Optical element, optical system, image pickup device, and method for manufacturing optical element
By using three layers of anti-reflective films of organic compound materials in the optical system, the specific refractive index and thickness conditions are met, and the problems of uneven films and insufficient reflectivity are solved, and the effective reflectivity reduction for different wavelength bands and incident angles are achieved.
Patent Information
- Application Number
- CN202410628983.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-03-13
- Filing Date
- 2024-05-21
- Publication Date
- 2024-11-26
AI Technical Summary
In the existing optical system, the anti-reflective film has uneven films in large opening lenses, resulting in a decrease in reflectivity, and the refractive index of the materials used is not sufficient to effectively suppress glare and ghosting.
An optical element consisting of three layers of anti-reflective films, wherein the refractive index and thickness of each layer meet specific inequality, including that the film layer is made of organic compound material and is formed by wet coating to ensure the uniformity of the film and Efficiency.
The reflectivity is significantly reduced, especially at different incident angles, the reflectivity of the light in the 420nm to 680nm band is less than 0.2%, improving the performance of the optical system.
Smart Images

Figure CN119024468A_ABST
Abstract
Description
Technical Field
[0001] One aspect of the embodiment relates to an optical element, an optical system, an imaging device, and a method of manufacturing an optical element. Background Art
[0002] In order to prevent glare and ghost caused by unnecessary reflection, a dielectric multilayer film (anti-reflection film) with anti-reflection function can be formed on the surface of an optical element (e.g., a lens or a filter) of an optical system. The anti-reflection film can exhibit high anti-reflection performance when its top layer is made of a material with a low refractive index. It is known that the material with a low refractive index is an inorganic material (such as silicon dioxide or magnesium fluoride), or an organic material (e.g., silicone resin or amorphous fluororesin). The refractive index of such a material can be reduced by forming a gap in a layer formed by the material.
[0003] Japanese Patent Laid-Open No. 2009-162989 discloses a double-layer antireflection film composed of a first layer including aluminum oxide as a main component and a second layer of silica aerogel having a refractive index of 1.27, and formed on a substrate having a refractive index of 1.70 to 1.95.
[0004] In the anti-reflection film disclosed in Japanese Patent Publication No. 2009-162989, the first layer including aluminum oxide as a main component is formed by evaporation. Therefore, in a large aperture lens, film unevenness occurs on the lens surface, and the anti-reflection performance (e.g., reflectivity reduction) on the entire lens surface is insufficient. In addition, since the refractive index of the second layer (i.e., the top layer) is about 1.27, the anti-reflection performance is insufficient in the case where the substrate has a lower refractive index. Summary of the invention
[0005] An optical element according to one aspect of the present disclosure includes a substrate and an anti-reflection film. The anti-reflection film is composed of: a first layer formed on the substrate, a second layer formed on the first layer, and a third layer formed on the second layer. The first layer, the second layer, and the third layer each include an organic compound. The following inequality is satisfied: 1.10≤n3≤1.28 Where n3 is the refractive index of the third layer for light with a wavelength of 550 nm.
[0006] According to another aspect of the present disclosure, an optical element includes a substrate and an anti-reflection film. The anti-reflection film is composed of: a first layer formed on the substrate, a second layer formed on the first layer, and a third layer formed on the second layer. The following inequality is satisfied: 1.30≤n1≤1.50 1.56≤n2≤1.70 1.10≤n3≤1.28 10≤n1d1≤155 10≤n2d2≤155 100≤n3d3≤155 200≤n1d1+n2d2+n3d3≤300 Among them, n1 is the refractive index of the first layer for light with a wavelength of 550nm, n2 is the refractive index of the second layer for light with a wavelength of 550nm, n3 is the refractive index of the third layer for light with a wavelength of 550nm, d1 (nm) is the thickness of the first layer, d2 (nm) is the thickness of the second layer, and d3 (nm) is the thickness of the third layer.
[0007] An optical system having one of the above optical elements and an imaging device having one of the above optical elements also constitute other aspects of the present disclosure. A method for manufacturing one of the above optical elements also constitutes other aspects of the present disclosure.
[0008] Further features of various embodiments of the present disclosure will become apparent from the following description of the embodiments with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 is a schematic diagram of an optical element according to each of Examples 1 to 14.
[0010] Figure 2 is a schematic cross-sectional view of an optical element according to each of Examples 1, 2, 5, 7, 8, 11, and 13 and Comparative Examples 1 and 2.
[0011] Figure 3 is a schematic cross-sectional view of an optical element according to each of Examples 3, 4, 6, 9, 10, 12, and 14.
[0012] Figure 4 The reflectivity characteristics of the optical element according to Example 1 at the position C when the incident angles are 0°, 15°, 30°, 45°, and 60° are shown.
[0013] Figure 5 The reflectivity characteristics of the optical element according to Example 1 at positions C and Q when the incident angle is 0° are shown.
[0014] Figure 6 The reflectivity characteristics of the optical element according to Example 2 at the position C when the incident angles are 0°, 15°, 30°, 45°, and 60° are shown.
[0015] Figure 7 The reflectivity characteristics of the optical element according to Example 2 at positions C and Q when the incident angle is 0° are shown.
[0016] Figure 8 The reflectivity characteristics of the optical element according to Example 3 at the position C when the incident angles are 0°, 15°, 30°, 45°, and 60° are shown.
[0017] Fig. 9 The reflectivity characteristics of the optical element according to Example 3 at positions C and Q when the incident angle is 0° are shown.
[0018] Fig.10 The reflectivity characteristics of the optical element according to Example 4 at the position C when the incident angles are 0°, 15°, 30°, 45° and 60° are shown.
[0019] Fig.11 The reflectivity characteristics of the optical element according to Example 4 at positions C and Q when the incident angle is 0° are shown.
[0020] Fig.12 The reflectivity characteristics of the optical element according to Example 5 at the position C when the incident angles are 0°, 15°, 30°, 45° and 60° are shown.
[0021] Fig.13 The reflectivity characteristics of the optical element according to Example 5 at positions C and Q when the incident angle is 0° are shown.
[0022] Fig.14 The reflectivity characteristics of the optical element according to Example 6 at the incident angles of 0°, 15°, 30°, 45° and 60° at position C are shown.
[0023] Fig.15 The reflectivity characteristics of the optical element according to Example 6 at positions C and Q when the incident angle is 0° are shown.
[0024] Fig.16 The reflectivity characteristics of the optical element according to Example 7 at the incident angles of 0°, 15°, 30°, 45° and 60° at position C are shown.
[0025] Fig.17 The reflectivity characteristics of the optical element according to Example 7 at positions C and Q when the incident angle is 0° are shown.
[0026] Fig.18 The reflectivity characteristics of the optical element according to Example 8 at the incident angles of 0°, 15°, 30°, 45° and 60° at position C are shown.
[0027] Fig.19 The reflectivity characteristics of the optical element according to Example 8 at positions C and Q when the incident angle is 0° are shown.
[0028] Fig. 20The reflectivity characteristics of the optical element according to Example 9 at the incident angles of 0°, 15°, 30°, 45° and 60° at position C are shown.
[0029] Fig.21 The reflectivity characteristics of the optical element according to Example 9 at positions C and Q when the incident angle is 0° are shown.
[0030] Fig. 22 The reflectivity characteristics of the optical element according to Example 10 at the incident angles of 0°, 15°, 30°, 45° and 60° at position C are shown.
[0031] Fig.23 The reflectivity characteristics of the optical element according to Example 10 at positions C and Q when the incident angle is 0° are shown.
[0032] Fig.24 The reflectivity characteristics of the optical element according to Example 11 when the incident angles at position C are 0°, 15°, 30°, 45°, and 60° are shown.
[0033] Fig.25 The reflectivity characteristics of the optical element according to Example 11 at positions C and Q when the incident angle is 0° are shown.
[0034] Fig.26 The reflectivity characteristics of the optical element according to Example 12 when the incident angles at position C are 0°, 15°, 30°, 45°, and 60° are shown.
[0035] Fig. 27 The reflectivity characteristics of the optical element according to Example 12 at positions C and Q when the incident angle is 0° are shown.
[0036] Fig.28 The reflectivity characteristics of the optical element according to Example 13 when the incident angles at position C are 0°, 15°, 30°, 45°, and 60° are shown.
[0037] Fig.29 The reflectivity characteristics of the optical element according to Example 13 at positions C and Q when the incident angle is 0° are shown.
[0038] Fig.30 The reflectivity characteristics of the optical element according to Example 14 when the incident angles at position C are 0°, 15°, 30°, 45°, and 60° are shown.
[0039] Fig.31 The reflectivity characteristics of the optical element according to Example 14 at positions C and Q when the incident angle is 0° are shown.
[0040] Fig.32 It is a cross-sectional view of the optical system according to Example 15.
[0041] Fig.33 is an external perspective view of an image pickup device according to Embodiment 16.
[0042] Fig.34 The reflectivity characteristics of the optical element as Comparative Example 1 at the position C when the incident angles are 0°, 15°, 30°, 45°, and 60° are shown.
[0043] Fig.35 The reflectance characteristics of the optical element as Comparative Example 1 at positions C and Q when the incident angle is 0° are shown.
[0044] Fig.36 The reflectivity characteristics of the optical element as Comparative Example 2 at the position C when the incident angles are 0°, 15°, 30°, 45°, and 60° are shown.
[0045] Fig.37 is a schematic diagram of an optical element according to each of Examples 17 to 25.
[0046] Fig.38 is a schematic cross-sectional view of the optical element of each of Examples 17, 19, 21 and 22 and Comparative Examples 1 and 2.
[0047] Fig.39 is a schematic cross-sectional view of an optical element according to each of Examples 18, 20 and 23.
[0048] Fig.40 is a schematic cross-sectional view of an optical element according to Example 24.
[0049] Fig.41 is a schematic cross-sectional view of an optical element according to Example 25.
[0050] Fig.42 The reflectivity characteristics of the optical element according to Example 17 when the incident angles at position C are 0°, 15°, 30°, 45°, and 60° are shown.
[0051] Fig.43 The reflectivity characteristics of the optical element according to Example 17 at positions C and Q when the incident angle is 0° are shown.
[0052] Fig.44 The reflectivity characteristics of the optical element according to Example 18 when the incident angles at position C are 0°, 15°, 30°, 45° and 60° are shown.
[0053] Fig.45 The reflectivity characteristics of the optical element according to Example 18 at positions C and Q when the incident angle is 0° are shown.
[0054] Fig.46 The reflectivity characteristics of the optical element according to Example 19 when the incident angles at position C are 0°, 15°, 30°, 45° and 60° are shown.
[0055] Fig.47 The reflectivity characteristics of the optical element according to Example 19 at positions C and Q when the incident angle is 0° are shown.
[0056] Fig.48 The reflectivity characteristics of the optical element according to Example 20 at the incident angles of 0°, 15°, 30°, 45° and 60° at position C are shown.
[0057] Fig.49 The reflectivity characteristics of the optical element according to Example 20 at positions C and Q when the incident angle is 0° are shown.
[0058] Fig.50 The reflectivity characteristics of the optical element according to Example 21 at incident angles of 0°, 15°, 30°, 45°, and 60° at position C are shown.
[0059] Fig.51 The reflectivity characteristics of the optical element according to Example 21 at positions C and Q when the incident angle is 0° are shown.
[0060] Fig.52 The reflectivity characteristics of the optical element according to Example 22 when the incident angles at position C are 0°, 15°, 30°, 45° and 60° are shown.
[0061] Fig.53 The reflectivity characteristics of the optical element according to Example 22 at positions C and Q when the incident angle is 0° are shown.
[0062] Fig.54 The reflectivity characteristics of the optical element according to Example 23 when the incident angles at position C are 0°, 15°, 30°, 45° and 60° are shown.
[0063] Fig.55 The reflectivity characteristics of the optical element according to Example 23 at positions C and Q when the incident angle is 0° are shown.
[0064] Fig.56 The reflectivity characteristics of the optical element according to Example 24 at incident angles of 0°, 15°, 30°, 45° and 60° at position C are shown.
[0065] Fig.57 The reflectivity characteristics of the optical element according to Example 24 at positions C and Q when the incident angle is 0° are shown.
[0066] Fig.58The reflectivity characteristics of the optical element according to Example 25 at the incident angles of 0°, 15°, 30°, 45° and 60° at position C are shown.
[0067] Fig.59 The reflectivity characteristics of the optical element according to Example 25 at positions C and Q when the incident angle is 0° are shown.
[0068] Fig.60 The reflectivity characteristics of the optical element as Comparative Example 3 at the position C when the incident angles are 0°, 15°, 30°, 45°, and 60° are shown.
[0069] Fig.61 The reflectance characteristics of the optical element as Comparative Example 3 at positions C and Q when the incident angle is 0° are shown.
[0070] Fig.62 The reflectivity characteristics of the optical element as Comparative Example 4 at the position C when the incident angles are 0°, 15°, 30°, 45°, and 60° are shown. DETAILED DESCRIPTION
[0071] Embodiments will now be described in detail with reference to the accompanying drawings.
[0072] Reference now Figure 1 , a schematic description will be given of an optical element 300 according to each of Embodiments 1 to 14. Figure 1 is a schematic diagram of an optical element 300. The optical element 300 includes a transparent substrate (substrate) 200 and an anti-reflection film 100 consisting of three layers. As used herein, "layer" refers to a group of parts made of the same material. That is, two adjacent layers are made of different materials and there is an interface between them. The anti-reflection film 100 is composed of a thin film layer (first layer) 01, a thin film layer (second layer) 02, and a thin film layer (third layer) 03 in order from the transparent substrate 200 to the air side.
[0073] In an embodiment, the thin film layers 01, 02, and 03 of the optical element 300 may be made of a material including an organic compound. An organic compound is a compound including carbon, except for compounds having a simple structure such as carbon monoxide and carbon dioxide. The material including the organic compound can be easily formed by a wet coating method.
[0074] In various embodiments, the following inequality (1) may be satisfied: 1.10≤n3≤1.28 (1) The reference wavelength λ is 550 nm, and n3 is the refractive index of the thin film layer 03 for a wavelength of 550 nm.
[0075] In each embodiment, n1 is the refractive index of the thin film layer 01 for a wavelength of 550 nm, n2 is the refractive index of the thin film layer 02 for a wavelength of 550 nm, and n3 is the refractive index of the thin film layer 03 for a wavelength of 550 nm. d1 (nm) is the physical thickness of the thin film layer 01, d2 (nm) is the physical thickness of the thin film layer 02, and d3 (nm) is the physical thickness of the thin film layer 03. At this time, the following inequalities (2) to (8) can be satisfied: 1.30≤n1≤1.50 (2) 1.56≤n2≤1.70 (3) 1.10≤n3≤1.28 (4) 10≤n1d1≤155 (5) 10≤n2d2≤155 (6) 100≤n3d3≤155 (7) 200≤n1d1+n2d2+n3d3≤300 (8)
[0076] In the case where the refractive index or physical thickness of each material is outside the range of inequalities (2) to (8), sufficient antireflection performance cannot be obtained.
[0007] Inequality (1) or (4) can be replaced by the following inequality (9): 1.12≤n3≤1.22 (9)
[0078] Inequality (1) or (4) can be replaced by the following inequality (9a): 1.15≤n3≤1.2 (9a)
[0079] Reference now Figure 2 and Figure 3 , a description will be given of an optical element 300 ( 301 , 302 ) in which an antireflection film 100 ( 101 , 102 ) is formed on a transparent substrate 200 ( 201 , 202 ). Figure 2 : is a schematic cross-sectional view of an optical element 301 according to Examples 1, 2, 5, 7, 8, 11, and 13 and Comparative Examples 1 and 2 described below. Figure 3 is a schematic cross-sectional view of an optical element 302 according to each of Embodiments 3, 4, 6, 9, 10, 12, and 14 described below.
[0080] exist Figure 2 In the optical element 301 shown, the transparent substrate 201 has a concave shape, and an anti-reflection film 101 composed of a thin film layer (first layer) 11, a thin film layer (second layer) 12, and a thin film layer (third layer) 13 is formed on the concave shape. Figure 3In the optical element 302 shown, the transparent substrate 202 has a convex shape, and an anti-reflection film 102 composed of a thin film layer (first layer) 21, a thin film layer (second layer) 22, and a thin film layer (third layer) 23 is formed on the convex shape. Figure 2 , but the description is similarly applicable to Figure 3 The optical element 302 is shown in FIG.
[0081] The shape of the optical surface of the optical element 301 used to form the anti-reflection film 101 has a rotationally symmetric axis (e.g., a reference axis; for example, a surface normal passing through an origin (e.g., a surface vertex)), in other words, it has a rotationally symmetric shape. However, the embodiments are not limited to this implementation, and the optical surface used to form the anti-reflection film 101 may not have rotational symmetry, for example, a partially notched shape of a rotationally symmetric shape. Figure 2 , position C is the rotation center of the lens surface of the transparent substrate 201 on which the anti-reflection film 101 is provided. In other words, position C is the position (e.g., intersection) where the rotational symmetry axis (e.g., reference axis, optical axis L) of the lens surface intersects with the lens surface of the transparent substrate 201. Position Q is located at the farthest point from position C in the optically effective area on the lens surface of the transparent substrate 201. The optically effective area is an area (e.g., effective diameter) on the optical surface through which an effective light beam that contributes to imaging passes.
[0082] When φ is the angle between the optical axis L and the normal at the position Q (hereinafter referred to as the half-open angle), the half-open angle φ has a maximum value in the optically effective area. The anti-reflection film 101 is composed of thin film layers 11, 12 and 13 in order from the transparent substrate 201. At the position C, d1c (nm) is the physical thickness of the thin film layer 11, d2c (mm) is the physical thickness of the thin film layer 12, and d3c (nm) is the physical thickness of the thin film layer 13. At the position Q, d1q (nm) is the physical thickness of the thin film layer 11, d2q (nm) is the physical thickness of the thin film layer 12, and d3q (nm) is the physical thickness of the thin film layer 13. In this case, the following inequalities (10) to (12) can be satisfied: 1.0<d1q / d1c≤1.3 (10) 1.0<d2q / d2c≤1.3 (11) 1.0<d3q / d3c≤1.3 (12)
[0083] In each embodiment, the film thickness of each of the thin film layers 11, 12 and 13 constituting the antireflection film 101 may be smallest at a position C which is the center of the antireflection film 101 (eg, the optical axis center) and increase as the position is away from the optical axis center.
[0084] In various embodiments, the half-opening angle φ (°) at position Q may satisfy the following inequality (13): φ≥25 (13)
[0085] Thin film layer 03,13 and 23 can have a gap. The gap (in other words, air) with a refractive index of 1.0 can reduce the refractive index to the scope that satisfies inequality (1), (4) and (9). When the refractive index is less than 1.10, the ratio of the gap included in the layer is high, so the film strength becomes low. When the refractive index is greater than 1.30, enough anti-reflection properties can not be obtained. If necessary, anti-fouling film etc. can be provided on the surface (for example, the surface of thin film layer 03,13 and 23) of the anti-reflection film according to each embodiment. The example of anti-fouling film includes the film containing fluoropolymer, fluorosilane monomolecule, titanium oxide particles etc.
[0086] In each embodiment, the film layers 03, 13 and 23 can be made of solid particles, chain particles or hollow particles. The film layers 03, 13 and 23 can be made of hollow particles with voids inside. The void can be a single hole or multiple holes, which can be selected as needed. The material of the solid particles, chain particles or hollow particles can have a low refractive index. The material is, for example, an organic resin made of SiO2, MgF2, fluorine or silicon, but SiO2 (which can easily manufacture its particles) can also be used. The average particle size of the hollow particles can be equal to or greater than 15nm and equal to or less than 100nm, or can be equal to or higher than 15nm and less than or equal to 80nm. In the case where the average particle size of the hollow particles is less than 15nm, it is difficult to reliably produce particles as the core. In the case where the average particle size of the hollow particles is greater than 100nm, the size of the voids between the particles becomes larger, so large voids may appear, and scattering with the particle size may occur.
[0087] The film layers 01, 11 and 21 may be made of a material comprising solid particles, in particular solid silica particles, bonded to a binder such as siloxane bonds. Alternatively, the material may comprise an acrylic resin as the "acrylate or methacrylate polymer".
[0088] The film layers 02, 12, and 22 may be made of a material including a polyimide resin, which is a "polymer compound containing an imide (-CO-NR-CO-) bond." Alternatively, the film layers may be made of a material including an epoxy resin, which is a "resin cross-linked and cured with an epoxy group having oxirane (ethylene oxide) as a three-membered cyclic ether in the structural formula."
[0089] In each embodiment, the optical element 300 is manufactured by forming a thin film layer 01 on a transparent substrate 200, forming a thin film layer 02 on the thin film layer 01, and forming a thin film layer 03 on the thin film layer 02. In each embodiment, the thin film layers 01, 11 and 21, the thin film layers 02, 12 and 22, and the thin film layers 03, 13 and 23 can be formed by a wet film forming method, which involves applying a coating solution containing a film material, and then drying and calcining. The wet film forming method can be cheaply coated over a large area. In particular, a spin coating method can be used because the method can flatten the film thickness distribution in a plane by coating while rotating around the rotation axis of the coating surface. A dry film forming method (such as an evaporation method or a sputtering method) forms a film in a positional relationship in which the evaporation source and the central part of the lens face each other. In a wide-angle lens, the incident angle of the evaporated material on the lens surface is large at the peripheral portion, so the film thickness at the peripheral portion is smaller than the film thickness at the central portion. Therefore, film (thickness) unevenness occurs in the lens surface, and anti-reflection performance has a bias. In order to form a film without (thickness) unevenness, a mask is provided or a substrate position and rotation operation are controlled.
[0090] The organic solvent that can be used for coating solution is not particularly limited, as long as coating is simple, performance etc. are not deteriorated, and any known solvent can be used.For example, the organic solvent can include monohydric alcohol, such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methylpropanol, 1-pentanol and 2-pentanol, cyclopentanol and 2-methylbutanol.The organic solvent can include 3-methylbutanol, 1-hexanol, 2-hexanol, 3-hexanol, 4-methyl-2-pentanol, 2-methyl-1-pentanol or 2-ethylbutanol.The organic solvent can include 2,4-dimethyl-3-pentanol, 3-ethylbutanol, 1-heptanol, 2-heptanol, 1-octanol or 2-octanol.The organic solvent can include polyhydric alcohol, such as ethylene glycol and triethylene glycol.
[0091] The organic solvent can include ether alcohols, such as methoxyethanol, ethoxyethanol, propoxyethanol, isopropoxyethanol, butoxyethanol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol and 1-propoxy-2-propanol. The organic solvent can include ethers, such as dimethoxyethane, diglyme, tetrahydrofuran, dioxane, diisopropyl ether, dibutyl ether and cyclopentyl methyl ether. The organic solvent can include esters, such as ethyl formate, ethyl acetate, n-butyl acetate, methyl lactate, ethyl lactate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate and propylene glycol monomethyl ether acetate.
[0092] The organic solvent may include various aliphatic hydrocarbons or cycloaliphatic hydrocarbons, such as n-hexane, n-octane, cyclohexane, cyclopentane and cyclooctane. The organic solvent may include various aromatic hydrocarbons, such as toluene, xylene and ethylbenzene. The organic solvent may include various ketones, such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone and cyclohexanone. The organic solvent may include various chlorinated hydrocarbons, such as chloroform, methylene chloride, carbon tetrachloride and tetrachloroethane. The organic solvent may include aprotic polar solvents, such as N-methyl pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide and ethylene carbonate. In these solvents, two or more solvents may be used in combination.
[0093] In the case where solid particles, chain particles or hollow particles are used for film layers 03, 13 and 23 and solid particles are used for film layers 01, 11 and 21, an adhesive for bonding may be used to improve strength. The adhesive may utilize a siloxane bond, particularly in the case of using silica particles having abundant hydroxyl groups on the surface.
[0094] In each embodiment, the thin film layers 01 and 11, the thin film layers 02 and 12, and the thin film layers 03 and 13 are made of a material that can be formed by a wet film forming method, so the material or the adhesive includes an organic compound. In addition, the anti-reflection film according to each embodiment will not be calcined at a high temperature during the drying process after coating. Therefore, for example, plastics and photocurable resins that are easily deformed by heat can be used for the transparent substrates 200, 201, and 202.
[0095] The following inequality (14) can be satisfied: 1.45≤nS≤2.10 (14) Where nS is the refractive index of the transparent substrates 200 , 201 and 202 .
[0096] Specific embodiments will be described below. These embodiments are merely illustrative, and the present disclosure is not limited to the scope of the embodiments. Example 1
[0097] First, Embodiment 1 will now be described. Figure 2: is a schematic cross-sectional view of an optical element 301 according to this embodiment. The optical element 301 according to this embodiment is an optical element in which an anti-reflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-TIL26 (manufactured by OHARA INC.) having a refractive index of 1.57 (for light of 550 nm wavelength). The lens surface of the transparent substrate 201 on which the anti-reflection film 101 is formed has a concave shape. The half-open angle φ at position Q on the maximum light effective diameter is 45°. Regarding the layer materials, the thin film layer 11 is made of a material including solid silica as a main component, the thin film layer 12 is made of a material including polyimide resin as a main component, and the thin film layer 13 is made of a material including hollow silica as a main component. Table 1 lists the details of the film configuration of the optical element 301 according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (1) to (8) and (10) to (12). The thin film layers 11, 12 and 13 each include an organic compound.
[0098] The antireflection film 101 according to this embodiment is formed by the following method. Hollow silica coating solution 1
[0099] 580 g of an isopropanol dispersion solution of hollow silica particles (THRULYA 4110 manufactured by JGC Catalysts and Chemicals Ltd.; average particle size of about 60 nm, shell thickness of about 12 nm, solid concentration of 20.5 wt% (mass percentage)) was used. The isopropanol dispersion solution was heated to distill off the isopropanol, and 1-ethoxy-2-propanol (hereinafter abbreviated as 1E2P) was added. The isopropanol was distilled to a solid concentration of 19.5 wt% to prepare 610 g of a 1E2P solvent replacement solution of hollow silica particles (hereinafter referred to as solvent replacement 1). An organic acid including fluorine was added to the solvent replacement solution 1 thus obtained so that the component ratio of the hollow silica particles and the organic acid including fluorine (trifluoroacetic acid having three fluorine atoms manufactured by Tokyo Chemical Industry Co., Ltd.) became 100 / 1, thereby obtaining a hollow particle dispersion solution 1.
[0100] In another container, 3.6 g of phosphonic acid diluted to 0.1% concentration in pure water, 11.4 g of 1-propoxy-2-propanol and 4.5 g of methyl polysilicate (methyl silicate 53A manufactured by Colcoat Co., Ltd.) were slowly added and stirred at room temperature for 120 minutes. Thus, a silica sol having a solid content concentration of 12 wt% (hereinafter referred to as silica sol 1) was prepared.
[0101] The hollow particle dispersion solution 1 was diluted with ethyl lactate to a solid content concentration of 4.5 wt%, and then silica sol 1 was added to a composition ratio of hollow silica particles to silica sol of 100 / 12. By subsequently stirring the mixture at room temperature for two hours, a hollow silica coating solution 1 including hollow silica particles was obtained. Solid silica coating solution 1
[0102] A solid silica coating solution 1 was prepared by adding 300 g of 1-methoxy-2-propanol and 4 g of Silica Sol 1 to 25 g of a silica particle dispersion solution PL-1 (manufactured by Fuso Chemical Co., Ltd.). Polyimide coating solution 1
[0103] Hexane was gradually added to 200 g of 4,4'-methylenebis(aminocyclohexane) (hereinafter referred to as DADCM; manufactured by Tokyo Chemical Industry Co., Ltd.) while refluxed until completely dissolved. After stopping the heating and leaving the solution at room temperature for a few days, the precipitate was filtered and dried under reduced pressure. 58 g of white solid cyclic diamine DADCM purified in this way was obtained.
[0104] A total of 12 mmol of the three diamines were dissolved in N,N-dimethylacetamide (hereinafter referred to as DMAc) to prepare a diamine solution. One of the three diamines was a cyclic diamine DADCM. The other two were an aromatic diamine 4,4'-bis(4-aminophenoxy)biphenyl (product name BODA; manufactured by Wakayama Seiko Co., Ltd.) and a siloxane-containing diamine 1,3-bis(3-aminopropyl)tetramethyldisiloxane (product name PAM-E; manufactured by Shin-Etsu Chemical Co., Ltd.).
[0105] About 12 mmol of anhydride was added to the water-cooled diamine solution. The anhydride was 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic anhydride (product name TDA-100; manufactured by Shin Nippon Rika Co., Ltd.). Alternatively, the anhydride was 5-(2,5-dioxotetrahydrofuranyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride (product name B-4400; manufactured by DIC). The amount of DMAc was adjusted so that the total mass of the diamine and the anhydride was 20% by weight.
[0106] The solution was stirred at room temperature for 15 hours to perform polymerization. In addition, the solution was adjusted to 8 wt % by dilution with DMAc, and then stirred at room temperature for 1 hour while adding 7.4 ml of pyridine and 3.8 ml of acetic anhydride. The solution was further stirred for 4 hours while heating from 60° C. to 70° C. in an oil bath. The polymer was reprecipitated from the polymerization solution with methanol or methanol, and then washed several times in methanol. After drying at 60° C. for 24 hours, polyimide 1 was obtained in the form of a white to light yellow powder.
[0107] The obtained Polyimide 1 was dissolved in cyclohexanone so that the solid content concentration became 2.5 wt %, thereby producing a Polyimide Coating Solution 1 .
[0108] The antireflection film 101 is formed using the solid silica coating solution 1 , the polyimide coating solution 1 , and the hollow silica coating solution 1 .
[0109] 0.2 ml of the solid silica coating solution 1 was dropped on the lens surface of the transparent substrate 201 and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating solution 1 was continuously dropped on the lens surface of the transparent substrate 201 and spin-coated at 4000 rpm for 20 seconds. In addition, 0.2 ml of the hollow silica coating solution 1 was dropped on the lens surface of the transparent substrate 201 and spin-coated at 4000 rpm for 20 seconds. Thereafter, drying was performed in a clean room at room temperature of 23° C. for more than 24 hours.
[0110] Figure 4 The reflectivity characteristics of the optical element 301 according to this embodiment are shown when the incident angles at position C are 0°, 15°, 30°, 45°, and 60°. Figure 4 In FIG. 1 , the horizontal axis represents wavelength (nm) and the vertical axis represents reflectivity (%). This is similarly applicable to other reflectivity characteristic graphs. For light in the 420nm to 680nm band when the incident angle is 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Figure 5 The reflectivity characteristics of the optical element 301 according to this embodiment when the incident angle is 0° at positions C and Q are shown. According to Table 1, the film thickness of each thin film layer at position Q is larger than the film thickness of each thin film layer at position C by about 6%, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectivity characteristics are equal to or less than 0.2% and this is excellent. Table 1 Example 2
[0111] Embodiment 2 will now be described. Figure 2: is a schematic cross-sectional view of an optical element 301 according to this embodiment. The optical element 301 according to this embodiment is an optical element in which an anti-reflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-LAL12 (manufactured by OHARA INC.) having a refractive index of 1.68 (for light of 550 nm wavelength). The lens surface of the transparent substrate 201 on which the anti-reflection film 101 is formed has a concave shape. The half-open angle φ at position Q on the maximum light effective diameter is 70°. Regarding the layer materials, the thin film layer 11 is made of a material including solid silica as a main component, the thin film layer 12 is made of a material including polyimide resin as a main component, and the thin film layer 13 is made of a material including hollow silica as a main component. Table 2 lists the details of the film configuration of the optical element 301 according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (1) to (8) and (10) to (12). The thin film layers 11, 12 and 13 each include an organic compound.
[0112] The antireflection film 101 according to this embodiment is formed by the following method. Hollow silica coating solution 2
[0113] Hollow particle dispersion solution 1 and silica sol 1 were prepared in a similar manner to hollow particle coating solution 1. Hollow particle dispersion solution 1 was diluted with ethyl lactate so that the solid content concentration became 4.5 wt%, and then silica sol 1 was added so that the component ratio of hollow silica particles and silica sol became 100 / 9. By subsequently stirring the mixture at room temperature for two hours, hollow silica coating solution 2 including hollow silica particles was obtained. Antireflection film 101 was formed from solid silica coating solution 1, polyimide coating solution 1, and hollow silica coating solution 2.
[0114] 0.2 ml of solid silica coating solution 1 was dropped on the lens surface of the transparent substrate 201 and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of polyimide coating solution 1 was continuously dropped on the lens surface of the transparent substrate 201 and spin-coated at 4000 rpm for 20 seconds. In addition, 0.2 ml of hollow silica coating solution 2 was dropped on the lens surface of the transparent substrate 201 and spin-coated at 4000 rpm for 20 seconds. Thereafter, drying was performed in a clean room at room temperature of 23° C. for more than 24 hours.
[0115] Figure 6 The reflectivity characteristics of the optical element 301 according to this embodiment are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Figure 7The reflectance characteristics of the optical element 301 according to this embodiment when the incident angle is 0° at positions C and Q are shown. According to Table 2, the film thickness of each thin film layer at position Q is 20% greater than the film thickness of each thin film layer at position C, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectance characteristics are equal to or less than 0.2% and this is excellent. Table 2 Example 3
[0116] Embodiment 3 will now be described. Figure 3 : is a schematic cross-sectional view of an optical element 302 according to this embodiment. The optical element 302 according to this embodiment is an optical element in which an anti-reflection film 102 is formed on a transparent substrate 202. The transparent substrate 202 is S-LAH53 (manufactured by OHARA INC.) having a refractive index of 1.81 (for light of 550 nm wavelength). The lens surface of the transparent substrate 202 on which the anti-reflection film 102 is formed has a convex shape. The half-open angle φ at position Q on the maximum light effective diameter is 30°. Regarding the layer materials, the thin film layer 21 is made of a material including an acrylic resin as a main component, and the thin film layer 22 is made of a material including hollow silica as a main component. Table 3 lists the details of the film configuration of the optical element 302 according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (1) to (8) and (10) to (12). The thin film layers 21, 22 and 23 each include an organic compound.
[0117] The antireflection film 102 according to this embodiment is formed by the following method. Chain silica coating solution 1
[0118] Using an evaporator, 2-propanol in a 2-propanol (IPA) dispersion solution of chain silica particles (IPA-ST-UP manufactured by Nissan Chemical Industries, Ltd.; average particle size of 12 nm, solid concentration of 15 wt%) was replaced with 1-propoxy-2-propanol (manufactured by SIGMA Corporation). Thus, a 1-propoxy-2-propanol dispersion solution (solid concentration 17 wt%) was produced. This will be referred to as dispersion solution 2. Next, 18.5 g of tetraethoxysilane (TEOS; manufactured by Tokyo Chemical Industry Co., Ltd.) and 16.0 g of 0.1 wt% phosphonic acid in an amount of 10 equivalents relative to TEOS were added as catalyst water, and mixed and stirred in a water bath at 20° C. for 60 minutes to obtain a binder solution 2.
[0119] 33.4 g of the binder solution 2 was added to 251.3 g of the dispersion solution 2. Then, 174.5 g of 1-propoxy-2-propanol and 546.5 g of ethyl lactate were added and stirred for 60 minutes to obtain a chain silica coating solution 1. Acrylic coating solution
[0120] 6.1 g of N-cyclohexylmaleimide (hereinafter referred to as CHMI) and 4.0 g of 2,2,2-trifluoroethyl methacrylate (product name M-3F; manufactured by Kyoeisha Chemical Co., Ltd.) were used. In addition, 0.45 g of 3-(methacryloyloxy)propyltrimethoxysilane (product name LS-3380; manufactured by Shin-Etsu Chemical Co., Ltd.) was used. In addition, 0.08 g of 2,2'-azobis(isobutyronitrile) (hereinafter referred to as AIBN) was used. They were stirred and dissolved in 24.8 g of toluene to obtain a solution. The solution was repeatedly degassed and nitrogen purged while cooling with ice water, and then stirred for seven hours under a nitrogen flow of 60 to 70°C. The polymerization solution was slowly introduced into strongly stirred methanol, the polymer thus precipitated was filtered, and then stirred and washed several times in methanol. The polymer collected by filtration was dried at 80°C to 90°C in a vacuum. 8.3 g of a white powdery maleimide copolymer was obtained (yield 81%), and the maleimide copolymerization ratio was 0.57. 2.2 g of the powder of maleimide copolymer 1 was dissolved in 97.8 g of a cyclopentanone / cyclohexanone mixed solvent to prepare a solution of maleimide copolymer 1, thereby producing an acrylic coating solution. Polyimide coating solution 2
[0121] 50 g of white solid cyclic diamine DADCM (hereinafter referred to as DADCM; manufactured by Tokyo Chemical Industry Co., Ltd.) was obtained by refining 4,4'-methylenebis(aminocyclohexane). A total of 12 mmol of the three diamines were dissolved in N,N-dimethylacetamide (hereinafter abbreviated as DMAc). One of the three diamines was the cyclic diamine DADCM. The other two were aromatic diamine 4,4'-bis(4-aminophenoxy)biphenyl (product name BODA; manufactured by Wakayama Seiko Co., Ltd.) and siloxane-containing diamine 1,3-bis(3-aminopropyl)tetramethyldisiloxane (product name PAM-E; manufactured by Shin-Etsu Chemical Co., Ltd.).
[0122] The following method is similar to that of the polyimide coating solution 1. Polyimide 2 having a different ratio of three diamines from that of the polyimide coating solution 1 is obtained. The obtained polyimide 2 is dissolved in cyclohexanone so that the solid concentration becomes 2.5 wt %, thereby producing a polyimide coating solution 2.
[0123] The antireflection film 102 is formed of an acrylic coating solution, a polyimide coating solution 2 , and a chain silica coating solution 1 .
[0124] 0.2 ml of the acrylic coating solution was dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating solution 2 was continuously dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. In addition, 0.2 ml of the chain silica coating solution 1 was dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. Thereafter, drying was performed in a clean room at room temperature of 23° C. for more than 24 hours.
[0125] Figure 8 The reflectivity characteristics of the optical element 302 according to this embodiment are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig. 9 The reflectivity characteristics of the optical element 302 according to this embodiment when the incident angle is 0° at positions C and Q are shown. According to Table 3, the film thickness of each thin film layer at position Q is larger than the film thickness of each thin film layer at position C by about 2%, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectivity characteristics are equal to or less than 0.2%, and this is excellent. Table 3 Example 4
[0126] Embodiment 4 will now be described. Figure 3 : is a schematic cross-sectional view of an optical element 302 according to this embodiment. The optical element 302 according to this embodiment is an optical element in which an anti-reflection film 102 is formed on a transparent substrate 202. The transparent substrate 202 is S-LAH79 (manufactured by OHARA INC.) having a refractive index of 2.00 (for light of 550 nm wavelength). The lens surface of the transparent substrate 202 on which the anti-reflection film 102 is formed has a convex shape. The half-open angle φ at position Q on the maximum light effective diameter is 45°. Regarding the layer materials, the thin film layer 11 is made of a material including solid silica as a main component, the thin film layer 12 is made of a material including polyimide resin as a main component, and the thin film layer 13 is made of a material including hollow silica as a main component. Table 4 lists the details of the film configuration of the optical element according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (1) to (8) and (10) to (12). The thin film layers 21, 22 and 23 each include an organic compound.
[0127] The antireflection film 102 according to this embodiment is formed by the following method.
[0128] The antireflection film 102 is formed using the solid silica coating solution 2 , the polyimide coating solution 2 , and the hollow silica coating solution 1 .
[0129] 0.2 ml of the solid silica coating solution 2 was dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating solution 2 was dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. In addition, 0.2 ml of the hollow silica coating solution 1 was dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. Thereafter, drying was performed in a clean room at room temperature of 23° C. for more than 24 hours.
[0130] Fig.10 The reflectivity characteristics of the optical element 302 according to this embodiment are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig.11 The reflectivity characteristics of the optical element 302 according to this embodiment when the incident angle is 0° at positions C and Q are shown. According to Table 4, the film thickness of each thin film layer at position Q is larger than the film thickness of each thin film layer at position C by about 6%, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectivity characteristics are equal to or less than 0.2%, and this is excellent. Table 4 Example 5
[0131] Embodiment 5 will now be described. Figure 2 : is a schematic cross-sectional view of an optical element 301 according to this embodiment. The optical element 301 according to this embodiment is an optical element in which an anti-reflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-LAH53 (manufactured by OHARA INC.) having a refractive index of 1.81 (for light of 550 nm wavelength). The lens surface of the transparent substrate 201 on which the anti-reflection film 101 is formed has a concave shape. The half-open angle φ at position Q on the maximum light effective diameter is 45°. Regarding the layer materials, the thin film layer 11 is made of a material including an acrylic resin as a main component, the thin film layer 12 is made of a material including a polyimide resin as a main component, and the thin film layer 13 is made of a material including hollow silica as a main component. Table 5 lists the details of the film configuration of the optical element according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (1) to (8) and (10) to (12). The thin film layers 11, 12 and 13 each include an organic compound.
[0132] The antireflection film 101 according to this embodiment is formed by the following method.
[0133] The anti-reflection film 101 is formed using an acrylic coating solution, a polyimide coating solution 1, and a hollow silica coating solution 2. 0.2 ml of the acrylic coating solution is dropped on the lens surface of the transparent substrate 201 and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating solution 1 is dropped on the lens surface of the transparent substrate 201 and spin-coated at 4000 rpm for 20 seconds. In addition, 0.2 ml of the hollow silica coating solution 2 is continuously dropped on the lens surface of the transparent substrate 201 and spin-coated at 4000 rpm for 20 seconds. After that, drying is performed in a clean room at a room temperature of 23°C for more than 24 hours.
[0134] Fig.12 The reflectivity characteristics of the optical element 301 according to this embodiment are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig.13 The reflectivity characteristics of the optical element 301 according to this embodiment when the incident angle is 0° at positions C and Q are shown. According to Table 5, the film thickness of each thin film layer at position Q is larger than the film thickness of each thin film layer at position C by about 6%, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectivity characteristics are equal to or less than 0.2%, and this is excellent. Table 5 Example 6
[0135] Embodiment 6 will now be described. Figure 3: is a schematic cross-sectional view of an optical element 302 according to this embodiment. The optical element 302 according to this embodiment is an optical element in which an anti-reflection film 102 is formed on a transparent substrate 202. The transparent substrate 202 is S-LAH66 (manufactured by OHARA INC.) having a refractive index of 1.77 (for light of 550 nm wavelength). The lens surface of the transparent substrate 202 on which the anti-reflection film 102 is formed has a convex shape. The half-open angle φ at position Q on the maximum light effective diameter is 60°. Regarding the layer materials, the thin film layer 21 is made of a material including solid silica as a main component, the thin film layer 22 is made of a material including epoxy resin as a main component, and the thin film layer 23 is made of a material including hollow silica as a main component. Table 6 lists the details of the film configuration of the optical element 302 according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (1) to (8) and (10) to (12). The thin film layers 21, 22 and 23 each include an organic compound.
[0136] The antireflection film 102 according to this embodiment is formed by the following method. Epoxy coating solution
[0137] An intermediate layer coating solution 3 was prepared by adding 500 g of 1-methoxy-2-propanol to 25 g of epoxy resin jER828 (manufactured by Mitsubishi Chemical Corporation). An antireflection film 102 was formed using the solid silica coating solution 2 , the epoxy resin coating solution, and the hollow silica coating solution 1 .
[0138] 0.2 ml of solid silica coating solution 2 was dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of epoxy resin coating solution was dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. In addition, 0.2 ml of hollow silica coating solution 1 was continuously dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. Thereafter, drying was performed in a clean room at room temperature of 23° C. for more than 24 hours.
[0139] Fig.14 The reflectivity characteristics of the optical element 302 according to this embodiment are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig.15The reflectivity characteristics of the optical element 302 according to this embodiment when the incident angle is 0° at positions C and Q are shown. According to Table 6, the film thickness of each thin film layer at position Q is larger than the film thickness of each thin film layer at position C by about 12%, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectivity characteristics are equal to or less than 0.2%, and this is excellent. Table 6 Example 7
[0140] Embodiment 7 will now be described. Figure 2 : is a schematic cross-sectional view of an optical element 301 according to this embodiment. The optical element 301 according to this embodiment is an optical element in which an anti-reflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is ZEONEX K22R (manufactured by Zeon Co., Ltd., Japan) with a refractive index of 1.54 (for light of 550nm wavelength). The lens surface of the transparent substrate 201 on which the anti-reflection film 101 is formed has a concave shape. The half-open angle φ at position Q on the maximum light effective diameter is 30°. Regarding the layer materials, the thin film layer 11 is made of a material including solid silica as a main component, the thin film layer 12 is made of a material including polyimide resin as a main component, and the thin film layer 13 is made of a material including hollow silica as a main component. Table 7 lists the details of the film construction of the optical element 301 according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (1) to (8) and (10) to (12). The thin film layers 11, 12 and 13 each include an organic compound.
[0141] The antireflection film 101 according to this embodiment is formed by the following method.
[0142] The anti-reflection film 101 is formed using a solid silica coating solution 1, a polyimide coating solution 1, and a hollow silica coating solution 1. 0.2 ml of the solid silica coating solution 1 is dropped on the lens surface of the transparent substrate 201 and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating solution 1 is dropped on the lens surface of the transparent substrate 201 and spin-coated at 4000 rpm for 20 seconds. In addition, 0.2 ml of the hollow silica coating solution 1 is continuously dropped on the lens surface of the transparent substrate 201 and spin-coated at 4000 rpm for 20 seconds. After that, drying is performed in a clean room at a room temperature of 23° C. for more than 24 hours.
[0143] Fig.16The reflectivity characteristics of the optical element 301 according to this embodiment are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig.17 The reflectivity characteristics of the optical element 301 according to this embodiment when the incident angle is 0° at positions C and Q are shown. According to Table 7, the film thickness of each thin film layer at position Q is larger than the film thickness of each thin film layer at position C by about 2%, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectivity characteristics are equal to or less than 0.2%, and this is excellent. Table 7 Example 8
[0144] Embodiment 8 will now be described. Figure 2 : is a schematic cross-sectional view of an optical element 301 according to this embodiment. The optical element 301 according to this embodiment is an optical element in which an anti-reflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is EP-5000 (manufactured by Mitsubishi Gas Chemical Co., Ltd.) with a refractive index of 1.64 (for light of 550nm wavelength). The lens surface of the transparent substrate 201 on which the anti-reflection film 101 is formed has a concave shape. The half-open angle φ at position Q on the maximum light effective diameter is 45°. Regarding the layer materials, the thin film layer 11 is made of a material including solid silica as a main component, the thin film layer 12 is made of a material including polyimide resin as a main component, and the thin film layer 13 is made of a material including hollow silica as a main component. Table 8 lists the details of the film construction of the optical element 301 according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (1) to (8) and (10) to (12). The thin film layers 11, 12 and 13 each include an organic compound.
[0145] The antireflection film 101 according to this embodiment is formed by the following method.
[0146] The antireflection film 101 is formed using the solid silica coating solution 2 , the polyimide coating solution 2 , and the hollow silica coating solution 2 .
[0147] 0.2 ml of the solid silica coating solution 2 was dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating solution 2 was dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. 0.2 ml of the hollow silica coating solution 2 was continuously dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. Thereafter, drying was performed in a clean room at room temperature of 23° C. for more than 24 hours.
[0148] Fig.18 The reflectivity characteristics of the optical element 301 according to this embodiment are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig.19 The reflectance characteristics of the optical element 301 according to this embodiment when the incident angle is 0° at positions C and Q are shown. According to Table 8, the film thickness of each thin film layer at position Q is 6% greater than the film thickness of each thin film layer at position C, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectance characteristics are equal to or less than 0.2%, and this is excellent. Table 8 Example 9
[0149] Embodiment 9 will now be described. Figure 3 : is a schematic cross-sectional view of an optical element 302 according to this embodiment. The optical element 302 according to this embodiment is an optical element in which an anti-reflection film 102 is formed on a transparent substrate 202. The transparent substrate 202 is EP-9000 (manufactured by Mitsubishi Gas Chemical Co., Ltd.) with a refractive index of 1.64 (for light of 550nm wavelength). The lens surface of the transparent substrate 202 on which the anti-reflection film 102 is formed has a convex shape. The half-open angle φ at position Q on the maximum light effective diameter is 30°. Regarding the layer materials, the thin film layer 21 is made of a material including solid silica as a main component, the thin film layer 22 is made of a material including polyimide resin as a main component, and the thin film layer 23 is made of a material including hollow silica as a main component. Table 9 lists the details of the film configuration of the optical element 302 according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (1) to (8) and (10) to (12). The thin film layers 21, 22 and 23 each include an organic compound.
[0150] The antireflection film 102 according to this embodiment is formed by the following method.
[0151] The anti-reflection film 102 is formed using a solid silica coating solution 1, a polyimide coating solution 1, and a chain silica coating solution 1. 0.2 ml of the solid silica coating solution 1 is dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating solution 1 is dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. 0.2 ml of the chain silica coating solution 1 is continuously dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. Thereafter, drying is performed in a clean room at a room temperature of 23° C. for more than 24 hours.
[0152] Fig. 20 The reflectivity characteristics of the optical element 302 according to this embodiment are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig.21 The reflectance characteristics of the optical element 302 according to this embodiment when the incident angle is 0° at positions C and Q are shown. According to Table 9, the film thickness of each thin film layer at position Q is 2% greater than the film thickness of each thin film layer at position C, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectance characteristics are equal to or less than 0.2%, and this is excellent. Table 9 Example 10
[0153] Embodiment 10 will now be described. Figure 3: is a schematic cross-sectional view of an optical element 302 according to this embodiment. The optical element 302 according to this embodiment is an optical element in which an anti-reflection film 102 is formed on a transparent substrate 202. The transparent substrate 202 is an optical element called a replica element, in which the transparent substrate 202 is formed on the surface of a glass substrate (not shown in the figure) as a substrate. The transparent substrate 202 is LPQ-1500 (manufactured by Mitsubishi Gas Chemical Co., Ltd.) having a refractive index of 1.59 (for light of a wavelength of 550nm). The lens surface of the transparent substrate 202 on which the anti-reflection film 102 is formed has a convex shape. The half-open angle φ at the position Q on the maximum light effective diameter is 30°. Regarding the layer materials, the thin film layer 21 is made of a material including solid silica as a main component, the thin film layer 22 is made of a material including a polyimide resin as a main component, and the thin film layer 23 is made of a material including hollow silica as a main component. Table 10 lists the details of the film configuration of the optical element 302 according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (1) to (8) and (10) to (12). The thin film layers 21, 22, and 23 each include an organic compound.
[0154] The antireflection film 102 according to this embodiment is formed by the following method.
[0155] The anti-reflection film 102 is formed using a solid silica coating solution 1, a polyimide coating solution 2, and a hollow silica coating solution 1. 0.2 ml of the solid silica coating solution 1 is dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating solution 2 is dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. 0.2 ml of the hollow silica coating solution 1 is continuously dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. After that, drying is performed in a clean room at a room temperature of 23° C. for more than 24 hours.
[0156] Fig. 22 The reflectivity characteristics of the optical element 302 according to this embodiment are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig.23 The reflectance characteristics of the optical element 302 according to this embodiment when the incident angle is 0° at positions C and Q are shown. According to Table 10, the film thickness of each thin film layer at position Q is 2% greater than the film thickness of each thin film layer at position C, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectance characteristics are equal to or less than 0.2%, and this is excellent. Table 10 Embodiment 11
[0157] Embodiment 11 will now be described. Figure 2 : is a schematic cross-sectional view of an optical element 301 according to this embodiment. The optical element 301 according to this embodiment is an optical element in which an anti-reflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-LAH66 (manufactured by OHARA INC.) having a refractive index of 1.77 (for light of 550 nm wavelength). The lens surface of the transparent substrate 201 on which the anti-reflection film 101 is formed has a concave shape. The half-open angle φ at position Q on the maximum light effective diameter is 30°. Regarding the layer materials, the thin film layer 11 is made of a material including a polyimide resin as a main component, the thin film layer 12 is made of a material including solid silica as a main component, and the thin film layer 13 is made of a material including hollow silica as a main component. Table 11 lists the details of the film configuration of the optical element according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (1) and (10) to (12). The thin film layers 11, 12 and 13 each include an organic compound.
[0158] The antireflection film 101 according to this embodiment is formed by the following method: The antireflection film 101 is formed using the polyimide coating solution 1 , the solid silica coating solution 1 , and the hollow silica coating solution 1 .
[0159] 0.2 ml of the polyimide coating solution 1 was dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the solid silica coating solution 1 was dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. 0.2 ml of the hollow silica coating solution 1 was continuously dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. Thereafter, drying was performed in a clean room at room temperature of 23° C. for more than 24 hours.
[0160] Fig.24 The reflectivity characteristics of the optical element 301 according to this embodiment are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig.25The reflectance characteristics of the optical element 301 according to this embodiment when the incident angle is 0° at positions C and Q are shown. According to Table 11, the film thickness of each thin film layer at position Q is 6% greater than the film thickness of each thin film layer at position C, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectance characteristics are equal to or less than 0.2%, and this is excellent. Table 11 Example 12
[0161] Embodiment 12 will now be described. Figure 3 : is a schematic cross-sectional view of an optical element 302 according to this embodiment. The optical element 302 according to this embodiment is an optical element in which an anti-reflection film 102 is formed on a transparent substrate 202. The transparent substrate 202 is S-TIH53 (manufactured by OHARA INC.) having a refractive index of 1.85 (for light of 550 nm wavelength). The lens surface of the transparent substrate 202 on which the anti-reflection film 102 is formed has a concave shape. The half-open angle φ at position Q on the maximum light effective diameter is 30°. Regarding the layer materials, the thin film layer 21 is made of a material including a polyimide resin as a main component, the thin film layer 22 is made of a material including solid silica as a main component, and the thin film layer 23 is made of a material including hollow silica as a main component. Table 12 lists the details of the film configuration of the optical element 302 according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (1) and (10) to (12). The thin film layers 21, 22 and 23 each include an organic compound.
[0162] The antireflection film 102 according to this embodiment is formed by the following method.
[0163] The anti-reflection film 102 is formed using a polyimide coating solution 2, a solid silica coating solution 1, and a hollow silica coating solution 2. 0.2 ml of the polyimide coating solution 2 is dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the solid silica coating solution 1 is dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. 0.2 ml of the hollow silica coating solution 2 is continuously dropped on the lens surface of the transparent substrate 202 and spin-coated at 4000 rpm for 20 seconds. After that, drying is performed in a clean room at a room temperature of 23° C. for more than 24 hours.
[0164] Fig.26The reflectivity characteristics of the optical element 302 according to this embodiment are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig. 27 The reflectance characteristics of the optical element 302 according to this embodiment when the incident angle is 0° at positions C and Q are shown. According to Table 12, the film thickness of each thin film layer at position Q is 2% greater than the film thickness of each thin film layer at position C, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectance characteristics are equal to or less than 0.2%, and this is excellent. Table 12 Example 13
[0165] Embodiment 13 will now be described. Figure 2 : is a schematic cross-sectional view of an optical element 301 according to this embodiment. The optical element 301 according to this embodiment is an optical element in which an anti-reflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-TIL26 (manufactured by OHARA INC.) having a refractive index of 1.57 (for light of 550 nm wavelength). The lens surface on which the anti-reflection film 101 is formed on the transparent substrate 201 has a concave shape. The half-open angle φ at position Q on the maximum light effective diameter is 45°. Regarding the layer materials, the thin film layer 11 is made of a material including magnesium fluoride as a main component, the thin film layer 12 is made of a material including aluminum oxide as a main component, and the thin film layer 13 is made of a material including hollow silica as a main component. Table 13 lists the details of the film configuration of the optical element 301 according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (1) to (8) and (10) to (12).
[0166] The antireflection film 101 according to this embodiment is formed by the following method.
[0167] The thin film layers 11 and 12 were formed by evaporation. The evaporated material was heated using an electron beam. In addition, an ion beam assisted evaporation method was performed to form a denser film. The vacuum chamber of the evaporation apparatus was evacuated to 2×10 -3 After confirming the high vacuum state inside the vacuum chamber, Ar as an inert gas was introduced into the ion gun, and then the ion gun was discharged. After the ion gun became stable, oxygen was introduced into the vacuum chamber, and at about 1×10 -2Ion-assisted evaporation is performed using oxygen ions under a vacuum pressure of 1.5 Pa. Typically, the problem with the evaporation method is that the film thickness of a lens having a large half-open angle decreases as the position moves toward the peripheral portion. During evaporation, Example 13 provides a mask having an arbitrary shape on the film-forming surface side of the transparent substrate 201 to avoid a decrease in film thickness at the peripheral portion and to make the film thickness distribution within the surface substantially uniform.
[0168] After the thin film layer 11, the thin film layer 12 was formed by evaporation, and then 0.2 ml of the hollow silica coating solution 1 was dropped on the lens surface of the transparent substrate 202 on which the thin film layers 11 and 12 were formed, and spin-coated at 4000 rpm for 20 seconds. Thereafter, drying was performed in a clean room at room temperature of 23° C. for more than 24 hours.
[0169] Fig.28 The reflectivity characteristics of the optical element 301 according to this embodiment are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig.29 The reflectance characteristics of the optical element 301 according to this embodiment when the incident angle is 0° at positions C and Q are shown. According to Table 13, the film thickness of each thin film layer at position Q is 6% greater than the film thickness of each thin film layer at position C, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectance characteristics are equal to or less than 0.2%, and this is excellent. Table 13 Embodiment 14
[0170] Embodiment 14 will now be described. Figure 3 : is a schematic cross-sectional view of an optical element 302 according to this embodiment. The optical element 302 according to this embodiment is an optical element in which an anti-reflection film 102 is formed on a transparent substrate 202. The transparent substrate 202 is S-LAH79 (manufactured by OHARA INC.) having a refractive index of 2.00 (for light of 550 nm wavelength). The lens surface of the transparent substrate 202 on which the anti-reflection film 102 is formed has a concave shape. The half-open angle φ at position Q on the maximum light effective diameter is 30°. Regarding the layer materials, the thin film layer 21 is made of a material including magnesium fluoride as a main component, the thin film layer 22 is made of a material including zirconium oxide and aluminum oxide as main components, and the thin film layer 23 is made of a material including hollow silica as a main component. Table 14 lists the details of the film configuration of the optical element 302 according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (1) to (8) and (10) to (12).
[0171] The anti-reflection film 102 according to this embodiment is formed by the following method. The thin film layers 21 and 22 are formed by an evaporation method. The evaporation method is similar to the evaporation method of Example 13. This embodiment also uses a mask so that the film thickness distribution is substantially uniform within the surface. After the thin film layer 21, the thin film layer 22 is formed by evaporation, and then 0.2 ml of the hollow silica coating solution 1 is dropped on the lens surface of the transparent substrate 202 on which the thin film layers 21 and 22 are formed, and spin coated at 4000 rpm for 20 seconds. Afterwards, drying is performed in a clean room at a room temperature of 23°C for more than 24 hours.
[0172] Fig.30 The reflectivity characteristics of the optical element 302 according to this embodiment are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig.31 The reflectance characteristics of the optical element 302 according to this embodiment when the incident angle is 0° at positions C and Q are shown. According to Table 13, the film thickness of each thin film layer at position Q is 2% greater than the film thickness of each thin film layer at position C, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectance characteristics are equal to or less than 0.2%, and this is excellent. Table 14 Embodiment 15
[0173] Reference now Fig.32 , a description will be given of the optical system 401 according to Embodiment 15. Fig.32 It is a cross-sectional view of the optical system 401. The optical system 401 includes a plurality of optical elements G401 to G416. Reference numeral 402 represents an aperture stop (aperture), and reference numeral 403 represents an imaging surface. The optical elements G401 to G411 are each a lens. The anti-reflection film according to any one of Examples 1 to 14 is disposed on at least one of the incident surface and the exit surface of each lens. That is, the optical system 401 includes a plurality of optical elements G401 to G411, and a plurality of optical elements G403, G412 and G143 include an optical element 301 or 302, and the anti-reflection film according to any one of Examples 1 to 14 is formed on the optical element 301 or 302.
[0174] The optical system 401 according to this embodiment is not limited to an imaging optical system included in an imaging device to be described below, but can also be applied to optical systems of various applications such as binoculars, projectors, and telescopes. Example 16
[0175] Reference now Fig.33 , a description will be given of an imaging device according to Embodiment 16. Fig.33 1 is an external perspective view of an imaging device (digital camera 500). The digital camera 500 includes a camera body 502, and a lens device 501 integrated with the camera body 502. However, the embodiment is not limited to this implementation, and the lens device 501 may be an interchangeable lens connected to and detachable from the camera body 502, such as an interchangeable lens for a single-lens reflex camera, a mirrorless camera, or the like. The lens device 501 includes an optical system 401 according to any one of Embodiments 1 to 15. The camera body 502 includes an image sensor 503, such as a CMOS sensor or a CCD sensor. The image sensor 503 is disposed on an imaging surface 403 of the optical system 401. Comparative Example 1
[0176] Next, Comparative Example 1 will be described. Figure 2 : is a schematic cross-sectional view of an optical element 301 according to this comparative example. The optical element 301 according to this comparative example is an optical element in which an anti-reflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-TIL26 (manufactured by OHARA INC.) having a refractive index of 1.57 (for light of 550 nm wavelength). The lens surface of the transparent substrate 201 on which the anti-reflection film 101 is formed has a concave shape. The half-open angle φ at position Q on the maximum light effective diameter is 45°. Regarding the layer materials, the thin film layer 11 is made of a material including magnesium fluoride as a main component, the thin film layer 12 is made of a material including aluminum oxide as a main component, and the thin film layer 13 is made of a material including hollow silica as a main component. Table 15 lists the details of the film configuration of the optical element according to this comparative example. The refractive index and film thickness of the material satisfy inequalities (1) to (8), but do not satisfy inequalities (10) and (11).
[0177] The anti-reflection film 101 according to this comparative example is formed by the following method. The thin film layers 11 and 12 are formed by an evaporation method. The evaporation method is similar to the evaporation method of Example 13. This comparative example does not use a mask to make the film thickness distribution substantially uniform within the surface. After the thin film layer 11, the thin film layer 12 is formed by evaporation, and then 0.2 ml of the hollow silica coating solution 1 is dropped on the lens surface of the transparent substrate 201 on which the thin film layers 11 and 12 are formed, and spin coated at 4000 rpm for 20 seconds. Afterwards, drying is performed in a clean room at a room temperature of 23°C for more than 24 hours.
[0178] Fig.34The reflectivity characteristics of the optical element 301 according to this comparative example at the incident angles of 0°, 15°, 30°, 45°, and 60° at position C are shown. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. However, when Fig.35 When the reflectance characteristics at an incident angle of 0° are compared between positions C and Q in Table 14, the reflectance characteristics at position Q are lower than those at position C. According to Table 14, the film thickness of the thin film layer 12 at position Q is 6% greater than that at position C, but the film thicknesses of the thin film layers 11 and 12 at position Q are 30% less than that at position C. Therefore, the reflectance characteristics at position Q are deteriorated. Table 15 Comparative Example 2
[0179] Next, Comparative Example 2 will be described. Figure 2 : is a schematic cross-sectional view of an optical element 301 according to this comparative example. The optical element 301 according to this comparative example is an optical element in which an anti-reflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-TIL26 (manufactured by OHARA INC.) having a refractive index of 1.57 (for light of 550 nm wavelength). The lens surface of the transparent substrate 201 on which the anti-reflection film 101 is formed has a concave shape. The half-open angle φ at the position Q on the maximum light effective diameter is 45°. With respect to the layer materials, the thin film layer 11 is made of a material including solid silica as a main component, the thin film layer 12 is made of a material including a polyimide resin as a main component, and the thin film layer 13 is made of a material including hollow silica as a main component.
[0180] Details of the film configuration of the optical element 301 according to this comparative example are listed in Table 16. The refractive index of the thin film layer 13 does not satisfy the inequalities (1) and (4).
[0181] The antireflection film 101 according to this comparative example was formed by the following method. Chain silica coating solution 2
[0182] A chain particle dispersion solution 2 and a binder solution 2 were prepared by a method similar to the hollow particle coating solution 1. 78.0 g of the chain particle binder solution 2 was added to 251.3 g of the dispersion solution 2. Then, 174.5 g of 1-propoxy-2-propanol and 510.8 g of ethyl lactate were added and stirred for 60 minutes to obtain a chain silica coating solution 2.
[0183] The antireflection film 101 is formed using the solid silica coating solution 1 , the polyimide coating solution 1 , and the chain silica coating solution 2 .
[0184] 0.2 ml of the solid silica coating solution was dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating solution 1 was dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. In addition, 0.2 ml of the chain silica coating solution 2 was continuously dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. After that, drying was performed in a clean room at room temperature of 23° C. for more than 24 hours.
[0185] Fig.36 The reflectivity characteristics of the optical element 301 according to this comparative example are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or greater than 0.2%, and therefore sufficient antireflection performance cannot be obtained. Table 16
[0186] Each embodiment can provide an optical element, an optical system, an imaging device, and a method of manufacturing an optical element, each of which can sufficiently reduce the reflectivity regardless of the refractive index of the base (substrate).
[0187] Reference now Fig.37 , a schematic description will be given of an optical element 300 according to any one of Embodiments 17 to 25. Fig.37 is a schematic diagram of an optical element 300. The optical element 300 includes a transparent substrate (base material) 200 and an anti-reflection film 100 composed of four layers. The anti-reflection film 100 is composed of the following in order from the transparent substrate 200 to the air side: a thin film layer (first layer) 01, a thin film layer (second layer) 02, a thin film layer (third layer) 03, and a thin film layer (fourth layer) 04.
[0188] For light of 550 nm wavelength, n1 is the refractive index of thin film layer 01, n2 is the refractive index of thin film layer 02, n3 is the refractive index of thin film layer 03, and n4 is the refractive index of thin film layer 04. d1 (nm) is the physical thickness of thin film layer 01, d2 (nm) is the physical thickness of thin film layer 02, d3 (nm) is the physical thickness of thin film layer 03, and d4 (nm) is the physical thickness of thin film layer 04. In this case, at least one of the following inequalities (15) to (22) may be satisfied: 1.56≤n1≤1.70 (15) 1.30≤n2≤1.50 (16) 1.56≤n3≤1.70 (17) 1.10≤n4≤1.28 (18) 40≤n1d1≤250 (19) 10≤n2d2≤100 (20) 10≤n3d3≤100 (21) 100≤n4d4≤155 (22) 200≤n1d1+n2d2+n3d3+n4d4≤550 (23)
[0189] In the case where the refractive index or physical thickness of any material is outside the range of inequalities (15) to (23), sufficient antireflection performance cannot be obtained.
[0190] Inequality (18) can be replaced by the following inequality (24): 1.12≤n4≤1.22 (24)
[0191] Inequality (18) can be replaced by the following inequality (24a): 1.15≤n4≤1.22(24a)
[0192] The thin film layers 02, 03, and 04 of the optical element 300 according to each embodiment may be composed of a material including an organic compound. The "organic compound" in this embodiment is a compound including carbon, except for compounds having a simple structure such as carbon monoxide and carbon dioxide. The material including the "organic compound" can be easily formed by a wet coating method.
[0193] Fig.38 The optical element 301 or 302 according to an embodiment of the present disclosure shown in FIG. 39 is a schematic diagram in which the surface of the transparent substrate 201 or 202 on which the anti-reflection film 101 or 102 is formed has a concave or convex shape. The following description will only discuss Fig.38 The concave shape shown, but the description is similarly applicable to Fig.39 Convex shape shown.
[0194] The shape of the optical surface of the optical element 301 for forming the anti-reflection film 101 has a rotationally symmetric axis (e.g., a reference axis; for example, a surface normal passing through an origin (e.g., a surface vertex)), in other words, it has a rotationally symmetric shape. However, the embodiments are not limited to this implementation, and the optical surface for forming the anti-reflection film 101 may not have rotational symmetry. Fig.38, position C is the rotation center of the lens surface of the transparent substrate 201 on which the anti-reflection film 101 is provided. In other words, position C is the position (intersection point) where the rotational symmetry axis (optical axis L) of the lens surface intersects with the lens surface of the transparent substrate 201. On the other hand, position Q is located at the farthest point from position C in the optically effective area on the lens surface of the transparent substrate 201. The optically effective area is an area (e.g., effective diameter) on the optical surface through which an effective light beam contributing to imaging passes.
[0195] When φ is the angle between the optical axis L and the normal at the position Q (hereinafter referred to as the half-open angle), the half-open angle φ has a maximum value in the optically effective area. The anti-reflection film 101 is composed of a thin film layer (first layer) 11, a thin film layer (second layer) 12, a thin film layer (third layer) 13, and a thin film layer (fourth layer) 14 in order from the transparent substrate 201. At the position C, d2c (nm) is the physical thickness of the thin film layer 12, d3c (mm) is the physical thickness of the thin film layer 13, and d4c (nm) is the physical thickness of the thin film layer 14. At the position Q, d2q (nm) is the physical thickness of the thin film layer 12, d3q (nm) is the physical thickness of the thin film layer 13, and d4q (nm) is the physical thickness of the thin film layer 14. In this case, at least one of the following inequalities (25) to (27) may be satisfied: 1.0<d2q / d2c≤1.3 (25) 1.0<d3q / d3c≤1.3 (26) 1.0<d4q / d4c≤1.3 (27)
[0196] In each embodiment, the film thickness of the thin film layers 12, 13 and 14 constituting the antireflection film 101 may each be smallest at a position C which is the center (optical axis center) of the antireflection film 101 and become larger at a position farther from the optical axis center.
[0197] In various embodiments, the half-opening angle φ (°) at position Q may satisfy the following inequality (28): 25≤φ<90 (28)
[0198] The following inequality (29) can be satisfied: 1.45≤nS≤2.10 (29) Where nS is the refractive index of the transparent substrate 201 .
[0199] Similar to the film layers 12, 13 and 14 and the film layers 22, 23 and 24, Fig.38 and 39The thin film layer 11 of the anti-reflection film 101 and the thin film layer 21 of the anti-reflection film 102 may be made of a material including an organic compound. Similarly, the film forming method may be a wet film forming method, in particular, a spin coating method.
[0200] The following description will only discuss Fig.38 The concave shape shown in , but similarly applicable to Fig.39 The convex shape shown in .
[0201] For the thin film layer 11, the following inequality (30) can be satisfied: 1.0<d1q / d1c≤1.3 (30) Wherein d1c (nm) is the physical thickness of the thin film layer 11 at position C, and d1q (nm) is the physical thickness of the thin film layer 11 at position Q.
[0202] The thin film layers 11 and 13 may satisfy the following inequality (31): 0.9≤d1 / d3≤1.1 (31)
[0203] The thin film layer 11 can be made of a material including a polyimide resin, which is a "polymer compound containing an imide (-CO-NR-CO-) bond." The imide bond has a planar structure, and during the formation of a thin film layer having such a structure, the molecular chains tend to be oriented parallel to the substrate. Therefore, the adhesion in the longitudinal direction is weaker than the adhesion in the lateral direction, and the thin film layer can be easily peeled off by rubbing with a cloth to which an appropriate amount of a polishing agent containing an aluminum oxide-based mineral is applied. In an embodiment of the present disclosure, the thin film layers 12, 13 and 14 above the thin film layer 11, in other words, the entire anti-reflection film 101 can be peeled off from the transparent substrate 201, and the regeneration process in the manufacturing process becomes easy.
[0204] Fig.40 41 shows an optical element 303 or 304 according to an embodiment of the present disclosure. The optical element 303 or 304 is a schematic diagram in the case where the surface of the transparent substrate 203 or 204 on which the anti-reflection film 103 or 104 is formed has a concave or convex shape. The following description will only discuss Fig.40 The concave shape shown in , but similarly applicable to Fig.41 The convex shape shown in .
[0205] The anti-reflection film 103 is composed of a thin film layer 31, a thin film layer 32, a thin film layer 33, and a thin film layer 34 in order from the transparent substrate 203. Similar to the thin film layers 12, 13, and 14 of the above-mentioned anti-reflection film 101, the thin film layers 32, 33, and 34 can be composed of a material including an organic compound and satisfy inequalities (25) to (27).
[0206] The thin film layer 31 may include a material containing aluminum oxide. Aluminum oxide exhibits excellent vapor barrier properties and can prevent yellowing of the substrate surface. In this case, the following inequality (19a) may be satisfied: 120≤n1d1≤250(19a)
[0207] When the thin film layer 31 is formed by a dry film forming method such as vapor deposition or sputtering, the incident angle of the evaporated material on the lens surface is large at the peripheral portion of the wide-angle lens, and the film thickness at the peripheral portion is smaller than that at the central portion. Fig.40 , the physical thickness d31c (nm) of the thin film layer 31 at position C and the physical thickness d31q (nm) of the thin film layer 31 at position Q can satisfy the following inequality (32): 0.5≤d31q / d31c<1.0 (32)
[0208] The following inequality (33) can be satisfied: -0.1≤ns-n1≤0.1 (33) Wherein ns is the refractive index of the transparent substrate 203 for light having a wavelength of 550 nm.
[0209] In the case where the difference in refractive index between the transparent substrate 203 and the thin film layer 31 is small, the interface reflection is small. Any unevenness in the film thickness of the thin film layer 31 within the lens surface is unlikely to cause deviation in the reflection performance.
[0210] The following inequality (34) can be satisfied: 450≤Tg≤550 (34) Wherein Tg (° C.) is the glass transition temperature of the transparent substrate 203 .
[0211] A glass material having a low glass transition temperature is likely to have problems such as yellowing caused by the glass material. Using aluminum oxide as a layer directly provided on the glass material can prevent a decrease in reflectivity due to yellowing or the like.
[0212] The thin film layers 04, 14, 24, 34 and 44 may include voids. Since the voids are included, in other words, air with a refractive index of 1.0 is included, the refractive index can be reduced to inequalities (18) and (24). When the refractive index is less than 1.10, the ratio of the voids included in the layer is high, so the film strength is low. When the refractive index is greater than 1.28, sufficient anti-reflection performance cannot be obtained. In each embodiment, an anti-fouling layer or the like can be provided on the surface of the anti-reflection film (e.g., the surface of the thin film layers 04, 14, 24, 34 and 44) as needed. Examples of anti-fouling layers include fluoropolymer layers, fluorosilane monolayers and titanium oxide particle layers.
[0213] In each embodiment, the film layer 04, 14, 24, 34 and 44 can be made of solid particles, chain particles or hollow particles. The film layer can be made of hollow particles with voids inside. The void can be a single hole or multiple holes, which can be selected as needed. The material of the solid particles, chain particles or hollow particles can have a low refractive index. The material is, for example, an organic resin made of SiO2, MgF2, fluorine or silicon, but SiO2 (which can easily manufacture its particles) can also be used. The average particle size of the hollow particles can be equal to or greater than 15nm and equal to or less than 100nm, or can be equal to or greater than 15nm and less than or equal to 80nm. In the case where the average particle size of the hollow particles is less than 15nm, it is difficult to reliably produce particles as the core. In the case where the average particle size of the hollow particles exceeds 100nm, the size of the voids between the particles becomes larger, so large voids may appear, and scattering with the particle size may occur.
[0214] The film layers 02, 12, 22, 32 and 42 may be made of a material comprising solid particles bonded to a binder such as siloxane bonds, in particular solid silica particles. Alternatively, the material may include acrylic resin as the "acrylate or methacrylate polymer".
[0215] The film layers 03, 13, 23, 33 and 43 may be made of a material including a polyimide resin, which is a "polymer compound containing an imide (-CO-NR-CO-) bond". Alternatively, the film layers may be made of a material including an epoxy resin, which is a "resin cross-linked and cured with an epoxy group having oxirane (ethylene oxide) as a three-membered cyclic ether in the structural formula".
[0216] In each embodiment, the thin film layers 11, 21, the thin film layers 12, 22, 32 and 42, the thin film layers 13, 23, 33 and 43, and the thin film layers 14, 24, 34 and 44 can be formed by a wet film forming method, which involves applying a coating solution containing a film material, followed by drying and calcining. The wet film forming method can be cheaply coated over a large area. In particular, a spin coating method can be used because the method can flatten the film thickness distribution in a plane by coating while rotating around the rotation axis of the coating surface.
[0217] The organic solvent that can be used for coating solution is not particularly limited, as long as coating is simple, performance etc. are not deteriorated, and any known solvent can be used.For example, the organic solvent can include monohydric alcohols, such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methylpropanol, 1-pentanol, 2-pentanol and cyclopentanol.The organic solvent can include 2-methylbutanol, 3-methylbutanol, 1-hexanol, 2-hexanol, 3-hexanol, 4-methyl-2-pentanol, 2-methyl-1-pentanol and 2-ethylbutanol.The organic solvent can include 2,4-dimethyl-3-pentanol, 3-ethylbutanol, 1-heptanol, 2-heptanol, 1-octanol and 2-octanol.
[0218] The organic solvent may include polyols, such as ethylene glycol and triethylene glycol. The organic solvent may include ether alcohols, such as methoxyethanol, ethoxyethanol, propoxyethanol, isopropoxyethanol, butoxyethanol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol and 1-propoxy-2-propanol. The organic solvent may include ethers, such as dimethoxyethane, diglyme, tetrahydrofuran, dioxane, diisopropyl ether, dibutyl ether and cyclopentyl methyl ether.
[0219] The organic solvent can include esters, such as ethyl formate, ethyl acetate, n-butyl acetate, methyl lactate, ethyl lactate, ethylene glycol monomethyl ether acetate and ethylene glycol monoethyl ether acetate. The ester can be ethylene glycol monobutyl ether acetate and propylene glycol monomethyl ether acetate. The organic solvent can include various aliphatic hydrocarbons or cycloaliphatic hydrocarbons, such as normal hexane, normal octane, cyclohexane, cyclopentane and cyclooctane. The organic solvent can include various aromatic hydrocarbons, such as toluene, xylene and ethylbenzene.
[0220] The organic solvent can include various ketones, such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone and cyclohexanone. The organic solvent can include various chlorinated hydrocarbons, such as chloroform, methylene dichloride, carbon tetrachloride and tetrachloroethane. The organic solvent can include aprotic polar solvents, such as N-Methyl pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide and ethylene carbonate. In these solvents, two or more solvents can be used in combination.
[0221] In the case where solid particles, chain particles or hollow particles are used for the fourth film layer 04, 14, 24, 34 and 44 and solid particles are used for the second film layer 02, 12, 22, 32 and 42, a bonding adhesive may be used to improve strength. The adhesive may be a siloxane bond, especially in the case of using silica particles having abundant hydroxyl groups on the surface.
[0222] In each embodiment, the thin film layers 11 and 21, the thin film layers 12 and 22, the thin film layers 13 and 23, and the thin film layers 14 and 24 are made of a material that can be formed by a wet film forming method, and thus the material or the binder includes an organic compound. In addition, the anti-reflection film according to each embodiment is not calcined at a high temperature during the drying process after coating. Therefore, for example, plastics and photocurable resins that are easily deformed by heat can be used for the transparent substrates 201 and 202, and all layers thereof can be formed by a wet film forming method.
[0223] The thin film layers 31 and 41 can be formed by a dry film forming method (such as an evaporation method or a sputtering method). The dry film forming method (such as an evaporation method or a sputtering method) forms a film in a positional relationship in which the evaporation source and the center portion of the lens face each other. In a wide-angle lens, the incident angle of the evaporated material on the lens surface is larger at the peripheral portion, so the film thickness at the peripheral portion is smaller than the film thickness at the central portion. Therefore, film (thickness) unevenness occurs in the lens surface, and the anti-reflection performance has deviations. However, when inequality (19) is satisfied, the interface reflection between the transparent substrate 200 and the thin film layers 31 and 41 is reduced. Therefore, even when the film thickness of the thin film layers 31 and 41 has an in-plane variation, the deviation of the reflective performance is reduced.
[0224] Specific embodiments will be described below. However, these embodiments are merely illustrative, and the present disclosure is not limited to the scope of each embodiment. Embodiment 17
[0225] Fig.38 : is a schematic cross-sectional view of an optical element 301 according to Example 17. The optical element 301 according to this embodiment is an optical element in which an anti-reflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-TIL26 (manufactured by OHARA INC.) having a refractive index of 1.57 (for light of 550 nm wavelength). The lens surface of the transparent substrate 201 on which the anti-reflection film 101 is formed has a concave shape. The half-open angle φ at position Q on the maximum light effective diameter is 45°. Regarding the layer materials, the thin film layer 11 is made of a material including a polyimide resin as a main component, the thin film layer 12 is made of a material including solid silica as a main component, the thin film layer 13 is made of a material including a polyimide resin as a main component, and the thin film layer 14 is made of a material including hollow silica as a main component. Table 1 lists the details of the film configuration of the optical element according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (15) to (23), (25) to (37) and (30). The thin film layers 11, 12, 13, and 14 each include an organic compound.
[0226] The antireflection film 101 according to this embodiment is formed by the following method.
[0227] The antireflection film 101 was formed using the solid silica coating solution 1 , the polyimide coating solution 1 , and the hollow silica coating solution.
[0228] 0.2 ml of the polyimide coating solution 1 was dropped on the lens surface of the transparent substrate 201 and spun at 2000 rpm for 20 seconds. Next, 0.2 ml of the solid silica coating solution 1 was continuously dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. In addition, 0.2 ml of the polyimide coating solution 1 was continuously dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. Finally, 0.2 ml of the hollow silica coating solution 1 was dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. After that, drying was performed in a clean room at room temperature of 23°C for more than 24 hours.
[0229] Fig.42 Reflectivity characteristics are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig.43 The reflectivity characteristics at the incident angle of 0° at positions C and Q are shown. According to Table 17, the film thickness of each thin film layer at position Q is about 6% greater than the film thickness at position C, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectivity characteristics are equal to or less than 0.2%, and this is excellent. Table 17 Embodiment 18
[0230] Fig.39: is a schematic cross-sectional view of an optical element 302 according to Example 18. The optical element 302 according to this embodiment is an optical element in which an anti-reflection film 102 is formed on a transparent substrate 202. The transparent substrate 202 is S-LAH66 (manufactured by OHARA INC.) having a refractive index of 1.77 (for light of 550 nm wavelength). The lens surface of the transparent substrate 202 on which the anti-reflection film 102 is formed has a convex shape. The half-open angle φ at position Q on the maximum light effective diameter is 60°. Regarding the layer materials, the thin film layer 21 is made of a material including a polyimide resin as a main component, the thin film layer 22 is made of a material including solid silica as a main component, the thin film layer 23 is made of a material including a polyimide resin as a main component, and the thin film layer 24 is made of a material including hollow silica as a main component. Table 18 lists the details of the film configuration of the optical element according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (15) to (23), (25) to (27) and (30). The thin film layers 21, 22, 23, and 24 each include an organic compound.
[0231] The antireflection film 102 according to this embodiment is formed by the following method.
[0232] The antireflection film 102 was formed using the solid silica coating solution, the polyimide coating solution 1, and the hollow silica coating solution.
[0233] 0.2 ml of polyimide coating solution 1 was dropped on the lens surface of transparent substrate 202 and spun at 3000 rpm for 20 seconds. Next, 0.2 ml of solid silica coating solution was continuously dropped on the lens surface of transparent substrate 201 and spun at 4000 rpm for 20 seconds. In addition, 0.2 ml of polyimide coating solution 1 was continuously dropped on the lens surface of transparent substrate 202 and spun at 4000 rpm for 20 seconds. Finally, 0.2 ml of hollow silica coating solution was dropped on the lens surface of transparent substrate 202 and spun at 4000 rpm for 20 seconds. After that, drying was performed in a clean room at room temperature of 23°C for more than 24 hours.
[0234] Fig.44 Reflectivity characteristics are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig.45The reflectivity characteristics when the incident angle is 0° at positions C and Q are shown. According to Table 18, the film thickness of each thin film layer at position Q is about 12% greater than the film thickness at position C, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectivity is equal to or less than 0.2%, and this is excellent. Table 18 Embodiment 19
[0235] Fig.38 : is a schematic cross-sectional view of an optical element 301 according to Example 19. The optical element 301 according to this embodiment is an optical element in which an anti-reflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-TIH53 (manufactured by OHARA INC.) having a refractive index of 1.85 (for light of 550 nm wavelength). The lens surface of the transparent substrate 201 on which the anti-reflection film 101 is formed has a concave shape. The half-open angle φ at position Q on the maximum light effective diameter is 30°. Regarding the layer materials, the thin film layer 11 is made of a material including a polyimide resin as a main component, the thin film layer 12 is made of a material including solid silica as a main component, the thin film layer 13 is made of a material including a polyimide resin as a main component, and the thin film layer 14 is made of a material including hollow silica as a main component. Table 19 lists the details of the film configuration of the optical element according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (15) to (23), (25) to (27) and (30). The thin film layers 11, 12, 13, and 14 each include an organic compound.
[0236] The antireflection film 101 according to this embodiment is formed by the following method.
[0237] The antireflection film 101 is formed using the solid silica coating solution 1 , the polyimide coating solution 2 , and the hollow silica coating solution.
[0238] 0.2 ml of polyimide coating solution 2 was dropped on the lens surface of the transparent substrate 201 and spun at 3000 rpm for 20 seconds. Next, 0.2 ml of solid silica coating solution 1 was dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. In addition, 0.2 ml of polyimide coating solution 2 was continuously dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. In addition, 0.2 ml of hollow silica coating solution 1 was dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. After that, drying was performed in a clean room at room temperature of 23°C for more than 24 hours.
[0239] Fig.46Reflectivity characteristics are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig.47 The reflectivity characteristics at the incident angle of 0° at positions C and Q are shown. According to Table 19, the film thickness of each thin film layer at position Q is about 2% greater than the film thickness at position C, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectivity characteristics are equal to or less than 0.2%, and this is excellent. Table 19 Embodiment 20
[0240] Fig.39 : is a schematic cross-sectional view of an optical element 302 according to Example 20. The optical element 302 according to this embodiment is an optical element in which an anti-reflection film 102 is formed on a transparent substrate 202. The transparent substrate 202 is LPQ-1500 (manufactured by Mitsubishi Gas Chemical Co., Ltd.) having a refractive index of 1.59 (for light of a wavelength of 550 nm). The lens surface of the transparent substrate 202 on which the anti-reflection film 102 is formed has a convex shape. The half-open angle φ at position Q on the maximum light effective diameter is 30°. Regarding the layer materials, the thin film layer 21 is made of a material including a polyimide resin as a main component, the thin film layer 22 is made of a material including solid silica as a main component, the thin film layer 23 is made of a material including a polyimide resin as a main component, and the thin film layer 24 is made of a material including hollow silica as a main component. Table 20 lists the details of the film configuration of the optical element according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (15) to (23), (25) to (27) and (30). The thin film layers 11, 12, 13 and 14 each include an organic compound.
[0241] The antireflection film 101 according to this embodiment is formed by the following method.
[0242] The antireflection film 102 is formed using the solid silica coating solution 1 , the polyimide coating solution 2 , and the hollow silica coating solution 1 .
[0243] 0.2 ml of polyimide coating solution 2 was dropped on the lens surface of the transparent substrate 202 and spun at 3500 rpm for 20 seconds. Next, 0.2 ml of solid silica coating solution 1 was dropped on the lens surface of the transparent substrate 202 and spun at 4000 rpm for 20 seconds. Next, 0.2 ml of polyimide coating solution 2 was dropped on the lens surface of the transparent substrate 202 and spun at 4000 rpm for 20 seconds. In addition, 0.2 ml of hollow silica coating solution 1 was dropped on the lens surface of the transparent substrate 202 and spun at 4000 rpm for 20 seconds. After that, drying was performed in a clean room at room temperature of 23°C for more than 24 hours.
[0244] Fig.48 Reflectivity characteristics are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig.49 The reflectivity characteristics at the incident angle of 0° at positions C and Q are shown. According to Table 20, the film thickness of each thin film layer at position Q is about 3% greater than the film thickness at position C, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectivity is equal to or less than 0.2%, and this is excellent. Table 20 Embodiment 21
[0245] Fig.38 : is a schematic cross-sectional view of an optical element 301 according to Example 21. The optical element 301 according to this embodiment is an optical element in which an anti-reflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is EP-9000 (manufactured by Mitsubishi Gas Chemical Co., Ltd.) having a refractive index of 1.68 (for light of a wavelength of 550 nm). The lens surface of the transparent substrate 201 on which the anti-reflection film 101 is formed has a concave shape. The half-open angle φ at position Q on the maximum light effective diameter is 45°. The thin film layer 11 is made of a material including a polyimide resin as a main component, the thin film layer 12 is made of a material including solid silica as a main component, the thin film layer 13 is made of a material including a polyimide resin as a main component, and the thin film layer 14 is made of a material including hollow silica as a main component. Table 21 lists the details of the film configuration of the optical element according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (15) to (23), (25) to (27), (30) and (31). The thin film layers 11, 12, 13 and 14 each include an organic compound.
[0246] The antireflection film 101 according to this embodiment is formed by the following method.
[0247] The antireflection film 101 is formed using the solid silica coating solution 1 , the polyimide coating solution 1 , and the hollow silica coating solution 1 .
[0248] 0.2 ml of the polyimide coating solution 1 was dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. Next, 0.2 ml of the solid silica coating solution 1 was dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. In addition, 0.2 ml of the polyimide coating solution 1 was dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. Finally, 0.2 ml of the hollow silica coating solution 1 was continuously dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. After that, drying was performed in a clean room at room temperature of 23°C for more than 24 hours.
[0249] Fig.50 Reflectivity characteristics are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig.51 The reflectivity characteristics at the incident angle of 0° at positions C and Q are shown. According to Table 21, the film thickness of each thin film layer at position Q is about 6% greater than the film thickness at position C, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectivity characteristics are equal to or less than 0.2%, and this is excellent. Table 21 Embodiment 22
[0250] Fig.38: is a schematic cross-sectional view of an optical element 301 according to Example 22. The optical element 301 according to this embodiment is an optical element in which an anti-reflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-BSL7 (manufactured by OHARA INC.) having a refractive index of 1.52 (for light of 550 nm wavelength). The lens surface of the transparent substrate 201 on which the anti-reflection film 101 is formed has a concave shape. The half-open angle φ at position Q on the maximum light effective diameter is 30°. Regarding the layer materials, the thin film layer 11 is made of a material including a polyimide resin as a main component, the thin film layer 12 is made of a material including solid silica as a main component, the thin film layer 13 is made of a material including a polyimide resin as a main component, and the thin film layer 14 is made of a material including hollow silica as a main component. Table 22 lists the details of the film configuration of the optical element according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (15) to (23), (25) to (27), (30) and (31). The thin film layers 11, 12, 13 and 14 each include an organic compound.
[0251] The antireflection film 101 according to this embodiment is formed by the following method.
[0252] The antireflection film 101 is formed using the solid silica coating solution 1 , the polyimide coating solution 2 , and the hollow silica coating solution 1 .
[0253] 0.2 ml of polyimide coating solution 2 was dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. Next, 0.2 ml of solid silica coating solution 1 was dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. In addition, 0.2 ml of polyimide coating solution 2 was dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. Finally, 0.2 ml of hollow silica coating solution 1 was continuously dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. After that, drying was performed in a clean room at room temperature of 23°C for more than 24 hours.
[0254] Fig.52 Reflectivity characteristics are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig.53The reflectivity characteristics at the incident angle of 0° at positions C and Q are shown. According to Table 22, the film thickness of each thin film layer at position Q is about 3% greater than the film thickness at position C, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectivity characteristics are equal to or less than 0.2%, and this is excellent. Table 22 Embodiment 23
[0255] Fig.39 : is a schematic cross-sectional view of an optical element 302 according to Example 23. The optical element 302 according to this embodiment is an optical element in which an anti-reflection film 102 is formed on a transparent substrate 202. The transparent substrate 202 is S-BAM12 (manufactured by OHARA INC.) having a refractive index of 1.64 (for light of 550 nm wavelength). The lens surface of the transparent substrate 202 on which the anti-reflection film 102 is formed has a convex shape. The half-open angle φ at position Q on the maximum light effective diameter is 45°. Regarding the layer materials, the thin film layer 21 is made of a material including a polyimide resin as a main component, the thin film layer 22 is made of a material including solid silica as a main component, the thin film layer 23 is made of a material including a polyimide resin as a main component, and the thin film layer 24 is made of a material including hollow silica as a main component. Table 23 lists the details of the film configuration of the optical element according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (15) to (23), (25) to (27), (30) and (31). The thin film layers 21, 22, 23 and 24 each include an organic compound.
[0256] The antireflection film 102 according to this embodiment is formed by the following method.
[0257] The antireflection film 102 is formed using the solid silica coating solution 1 , the polyimide coating solution 1 , and the hollow silica coating solution 1 .
[0258] 0.2 ml of the polyimide coating solution 1 was dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. Next, 0.2 ml of the solid silica coating solution 1 was dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. In addition, 0.2 ml of the polyimide coating solution 1 was dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. Finally, 0.2 ml of the hollow silica coating solution 1 was continuously dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. After that, drying was performed in a clean room at room temperature of 23°C for more than 24 hours.
[0259] Fig.54Reflectivity characteristics are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig.55 The reflectivity characteristics at the incident angle of 0° at positions C and Q are shown. According to Table 23, the film thickness of each thin film layer at position Q is about 6% greater than the film thickness at position C, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectivity is equal to or less than 0.2%, and this is excellent. Table 23 Embodiment 24
[0260] Fig.40 : is a schematic cross-sectional view of an optical element 303 according to Example 24. The optical element 303 according to this embodiment is an optical element in which an anti-reflection film 103 is formed on a transparent substrate 203. The transparent substrate 203 is L-BAL43 (manufactured by OHARA INC.) having a refractive index of 1.59 (for light of 550 nm wavelength). The glass transition temperature Tg (°C) of L-BAL43 is 493°C. The lens surface of the transparent substrate 203 on which the anti-reflection film 103 is formed has a concave shape. The half-open angle φ at position Q on the maximum light effective diameter is 30°. Regarding the layer materials, the thin film layer 31 is made of a material including aluminum oxide as a main component, the thin film layer 32 is made of a material including solid silica as a main component, the thin film layer 33 is made of a material including a polyimide resin as a main component, and the thin film layer 34 is made of a material including hollow silica as a main component. Table 24 lists the details of the film configuration of the optical element according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (15) to (23), (25) to (27), and (32) to (34). The thin film layers 32, 33, and 34 each include an organic compound.
[0261] The antireflection film 103 according to this embodiment is formed by the following method.
[0262] The thin film layer 31 is formed by evaporation. The evaporated material is heated using an electron beam. In addition, an ion beam assisted evaporation method is performed to form a denser film. The vacuum chamber of the evaporation device is evacuated to 2×10 -3 After confirming the high vacuum state inside the vacuum chamber, Ar as an inert gas was introduced into the ion gun, and then the ion gun was discharged. After the ion gun became stable, oxygen was introduced into the vacuum chamber, and at about 1×10 -2Ion-assisted evaporation was performed using oxygen ions under a vacuum pressure of 1.5 Pa. According to the evaporation method, the film thickness of a lens having a large half-opening angle decreases as the position moves toward the peripheral portion.
[0263] After the thin film layer 31 was formed by evaporation, 0.2 ml of the solid silica coating solution 1 was dropped on the lens surface of the transparent substrate 203 on which the thin film layer 31 was formed, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating solution 1 was dropped on the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Finally, 0.2 ml of the hollow silica coating solution 1 was continuously dropped on the lens surface of the transparent substrate 203, and spin-coated at 4000 rpm for 20 seconds. Thereafter, drying was performed in a clean room at room temperature of 23° C. for more than 24 hours.
[0264] Fig.56 Reflectivity characteristics are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig.57 The reflectivity characteristics at the incident angle of 0° at positions C and Q are shown. According to Table 24, the film thickness of the thin film layer 31 at position Q is about 13% smaller than the film thickness at position C, and the film thickness of the thin film layers 32, 33, and 34 at position Q is about 3% larger than the film thickness at position C, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectivity characteristics are equal to or less than 0.2%, and this is excellent. Table 24 Embodiment 25
[0265] Fig.41: is a schematic cross-sectional view of an optical element 304 according to Example 25. The optical element 304 according to this embodiment is an optical element in which an anti-reflection film 104 is formed on a transparent substrate 204. The transparent substrate 204 is L-TIL28 (manufactured by OHARA INC.) having a refractive index of 1.69 (for light of 550 nm wavelength). The lens surface of the transparent substrate 204 on which the anti-reflection film 104 is formed has a convex shape. The half-open angle φ at position Q on the maximum light effective diameter is 40°. Regarding the layer materials, the thin film layer 41 is made of a material including aluminum oxide as a main component, the thin film layer 42 is made of a material including solid silica as a main component, the thin film layer 43 is made of a material including a polyimide resin as a main component, and the thin film layer 44 is made of a material including hollow silica as a main component. Table 25 lists the details of the film configuration of the optical element according to this embodiment. The refractive index and film thickness of the material satisfy inequalities (15) to (23), (25) to (27), and (32) to (34). The thin film layers 42, 43, and 44 each include an organic compound.
[0266] The antireflection film 104 according to this embodiment is formed by the following method.
[0267] The thin film layer 41 is formed by an evaporation method similar to the evaporation method used for the thin film layer 31 according to the eighth embodiment.
[0268] After the thin film layer 41 was formed by evaporation, 0.2 ml of the solid silica coating solution 1 was dropped on the lens surface of the transparent substrate 204 on which the thin film layer 41 was formed, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating solution 2 was continuously dropped on the lens surface of the transparent substrate 204, and spin-coated at 4000 rpm for 20 seconds. Finally, 0.2 ml of the hollow silica coating solution 1 was continuously dropped on the lens surface of the transparent substrate 204, and spin-coated at 4000 rpm for 20 seconds. Thereafter, drying was performed in a clean room at room temperature of 23° C. for more than 24 hours.
[0269] Fig.58 Reflectivity characteristics are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. Fig.59The reflectivity characteristics at the incident angle of 0° at positions C and Q are shown. According to Table 25, the film thickness of the thin film layer 41 at position Q is about 23% smaller than the film thickness at position C, and the film thickness of the thin film layers 32, 33, and 34 at position Q is 5% larger than the film thickness at position C, however, it can be confirmed that for light in the 420nm to 680nm band, the reflectivity characteristics are equal to or less than 0.2%, and this is excellent. Table 25
[0270] The optical elements of Examples 17 to 25 can also be applied to the above reference Fig.32 The optical system 401 of the embodiment 15 described above. The optical system 400 includes the optical element 301, 302, 303 or 304 on which the anti-reflection film according to any one of the embodiments 17 to 25 is formed. In addition, the optical element according to any one of the embodiments 17 to 25 can also be applied to the above reference Fig.33 An image pickup apparatus (digital camera 500) according to Embodiment 16 is described. Comparative Example 3
[0271] Fig.38 A schematic cross-sectional view of an optical element 301 according to Comparative Example 3 is shown. The optical element 301 according to this comparative example is an optical element in which an anti-reflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-TIL26 (manufactured by OHARA INC.) having a refractive index of 1.57 (for light of 550 nm wavelength). The lens surface of the transparent substrate 201 on which the anti-reflection film 101 is formed has a concave shape. The half-open angle φ at position Q on the maximum light effective diameter is 45°. Regarding the layer materials, the thin film layer 11 is made of a material including aluminum oxide as a main component, the thin film layer 12 is made of a material including magnesium fluoride as a main component, the thin film layer 13 is made of a material including aluminum oxide as a main component, and the thin film layer 14 is made of a material including hollow silica as a main component. Table 26 lists the details of the film configuration of the optical element according to this comparative example. The refractive index and film thickness of the material satisfy inequalities (15) to (23), but do not satisfy inequalities (25) to (27).
[0272] The anti-reflection film 101 according to this comparative example is formed by the following method. The thin film layers 11, 12 and 13 are formed by an evaporation method. The evaporation method is similar to that of Example 8. After the thin film layers 11, 12 and 13 are formed in the order described by evaporation, 0.2 ml of the hollow silica coating solution 1 is dropped on the lens surface of the transparent substrate 201 on which the thin film layers 11, 12 and 13 are formed, and spin-coated at 4000 rpm for 20 seconds. Thereafter, drying is performed in a clean room at a room temperature of 23° C. for more than 24 hours.
[0273] Fig.60 The reflectivity characteristics at the incident angles of 0°, 15°, 30°, 45°, and 60° at position C are shown. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or less than 0.2%, and it can be understood that this reflectivity characteristic is very favorable. However, at Fig.61 , the reflectivity characteristics at an incident angle of 0° between positions C and Q are compared, and the reflectivity characteristics at position Q are lower than those at position C. According to Table 26, the film thickness of the thin film layer 14 at position Q is 6% greater than that at position C, but the film thickness of the thin film layers 11, 12, and 13 at position Q is 30% less than that at position C. Therefore, the reflectivity characteristics at position Q are deteriorated. Table 26 Comparative Example 4
[0274] Fig.62 A schematic cross-sectional view of an optical element 301 according to Comparative Example 4 is shown. The optical element 301 according to this comparative example is an optical element in which an anti-reflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-TIL26 (manufactured by OHARA INC.) having a refractive index of 1.57 (for light of 550 nm wavelength). The lens surface of the transparent substrate 201 on which the anti-reflection film 101 is formed has a concave shape. The half-open angle φ at position Q on the maximum light effective diameter is 45°. Regarding the layer materials, the thin film layer 11 is made of a material including a polyimide resin as a main component, the thin film layer 12 is made of a material including solid silica as a main component, the thin film layer 13 is made of a material including a polyimide resin as a main component, and the thin film layer 14 is made of a material including chain silica as a main component. Table 27 lists the details of the film configuration of the optical element according to this comparative example. The refractive index of the thin film layer 13 does not satisfy inequality (18).
[0275] The antireflection film 101 according to this embodiment is formed by the following method.
[0276] The antireflection film 101 is formed using the solid silica coating solution 1 , the polyimide coating solution 1 , and the chain silica coating solution 2 .
[0277] 0.2 ml of polyimide coating solution 1 was dropped on the lens surface of the transparent substrate 201 and spun at 3000 rpm for 20 seconds. Next, 0.2 ml of solid silica coating solution 1 was dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. In addition, 0.2 ml of polyimide coating solution 1 was dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. In addition, 0.2 ml of chain silica coating solution 2 was continuously dropped on the lens surface of the transparent substrate 201 and spun at 4000 rpm for 20 seconds. After that, drying was performed in a clean room at room temperature of 23°C for more than 24 hours.
[0278] Fig.62 Reflectivity characteristics are shown when the incident angles are 0°, 15°, 30°, 45°, and 60° at position C. For light in the 420nm to 680nm band at an incident angle of 0°, the reflectivity is equal to or greater than 0.2%, and thus sufficient antireflection characteristics cannot be obtained. Table 27
[0279] Although this disclosure describes example embodiments, it is to be understood that some embodiments are not limited to the disclosed embodiments.The scope of the following claims is to be accorded the broadest interpretation so as to encompass all such modifications and equivalent structures and functions.
[0280] Various embodiments can provide an optical element that can substantially reduce reflectivity regardless of the refractive index of a substrate.
Claims
1. An optical element, comprising: Base material; and Anti-reflective film, The antireflection film is characterized in that the antireflection film is composed of a first layer formed on a substrate, a second layer formed on the first layer, and a third layer formed on the second layer. wherein the first layer, the second layer and the third layer each comprise an organic compound, and The following inequality is satisfied: 1.10≤n3≤1.28 Where n3 is the refractive index of the third layer for light with a wavelength of 550 nm.
2. An optical element, comprising: Base material; and Anti-reflective film, The antireflection film is characterized in that the antireflection film is composed of a first layer formed on a substrate, a second layer formed on the first layer, and a third layer formed on the second layer. The following inequality is satisfied: 1.30≤n1≤1.50 1.56≤n2≤1.70 1.10≤n3≤1.28 10≤n1d1≤155 10≤n2d2≤155 100≤n3d3≤155 200≤n1d1+n2d2+n3d3≤300 Wherein n1 is the refractive index of the first layer for light with a wavelength of 550nm, n2 is the refractive index of the second layer for light with a wavelength of 550nm, n3 is the refractive index of the third layer for light with a wavelength of 550nm, d1 (nm) is the thickness of the first layer, d2 (nm) is the thickness of the second layer, and d3 (nm) is the thickness of the third layer.
3. The optical element according to claim 2, characterized in that The first layer, the second layer, and the third layer each include an organic compound.
4. The optical element according to claim 1, characterized in that The following inequality is satisfied: 1.0<d1q / d1c≤1.3 1.0<d2q / d2c≤1.3 1.0<d3q / d3c≤1.3 Wherein d1c (nm), d2c (nm) and d3c (nm) are respectively the thickness of the first layer, the thickness of the second layer and the thickness of the third layer at the intersection of a reference axis and the optical surface, wherein the reference axis passes through the surface vertex of the optical surface of the substrate on which the anti-reflection film is formed, and d1q (nm), d2q (nm) and d3q (nm) are respectively the thickness of the first layer, the thickness of the second layer and the thickness of the third layer at the position farthest from the intersection in the effective area of the optical surface.
5. The optical element according to claim 1, characterized in that The thickness of each of the first layer and the second layer is smallest at the center of the antireflection film and becomes larger at a position away from the center.
6. The optical element according to claim 1, characterized in that The first layer includes acrylic resin.
7. The optical element according to claim 1, characterized in that The first layer includes solid particles.
8. The optical element according to claim 1, characterized in that The second layer includes epoxy resin or polyimide resin.
9. The optical element according to claim 1, characterized in that The following inequality is satisfied: 1.45≤ns≤2.10 where ns is the refractive index of the substrate for light with a wavelength of 550 nm.
10. The optical element according to claim 2, characterized in that The following inequality is satisfied: 0.9≤d1 / d3≤1.
1.
11. The optical element according to claim 1, characterized in that The following inequality is satisfied: 1.55≤ns≤1.70 where ns is the refractive index of the substrate for light with a wavelength of 550 nm.
12. The optical element according to claim 1, characterized in that The following inequality is satisfied: 450≤Tg≤550 Where Tg (°C) is the glass transition temperature of the substrate.
13. The optical element according to claim 4, characterized in that In a wavelength band between 450 nm and 650 nm, the antireflection film has a reflectivity of 0.5% or less for light incident on the intersection at an incident angle of 0°, and has a reflectivity of 1.0% or less for light incident on the intersection at an incident angle of 30°.
14. The optical element according to claim 1, characterized in that The following inequality is satisfied: 1.12≤n3≤1.25。 15. The optical element according to claim 1, characterized in that The layer of the antireflective film farthest from the substrate includes voids.
16. The optical element according to claim 1, characterized in that The layer of the antireflection film farthest from the substrate includes at least one of solid particles, chain particles, and hollow particles.
17. The optical element according to claim 16, characterized in that At least one of the solid particles, chain particles and hollow particles is made of silicon dioxide. 18 . The optical element according to claim 1 , further comprising a film including a fluorine resin formed on the antireflection film.
19. An optical system comprising a plurality of optical elements, the plurality of optical elements comprising the optical element according to any one of claims 1 to 18.
20. The optical system according to claim 19, characterized in that The following inequality is satisfied: 25≤φ<90 Wherein φ (degrees) is the half-open angle at the position of the effective diameter of the optical surface on which the antireflection film is formed on the substrate.
21. A camera device, comprising: An optical system according to claim 19 or 20; and An image sensor is configured to photograph a subject through the optical system.
22. A method for manufacturing an optical element, the optical element comprising a substrate and an anti-reflection film, the anti-reflection film comprising a first layer, a second layer and a third layer, the manufacturing method comprising the following steps: forming a first layer on a substrate using a wet coating method; forming a second layer on the first layer using a wet coating method; and The third layer is formed on the second layer by a wet coating method, It is characterized by satisfying the following inequality: 1.10≤n3≤1.28 Where n3 is the refractive index of the third layer for light with a wavelength of 550 nm.
23. The manufacturing method according to claim 22, characterized in that: The wet coating method is a spin coating method.