Coating device and coating method for enhancing oxidation resistance of total cross section of soft copper conductor

By using antioxidant coating solution prepared by 96-97% industrial alcohol and benzotriazole on cable conductors, combined with a special coating device, a metal chelate protective film is formed, which solves the conductor oxidation problem and improves the Antioxidant ability and prevent white objects from precipitating.

CN119028665AActive Publication Date: 2024-11-26HUNAN HUATAI CABLE CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411325093.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-11-26
Estimated Expiration
2044-09-23

AI Technical Summary

Technical Problem

Existing cable conductors are prone to oxidation in moisture environments, causing blackening, affecting quality and vision. In addition, the antioxidant ability of existing antioxidants decreases during annealing and twisting, making it difficult to effectively prevent full-section oxidation.

Method used

Using 96-97% industrial alcohol as solvent and benzotriazole as solute, the antioxidant coating liquid is prepared in a ratio of 1:1.2-1.6, and the size and drip of the liquid outlet are controlled through a special coating device. The length of the infusion needle forms a metal chelate protective film that isolates oxygen and prevents copper oxidation.

Benefits of technology

Effectively prevent the full cross-section of soft copper conductors, reduce the occurrence of mass problems, and prevent the crystallization and precipitation of antioxidants white substances, thereby improving the antioxidant ability of the conductor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028665A_ABST
    Figure CN119028665A_ABST
Patent Text Reader

Abstract

The invention provides a coating device and a coating method for enhancing the oxidation resistance of the total cross section of a soft copper conductor. The device comprises an antioxidant liquid storage tank, an alcohol box, a support column, a liquid outlet pipe, a liquid conveying pipe, a spray head, an electric control box and a motor, the alcohol box is arranged above the antioxidant liquid storage tank through the supporting column, one end of the liquid outlet pipe is arranged in the antioxidant liquid storage tank, and the other end of the liquid outlet pipe is connected with the liquid conveying pipe; one end in the alcohol box is provided with a wire inlet die, the other end in the alcohol box is provided with a wire outlet die, a group of wire passing guide wheels are arranged between the wire inlet die and the wire outlet die, and a bunch-stranded conductor to be coated passes through the wire inlet die, the wire passing guide wheels and the wire outlet die to spray coating liquid on the surface of the bunch-stranded conductor. Alcohol with the concentration of 96-97% is used as a solvent, benzotriazole is used as a solute, the antioxidant coating liquid is prepared according to the mass ratio of 1: 1.2-1.6%, meanwhile, the soft copper conductor is coated through a matched coating device, the total cross section of the soft copper conductor can be prevented from being oxidized, and the antioxidant can be prevented from being crystallized and separated out in the form of white matter.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cable conductor anti-oxidation, in particular to a coating device and a coating method for enhancing the anti-oxidation capability of the entire cross-section of a soft copper conductor. Background Art

[0002] Common oxidation situations of existing wire and cable conductors include: BVR or RV electrical equipment wires are selected in home decoration, industrial equipment or wind power switch cabinet distribution lines. During the cable manufacturing and long-term installation process, the inner conductor is oxidized and discolored (red or black) due to the presence of moisture or mixed gas in the air or pipeline; the inner conductor of the copper core silicone rubber cable turns black about a week after insulation; the inner conductor of the mining rubber sheathed flexible cable oxidizes to red, yellow, purple or even black due to the sulfur or sulfur-containing groups in the rubber formula.

[0003] Conductor oxidation and blackening is a common quality problem in the cable industry or in transmission and distribution lines. This problem is very likely to cause customer complaints and affect the supply and demand relationship. There are countless returns and quality claims caused by this problem every year. According to incomplete statistics, various losses amount to tens of billions of yuan. Therefore, conductor oxidation is a pain point and difficulty in the industry. In addition, conductor oxidation and blackening generally occur at the ends. The thickness of the conductor oxide layer is very thin, and the resistance increases by about 2%. On the one hand, the oxidized and discolored conductor affects people's vision and is an important certificate for project acceptance products.

[0004] Therefore, solving the conductor oxidation problem is an urgent and realistic problem facing every technician in the cable industry. From the perspective of the conductor oxidation mechanism, the most critical thing is to enhance the conductor's antioxidant capacity. In practice, adding antioxidants to the drawing liquid and annealing liquid or using a wrapping film to isolate the conductor from the air has a certain effect, but it cannot eliminate the root cause of the conductor's reduced antioxidant capacity caused by annealing, twisting, and secondary vulcanization. Especially for conductors with multiple soft wires, it is very difficult to solve because the conductor gaps have oxygen and are very easy to oxidize in a humid environment. In addition to preparing special antioxidants, it is also important to consider that the solvent has good volatility and environmental protection. The conductor is coated with a thin layer of protective film similar to a metal chelate through the mixed liquid, which isolates the oxygen in the air and prevents copper oxidation reaction, thereby enhancing the copper conductor's antioxidant capacity and reducing the occurrence of quality problems.

[0005] Therefore, the industry is in urgent need of a new technology of a coating device and a coating method for enhancing the oxidation resistance of the entire cross-section of a soft copper conductor. Summary of the invention

[0006] In order to solve the technical problem of conductor oxidation and blackening in the prior art, the present invention provides a coating device and a coating method for enhancing the anti-oxidation ability of the full cross-section of a soft copper conductor. The present invention takes into account that the solvent has good volatility and environmental protection. The conductor is coated with a mixed liquid to form a thin metal chelate protective film, which isolates oxygen in the air and does not cause copper oxidation reaction, thereby enhancing the anti-oxidation ability of the copper conductor and reducing the occurrence of quality problems. Specifically, the present invention uses industrial alcohol with a concentration of 96-97% as a solvent and benzotriazole as a solute. The two are mixed in a mass ratio of 1:1.2-1.6% to form an antioxidant coating liquid unique to the soft copper conductor bundle twisting process. At the same time, the coating device of the present invention is used to coat the soft copper conductor by controlling the size of the liquid outlet tube, the dripping speed and the length of the infusion needle, which can prevent the full cross-section of the soft copper conductor from being oxidized and prevent the antioxidant from crystallizing and precipitating in the form of white matter.

[0007] To achieve the above object, the present invention provides a coating device for enhancing the anti-oxidation ability of the entire cross-section of a soft copper conductor, the coating device comprising an antioxidant storage tank, an alcohol box, a support, a liquid outlet pipe, a liquid infusion pipe, an adjustable alcohol nozzle, an electric control box and a motor;

[0008] The antioxidant liquid storage tank is an open container for storing the antioxidant coating liquid and recovering excess antioxidant coating liquid;

[0009] The alcohol box is a closed container, which is used to spray the antioxidant coating liquid on the soft copper stranded conductor of the cable to be coated and collect the excess antioxidant coating liquid;

[0010] The alcohol box is arranged above the antioxidant storage tank through a support, one end of the liquid outlet pipe is arranged in the antioxidant storage tank, the other end of the liquid outlet pipe is connected to an infusion pipe, the infusion pipe is connected to an adjustable alcohol nozzle, a control valve is arranged on the infusion pipe, and a needle is arranged on the adjustable alcohol nozzle;

[0011] A wire entry die is provided at one end of the alcohol box in the horizontal direction, and a wire exit die is provided at the other end. A set of wire guide wheels is provided between the wire entry die and the wire exit die. The soft copper stranded conductor of the cable to be coated enters the alcohol box through the wire entry die, and then enters the wire exit die through the wire guide wheel. The alcohol spray head can be adjusted to spray the coating liquid on the surface of the stranded conductor.

[0012] The motor is connected to the liquid outlet pipe and is used to pump the antioxidant coating liquid to the liquid infusion pipe;

[0013] The electric control box is electrically connected to the motor.

[0014] Furthermore, a hole is provided at the bottom of the alcohol box, the hole is connected to one end of a reflux pipe, and the other end of the reflux pipe is provided in an antioxidant storage tank for conveying excess antioxidant coating liquid collected in the alcohol box to the antioxidant storage tank for recycling and reuse.

[0015] Furthermore, there are one or at least two adjustable alcohol nozzles; when there are two adjustable alcohol nozzles, the other end of the liquid outlet pipe is connected to two infusion tubes through a three-way pipe, and the infusion tubes are connected to multiple adjustable alcohol nozzles.

[0016] Furthermore, a drain port is provided at the bottom of the antioxidant liquid storage tank; a liquid level sensor is provided inside the antioxidant liquid storage tank, and the liquid level sensor is electrically connected to the electric control box.

[0017] The present invention also provides a method for coating a bundle of soft copper conductors of a cable for anti-oxidation, wherein the soft copper bundle of the cable conductor to be coated is transported to the inlet die of the alcohol box in the coating device, enters the alcohol box, and then passes through the wire guide wheel, and the alcohol nozzle can be adjusted to spray the coating liquid on the surface of the bundle of conductors through the infusion tube, and the liquid outlet speed is adjusted to match the stranding speed, and finally the bundle of conductors enters the outlet die, and the coating is completed;

[0018] The antioxidant coating liquid comprises benzotriazole and alcohol, the alcohol concentration is 96-97%, and the mass percentage of benzotriazole is 1.2-1.6% of the mass of alcohol.

[0019] Furthermore, the infusion tube is a hospital infusion tube, and the dripping speed is 1-3 drops per second.

[0020] Furthermore, the angle at which the adjustable alcohol spray head and the coating liquid are sprayed on the bundled conductor is 45-55°.

[0021] Furthermore, the size of the needle is 0.3-0.6 mm; the length of the needle is 1.5-3 mm.

[0022] Furthermore, the adjustable alcohol spray nozzle is an infusion needle; the infusion needle includes special, No. 7, No. 6, and No. 5 needles, wherein the diameter of the special needle is 0.6 mm, the diameter of the No. 7 needle is 0.51 mm, the diameter of the No. 6 needle is 0.34 mm, and the diameter of the No. 5 needle is 0.30 mm.

[0023] Furthermore, the cable soft copper stranded conductor to be coated is a Category 5 or Category 6 soft copper conductor strand of wires and cables; the specification of the soft copper wire is 0.15-0.5 mm.

[0024] The present invention has the following beneficial effects:

[0025] The present invention adopts industrial alcohol with a concentration of 96-97% as a solvent and benzotriazole as a solute, and the two are mixed in a ratio of 1:1.2-1.6% to prepare an antioxidant coating liquid with a unique soft copper conductor bundle twisting process. At the same time, the coating device of the present invention is used to control the size of the liquid outlet pipe, the switching speed and the length of the infusion needle to coat the soft copper conductor, which can prevent the full cross-section of the soft copper conductor from being oxidized and the antioxidant from being crystallized and precipitated in the form of white matter. Because when the antioxidant prepared in the same proportion as above with alcohol with a concentration of more than 97% is easy to precipitate in large quantities and easily clog the needle, the needle needs to be replaced or cleaned every 15 minutes or so, which is not conducive to the continuous production of soft copper conductors. The configuration of the antioxidant for the copper conductor of the enhanced cable is to use benzotriazole to form a covalent bond and a coordination bond with the copper atom, and mutually form a chain metal chelate protective film, which isolates oxygen in the air and does not cause copper oxidation reaction, thereby enhancing the antioxidant capacity of the copper conductor. Benzotriazole is a crystalline chemical reagent, slightly soluble in water and alcohol. Therefore, the liquid containing benzotriazole must have good volatility and a certain limit on water content, because water remaining in the conductor will accelerate its oxidation. Therefore, industrial alcohol is used as its solvent. The content of benzotriazole should be appropriate. Too much benzotriazole content is very easy to precipitate as white crystals and stick to the surface of the conductor, affecting the conductor's smoothness. Too much benzotriazole content will cause its antioxidant capacity to be insufficient and lack of protection. The best effect is in the range of 1.2-1.6%.

[0026] In addition to the above-described purposes, features and advantages, the present invention has other purposes, features and advantages. The present invention will be further described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0028] Figure 1 It is a structural schematic diagram of a coating device for enhancing the anti-oxidation capability of the entire cross-section of a soft copper conductor according to the present invention;

[0029] Among them, 1-antioxidant storage tank, 2-motor, 3-liquid outlet pipe, 4-electric control box, 5-pillar, 6-alcohol box, 7-cable soft copper bundle stranded conductor to be coated, 8-inlet mold, 9-adjustable alcohol nozzle, 10-tee pipe, 11-infusion tube, 12-connector, 13-outlet mold, 14-wire guide wheel, 15-reflux pipe, 16-drain outlet. DETAILED DESCRIPTION

[0030] The embodiments of the present invention are described in detail below with reference to the accompanying drawings, but the present invention can be implemented in many different ways as defined and covered by the claims.

[0031] The purpose of the present invention is to provide an economical and effective coating device and coating method for preventing the oxidation resistance of the entire cross-section (including the inner and outer surfaces) of the soft copper stranded conductor of the cable category 5 and category 6. Usually, soft copper wire refers to a combination of multiple fine copper wires of the same diameter. According to different cross-sections, the conductor positions are divided into multiple structures such as inner layer, adjacent outer layer and outer layer. The so-called full cross-section of soft copper wire refers to the general term for the surface and gap of the single wire conductor of the outer layer including the adjacent outer layer and the surface and gap of the single wire conductor of the inner layer. After passing through the stranding die, the gap between the conductors becomes smaller accordingly, and the stranding outer diameter becomes smaller, which is conducive to the saving of subsequent materials.

[0032] The conductor processing method of twisting multiple soft copper single wires together in the same direction and pitch is called bundled wire. The standard stipulates that the 5th or 6th category conductors are twisted in bundles, which are usually used in occasions such as mobile cable conductors that require relatively softness. According to the size of the conductor cross-section, different numbers of single wires are used for bundle twisting, and then the conductors are twisted in a re-twisted manner to obtain a larger cross-section.

[0033] See also Figure 1 The present invention provides a coating device for enhancing the antioxidant capacity of the entire cross-section of a soft copper conductor, and is particularly suitable for processing equipment assisting in the twisting process of Category 5 or Category 6 soft copper conductors of wires and cables. The coating device includes an antioxidant storage tank 1, an alcohol box 6, a support 5, a liquid outlet pipe 3, an infusion pipe 11, an adjustable alcohol nozzle 9, an electric control box 4 and a motor 2.

[0034] The antioxidant liquid storage tank 1 is an open container for storing the antioxidant coating liquid and recovering excess antioxidant coating liquid;

[0035] The alcohol box 6 is a closed container, and an inlet mold 8 and an outlet mold 13 are arranged in the alcohol box 6. A group of wire guide wheels 14 are arranged between the inlet mold 8 and the outlet mold 13, which are used to spray the antioxidant coating liquid on the cable soft copper bundle stranded conductor 7 to be coated and collect excess antioxidant coating liquid.

[0036] The alcohol box 6 is arranged above the antioxidant storage tank 1 through the support 5, one end of the liquid outlet pipe 3 is arranged in the antioxidant storage tank 1, and the other end of the liquid outlet pipe 3 is connected to the infusion pipe 11, and the infusion pipe 11 is connected to the adjustable alcohol nozzle 9. The adjustable alcohol nozzle 9 is one or at least two; when the adjustable alcohol nozzle 9 is at least two, the other end of the liquid outlet pipe 3 is connected to multiple infusion pipes 11 through a three-way pipe 10, and each infusion pipe 11 can also continue to connect multiple infusion pipes 11 through the three-way pipe 10, and multiple infusion pipes 11 are connected to multiple adjustable alcohol nozzles 9.

[0037] The infusion tube 11 is provided with a control valve, and the adjustable alcohol nozzle 9 is provided with a needle; the infusion tube 11 is connected to the adjustable alcohol nozzle 9 via a connector 12 .

[0038] An inlet mold 8 is provided at one horizontal end of the alcohol box 6, and an outlet mold 13 is provided at the other end. A group of wire guide wheels 14 are provided between the inlet mold 8 and the outlet mold 13. The soft copper stranded conductor 7 of the cable to be coated enters the alcohol box 6 through the inlet mold 8, and then enters the outlet mold 13 through the wire guide wheels 14. The alcohol spray head 9 can be adjusted to spray the coating liquid on the surface of the stranded conductor.

[0039] The motor 2 is connected to the liquid outlet pipe 3 and is used to pump the antioxidant coating liquid to the liquid infusion pipe 11 ; the electric control box 4 is electrically connected to the motor 2 .

[0040] The bottom of the alcohol box 6 is provided with a hole, and the hole is connected to one end of the reflux pipe 15 , and the other end of the reflux pipe 15 is arranged in the antioxidant storage tank 1 .

[0041] The bottom of the antioxidant liquid storage tank 1 is provided with a drain port 16. A liquid level sensor is provided inside the antioxidant liquid storage tank 1, and the liquid level sensor is electrically connected to the electric control box 4.

[0042] In a specific embodiment, the antioxidant liquid storage tank 1 is a rectangular stainless steel metal container, which is open on the top and has a liquid outlet pipe 3 connected to the motor 2. The antioxidant liquid storage tank 1 is the main station for storing antioxidant coating liquid, and provides antioxidant coating liquid for the continuous production of the cable soft copper bundle stranded conductor 7 to be coated. The motor 2 provides power for coating through the switch, and the antioxidant coating liquid is pumped from the liquid outlet hole of the motor pump to the infusion pipe 11 through the liquid outlet pipe 3. The adjustable alcohol nozzle 9 passes the antioxidant coating liquid through the infusion pipe 11, the control valve and the needle in sequence, and directly smears it on the stranded copper conductor. The stranded conductor in the alcohol box 6 presents two forms of movement: linear motion and spiral motion through the wire inlet mold 8, the wire outlet mold 13 and a group of wire guide wheels 14. Therefore, the antioxidant coating liquid can easily enter the conductor and wet the inner conductor surface. The flow rate is adjusted by the control valve, and the nozzle is fixed on the support 5 with a base, so that the antioxidant coating liquid is sprayed on the moving conductor without deviation, that is, it has a positioning function. At the same time, two nozzles (one in front and one behind or one large and one small) or one nozzle are selected according to the size of the conductor cross-section, depending on the effect, to prevent excess antioxidant liquid from remaining on the conductor without completely volatilizing and causing insulation bubbling. Therefore, the number of drops needs to match the speed of the conductor. When shutting down, the switch of the motor pump and the switch on the control valve on the infusion tube are both in the closed state, which reduces the consumption of the antioxidant coating liquid on the one hand and reduces the precipitation of the antioxidant coating liquid on the other hand.

[0043] In one embodiment, a heating ring is further provided inside the outlet mold 13, which is heated by low voltage and high current so that the alcohol and water on the surface of the twisted conductor passing through it evaporate quickly to form a dense anti-oxidation mold.

[0044] The electric control box 4 includes a start button, a stop button and a liquid level alarm button. This part is wired to control the motor and the liquid level, making the switch operation convenient. The upper end of the pillar 5 is connected to the alcohol box 6, the middle part is connected to the control box, and a metal gravity balance plate is welded at the lower end. The pillar 5 is made of a light aluminum alloy material. Among them, the alcohol box 6 can be used to collect excess dripping antioxidant coating liquid so that it can flow into the antioxidant storage tank 1 through the reflux pipe 15. There are an inlet mold 8 and an outlet mold 13 at both ends of the alcohol box 6, which have the function of sizing and preventing the core of the soft copper bundle stranded conductor of the cable to be coated from swinging. There is also a set of upper and lower guide wheels to support the conductor and limit the deviation of the conductor.

[0045] The coating device is used to apply an anti-oxidation coating to a bundle of soft copper conductors of a cable. The soft copper conductors of the cable to be coated are passed through an inlet die into an alcohol box, and then passed through a wire guide wheel into an outlet die. The coating liquid is sprayed on the surface of the bundle of conductors through an adjustable alcohol nozzle through an infusion tube.

[0046] The coating liquid comprises benzotriazole and alcohol, the alcohol concentration is 96-97%, and the mass percentage of benzotriazole is 1.2-1.6% of the mass of alcohol.

[0047] Specific implementation methods: Figure 1 As shown, several copper conductors pass through the distribution board from left to right into the bundle assembly mold to form a bundle copper conductor, that is, the cable soft copper bundle twisted conductor to be coated. Then turn on the electric switch and the manual infusion switch. After passing the positioning guide wheel, pass through the outlet mold, adjust the nozzle position, quantity and dripping speed, check the conductor surface and inner layer coating, and turn on the machine after it is normal. The dripping liquid is controlled by the manual control valve and the size of the infusion needle. The nozzle and the conductor are at an angle of 45-55 degrees. The best position is before the stranded wire is about to enter the mold. There is a little gap between the conductors to facilitate the liquid to infiltrate the conductor surface. The infusion tube is a hospital infusion tube. The dripping speed is 1-3 drops / second. The size of the needle is 0.3-0.6mm; the length of the needle is 1.5-3mm. The adjustable alcohol nozzle is an infusion needle; the infusion needle includes a special needle, a No. 7 needle, a No. 6 needle and a No. 5 needle; among them, the diameter of the special needle is 0.6mm, the diameter of the No. 7 needle is 0.51mm, the diameter of the No. 6 needle is 0.34mm, and the diameter of the No. 5 needle is 0.30mm. It is selected according to the size of the thin and soft copper wire specification of 0.15-0.5mm, and the liquid discharge speed is adapted to the twisting speed.

[0048] Since online spraying increases the pumping pressure, the design model of hospital infusion tubes was adopted for the first time. In particular, the size of the outlet tube, the control of the switching speed and the length of the infusion needle were the key cores of the implementation.

[0049] Furthermore, the switch control requires the infusion rate to be 1-3 drops per second, and not higher than 4-5 drops. Otherwise, antioxidants will remain inside the conductor. After the alcohol evaporates, the antioxidants will attach to the conductor surface in the form of white crystals, increasing the DC resistance of the conductor.

[0050] Furthermore, there are four types of infusion needles to choose from: special, No. 7, No. 6, and No. 5. They are selected based on the size of the soft copper wire (0.15-0.5mm) and the number of conductors. Special needles and No. 7 needles are preferred for the type of needle. The length of the needle is maintained at 1.5-3mm, which can maintain a certain pressure on the liquid while allowing it to pass through the needle quickly, preventing benzotriazole crystals from clogging the needle due to replacement of the conductor, breakage of the wire, and other accidents, resulting in poor coating effect.

[0051] The present invention is explained below in conjunction with specific embodiments.

[0052] Embodiment 1:

[0053] The soft copper stranded cable conductor to be coated is delivered to Figure 1 After the alcohol box in the coating device enters the wire entry mold, it enters the alcohol box, and then passes through the wire guide wheel. The adjustable alcohol nozzle sprays the coating liquid on the surface of the bundled conductor through the hospital infusion tube, and at the same time adjusts the liquid outlet speed to match the stranding speed. Finally, the bundled conductor enters the wire exit mold, and the coating is completed. The infusion tube is a hospital infusion tube, and the adjustable alcohol nozzle is an infusion needle. The length of the needle is maintained at 1.5-3mm. The dripping liquid is controlled by the manual control valve and the size of the infusion needle. The needle and the coating liquid are sprayed on the bundled conductor at an angle of 45-55°. The best position is before the stranded wire is about to enter the mold. There is a little gap between the conductors, which is convenient for the liquid to infiltrate the conductor surface. The dripping speed is 1-3 drops / second. The needle is a No. 7 needle, which is selected according to the size of the fine and soft copper wire specification 0.15-0.5mm. The liquid outlet speed is adapted to the stranding speed.

[0054] The antioxidant coating liquid is prepared by mixing benzotriazole and 96% industrial alcohol in a ratio of 1.2:100, and then put into a special container for fireproof sealing and storage.

[0055] Embodiment 2:

[0056] The soft copper stranded cable conductor to be coated is delivered to Figure 1After the alcohol box in the coating device enters the wire entry mold, it enters the alcohol box, and then passes through the wire guide wheel. The adjustable alcohol nozzle sprays the coating liquid on the surface of the bundled conductor through the hospital infusion tube, and at the same time adjusts the liquid outlet speed to match the stranding speed. Finally, the bundled conductor enters the wire exit mold, and the coating is completed. The infusion tube is a hospital infusion tube, and the adjustable alcohol nozzle is an infusion needle. The length of the needle is maintained at 1.5-3mm. The dripping liquid is controlled by the manual control valve and the size of the infusion needle. The needle and the coating liquid are sprayed on the bundled conductor at an angle of 45-55°. The best position is before the stranded wire is about to enter the mold. There is a little gap between the conductors, which is convenient for the liquid to infiltrate the conductor surface. The dripping speed is 1-3 drops / second. The needle is a No. 6 needle, which is selected according to the size of the fine and soft copper wire specification 0.15-0.5mm. The liquid outlet speed is adapted to the stranding speed.

[0057] The antioxidant coating liquid is prepared by mixing benzotriazole and 96% industrial alcohol in a ratio of 1.3:100, and then put into a special container for fireproof sealing and storage.

[0058] Embodiment 3:

[0059] The soft copper stranded cable conductor to be coated is delivered to Figure 1 After the alcohol box in the coating device enters the wire entry mold, it enters the alcohol box, and then passes through the wire guide wheel. The adjustable alcohol nozzle sprays the coating liquid on the surface of the bundled conductor through the hospital infusion tube, and at the same time adjusts the liquid outlet speed to match the stranding speed. Finally, the bundled conductor enters the wire exit mold, and the coating is completed. The infusion tube is a hospital infusion tube, and the adjustable alcohol nozzle is an infusion needle. The length of the needle is maintained at 1.5-3mm. The dripping liquid is controlled by the manual control valve and the size of the infusion needle. The needle and the coating liquid are sprayed on the bundled conductor at an angle of 45-55°. The best position is before the stranded wire is about to enter the mold. There is a little gap between the conductors to facilitate the liquid to infiltrate the conductor surface. The dripping speed is 1-3 drops / second. The needle is a No. 5 needle. It is selected according to the size of the fine and soft copper wire specification 0.15-0.5mm. The liquid outlet speed is adapted to the stranding speed.

[0060] The antioxidant coating liquid is prepared by mixing benzotriazole and 96% industrial alcohol in a ratio of 1.4:100, and then put into a special container for fireproof sealing and storage.

[0061] Embodiment 4:

[0062] The soft copper stranded cable conductor to be coated is delivered to Figure 1After the alcohol box in the coating device enters the wire entry mold, it enters the alcohol box, and then passes through the wire guide wheel. The adjustable alcohol nozzle sprays the coating liquid on the surface of the bundled conductor through the hospital infusion tube, and at the same time adjusts the liquid outlet speed to match the stranding speed. Finally, the bundled conductor enters the wire exit mold, and the coating is completed. The infusion tube is a hospital infusion tube, and the adjustable alcohol nozzle is an infusion needle. The length of the needle is maintained at 1.5-3mm. The dripping liquid is controlled by the manual control valve and the size of the infusion needle. The needle and the coating liquid are sprayed on the bundled conductor at an angle of 45-55°. The best position is before the stranded wire is about to enter the mold. There is a little gap between the conductors, which is convenient for the liquid to infiltrate the conductor surface. The dripping speed is 1-3 drops / second. The needle is a special needle, which is selected according to the size of the fine and soft copper wire specification 0.15-0.5mm, and the liquid outlet speed is adapted to the stranding speed.

[0063] The antioxidant coating liquid is prepared by mixing benzotriazole and 96% industrial alcohol in a ratio of 1.5:100, and then put into a special container for fireproof sealing and storage.

[0064] Embodiment 5:

[0065] The difference between Example 5 and Example 1 is that the antioxidant coating liquid is prepared by mixing benzotriazole and 96% industrial alcohol in a ratio of 1.6:100, and then put into a special container for fireproof sealing and storage.

[0066] Comparative Example 1:

[0067] The difference between Comparative Example 1 and Example 1 is that the antioxidant coating liquid used is prepared by mixing benzotriazole and 96% industrial alcohol in a mass ratio of 1.0:100, and the rest is the same as Example 1.

[0068] Comparative Example 2:

[0069] The difference between Comparative Example 2 and Example 1 is that the antioxidant coating liquid used is prepared by mixing benzotriazole and 96% industrial alcohol in a mass ratio of 1.1:100, and the rest is the same as Example 1.

[0070] Comparative Example 3:

[0071] The difference between Comparative Example 3 and Example 1 is that the antioxidant coating liquid used is prepared by mixing benzotriazole and 96% industrial alcohol in a mass ratio of 1.7:100, and the rest is the same as Example 1.

[0072] Comparative Example 4:

[0073] The difference between Comparative Example 4 and Example 1 is that the antioxidant coating liquid used is prepared by mixing benzotriazole and 96% industrial alcohol in a mass ratio of 1.8:100, and the rest is the same as Example 1.

[0074] Comparative Example 5:

[0075] The difference between Comparative Example 4 and Example 1 is that the antioxidant coating liquid used is prepared by mixing benzotriazole and 96% industrial alcohol in a mass ratio of 2.0:100, and the rest is the same as Example 1.

[0076] Comparative Example 6:

[0077] The difference between Comparative Example 6 and Example 1 is that the dripping speed is 0.5 drops / second, and the rest is the same as Example 1.

[0078] Comparative Example 7:

[0079] The difference between Comparative Example 7 and Example 1 is that the dripping speed is 5 drops / second, and the rest is the same as Example 1.

[0080] Comparative Example 8:

[0081] The difference between Comparative Example 7 and Example 1 is that a No. 4 needle (with a diameter of 0.21 mm) is selected as the needle, and the rest is the same as Example 1.

[0082] Comparative Example 9:

[0083] The difference between Comparative Example 7 and Example 1 is that the selected needle is larger than the special needle (with a diameter of 0.65 mm), and the rest is the same as Example 1.

[0084] The following is an antioxidant performance verification test for Examples 1-5 and Comparative Examples 1-9, to determine whether the color of the soft wire stranded conductor does not change (including turning red, i.e. slight oxidation, turning purple, and turning black, i.e. deep oxidation) after the first continuous vulcanization of the rubber insulation and the second continuous vulcanization of the rubber sheath in a vulcanization tube of about 120 meters with 175-200°C steam (steam pressure 15kg) as evidence of process verification of whether the antioxidant is effective.

[0085] Comparative Example 10: Take a soft copper conductor without adding an antioxidant, mark it with Comparative Example 10, place it in a rubber extrusion vulcanization workshop, and observe the oxidation time of the conductor.

[0086] Comparative Example 11: Take a soft copper conductor without adding an antioxidant, mark it with Comparative Example 11, extrude a vulcanized rubber insulation layer, and observe the oxidation time of the conductor.

[0087] Application example: The soft copper stranded wires coated in comparative examples 1-2 and embodiments 1-3 are respectively produced into samples of about 500 meters, which are marked as samples 1-5, and are respectively subjected to a vulcanization extrusion rubber insulation layer, and the oxidation time of the conductor, whether colored crystals are precipitated on the conductor, and the resistance of the conductor are tested to see the percentage increase of resistance;

[0088] Application example: The soft copper stranded wires coated in Examples 4-5 and Comparative Examples 3-9 were respectively produced into samples of about 500 meters, labeled as samples 6-10, and respectively subjected to secondary vulcanization, i.e., extruded rubber insulation layer + rubber sheath, to observe the conductor oxidation time, whether colored crystals were precipitated on the conductor, and the test conductor resistance ratio and resistance increase percentage. The test results are shown in Table 1 (the observation period is 8 months). The experimental results are shown in Table 1:

[0089] Table 1

[0090]

[0091]

[0092] It can be seen from Table 1 that the present invention uses alcohol with a concentration of 90-97% as a solvent and benzotriazole as a solute, and the two are mixed in a ratio of 1:1.2-1.6% to prepare a unique antioxidant coating liquid for the soft copper conductor bundle twisting process. At the same time, the coating device of the present invention is used to control the size of the liquid outlet tube, the switching speed and the length of the infusion needle to coat the soft copper conductor, which can prevent the full cross-section of the soft copper conductor from being oxidized and the antioxidant from crystallizing and precipitating in the form of white matter. Because the configuration of the antioxidant for the copper conductor of the enhanced cable is to form a covalent bond and a coordination bond between benzotriazole and copper atoms, and form a chain metal chelate protective film to isolate oxygen in the air, and no copper oxidation reaction will occur, thereby enhancing the antioxidant capacity of the copper conductor. Benzotriazole is a crystalline chemical reagent, which is slightly soluble in water and alcohol. Therefore, the liquid containing benzotriazole must have good volatility and a certain limit on water content, because water remaining in the conductor will accelerate its oxidation. Therefore, industrial alcohol is selected as its solvent. The content of benzotriazole in the antioxidant coating liquid is very important. When the content of benzotriazole is too much, it is very easy to precipitate as white crystals and stick to the surface of the conductor, affecting the smoothness of the conductor; when the content of benzotriazole is too little, it will cause its antioxidant capacity to be insufficient and lack of protection. Therefore, the best effect is achieved when the concentration is in the range of 1.2-1.6%.

[0093] During the coating process, the speed of adding the antioxidant coating liquid is also very important. When the dripping speed is 0.5 drops / second (Comparative Example 6), the stranding speed of the bundled conductor is faster than the dripping speed, resulting in the risk of oxidation of some conductors that are not dipped in the protective liquid, while the conductors coated with the antioxidant are not oxidized. For wires and cables used in sections, this leads to an increase in customer complaints about conductor oxidation.

[0094] When the dripping speed is 5 drops / second (Comparative Example 7), the conductor stranding speed is slower than the dripping speed, and liquid overflows from the inner and outer surfaces of the conductor, forming a saturated dip coating. Part of the overflowed liquid flows back to the receiver, part of it hangs on the guide wheel, the assembly mold and the take-up reel, polluting the production equipment, and part of it remains inside the conductor, which will cause the conductor to oxidize and turn black over time.

[0095] During the coating process, the selection of the needle size of the antioxidant coating liquid is also very important. When the needle is too small and a needle smaller than No. 5 is selected (Comparative Example 8), the dripping speed can be fine-tuned by the switch, but the antioxidant is completely dissolved into liquid in alcohol from the naked eye. It is slightly soluble in alcohol, and the excess part is very easy to precipitate and block the filter membrane at the front end of the syringe. Especially when the machine is unexpectedly shut down and then turned on again after a few minutes, it is found that it is completely blocked and no liquid can come out. The needle part needs to be cleaned again, and the production is not continuous enough.

[0096] When the needle is too large and a needle larger than the extra-large needle (Comparative Example 9) is selected, the antioxidant quickly flows to the conductor to form a saturated dip coating, just like a large-sized faucet. Part of the overflowed liquid flows back to the receiver, part of it hangs on the guide wheel, the assembly mold and the take-up reel, polluting the production equipment, and part of it remains inside the conductor. This will cause the conductor to oxidize and turn black over time, and the effect is the same as that of Comparative Example 7.

[0097] In summary, through the above-mentioned performance tests in different environments and different ratios, the present invention can find that benzotriazole imidazole used as cable Category 5 and Category 6 conductor bundles can effectively prevent the oxidation of the inner and outer layers of soft copper conductors, and is very effective in the primary continuous vulcanization of rubber insulation and the secondary continuous vulcanization of rubber sheaths of conductors coated with antioxidants, without oxidation and discoloration, thus fundamentally solving the problems that have plagued the industry.

[0098] In order to further optimize the antioxidant dripping process and improve production efficiency and product quality, the following measures can be taken to adjust the nozzle position, quantity and dripping speed:

[0099] First, adjust the position of the nozzle: Specifically, make sure the nozzle is in the best position just above the soft copper conductor and before it enters the molded stranded wire. This allows the liquid to fully soak the surface of each conductor and prevents the liquid from gathering or flowing unevenly on the conductor. At the same time, according to the arrangement and twisting method of the conductor, adjust the position of the nozzle appropriately so that each conductor can be evenly covered by the liquid.

[0100] Secondly, adjust the number of nozzles: Specifically, according to the number and arrangement of conductors, reasonably configure the number of nozzles. If there are many conductors or the arrangement is more complicated, the number of nozzles can be appropriately increased to ensure that each conductor can be evenly covered by the liquid. Consider production efficiency and cost, and reasonably select the number of nozzles. Too many nozzles may lead to waste of resources, while too few may affect the uniform distribution of the liquid.

[0101] In addition, the dripping speed should be adjusted according to the specifications of the conductor and the viscosity of the liquid. For thinner copper wires (such as 0.15-0.5mm), the dripping speed should be controlled within the range of 1-3 drops per second to ensure that the liquid can be evenly coated on the conductor surface.

[0102] Finally, the choice of needle size: Specifically, according to the specifications of the thin and soft copper wire, choose the appropriate needle size. Special, No. 7, No. 6, and No. 5 needles each have their own application scenarios and should be selected according to the thickness of the copper wire and production requirements. For thinner copper wires, it is recommended to use a small needle (such as No. 5 or No. 6) to reduce liquid waste and improve the uniformity of the coating.

[0103] Through the above measures, the nozzle position, quantity and dripping speed can be effectively adjusted to optimize the liquid coating effect, improve production efficiency and product quality. At the same time, the process parameters should be continuously adjusted and optimized according to the specific conditions and experience in actual operation to achieve the best production effect.

[0104] Further specific embodiments adjust the dripping speed to be compatible with the stranding speed: The dripping speed is adapted to the stranding speed to ensure that the conductor surface can be evenly covered with liquid during the stranding process to form a continuous and uniform coating. To achieve this, the following specific control methods can be adopted: According to the speed matching principle, first, it is necessary to understand the operating speed range of the stranding machine and select a suitable dripping speed based on the speed range. Normally, the dripping speed should be slightly lower than the stranding speed to ensure that the liquid has enough time to form a uniform coating on the conductor.

[0105] In a specific example, the dripping speed can be adjusted to be compatible with the stranding speed according to the thickness of the coating formed by dripping on the conductor. Specifically, the thickness of the coating is greater than a set threshold value (obtained based on an empirical value), the flow rate per unit coating width of the coating liquid passing through the strand is controlled to be constant before and after the coating width is changed, and the supply flow rate and the discharge flow rate are controlled to be less than the supply flow rate and the discharge flow rate before the coating width is changed. When the thickness of the coating film is less than the thickness of the coating film before the coating width is changed, the flow rate is controlled to be constant before and after the coating width is changed, and the supply flow rate and the discharge flow rate are controlled to be greater than the supply flow rate and the discharge flow rate before the coating width is changed. The supply unit has a pump, and the supply flow rate is changed by the pump. The discharge unit has a pump, and the discharge flow rate is changed by the pump.

[0106] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A coating device for enhancing the anti-oxidation ability of the entire cross-section of a soft copper conductor, characterized in that: The coating device comprises an antioxidant liquid storage tank, an alcohol box, a support, a liquid outlet pipe, a liquid infusion pipe, an adjustable alcohol nozzle, an electric control box and a motor; The antioxidant liquid storage tank is an open container for storing the antioxidant coating liquid and recovering excess antioxidant coating liquid; The alcohol box is a closed container, which is used to spray the antioxidant coating liquid on the soft copper stranded conductor of the cable to be coated and collect the excess antioxidant coating liquid; The alcohol box is arranged above the antioxidant storage tank through a support, one end of the liquid outlet pipe is arranged in the antioxidant storage tank, the other end of the liquid outlet pipe is connected to an infusion pipe, the infusion pipe is connected to an adjustable alcohol nozzle, a control valve is arranged on the infusion pipe, and a needle is arranged on the adjustable alcohol nozzle; A wire entry die is provided at one end of the alcohol box in the horizontal direction, and a wire exit die is provided at the other end. A set of wire guide wheels is provided between the wire entry die and the wire exit die. The soft copper stranded conductor of the cable to be coated enters the alcohol box through the wire entry die, and then enters the wire exit die through the wire guide wheel. The alcohol spray head can be adjusted to spray the coating liquid on the surface of the stranded conductor. The motor is connected to the liquid outlet pipe and is used to pump the antioxidant coating liquid to the liquid infusion pipe; The electric control box is electrically connected to the motor.

2. A coating device for enhancing the full cross-section oxygen resistance of soft copper conductor according to claim 1, characterized in that: A hole is arranged at the bottom of the alcohol box, and the hole is connected to one end of a reflux pipe, and the other end of the reflux pipe is arranged in the antioxidant storage tank.

3. A coating device for enhancing the full cross-section oxygen resistance of soft copper conductor according to claim 1, characterized in that: There is one or at least two adjustable alcohol nozzles; when there are two adjustable alcohol nozzles, the other end of the liquid outlet pipe is connected to two infusion tubes through a three-way pipe, and the infusion tubes are connected to multiple adjustable alcohol nozzles.

4. A coating device for enhancing the anti-oxidation capability of the entire cross-section of a soft copper conductor according to any one of claims 1 to 3, characterized in that: A drain port is arranged at the bottom of the antioxidant liquid storage tank; a liquid level sensor is arranged inside the antioxidant liquid storage tank, and the liquid level sensor is electrically connected to the electric control box.

5. A method for coating cable soft copper conductor bundles for anti-oxidation, characterized in that: After the soft copper stranded conductor of the cable to be coated is conveyed to the wire inlet die of the alcohol box in the coating device according to any one of claims 1 to 4, it enters the alcohol box, and then passes through the wire guide wheel, and the alcohol nozzle can be adjusted to spray the coating liquid on the surface of the stranded conductor through the infusion tube, and the liquid outlet speed is adjusted to match the stranding speed, and finally the stranded conductor enters the wire outlet die, and the coating is completed; The antioxidant coating liquid comprises benzotriazole and alcohol, the alcohol concentration is 96-97%, and the mass percentage of benzotriazole is 1.2-1.6% of the mass of alcohol.

6. The coating method according to claim 5, characterized in that: The infusion tube is a hospital infusion tube, and the dripping speed is 1-3 drops per second.

7. The coating method according to claim 5, characterized in that: The angle at which the adjustable alcohol spray head and the coating liquid are sprayed on the bundled conductor is 45-55°.

8. The coating method according to claim 5, characterized in that: The size of the needle is 0.3-0.6mm; the length of the needle is 1.5-3mm.

9. The coating method according to claim 5, characterized in that: The adjustable alcohol spray nozzle is an infusion needle; the infusion needle includes a special needle, a No. 7 needle, a No. 6 needle and a No. 5 needle; among them, the diameter of the special needle is 0.6mm, the diameter of the No. 7 needle is 0.51mm, the diameter of the No. 6 needle is 0.34mm, and the diameter of the No. 5 needle is 0.30mm.

10. The coating method according to claim 5, characterized in that: The cable soft copper stranded conductor to be coated is a stranded soft copper conductor of Category 5 or Category 6 wire and cable; the specification of the soft copper wire is 0.15-0.5 mm.

Citation Information

Patent Citations

  • Anti-oxidation machining technology for copper wire production

    CN109047349A

  • Electric wire and cable conductor surface anti-oxidant

    CN1944711A

  • Copper wire twisting device

    CN221008660U