Electrolyte and application thereof in lithium ion battery

The in-situ reaction of the lithium salts containing fluorine and phosphorus elements in lithium-ion batteries with silicon-based oxalate compounds is formed to form a protective film, which solves the problem of insufficient high temperature and fast charging performance of lithium-ion batteries, and through Silicone compounds improve performance and reduce the cost of electrolyte.

CN119029314APending Publication Date: 2024-11-26SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411445187.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing lithium-ion batteries have shortcomings in high-temperature storage performance and fast charging and circulation performance, and the difficulty and cost of synthesis of lithium-salt additives limit the application of electrolytes.

Method used

The lithium salt containing fluorine and phosphorus elements is used to react in situ with silicon-based oxalate compounds to form oxalate phosphate compounds, forming a low-impedance protective film, improving the high temperature and fast charging performance of the battery, and using silicone compounds at the same time Further improve performance and reduce the cost of electrolyte.

Benefits of technology

It improves the high-temperature storage capacity retention rate, fast charging cycle performance and low high-temperature storage gas production expansion rate of lithium-ion batteries, reduces the cost of electrolyte, and maintains good performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005087545560000021
    Figure BDA0005087545560000021
  • Figure BDA0005087545560000031
    Figure BDA0005087545560000031
  • Figure BDA0005087545560000041
    Figure BDA0005087545560000041
Patent Text Reader

Abstract

The invention discloses an electrolyte and application thereof in a lithium ion battery, the electrolyte comprises an organic solvent, a lithium salt and an additive, the lithium salt comprises a lithium salt containing fluorine and phosphorus elements, and the additive comprises a silicon-based oxalate compound. In the electrolyte provided by the invention, the lithium salt can be respectively subjected to in-situ reaction with the bis (trimethylsilyl) oxalate compound and the hexamethyldisiloxane compound before formation to generate an oxalate phosphate compound and a fluorophosphate compound, and stable positive and negative electrode interface protection films are formed during formation, so that the performance of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion batteries and relates to an electrolyte and application thereof in lithium ion batteries. Background Art

[0002] In recent years, with the development of new energy technologies, lithium-ion power batteries for vehicles have put forward higher requirements on the performance of lithium-ion secondary batteries. In order to meet the long driving range and wide temperature range of electric vehicles, it is necessary to develop lithium-ion secondary batteries with higher energy density, better fast charging cycle and storage performance to meet the life requirements of more than 10 years for automotive power batteries. In addition, the development of fast-charging batteries with higher charging speed and high energy density has put forward higher requirements on the fast-charging performance of electrolyte materials.

[0003] In order to improve the power and life of lithium-ion batteries, a series of functional additives have been developed, among which lithium salt additives have the most outstanding performance, represented by lithium difluorophosphate, lithium monofluorophosphate, lithium difluorobisoxalate phosphate, and lithium difluorooxalate borate. However, these additives are difficult to synthesize and have high costs, which greatly increases the price of electrolytes and limits their applications.

[0004] Therefore, it is necessary to provide an electrolyte that has a lower preparation cost while improving the high temperature storage performance and fast charge cycle performance of the battery to facilitate its application. Summary of the invention

[0005] In view of the above technical problems existing in the prior art, the object of the present invention is to provide an electrolyte and its application in a lithium ion battery.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides an electrolyte, comprising an organic solvent, a lithium salt and an additive, wherein the lithium salt comprises a lithium salt containing fluorine and phosphorus elements, and the additive comprises a silicon-based oxalate compound.

[0008] In the electrolyte of the present invention, silicon-based oxalate compounds and lithium salts containing fluorine and phosphorus elements are added at the same time, and the two can react in situ before formation to generate oxalate phosphate compounds, and the in situ reaction generates different types of lithium salt additives. The oxalate and PF groups in the oxalate phosphate can form a low-impedance and dense protective film on the surface of the positive electrode and the negative electrode, inhibit the side reaction between the positive electrode and the electrolyte, increase the stability of the negative electrode SEI film, improve the high temperature performance and fast charging performance, the lithium ion battery has a high high temperature storage capacity retention rate, good fast charging cycle performance, low high temperature storage gas expansion rate, and low DC internal resistance.

[0009] The silicon-based oxalate compound raw material used in the electrolyte of the present invention has low cost. Compared with directly adding lithium salt additives, it not only ensures good performance but also greatly reduces the cost of the electrolyte.

[0010] For example, taking LiPF6 as an example, the mechanism of in-situ reaction between silicon-based oxalate compounds and lithium salts containing fluorine and phosphorus is described:

[0011]

[0012] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0013] Preferably, the lithium salt containing fluorine and phosphorus elements is lithium hexafluorophosphate.

[0014] Preferably, based on the mass of the electrolyte as 100%, the mass fraction of the lithium salt containing fluorine and phosphorus elements is 5-20%, for example, it can be 5%, 6%, 7%, 8%, 10%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%, etc.

[0015] Optionally, the lithium salt may also include other functional lithium salts, including at least one of lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), lithium perchlorate (LiClO4), lithium fluorosulfonate, lithium bis(oxalatoborate) (LiBOB) and lithium tetrafluoroborate (LiBF4).

[0016] In the present invention, other functional lithium salts are not essential components and may be added or not added, and those skilled in the art may select them according to their needs.

[0017] Preferably, the silicon-based oxalate compound comprises a compound represented by formula I;

[0018]

[0019] Wherein, R1-R6 are independently selected from any one of hydrogen, fluorine, C1-C10 alkyl, C6-C20 aromatic hydrocarbon, C2-C10 alkenyl or C2-C10 alkynyl, methoxy, ethoxy, cyano or sulfonate.

[0020] In the present invention, the C1-C10 alkyl group may be a C1, C2, C3, C4, C5, C6, C7, C8, C9 or C10 alkyl group, the C6-C20 aromatic hydrocarbon group may be a C6, C8, C10, C12, C14, C16, C18 or C20 aromatic hydrocarbon group, the C2-C10 alkenyl group may be a C2, C3, C4, C5, C6, C7, C8, C9 or C10 alkenyl group, and the C2-C10 alkynyl group may be a C2, C3, C4, C5, C6, C7, C8, C9 or C10 alkynyl group.

[0021] Preferably, R1-R6 are methyl groups. In this case, the silicon-based oxalate compound is a bis(trimethylsilyl)oxalate compound.

[0022] As a preferred technical solution of the electrolyte of the present invention, based on the mass of the electrolyte being 100%, the mass fraction of the silicon-based oxalate compound is a, the mass fraction of the lithium salt containing fluorine and phosphorus elements is m, and 0.005≤a / m≤0.5. For example, a / m can be 0.005, 0.01, 0.03, 0.05, 0.08, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45 or 0.5, etc., preferably 0.02≤a / m≤0.16.

[0023] As a preferred technical solution of the electrolyte of the present invention, the additive further includes a siloxane compound represented by formula II;

[0024]

[0025] Among them, R7-R 12 Any one independently selected from hydrogen, fluorine, C1-C10 alkyl, C6-C20 aromatic hydrocarbon, C2-C10 alkenyl or C2-C10 alkynyl, methoxy, ethoxy, cyano or sulfonate.

[0026] In the present invention, the sulfonate group may be, for example, -SO3CH3, -SO3C2H5, etc.

[0027] Preferably, R7-R 12 In this case, the siloxane compound is a hexamethyldisiloxane compound.

[0028] Siloxane compounds and lithium salts containing fluorine and phosphorus can react in situ before formation to generate fluorophosphate compounds, and different types of lithium salt additives are generated by the in situ reaction. The difluorophosphorous acid group (-POF2) in the fluorophosphate compounds can form a low-impedance and dense protective film on the surface of the positive electrode, inhibiting the side reaction between the positive electrode and the electrolyte, and improving high temperature performance and fast charging performance.

[0029] The siloxane compound raw material used in the electrolyte of the present invention has low cost. Compared with directly adding lithium salt additives, it not only ensures good performance but also greatly reduces the cost of the electrolyte.

[0030] For example, taking LiPF6 as an example, the mechanism of in-situ reaction between silicon-based oxalate compounds and lithium salts containing fluorine and phosphorus is described:

[0031]

[0032] Preferably, based on the mass of the electrolyte being 100%, the total mass fraction of the silicon-based oxalate compound and the siloxane compound is b, 0.005≤b / m≤0.5. Exemplarily, b / m may be 0.005, 0.01, 0.03, 0.05, 0.08, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45 or 0.5, etc., preferably 0.02≤b / m≤0.3.

[0033] Optionally, the additives also include other functional additives, which include any one or a combination of at least two of a cyclic carbonate compound containing an unsaturated bond, a halogen-substituted cyclic carbonate compound, a sulfate compound, a sulfite compound, a sultone compound, a nitrile compound, an aromatic compound, an isocyanate compound, a phosphazene compound, a cyclic anhydride compound, a phosphite compound, a phosphate compound or a borate compound.

[0034] In the present invention, other functional additives are not essential components and may be added or not, and those skilled in the art may select them according to their needs.

[0035] Preferably, the organic solvent comprises a carbonate solvent and / or a carboxylate solvent;

[0036] Preferably, the carbonate solvent includes any one or a combination of at least two of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC) or ethyl propyl carbonate;

[0037] Preferably, the carboxylic acid ester solvent includes any one of ethyl acetate (EA), ethyl propionate, methyl propionate, propyl propionate, etc., or a combination of at least two thereof.

[0038] In a second aspect, the present invention provides a lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the electrolyte is the electrolyte described in the first aspect.

[0039] The present invention does not limit the specific compositions of the positive electrode sheet, negative electrode sheet, and separator. Those skilled in the art can prepare them by referring to the methods disclosed in the prior art, or they can also be commercially available products.

[0040] In one embodiment, the positive electrode sheet includes at least one positive electrode material capable of intercalating and deintercalating lithium ions.

[0041] In one embodiment, the positive electrode material includes LiCoO2, LiNi x Co y Mn z O2 (where x + y + z = 1, 0 ≤ x ≤ 2, 0 ≤ y ≤ 2, 0 ≤ z ≤ 2), LiNi x Mn y O2 (where x + y = 1, 0 ≤ x ≤ 2, 0 ≤ y ≤ 2,), LiMn2O4, LiMnO2, Li2MnO4, Li 1+a Mn 1-x M x O2 (where M is selected from any one or a combination of at least two of Ni, Co, Mn, Al, Cr, Mg, Zr, Mo, V, Ti, 0 ≤ a < 0.2, 0 < x < 1), LiCo 1-x M x O2 (where M is selected from any one or a combination of at least two of Ni, Co, Mn, Al, Cr, Mg, Zr, Mo, V, Ti, 0 < x < 1), LiMn 1-x M x O4 (where M is selected from any one or a combination of at least two of Ni, Co, Mn, Al, Cr, Mg, Zr, Mo, V, Ti, 0 < x < 1) or Li2Mn 1-x O4 (0 < x < 1), or any one or more of them.

[0042] In one embodiment, the positive electrode material is a transition metal phosphate compound of lithium.

[0043] In one embodiment, the transition metal phosphate compound of lithium includes LiFePO4, LiMnPO4, LiCoPO4, LiFe 1-x M x PO4 (where M is selected from any one or a combination of at least two of Ni, Co, Mn, Al, Cr, Mg, Zr, Mo, V, Ti, 0 < x < 1.

[0044] In one embodiment, the negative electrode sheet includes at least one negative electrode material capable of intercalating and deintercalating lithium ions.

[0045] In one embodiment, the negative electrode material includes but is not limited to any one or a combination of at least two of soft carbon, hard carbon, artificial graphite, natural graphite, silicon-oxygen negative electrode material, silicon-carbon negative electrode material or metallic lithium.

[0046] In a third aspect, the present invention provides a method for preparing a lithium-ion battery, comprising: stacking a positive electrode, a negative electrode and a separator, winding or laminating to form a battery core, injecting the electrolyte described in the first aspect into the battery core, standing at high temperature, and forming to obtain the lithium-ion battery.

[0047] In the present invention, high-temperature standing refers to standing under heating conditions, and the heating temperature is higher than room temperature.

[0048] In the preparation process of lithium-ion batteries, since the electrolyte contains silicon-based oxalate compounds and lithium salts containing fluorine and phosphorus elements, the two react in situ during high-temperature standing to generate oxalate phosphate compounds. Furthermore, the electrolyte also includes siloxane compounds, and the siloxane compounds react in situ with lithium salts containing fluorine and phosphorus elements during high-temperature standing to generate fluorophosphate compounds.

[0049] In one embodiment, the charge is performed for the first time.

[0050] Preferably, the high temperature standing temperature is 40-65°C, for example, it can be 40°C, 42°C, 43°C, 44°C, 45°C, 46°C, 47°C, 48°C, 50°C, 52°C, 55°C, 57°C, 60°C, 61°C, 62°C, 63°C or 65°C, etc.

[0051] Preferably, the high-temperature standing time is 4-8 h, for example, it can be 4 h, 5 h, 5.5 h, 6 h, 6.5 h, 7 h, 7.5 h or 8 h.

[0052] Preferably, an alkaline solution is used to absorb the gas generated by the high-temperature standing, and the product is recovered and recycled.

[0053] In the present invention, during the high temperature standing process, gas may be generated. In this case, the gas may be discharged or absorbed by an alkaline solution, which is not specifically limited in the present invention and can be selected by those skilled in the art as needed.

[0054] In one embodiment, the alkaline solution is a NaOH solution, and the product generated after absorption is siloxane (such as hexamethyldisiloxane), which can be recycled.

[0055] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0056] Compared with the prior art, the present invention has the following beneficial effects:

[0057] (1) In the electrolyte of the present invention, a silicon-based oxalate compound and a lithium salt containing fluorine and phosphorus are added at the same time. The two can react in situ before formation to generate oxalate phosphate compounds, and the in situ reaction generates different types of lithium salt additives. The oxalate and PF groups in the oxalate phosphate can form a low-impedance and dense protective film on the surface of the positive electrode, inhibiting the side reactions between the positive electrode and the electrolyte, and improving high-temperature performance and fast-charging performance. The lithium-ion battery has a high high-temperature storage capacity retention rate, good fast-charging cycle performance, low high-temperature storage gas expansion rate, and low DC internal resistance. Furthermore, the electrolyte can also include siloxane compounds, which can further enhance the performance of the lithium-ion battery.

[0058] (2) The silicon-based oxalate compound raw materials and siloxane compound used in the electrolyte of the present invention are low in cost. Compared with directly adding lithium salt additives, it not only ensures good performance but also greatly reduces the cost of the electrolyte. DETAILED DESCRIPTION

[0059] The technical scheme of the present invention is further described below by specific implementation methods. Those skilled in the art should understand that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. In the following embodiments, bis(trimethylsilyl)oxalate compounds can be purchased from Aladdin reagent, Macklin reagent, Sigma-aldrich and other companies; hexamethyldisiloxane compounds can be purchased from Aladdin reagent, Macklin reagent, Sigma-aldrich and other companies.

[0060] Bis(trimethylsilyl)oxalate is abbreviated as Compound Ⅰ, hexamethyldisiloxane compounds are abbreviated as Compound Ⅱ, ethylene carbonate is abbreviated as EC, ethyl methyl carbonate is abbreviated as EMC, dimethyl carbonate is abbreviated as DMC, vinylene carbonate is abbreviated as VC, lithium difluorophosphate is abbreviated as LiPO2F2, lithium bis(fluorosulfonyl)imide is abbreviated as LiFSI, lithium perchlorate is abbreviated as LiClO4, lithium tetrafluoroborate is abbreviated as LiBF4, lithium bis(trifluorosulfonyl)imide is abbreviated as LiTFSI, vinyl sulfate is abbreviated as DTD, and acetonitrile is abbreviated as ACN.

[0061] Examples 1-12 and Comparative Examples 1-4

[0062] Provided is an electrolyte, comprising a lithium salt, an organic solvent and an additive, wherein the lithium salt comprises a first lithium salt and optionally other functional lithium salts, the additive comprises a first additive and optionally other functional additives, and the composition of the electrolyte is shown in Table 1. The contents thereof are all in mass percentage, based on the mass of the electrolyte. The cost of the electrolyte is shown in Table 2.

[0063] Table 1

[0064]

[0065]

[0066] (I) Battery production:

[0067] The positive electrode active material is lithium nickel cobalt manganese oxide (LiNi 0.6 Co 0.1 Mn 0.3 O2), conductive agent Super-P, and adhesive PVDF were dissolved in solvent N-methylpyrrolidone at a mass ratio of 94:3.0:3.0 and mixed evenly to form positive electrode slurry. The positive electrode slurry was evenly coated on the current collector aluminum foil with a coating amount of 18 mg / cm 2 , then dried at 85°C, cold pressed, trimmed, cut into pieces, and slit, and then dried at 85°C under vacuum conditions for 4 hours, and the tabs were welded to produce a positive electrode sheet for a lithium-ion secondary battery that meets the requirements;

[0068] The negative electrode active material hard carbon, conductive agent Super-P, thickener CMC, and binder SBR were dissolved in solvent deionized water at a mass ratio of 96.5:1.0:1.0:1.5 and mixed evenly to form a negative electrode slurry. The negative electrode slurry was evenly coated on the current collector copper foil with a coating amount of 8.3 mg / cm 2 , then dried at 85°C, cold pressed, trimmed, cut into pieces, and slit, and then dried at 110°C under vacuum conditions for 4 hours, and the tabs were welded to produce a negative electrode sheet for a lithium-ion secondary battery that meets the requirements;

[0069] The electrolyte, positive electrode sheet, negative electrode sheet and isolation film (PE film) obtained in Examples 1-12 and Comparative Examples 1-4 were laminated to form a battery with a thickness of 8 mm, a width of 60 mm, a length of 130 mm and a capacity of 2000 mAh, and then vacuum-baked at 85°C for 10 hours to remove moisture.

[0070] Inject 10g of electrolyte, let stand for 4h at room temperature, let stand for 4h at 60℃ (if gas is generated, discharge the gas or use sodium hydroxide solution to absorb the gas, and the product hexamethyldisiloxane generated after absorption can be recycled), and then let stand for 12h at room temperature. Then charge to 4.4V with a constant current of 0.1C (200mA), then charge at a constant voltage of 4.4V until the current drops to 0.05C (100mA), then discharge to 2.8V with a constant current of 0.1C (200mA), repeat the charge and discharge twice, and finally charge to 3.7V with a constant current of 0.1C (200mA) to obtain a lithium-ion battery.

[0071] (ii) Storage performance test, cycle performance test, high temperature storage gas generation and DC internal resistance test were performed on lithium ion batteries assembled using the electrolytes of Examples 1-13 and Comparative Examples 1-3.

[0072] (1) Storage performance test method:

[0073] At 25°C, the prepared lithium ion secondary batteries are first charged to 4.4V with a constant current of 1C, further charged to a current of 0.05C with a constant voltage of 4.4V, and then discharged to 2.8V with a constant current of 1C. The discharge capacity is the discharge capacity of the lithium ion secondary battery before high-temperature storage; the lithium ion secondary battery is then charged to 4.4V with a constant current of 1C, and the lithium ion secondary battery is stored at 60°C for 30 days. After the storage is completed, the lithium ion secondary battery is placed in a 25°C environment, and then discharged to 2.8V with a constant current of 0.5C. Thereafter, the lithium ion secondary battery is charged to 4.4V with a constant current of 1C, further charged to a current of 1C with a constant voltage of 4.4V, and then discharged to 2.8V with a constant current of 1C. The last discharge capacity is the discharge capacity of the lithium ion secondary battery after high-temperature storage. Capacity retention rate (%) of lithium ion secondary battery after high temperature (60° C.) storage=[discharge capacity of lithium ion secondary battery after high temperature storage / discharge capacity of lithium ion secondary battery before high temperature storage]×100%.

[0074] (2) Cyclic performance test method:

[0075] The fast charge cycle performance of the prepared lithium-ion secondary battery was tested respectively. The specific method was as follows: at 45°C, the lithium-ion secondary battery was first charged to 4.4V at a constant current of 4C (8000mA), then charged to a current of 0.05C at a constant voltage of 4.4V, and then discharged to 2.8V at a constant current of 1C (2000mA). This is a charge and discharge cycle process, and the discharge capacity this time is the discharge capacity C1 of the first cycle. The lithium-ion secondary battery was subjected to a cyclic charge and discharge test in the above manner, and the discharge capacity C of the 800th cycle was taken. 800 . 4C fast charge cycle capacity retention rate = (%) = [C 800 / C1]×100%.

[0076] (3) High temperature storage gas production test:

[0077] After the high-temperature storage test, the lithium-ion battery is stored at 60°C for 30 days. After the storage is completed, the lithium-ion secondary battery is placed in a 25°C environment, and the volume of the battery is tested by the drainage method, and the thickness of the battery is measured with a micrometer. The lithium-ion secondary battery is then discharged to 2.8V at a constant current of 0.5C, and then charged to 4.4V at a constant current of 1C, and further charged to a current of 1C at a constant voltage of 4.4V, and then discharged to 2.8V at a constant current of 1C. The last discharge capacity is the discharge capacity of the lithium-ion secondary battery after high-temperature storage. The gas expansion rate after 30 days of storage at 60°C = (volume after storage / volume before storage - 1)%.

[0078] (4) DC internal resistance test:

[0079] At 25°C, the lithium ion secondary batteries prepared in the embodiment and the comparative example are first charged to 4.4V at a constant current of 1C, and then further charged at a constant voltage of 4.4V to a current of 0.05C, and then discharged at a constant current of 0.5C for 1 hour, and the charge of the battery is maintained at 50% SOC. After standing for 10 minutes, the voltage V1 is recorded. At this time, the battery is discharged at a current of I (I = 5C) for 10 seconds, and the discharge termination voltage V2 is recorded. The calculation formula of the discharge DC internal resistance DCIR of the battery is: DCIR = (V1-V2) / I, in units of mΩ.

[0080] The test results are shown in Table 2:

[0081] Table 2

[0082]

[0083]

[0084] As can be seen from Table 1, it can be obtained from Examples 1 to 6 that in the electrolyte, a silicon-based oxalate compound and a lithium salt containing fluorine and phosphorus are used together. After standing at high temperature before formation, a lithium salt-type additive is generated in situ, and a dense positive electrode interface protective film is generated during formation, which greatly improves the cycle and storage performance of the battery and reduces the internal resistance. The internal resistance is below 18mΩ, the 60°C storage capacity retention rate is above 88%, the 4C fast charge cycle capacity retention rate is above 89%, and the gas expansion rate of 60°C storage for 30 days is below 27%. Moreover, the cost of the electrolyte is low, and the cost of the electrolyte is below 23 yuan / kg. In Comparative Example 1, since the first additive is not added, the internal resistance increases, the gas production is large during high-temperature storage, and the cycle performance and storage performance are reduced. In Comparative Example 3, the lithium salt containing fluorine and phosphorus elements is replaced by LiTFSI, resulting in a decrease in the cycle and storage performance of the battery.

[0085] From the comparison between Example 1 and Comparative Example 2, it can be seen that compared with the direct addition of the lithium salt additive lithium difluorobis(oxalyl)phosphate, the overall performance of the battery is basically the same and the cycle performance is slightly better, but the electrolyte cost is reduced by 10 yuan / kg, indicating that after adding the low-cost bis(trimethylsilyl) oxalate additive, after a high-temperature in-situ reaction process, the effect of directly adding a lithium salt additive can be achieved and the cost can be effectively reduced.

[0086] By comparing Example 1 with Comparative Example 4, it can be seen that if a siloxane compound is used to replace the silicon-based oxalate compound in Example 1, the cycling and storage performance of the battery will be reduced, indicating that the performance of the silicon-based oxalate compound is better than that of the siloxane in Comparative Example 4.

[0087] By comparing Example 1 with Example 2, it can be seen that the combination of a siloxane compound and a silicon-based oxalate compound can better form a protective film at the interface of the positive electrode and the negative electrode, inhibit side reactions, and thus help improve the performance of lithium-ion batteries, compared to a single silicon-based oxalate compound.

[0088] By comparing Example 1 with Examples 7-8, it can be seen that when the content of bis(trimethylsilyl)oxalate of Compound I is too low, the film-forming effect is insufficient and the battery performance is deteriorated. When the content is too high, the film is too thick and difficult to dissolve, which increases the internal resistance of the battery and reduces the performance.

[0089] By comparing Example 1 with Examples 9-10, it can be seen that when the content of the siloxane compound of Formula II is too low, the film-forming effect is insufficient and the battery performance is deteriorated. When the content is too high, the film is too thick and difficult to dissolve, which increases the internal resistance of the battery and reduces the performance.

[0090] By comparing Example 3 with Examples 11-12, it can be seen that when the mass fraction a of the silicon-based oxalate compound, the total mass fraction b of the silicon-based oxalate compound and the siloxane compound, and the mass fraction m of lithium hexafluorophosphate satisfy 0.02≤a / m≤0.16 and 0.02≤b / m≤0.3, it is more conducive to reducing the internal resistance and reducing the gas production during high-temperature storage, thereby improving the performance of the battery.

[0091] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

[0092] The applicant declares that the present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. An electrolyte, characterized in that: The electrolyte includes an organic solvent, a lithium salt and an additive, wherein the lithium salt includes a lithium salt containing fluorine and phosphorus elements, and the additive includes a silicon-based oxalate compound.

2. The electrolyte according to claim 1, characterized in that The lithium salt containing fluorine and phosphorus elements is lithium hexafluorophosphate; Preferably, based on the mass of the electrolyte being 100%, the mass fraction of the lithium salt containing fluorine and phosphorus elements is 5-20%; Preferably, the lithium salt further includes other functional lithium salts, and the other functional lithium salts include at least one of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium perchlorate, lithium fluorosulfonate, lithium bis(oxalatoborate) and lithium tetrafluoroborate.

3. The electrolyte according to claim 1 or 2, characterized in that The silicon-based oxalate compound includes a compound represented by formula I; Wherein, R1-R6 are independently selected from any one of hydrogen, fluorine, C1-C10 alkyl, C6-C20 aromatic hydrocarbon, C2-C10 alkenyl or C2-C10 alkynyl, methoxy, ethoxy, cyano or sulfonate; Preferably, R1-R6 are methyl groups.

4. The electrolyte according to any one of claims 1 to 3, characterized in that Based on the mass of the electrolyte being 100%, the mass fraction of the silicon-based oxalate compound is a, the mass fraction of the lithium salt containing fluorine and phosphorus elements is m, and 0.005≤a / m≤0.5, preferably 0.02≤a / m≤0.

16.

5. The electrolyte according to any one of claims 1 to 4, characterized in that The additive also includes a siloxane compound shown in formula II; Among them, R7-R 12 Any one independently selected from hydrogen, fluorine, C1-C10 alkyl, C6-C20 aromatic hydrocarbon, C2-C10 alkenyl or C2-C10 alkynyl, methoxy, ethoxy, cyano or sulfonate; Preferably, R7-R 12 is methyl; Preferably, based on 100% of the mass of the electrolyte, the total mass fraction of the silicon-based oxalate compound and the siloxane compound is b, 0.005≤b / m≤0.5, preferably 0.02≤b / m≤0.

3.

6. The electrolyte according to claim 5, characterized in that The additives also include other functional additives, which include any one or a combination of at least two of cyclic carbonate compounds containing unsaturated bonds, halogen-substituted cyclic carbonate compounds, sulfate compounds, sulfite compounds, sultone compounds, nitrile compounds, aromatic compounds, isocyanate compounds, phosphazene compounds, cyclic anhydride compounds, phosphite compounds, phosphate compounds or borate compounds.

7. The electrolyte according to any one of claims 1 to 6, characterized in that: The organic solvent includes a carbonate solvent and / or a carboxylate solvent; Preferably, the carbonate solvent includes any one of ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate or ethyl propyl carbonate, or a combination of at least two thereof; Preferably, the carboxylate solvent includes any one of ethyl acetate, ethyl propionate, methyl propionate, propyl propionate, etc., or a combination of at least two thereof.

8. A lithium ion battery comprising a positive electrode, a negative electrode, a separator and an electrolyte, characterized in that: The electrolyte is the electrolyte according to any one of claims 1 to 7.

9. A method for preparing a lithium ion battery, characterized in that: include: The positive electrode sheet, the negative electrode sheet and the separator are stacked, wound or laminated to form a battery core, and the electrolyte described in any one of claims 1 to 7 is injected into the battery core. After standing at high temperature, the electrolyte is formed to obtain the lithium-ion battery.

10. The method for preparing a lithium ion battery according to claim 9, characterized in that: The high temperature static temperature is 40-65°C; Preferably, the high temperature standing time is 4-8h; Preferably, an alkaline solution is used to absorb the gas generated by the high-temperature standing, and the product is recovered and recycled.

Citation Information

Patent Citations

  • Electrolyte for non-aqueous electrolyte battery, and non-aqueous electrolyte battery using same

    CN104380517A

  • Nonaqueous electrolyte compositions comprising silyl oxalates

    CN109643827A

  • Preparation method of lithium difluorobisoxalate phosphate solution

    CN109742447A

  • Synthetic method of oxalate lithium phosphate salt compound

    CN111943985A

  • Electrolyte and lithium ion battery containing same

    CN115020806A