Heat-shrinkable polyester film
By optimizing the composition and process of ethylene terephthalate film, combined with recycling and particle addition, the problems of low-temperature heat seal strength and automatic installation suitability are solved, and high-efficiency and environmentally friendly heat shrinkable polyester films are achieved. .
Patent Information
- Application Number
- CN202380029330.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-25
- Filing Date
- 2023-03-13
- Publication Date
- 2024-11-26
AI Technical Summary
The existing heat shrinkable polyester films have insufficient heat sealing strength at low temperatures, and the heat shrinkage rate in the width direction is not high enough, and it is difficult to take into account both the installation suitability and environmental friendliness of automatic machinery.
The heat-shrinkable polyester film with ethylene terephthalate as the main component is ensured that the width direction ring stiffness, heat shrinkage, heat seal strength and wetting tension are within the optimized range through specific component ratios and process treatment. , and use a recycled PET bottle for mechanical or chemical recycling, adding an appropriate amount of particles to improve slippage.
It realizes high heat seal strength at low temperature, high heat shrinkage rate in width and suitability for automatic mechanical installation, while taking into account environmental friendliness, improving the ring stiffness and heat seal strength of the film, and reducing production costs.
Smart Images

Figure CN119032123A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a heat-shrinkable polyester film having excellent heat-sealing properties, a label, and a package. Specifically, the present invention relates to a ring-shaped label suitable for noodle containers and the like in convenience stores and the like, and particularly to a label having excellent environmental compatibility and compatibility with automatic mounting machines. Background Art
[0002] In recent years, stretched films (so-called heat shrinkable films) formed of polyvinyl chloride resins, polystyrene resins, polyester resins, etc. have been increasingly widely used in label packaging for glass bottles, PET bottles, etc. that serves both protection and product display, bundle packaging for the purpose of fixing containers and lids of convenience store lunch boxes, and label packaging. Among such heat shrinkable films, polyvinyl chloride films have the following problems: not only do they have low heat resistance, but they also produce hydrogen chloride gas when burned, which causes dioxins. In addition, polystyrene films have the following problems: not only do they have poor solvent resistance, but they must use inks of special composition when printing, and they must be burned at high temperatures, which are accompanied by a foul odor and produce a large amount of black smoke when burned. Therefore, polyester heat shrinkable films that have high heat resistance, are easy to burn, and have excellent solvent resistance are increasingly widely used as shrink labels, and there is a tendency for their use to increase.
[0003] In recent years, the number of pre-cooked noodles such as udon and ramen noodles has been increasing in convenience stores, and a packaging method (so-called label packaging) has been adopted in which the pre-cooked noodles and other contents are placed in a deep plastic container, covered with a lid from the top, and the container and the lid are fixed from the top and bottom by an annular shrink film. As heat-shrinkable polyester films, those that shrink greatly in the width direction are widely used. When used as a label film for bottles or a label for bento, the film is formed into a ring, installed on the bottle or bento container, and then heat-shrunk to complete the product. As an example of making an annular label, the shrink film rolled out from the film roll is cut in the width direction, and the two ends of the cut film are bonded. When the two ends of the film are bonded (making an annular label), the process of covering the packaged object (noodle container, etc.) is often simultaneous. The annular film thus made is heated and shrunk by hot air or the like, so that it fits tightly with the packaged object and becomes a label that fixes the container and the lid.
[0004] As a property of a heat shrinkable film with a label, the ability to follow the container based on shrinkage is of course important, but in addition, it is also necessary that the bonded portion does not peel off. As a bonding method, heat sealing of the film itself is widely used. In the past, as a technology to prevent the heat-sealed portion from peeling off, methods such as improving the heat seal strength or reducing the shrinkage stress have gradually been adopted.
[0005] For example, Patent Document 1 discloses a polyester heat shrinkable film that shrinks along the length direction of a roll using a monomer that becomes an amorphous component. However, the film of Patent Document 1 cannot achieve the required heat seal strength at the current technical level. In recent years, in order to improve the yield rate when manufacturing labels, the equipment has been accelerated and the heat seal time has been reduced. In conjunction with this, the film is required to have a high heat seal strength at a lower temperature.
[0006] In contrast, Patent Document 2 discloses a film that reduces the degree of plane orientation by uniaxial stretching, thereby increasing the heat seal strength and reducing the shrinkage stress, thereby suppressing the peeling of the heat seal portion. However, the film of Patent Document 2 is uniaxially stretched, so the final area stretch ratio (vertical × horizontal) of the film will be lower, and there is room for improvement in productivity. As pointed out in Patent Document 2, when it is desired to improve productivity by biaxial stretching, it becomes inevitable to avoid the peeling of the seal portion due to the reduction in heat seal strength and the increase in shrinkage stress.
[0007] In addition to the above, heat shrinkable films used in labels require opposite characteristics such as thin-walled and stiff. Regarding the former, with the increase in environmental awareness in recent years, not only the business operators involved in the entire supply chain including retailers / food manufacturers, but also consumers have the desire to save packaging materials as much as possible. On the other hand, in recent years, the automation of food packaging machines has been particularly promoted in order to not only improve efficiency but also eliminate labor shortages, and the film is also required to be suitable for installation on automatic machines. The suitability for installation on machines in labels refers to the following characteristics: in the process of cutting the above-mentioned film in the width direction and heat-sealing it into a ring shape, for example, the film can be accurately held on the robot arm, or the film is loose on the high-speed moving label production line. These characteristics are closely related to the stiffness of the film, and there is a dilemma that the stiffness, that is, the suitability for installation on the machine, decreases as the aforementioned thinning is promoted.
[0008] In addition, Patent Document 3 describes a method for improving alkali-leaving properties when laminating an alkali-leaving skin layer on a film by subjecting the film to a predetermined surface treatment. However, this technique only slightly improves heat-sealing properties and does not have a sufficient effect.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent No. 4411556
[0012] Patent Document 2: Japanese Patent No. 6988440
[0013] Patent Document 3: Japanese Patent Application Publication No. 2004-139067
[0014] Non-patent literature
[0015] Non-patent document 1: A.Mahendrasingam et al "Effect of draw ratio and temperature on the strain induced crystallization of poly(ethyleneterephthalate)at fast draw rates" Polym.40 5556 (1999) Summary of the invention
[0016] Problem that the invention aims to solve
[0017] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a heat-shrinkable polyester film having excellent heat-sealing strength at low temperatures, high heat shrinkage in the width direction, and achieving both suitability for installation in automatic machinery and response to environmental issues.
[0018] Solutions for solving problems
[0019] The present inventors have conducted research to solve the above-mentioned problems. As a result, the present invention is configured as follows.
[0020] 1. A heat-shrinkable polyester film, characterized in that it contains ethylene terephthalate as a main component and satisfies the following conditions (1) to (4).
[0021] (1) Ring stiffness in the width direction is 6 mN / 25 mm or more and 200 mN / 25 mm or less
[0022] (2) The heat shrinkage rate in the width direction when shrinking in hot water at 80°C for 10 seconds is 20% or more and 70% or less
[0023] (3) When one side of the film is heat-sealed with the other side at a temperature of 140°C and a pressure of 0.1 MPa for 1 second, the strength of the film when peeled off in a shear test in the width direction is 20 N / 15 mm or more and 80 N / 15 mm or less
[0024] (4) The wetting tension of at least one outermost layer is 40 mN / m or more and 55 mN / m or less
[0025] 2. The heat-shrinkable polyester film according to 1., wherein the reversible heat capacity difference from 25°C to 140°C measured by a temperature modulation differential scanning calorimeter is 0.4 J / g·K or more and 1.4 J / g·K or less.
[0026] 3. A heat-shrinkable polyester film according to any one of 1. or 2., characterized in that the proportion of oxygen atoms on the film surface obtained from the peak of 285-290 eV in the C1s spectrum of X-ray photoelectron spectroscopy (ESCA) is greater than 27% and less than 31% in at least one outermost layer.
[0027] 4. The heat-shrinkable polyester film according to any one of 1. to 3., which has a thickness of 20 μm to 50 μm.
[0028] 5. The heat-shrinkable polyester film according to any one of 1. to 4., characterized in that the polyester constituting the film contains 1 mol % to 30 mol % of any one of isophthalic acid, neopentyl glycol, 1,4-cyclohexanedimethanol, butanediol, and diethylene glycol.
[0029] 6. The heat-shrinkable polyester film according to any one of 1. to 5., wherein a polyester raw material obtained by mechanically recycling and / or chemically recycling PET bottles is used as a raw material constituting the film.
[0030] 7. A label, characterized in that it is a ring-shaped label using the heat-shrinkable polyester film described in any one of 1. to 6. above in at least a part, the heat-shrinkable polyester film itself is bonded to each other or to other films, and the strength when the adhesive portion is peeled off in a shear test is greater than 20N / 15mm and less than 80N / 15mm.
[0031] Effects of the Invention
[0032] According to the present invention, it is possible to provide a heat-shrinkable polyester film which has excellent heat-sealing strength at low temperatures, a high heat shrinkage rate in the width direction, and which achieves both suitability for installation in automatic machinery and response to environmental issues. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 Schematic diagram for making the horizontal stretching by the tenter machine a single-stage stretching
[0034] Figure 2 Schematic diagram for making the transverse stretching by the tenter machine into three-stage stretching
[0035] Figure 3 Schematic diagram for measuring heat seal strength so that the peeling direction is the shear direction DETAILED DESCRIPTION
[0036] 1. Polyester raw materials used in heat shrinkable polyester films
[0037] The polyester used in the heat-shrinkable polyester film of the present invention has ethylene terephthalate units as main constituents, and the ethylene terephthalate units account for preferably 50 mol% or more, more preferably 55 mol% or more, and further preferably 60 mol% or more of 100 mol% of the constituent units of the polyester.
[0038] Examples of other dicarboxylic acid components constituting the polyester of the present invention include aromatic dicarboxylic acids such as isophthalic acid, phthalic acid, and 2,6-naphthalenedicarboxylic acid, aliphatic dicarboxylic acids such as adipic acid, azelaic acid, sebacic acid, and decanedicarboxylic acid, and alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid. Among these, isophthalic acid and phthalic acid are preferred.
[0039] When an aliphatic dicarboxylic acid (for example, adipic acid, sebacic acid, decanedicarboxylic acid, etc.) is contained in the polyester, the content is preferably less than 3 mol % (in 100 mol % of the dicarboxylic acid component).
[0040] In addition, it is preferred that the polyester does not contain a trivalent or higher polycarboxylic acid (eg, trimellitic acid, pyromellitic acid, and anhydrides thereof). In a heat-shrinkable polyester film obtained using a polyester containing such a polycarboxylic acid, it becomes difficult to achieve a desired high shrinkage ratio.
[0041] Examples of other diol components constituting the polyester of the present invention include alicyclic diols such as neopentyl glycol and 1,4-cyclohexanedimethanol, aliphatic diols such as 1,4-butanediol, diethylene glycol, 1,3-propylene glycol, and hexanediol, and aromatic diols such as bisphenol A. Among the above, neopentyl glycol, 1,4-cyclohexanedimethanol, 1,4-butanediol, and diethylene glycol are preferred.
[0042] The constituent components of the above-mentioned polyester preferably contain at least one selected from isophthalic acid, neopentyl glycol, 1,4-cyclohexanedimethanol, butanediol, and diethylene glycol in a total amount of 1 mol% or more and 50 mol% or less. If the total amount of these components is less than 1 mol%, it becomes difficult to make the heat shrinkage and heat sealing strength within the prescribed range, so it is not preferred. On the other hand, if the total amount of these components exceeds 50 mol%, although the thin-walling as the main purpose of the present invention is achieved, it becomes difficult to keep the ring stiffness as an indicator of stiffness at more than 6mN / 25mm. The total amount of the above-mentioned components is more preferably more than 5 mol% and less than 45 mol%, and further preferably more than 10 mol% and less than 40 mol%. The particularly preferred upper limit is less than 30 mol%.
[0043] In addition to the polyester raw material having the above-mentioned constituent components, a polyester elastomer may also be used in the film of the present invention. By using a polyester elastomer, the reversible thermal tolerance (ΔCp) of the film described later can be reduced, so it is preferred. Examples of the polyester elastomer include a copolymer of ε-caprolactone and 1,4-butanediol, polytetramethylene glycol, and the like.
[0044] Furthermore, for the purpose of environmental response of the present invention, in addition to the above polyester raw materials, it is also a preferred solution to use polyester raw materials that are recycled from used waste such as plastic bottles. For example, as polyester resins that are recycled plastic bottles, there can be mentioned: polyester resins obtained by a physical recycling method (hereinafter sometimes referred to as mechanically recycled polyester resins), wherein the used plastic bottles collected from the market and society are screened, crushed, and washed, and the dirt and foreign matter on the surface are fully removed, and then exposed to high temperatures to highly clean the pollutants and the like that remain inside the resin, and then pelletized again; and polyester resins obtained by decomposing the polyester resin contained in the used packaging container to the monomer level, removing the pollutants and the like, and polymerizing again (hereinafter sometimes referred to as chemically recycled polyester resins).
[0045] The main recycled raw materials that can be preferably used in the present invention are recycled products of containers with polyethylene terephthalate as the main body, for example, recycled products of beverage containers for tea beverages, refreshing drinks, etc. can be preferably used, which can be appropriately oriented, preferably colorless, and can also contain some coloring components.
[0046] The raw materials recycled from the market and society, including the plastic bottles that can be preferably utilized, are polyesters manufactured and molded by conventional polymerization methods and solid phase polymerization methods, preferably with polyethylene terephthalate as the main body, and may also contain other polyester components and copolymer components. Metal compounds such as antimony, germanium, and titanium as catalysts, and phosphorus compounds as stabilizers may be contained. In polyesters commonly used for plastic bottles, germanium is often used as a catalyst. If it is made into a film using recycled raw materials from plastic bottles, more than 1 ppm of germanium will be contained in the film. However, it is ultimately the content of the catalyst, so it is usually at most 100 ppm or less, and generally 50 ppm or less.
[0047] The polyester raw material used in the present invention may be added with various additives as needed. The additives are not particularly limited, and examples thereof include waxes, antioxidants, antistatic agents, crystal nucleating agents, thickeners, heat stabilizers, coloring pigments, anti-coloring agents, ultraviolet absorbers and other known additives.
[0048] In addition, the polyester raw material is preferably added with particles that act as a lubricant to make the workability (slippery) of the film good. As the above-mentioned particles, any type of inorganic particles and organic particles can be selected. As inorganic particles, for example, silica, alumina, titanium dioxide, calcium carbonate, kaolin, barium sulfate, etc. can be cited. As organic particles, for example, acrylic resin particles, melamine resin particles, silicone resin particles, cross-linked polystyrene particles, etc. can be cited. When the average particle size of the above-mentioned particles is measured with a Coulter counter, it is preferably in the range of about 0.05 to 3.0 μm. If the particle size is less than 0.05 μm, there is a concern that the slippery properties required for operation will not be satisfied. On the other hand, if the particle size exceeds 3.0 μm, the particles will aggregate / coarsen excessively and become foreign matter, and there is a concern that the appearance quality will be extremely poor. The particle size is more preferably 0.06 μm or more and 2.99 μm or less, and further preferably 0.07 μm or more and 2.98 μm or less. The amount of fine particles added is preferably within a range of 100 to 4000 ppm relative to the film.
[0049] The method of blending the microparticles into the polyester raw material is not particularly limited. For example, the microparticles may be added at any stage of the production of the polyester resin, but preferably added as a slurry dispersed in ethylene glycol or the like at the stage of esterification or after the end of the transesterification reaction and before the start of the polycondensation reaction to promote the polycondensation reaction. Alternatively, the method may be carried out by a method such as a method of blending a slurry of microparticles dispersed in ethylene glycol or water or the like with the polyester resin raw material using a kneading extruder with a vent, or a method of blending dried microparticles with the polyester resin raw material using a kneading extruder.
[0050] 2. Characteristics of the heat-shrinkable polyester film of the present invention
[0051] (1) Ring stiffness
[0052] The ring stiffness of the film of the present invention in the width direction must be 6mN / 25mm or more and 200mN / 25mm or less. Ring stiffness is an index indicating the stiffness of the film, and the lower the value, the less stiff it is. If the ring stiffness is lower than 6mN / 25mm, it becomes easy to cause poor installation when the film is heat-sealed with an installation machine, so it is not preferred. If the ring stiffness exceeds 200mN / 25mm, it is not preferred because consumers find it difficult to open the sealed label or it becomes easy to hurt their hands with the film. The ring stiffness is preferably 8mN / 25mm or more and 198mN / 25mm or less, and more preferably 10mN / 25mm or more and 196mN / 25mm or less.
[0053] (2) Thermal shrinkage
[0054] The film of the present invention must have a heat shrinkage rate in the width direction when it shrinks in hot water at 80°C for 10 seconds of 20% or more and 70% or less. Here, "width direction" refers to the direction orthogonal to the length direction (machine direction, Machine Direction; MD), also known as transverse direction (Transverse Direction; TD). If the heat shrinkage rate in the width direction at 80°C is less than 20%, the film will not shrink enough when shrinking to the object, and it will not fit perfectly, resulting in poor appearance, so it is not preferred. On the other hand, if the heat shrinkage rate in the width direction at 80°C exceeds 70%, there is a tendency for the shrinkage stress to increase during shrinkage, and there is a concern that the shrinkage stress will become more than MPa, so it is not preferred. The heat shrinkage rate in the width direction at 80°C is preferably 25% or more and 65% or less, more preferably 30% or more and 60% or less.
[0055] (3) Heat seal strength
[0056] The film of the present invention must have a strength of 20N / 15mm or more and 80N / 15mm or less when one side of the film is heat-sealed with the other side at a temperature of 140°C, a pressure of 0.1MPa, and 1 second, and peeled in a shear test. The value of the heat seal strength when peeled in a shear test shows a value different from the value when measured under the usual 90-degree peeling or 180-degree peeling. The inventors found that the value of the heat seal strength measured by this method becomes an indicator of the unsealing property of the label. If the heat seal strength is less than 20N / 15mm, the label will be easily unsealed, so it is not preferred. On the other hand, if the heat seal strength is more than 80N / 15mm, there is a concern that consumers will feel it is difficult to open when opening the label, so it is not preferred. The heat seal strength is preferably more than 25N / 15mm and less than 75N / 15mm, and more preferably more than 30N / 15mm and less than 70N / 15mm.
[0057] (4) Wetting tension
[0058] The wetting tension of at least one outermost layer of the film of the present invention must be 40mN / m or more and 55mN / m or less. By making the wetting tension of the outermost layer of the film 40mN / m, it becomes easy to make the above-mentioned heat seal strength 20N / 15mm or more. If the wetting tension is lower than 40mN / m, it becomes difficult to make the above-mentioned heat seal strength 20N / 15mm, so it is not preferred. On the other hand, if the wetting tension exceeds 55mN / 15mm, the surfaces of the film will adhere to each other during the period when the film is made into a roll and stored in a warehouse, etc., and it will become easy to cause adhesion. If adhesion occurs, it becomes easy to break when the film is unrolled from the roll, so it is not preferred. The wetting tension is preferably 41mN / 15mm or more and 54mN / 15mm or less, more preferably 42mN / 15mm or more and 53mN / 15mm or less.
[0059] (5) Reversible thermal tolerance (ΔCp)
[0060] The film of the present invention preferably has a reversible thermal capacity difference (hereinafter sometimes referred to as ΔCp) of 0.4 J / g·K or more and 1.4 J / g·K or less when measured from 25°C to 140°C using a temperature modulation differential scanning calorimeter (temperature modulation DSC). The correlation between ΔCp and heat seal strength is described below.
[0061] The high-order structure of polyester is roughly divided into two types: crystal and amorphous. In recent years, it is believed that amorphous molecules can be further divided into rigid amorphous and flexible amorphous according to their mobility. It is believed that flexible amorphous molecules move at the glass transition temperature (Tg) and belong to the amorphous molecules previously considered. The existence rate of flexible amorphous can be quantified by finding the reversible heat capacity difference before and after the start of glass transition from the reversible heat capacity curve measured in the heating mode based on temperature modulation DSC. Rigid amorphous is expected to exist between flexible amorphous and crystalline, and its mobility is also believed to be between flexible amorphous and crystalline. Rigid amorphous is considered to be a molecule that does not reflect glass transition, unlike flexible amorphous. However, the value of reversible heat capacity shows a slow rise from the glass transition to the melting point, so it is believed that rigid amorphous becomes flexible amorphous in the temperature range of glass transition and thereafter. From the above, it is believed that flexible amorphous and rigid amorphous move due to heat sealing, so that the heat sealing surfaces are tightly attached to each other, reflecting the heat sealing strength. In addition, in actual measurement data, the reversible heat capacity often increases at lower temperatures than the glass transition temperature (glass state). The mechanism is unclear, but it is believed that the change in reversible heat capacity at Tg from room temperature is also related to the manifestation of heat seal strength.
[0062] Therefore, the inventors of the present invention captured the reversible thermal capacity difference that increased from room temperature to heat sealing temperature as the sum of the changes in the flexible amorphous and rigid amorphous materials, and studied the relationship with the heat sealing strength. As a result, they found that by controlling the changes in the flexible amorphous and rigid amorphous materials within the specified ranges, appropriate heat sealing strength and heat resistance can be ensured.
[0063] By setting ΔCp to 0.4 J / g·K or more, it becomes easy to set the heat seal strength to 20 N / 15 mm or more. On the other hand, if ΔCp exceeds 1.4 J / g·K, the heat seal strength is improved, which is preferred, but there is a concern that the strength required for the film may be insufficient, so it is not preferred. ΔCp is more preferably 0.45 J / g·K or more and 1.35 J / g·K or less, and further preferably 0.5 J / g·K or more and 1.3 J / g·K or less.
[0064] The film forming method and conditions for making ΔCp fall within a preferred range will be described later.
[0065] (6) Thickness
[0066] The thickness of the film of the present invention is preferably 20 μm or more and 50 μm or less. By making the thickness 20 μm or more, it is easy to make the ring stiffness 6 mN / 25 mm or more, so it is preferred. On the other hand, if the film exceeds 50 μm, not only the ring stiffness becomes easy to exceed 200 mN / 25 mm, but also it becomes difficult to contribute to the environmental response (resource saving based on thin-walling) which is the main purpose of the present invention, so it is not preferred. The thickness is more preferably 22 μm or more and 48 μm or less, and further preferably 24 μm or more and 46 μm or less.
[0067] (7) Thermal shrinkage in the longitudinal direction
[0068] The film of the present invention preferably has a heat shrinkage rate in the longitudinal direction (machine direction, MD) when immersed in hot water at 80°C for 10 seconds of not less than -5% and not more than 8%. If the heat shrinkage rate in the longitudinal direction at 80°C is less than -5%, excessive elongation occurs when shrinking toward the object, wrinkles are easily formed, and a good shrinkage appearance cannot be obtained, so it is not preferred. On the other hand, if the heat shrinkage rate in the longitudinal direction at 80°C exceeds 8%, strain and shrinkage holes become easy to occur after shrinkage, so it is not preferred. The heat shrinkage rate in the longitudinal direction at 80°C is preferably not less than -4% and not more than 7%, more preferably not less than -3% and not more than 6%.
[0069] (8) Glass transition temperature (Tg)
[0070] The Tg of the film of the present invention is preferably 50°C or more and 100°C or less. If the Tg is lower than 50°C, it is not preferred because sticking is likely to occur when the film is stored as a roll. On the other hand, if the Tg exceeds 100°C, it is difficult to make ΔCp above 0.4 J / g·K and the above-mentioned heat seal strength 20N / 15mm. As mentioned above, the present invention assumes that ΔCp is related to the heat seal strength, and ΔCp is closely related to Tg. In the case of heat sealing with an actual installation machine, it can be said that even if the temperature of the sealing rod is as set, the temperature applied to the film is lower than the setting when sealing is performed at a high speed (for example, 1 second). Therefore, if the Tg of the film exceeds 100°C, the film will not undergo devitrification when heat sealing is performed at a low temperature / high speed (for example, 140°C·1 second), and it is difficult to make ΔCp above 0.4 J / g·K. Tg is more preferably 55°C or more and 95°C or less, and further preferably 60°C or more and 90°C or less.
[0071] (9) Intrinsic viscosity IV
[0072] The IV of the film of the present invention is preferably 0.6 dL / g or more and 1.2 dL / g or less. If the IV is less than 0.6 dL / g, not only the minimum mechanical strength required for the film becomes insufficient, but also it becomes easy to cause breakage when the film is made into a film. On the other hand, if the IV exceeds 1.2 dL / g, when the raw material is melted in the extruder, the pressure becomes high, and it becomes easy to cause deformation of the filter, etc., so it is not preferred. The IV is preferably 0.65 dL / g or more and 1.15 dL / g or less, and more preferably 0.7 dL / g or more and 1.1 dL / g or less.
[0073] (10) Maximum thermal shrinkage stress in the width direction
[0074] The maximum heat shrinkage stress in the width direction of the film of the present invention when it is shrunk in hot air at 90°C for 30 seconds is preferably 3 MPa or more and 22 MPa or less. During heat shrinkage, if the maximum heat shrinkage stress at 90°C in the width direction is higher than 22 MPa, even if the heat seal strength is set to 20N / 15mm or more, the possibility of the sealed portion with the label being peeled off during shrinkage will increase, so it is not preferred. On the other hand, if the maximum heat shrinkage stress in the width direction is lower than 3 MPa, even after shrinking to the object, the object becomes easy to fall off, so it is not preferred. The maximum heat shrinkage stress in the width direction is more preferably 4 MPa or more and 21 MPa or less, and further preferably 5 MPa or more and 20 MPa or less.
[0075] (11) Heat sealing starting temperature
[0076] The heat sealing start temperature of the film of the present invention when heat-sealing one side of the film with the other side is preferably 100°C or more and 150°C or less. The heat sealing start temperature is the temperature at which the strength when peeling in a shear test initially becomes 2N / 15mm or more when the heat sealing temperature is changed from 90°C to 160°C at intervals of 5°C under the conditions of a pressure of 0.1MPa and 1 second. A heat sealing start temperature exceeding 150°C means that there is no low-temperature sealing property, which is likely to become unfavorable for high-speed installation based on an automatic machine (poor yield of label manufacturing). On the other hand, if the heat sealing start temperature is lower than 100°C, the low-temperature sealing property is improved, which is preferred, but it is not preferred because it becomes easy to cause adhesion when the film is stored as a roll. The heat sealing start temperature is more preferably 105°C or more and 145 or less, and further preferably 110°C or more and 140 or less.
[0077] (12) Proportion of oxygen atoms on the film surface
[0078] The oxygen atom presence ratio on the film surface obtained by the peak representing oxygen atoms and the peak representing carbon atoms in the spectrum obtained by X-ray photoelectron spectroscopy (ESCA) of the film of the present invention is preferably 27% or more and 31% or less in at least one outermost layer. The detailed determination method of the oxygen atom presence ratio is described later. If the oxygen atom presence ratio is 27% or more, the wetting tension is easily called 40mN / m, and it becomes easy to achieve the above-mentioned heat seal strength of 20N / 15mm or more. The more the oxygen atom presence ratio, the better the wetting tension and heat seal strength, which is preferred, but when it is rolled up and stored in the form of a roll, it becomes easy to cause adhesion, so it is not preferred.
[0079] It is believed that if the oxygen atom exists in a large proportion, functional groups such as carboxyl and hydroxyl groups are more present on the film surface. These functional groups are polarized (for example, oxygen atoms are δ+ and hydrogen atoms are δ-), so it is believed that the electrical mutual attraction between the film surfaces when they are close to each other becomes stronger, and the heat seal strength is improved. Furthermore, these functional groups protrude three-dimensionally from the film surface, so it is believed that the functional groups also play a role like a wedge. As mentioned above, it is believed that the functional groups containing oxygen atoms interact electrically / physically, thereby improving the heat seal strength.
[0080] The oxygen atom abundance ratio is more preferably 27.5% to 30.5%, and further preferably 28% to 30%.
[0081] (13) Haze
[0082] The haze of the film of the present invention is preferably 2% or more and 20% or less. If the haze value exceeds 20%, the transparency becomes poor and the object (content) becomes difficult to be seen, so it is not preferred. The haze is more preferably 19% or less, and further preferably 18% or less. It should be noted that the smaller the haze value, the more preferred, but for the purpose of imparting the required slip properties in practical use, when considering that a specified amount of lubricant must be added to the film, about 2% becomes the lower limit.
[0083] 3. Method for producing the heat-shrinkable polyester film of the present invention
[0084] The film of the present invention can be produced by stretching the unstretched film obtained by melt-extruding the above polyester raw material using an extruder under the following method / conditions. It should be noted that the polyester can be obtained by polycondensing the above-mentioned suitable dicarboxylic acid component and diol component by a known method. In addition, two or more polyesters in small pieces are usually mixed and used as the raw materials of the film.
[0085] Hereinafter, each step will be described in detail.
[0086] 3.1. Melt extrusion
[0087] When the raw material resin is melt-extruded, it is preferred to dry the polyester raw material with a hopper dryer, a paddle dryer or a vacuum dryer. After the polyester raw material is dried in this way, it is melted at a temperature of 200 to 330° C. using an extruder and extruded into a film. When extruding, any existing method such as a T-die method or a tubular method is adopted.
[0088] The extruded sheet-shaped molten resin is then rapidly cooled to obtain an unstretched film. It should be noted that as a method for rapidly cooling the molten resin, a method is preferably used in which the molten resin is cast from a nozzle onto a rotating drum and rapidly cooled and solidified to obtain a substantially unoriented resin sheet.
[0089] The obtained unstretched film is stretched along the length (longitudinal) direction and the width (horizontal) direction by the method described in detail below, so as to obtain the film of the present invention. As the stretching direction, it can be either uniaxial stretching of only one of the longitudinal or transverse directions, biaxial stretching of the longitudinal and transverse directions, but if the productivity as the main purpose of the present invention is considered, biaxial stretching is preferred. In the case of biaxial stretching, it can be biaxial stretching in sequence in which the remaining direction is stretched after any one of the longitudinal or transverse directions, or biaxial stretching while the longitudinal and transverse directions are stretched simultaneously, either. Below, the method / condition of biaxial stretching in sequence in the longitudinal-transverse direction after being stretched in the transverse direction is recorded.
[0090] 3.2. Longitudinal stretching
[0091] In the manufacture of the film of the present invention, it is preferred that a substantially unoriented film is introduced into a longitudinal stretching machine in which a plurality of roller groups are continuously arranged, and after being heated on a preheating roller, it is longitudinally stretched in a manner of 1.0 times or more and 4.5 times or less. When the longitudinal stretching ratio is 1.0, it is substantially not longitudinally stretched. It is preferred that preheating is performed on the preheating roller until the film temperature reaches 60°C to 110°C. If the film temperature is lower than 60°C, it becomes difficult to stretch (i.e., it becomes easy to break) when stretched in the longitudinal direction, which is not preferred. In addition, if it is higher than 110°C, the film is easy to adhere to the roller, and the film is wound into a roll, thereby significantly reducing productivity, so it is not preferred.
[0092] After the film temperature reaches the above range, the film is stretched longitudinally by the speed difference of the rollers. At this time, by extending the roller spacing used in the longitudinal stretching, the longitudinal stretching ratio can be increased, and the ΔCp of the film can be suppressed at a lower level. It is believed that this is because the longer the roller spacing, the lower the speed of the longitudinal stretching, and the more crystallization and rigid amorphization can be suppressed. However, the longer the roller spacing, the larger the shrinkage (Poisson's ratio) in the direction orthogonal to the stretching direction (here is the width direction), so the problem of reduced productivity arises. That is, if the film width after longitudinal stretching is reduced, the inlet width in the transverse stretching in the tentering machine of the subsequent process will be narrowed, so the width at the tentering machine outlet will also be reduced accordingly. The roller spacing is preferably 80 mm or more and 500 mm or less, more preferably 90 mm or more and 490 mm. In order to compensate for the reduction in productivity and increase the transverse stretching ratio, ΔCp will become easy to be lower than 0.4 J / g·K. Therefore, even if the longitudinal stretching is made high-ratio, ΔCp is made 0.4 J / g·K or more, and the productivity is improved, therefore, in the present invention, it is preferred to divide the longitudinal stretching times into multiple times. Specifically, it is preferred to increase the configuration (stretching level) of the rollers used in the longitudinal stretching from the usual two types of low speed / high speed (primary stretching) to three types of low speed / medium speed / high speed (secondary stretching) and four types of low speed / medium-low speed / medium-high speed / high speed (three-stage stretching). The more the stretching level increases, the more significant the effect is and the more preferred it is, but the equipment becomes huge, so the preferred stretching level is 1 to 3 levels.
[0093] The stretching ratio per stage in the longitudinal stretching is preferably 1.0 times or more and 3.2 times or less, and more preferably 1.1 times or more and 3.1 times or less.
[0094] 3.3. Intermediate heat treatment after longitudinal stretching
[0095] After longitudinal stretching, an intermediate heat treatment is preferably performed for the purpose of reducing the heat shrinkage in the length direction. The intermediate heat treatment temperature is preferably 100°C or more and 160°C or more, more preferably 105°C or more and 155°C or less, and further preferably 110°C or more and 150°C or less. In addition, during the intermediate heat treatment, the shrinkage in the length direction of the film generated during the longitudinal stretching can be further reduced by relaxing the film in the length direction (relaxation in the length direction). Not only that, by relaxing in the length direction, the bow phenomenon (strain) occurring in the tenter can be reduced. The relaxation rate in the length direction is preferably 0% or more and 60% or less (relaxation rate 0% means no relaxation). The upper limit of the relaxation rate in the length direction is determined by the raw materials used and the longitudinal stretching conditions, and therefore, relaxation cannot be performed beyond this upper limit. Relaxation in the length direction can be implemented by heating the longitudinally stretched film at a temperature below 65°C to 100°C and adjusting the speed difference of the rollers. The heating means can use any of rollers, near infrared rays, far infrared rays, hot air heaters, etc. In addition, relaxation in the length direction can be implemented at any time, even if it is not just after longitudinal stretching. For example, it can be implemented by reducing the clamp spacing in the length direction during transverse stretching (including preheating zone) and final heat treatment (in this case, both ends of the film in the width direction are also relaxed in the length direction, so the bow strain is reduced).
[0096] After relaxation in the longitudinal direction (if no relaxation is performed, longitudinal stretching), the film is preferably cooled once, preferably on a cooling roll having a surface temperature of 20 to 40°C.
[0097] 3.2. Transverse stretching
[0098] The film after longitudinal stretching or relaxation in the length direction is continuously introduced into the tenter, preheated and then stretched transversely. The temperature of the preheating zone is preferably above 80°C and below 150°C. If the preheating temperature is lower than 80°C, the molecules become easily oriented and crystallized during transverse stretching, which not only makes it easy to make ΔCp lower than 0.4 J / g·K, but also makes the film easy to break, so it is not preferred. On the contrary, if the preheating temperature exceeds 150°C, the uneven thickness in the width direction will worsen, and the winding quality when winding in the form of a roll will be reduced, so it is not preferred.
[0099] The residence time in the preheating zone is preferably 2 seconds or more and 10 seconds or less. If the residence time is less than 2 seconds, it becomes difficult for the film to reach the temperature required for transverse stretching, and the same concern arises when the preheating zone temperature is less than 80°C. On the other hand, even if the residence time exceeds 10 seconds, transverse stretching itself is unlikely to cause problems, but there is a tendency to increase the scale of production equipment accordingly, so it is not preferred.
[0100] After the preheating zone, transverse stretching is performed in the transverse stretching zone where the distance between the clips in the width direction of the tenter is continuously expanded. The inventors have found that, in transverse stretching, the increase in the number of stretching stages, as in longitudinal stretching, can suppress the increase in ΔCp even if the stretch ratio is increased, and the required heat sealability can be ensured. Specifically, compared with the conventional one-stage stretching ( Figure 1 ) compared to multi-stage stretching (e.g. Figure 2 ; 3-stage stretching) can take into account both productivity and the specified ΔCp. It is believed that this is because the molecular chains extended by stretching are thermally relaxed under tension in the unstretched interval. For example, Figure 8 of Non-Patent Document 1 shows X-ray diffraction images of polyethylene terephthalate just after stretching at a stretching ratio of 2.0 (a, b) to 4.0 (i, j) (upper section) and about 0.2 seconds after the end of stretching (lower section), and it is possible to read the structural changes caused by the passage of time after the end of stretching. It can be seen here that when the stretching ratio is 4.0, crystallization occurs about 0.2 seconds after the end of stretching (j), while when the stretching ratio is up to about 2.2, no structural changes occur and the amorphous state is maintained (b, d). In addition, Figure 2 The X-ray diffraction images are shown in Figure 8 when the stretching temperature is changed from 85°C to 130°C, immediately after the stretching is completed (upper section) and about 0.2 seconds after the stretching is completed (lower section). Here, the X-ray diffraction images are read when the stretching is performed at 130°C and no crystallization occurs after a certain period of time has passed since the end of the stretching (p). Non-patent document 1 indicates that no oriented crystallization occurs after the end of the stretching (i, j, Figure 2 p) is because the relaxation speed of molecules based on heat is faster than the orientation speed of molecules based on stretching. In the present invention, a (non-crystalline) polyester that is less likely to crystallize than polyethylene terephthalate is used as a raw material. Therefore, the stretching ratio that causes oriented crystallization is greater than that of polyethylene terephthalate. It can be imagined that the oriented molecules after further stretching are in a state of easy thermal relaxation. In the past, in order to relax the oriented molecular chains, it can be achieved by shortening the clamp spacing in the width direction of the tenter (relaxation in the width direction), but the width of the tenter outlet will be reduced, so there is a problem that productivity is sacrificed. Therefore, various studies have been conducted on means to maintain or improve productivity and the ΔCp required for the residual film. As a result, the inventors found that: using an amorphous polyester raw material, further providing an unstretched section in the middle of the transverse stretching zone as described above (forming a multi-stage stretching), thereby, the oriented molecular chains are efficiently thermally relaxed and ΔCp is reduced. Based on such technical concept, it is preferred that the number of stretching stages is larger because ΔCp is within a predetermined range and productivity is improved, but there is a concern that the length of the tenter may increase. The number of stretching stages in the transverse direction is preferably 2 or more and 4 or less.
[0101] The stretching ratio per stage in transverse stretching is preferably 1.1 to 3 times, and the final stretching ratio (the value obtained by multiplying the stretching ratios in all stretching stages) is preferably 3.5 to 6 times.
[0102] The transverse stretching temperature is preferably 80° C. to 150° C., and the number of stretching stages may be any. The time for each stage in the transverse stretching is preferably 1 second to 10 seconds, but it depends on the stretching ratio and the line speed and can be changed appropriately.
[0103] Heat treatment
[0104] The film that has been transversely stretched as described above can be heat-treated in a tenter as needed in a state where both ends in the width direction are held by clamps. Heat treatment herein refers to heat treatment at a temperature of 80°C or more and 120°C or less for 1 second or more and 9 seconds or less. Such heat treatment improves the dimensional stability after storage over time, and therefore, it is preferably used. If the heat treatment temperature is lower than 80°C, the above-mentioned effect based on the heat treatment cannot be effectively exerted. On the other hand, if the heat treatment temperature is higher than 120°C, the heat shrinkage in the width direction becomes easy to be lower than the lower limit of 20%.
[0105] The longer the heat treatment time is, the easier it is to exert the effect. However, if the time is not too long, the equipment will become large, so it is preferably controlled to be 1 second or more and 9 seconds or less, and more preferably 5 seconds or more and 8 seconds or less.
[0106] In the heat treatment step, the distance between the holding clips in the tenter may be shortened to allow relaxation in the width direction. However, this will reduce productivity as described above, so the relaxation rate is preferably 0% to 10%.
[0107] Surface treatment
[0108] At least one outermost layer of the film is preferably treated for the purpose of increasing the heat seal strength. As surface treatment, corona treatment, plasma treatment, flame treatment, sandblasting, coating, etc. can be cited. Among these, corona treatment, plasma treatment, coating are preferred. In the case of corona treatment and plasma treatment, it becomes easy to make the wetting tension more than 40mN / m. The treatment degree (wetting tension) of corona treatment and plasma treatment varies according to the distance between the treatment electrode and the film, the discharge voltage, and the speed (linear velocity) of the film flow, and is determined by the combination of these conditions.
[0109] Regarding coating, for example, by applying a heat-sealable resin to the surface of the film, the low-temperature heat-sealability of the film is improved. As a heat-sealable resin, for example, the polyester resins listed in "1. Polyester raw materials used in heat-shrinkable polyester films" can be cited. A solution prepared by using these resins alone or using two or more of them and dissolving them in a solvent can be applied to the surface of the film. Among the constituent components of the above-mentioned polyester, isophthalic acid, neopentyl glycol, and 1,4-cyclohexanedimethanol are preferably used. In the case of coating, sebacic acid and 1,3-propylene glycol are further preferably used. It is preferred that the coating liquid contains more than 40 mol% and less than 100 mol% of one or more selected from these. If the total amount of these components is less than 40 mol%, it becomes difficult to dissolve in the solvent when preparing the coating liquid, so it is not preferred.
[0110] The step of applying the coating liquid may be performed at any timing in the film forming steps exemplified above.
[0111] The film having undergone the above-mentioned steps is preferably wound in a roll shape on a winding core such as a paper tube to form a film roll.
[0112] 4. Ring label
[0113] The heat-shrinkable polyester film of the present invention is used in at least a part of the annular label of the present invention. The heat-shrinkable polyester film of the present invention is bonded to each other or to other films, and the heat seal strength when the bonded part is peeled off in a shear test is 20N / 15mm or more and 80N / 15mm or less. In addition, the length (circumference) and the number of bonded parts of the annular label of the present invention can be arbitrary. Preferably, it is the aforementioned tape label.
[0114] As other films constituting the ring-shaped label of the present invention, any conventionally known films can be used with any length, regardless of the presence or absence of the characteristics listed in "2. Characteristics of the heat-shrinkable polyester film of the present invention". The raw material of the film can also be any, for example, polyester, polyolefin, polyamide, etc.
[0115] As the bonding method required to form the annular label of the present invention, heat sealing, ultrasonic sealing, a method using hot glue (hot melt) or cold glue, a solvent-based center seal, etc. can be cited. Among these, heat sealing or ultrasonic sealing is preferred, and heat sealing is more preferred. The heat seal strength varies according to the temperature, pressure, and sealing time of the heat seal rod (the surface in contact with the film), and is determined according to the combination of these conditions. For example, assuming that the heat seal temperature is increased and the sealing time becomes shorter, the temperature actually applied to the film also becomes lower. As an example, the heat seal temperature is preferably above 100°C and below 180°C, more preferably above 110°C and below 170°C, and further preferably above 120°C and above 160°C. If the heat seal temperature is lower than 100°C, it will become easy to make the heat seal strength lower than 20N / 15mm. If the heat seal temperature is higher than 180°C, the heat seal strength is improved, which is preferred, but the film becomes easy to heat shrink, the label size of the heat seal portion changes, and there is a concern about the deterioration of the appearance. The heat sealing pressure is preferably 0.05 MPa or more and 0.6 MPa or less, more preferably 0.1 MPa or more and 0.55 MPa or less, and further preferably 0.15 MPa or more and 0.5 MPa or less. If the pressure is lower than 0.05 MPa, it becomes difficult for the sealing rod to transfer sufficient heat to the film, and the heat sealing strength is likely to be lower than 20 N / 15 mm. If the pressure is higher than 0.05 MPa, the heat sealing strength does not change significantly based on the research of the present inventors, but if it is higher than 0.6 MPa, there is a concern that the film may break.
[0116] The heat sealing time is preferably 0.1 seconds to 3 seconds, more preferably 0.2 seconds to 2.9 seconds, and further preferably 0.3 seconds to 2.8 seconds. If the sealing time is less than 0.1 seconds, the heat sealing strength is likely to be less than 20 N / 15 mm. If the sealing time exceeds 3 seconds, the heat sealing strength is improved, which is preferred, but it goes against the improvement of productivity which is the main purpose of the present invention, so it is not preferred.
[0117] 5. Packaging
[0118] The packaging body of the present invention is characterized in that the annular label of the present invention is used. Specifically, the annular label of the present invention is covered on at least a portion of the packaging object, and the heat-shrinkable polyester film of the present invention is heat-shrunk. The heat shrinkage may be a part of the heat-shrinkable polyester film used for the annular label of the present invention.
[0119] The packaging object is not limited, and examples thereof include plastic containers and plastic bottles in square or round shapes.
[0120] Example
[0121] Next, the present invention will be specifically described using Examples and Comparative Examples. However, the present invention is not limited to the embodiments of these Examples and can be modified within a scope not departing from the gist of the present invention.
[0122] The following properties were evaluated for each polyester film described in Table 2 below.
[0123] [thickness]
[0124] The measurement was performed using a scale in accordance with JIS K7130-1999 Method A.
[0125] [Tg (glass transition point)]
[0126] The film to be the sample is weighed in a T-zero pan or an aluminum pan (flat pan shape) at 5.0±0.2 mg using a temperature modulation differential scanning calorimeter (DSC) "DSC250" (manufactured by TA Instruments). The film is measured in a MDSC (registered trademark) heating mode only with an average heating rate of 2°C / min and a modulation cycle of 40 seconds to obtain a reverse heat flow. It should be noted that when the sample is sealed in the pan, in order to achieve good adhesion to the bottom of the pan, an overlapping film is used and punched into a circular shape (diameter 4.5 mm) with a punch. "Good adhesion to the bottom of the pan" refers to the following state: when the sample is sealed in the pan, there is no bend in the film sample in the pan, and there is no space between the films that are firmly pressed and overlapped with the cover. It should be noted that wrinkles can also enter the film before punching, but it is preferred to stretch the wrinkles in advance when punching the sample. In addition, the shape and size of the punched sample (punch) are not limited to the above, as long as the sample is stored in the bottom of the pan without bending.
[0127] In the reverse heat flow obtained in the measurement, Tg is obtained as a signal that changes in a step-like manner from the baseline. Specifically, an extension line of the baseline of each heat flow is drawn on the low temperature side / high temperature side closer to Tg, and the intersection with the tangent line at the inflection point (Tg) is obtained, and the value of the horizontal axis at the intersection is read, and the average value of the low temperature side and the high temperature side is taken as Tg.
[0128] [Intrinsic viscosity IV (film, polyester raw materials)]
[0129] The film or polyester raw material (resin) was dissolved in a 6 / 4 (weight ratio) mixed solvent of phenol / 1,1,2,2-tetrachloroethane, and the measurement was performed at a temperature of 30°C.
[0130] [Wetting tension]
[0131] The wetting tension on the film surface was measured by the method described in JIS K 6768:1999 after aging the film at 23°C and a relative humidity of 50% for 24 hours.
[0132] [Oxygen atom presence ratio]
[0133] The film surface was measured using an X-ray photoelectron spectroscopy (ESCA) analyzer (K-Alpha manufactured by Thermo Fisher Scientific).
[0134] Excitation X-ray: Monochromatized ALKα ray
[0135] X-ray power: 12kV, 6mA
[0136] Photoelectron separation angle: 90°
[0137] Point size:
[0138] Pulse energy: 50eV (narrow scan), 200eV (full element scan)
[0139] Step size: 0.1eV (narrow scan), 1eV (full element scan)
[0140] A narrow scan was performed for C, N, O, and Si, and the peak intensity ratio obtained by dividing the peak intensity of 530 to 540 eV representing oxygen atoms by the peak intensity of 280 to 290 eV representing carbon atoms was obtained from the obtained spectral data, and this was used as the oxygen atom existence ratio on the film surface. It should be noted that the measurement was repeated 4 times, and the average value of the peak intensity ratio was obtained.
[0141] [Ring stiffness]
[0142] As a sample for measuring the ring stiffness, the laminated film prepared in the embodiment and the comparative example is cut into a strip film with a width of 25.4 mm and 110 mm. At this time, the length direction of the strip film is made consistent with the direction of the measurement object. The cut strip film is installed in a ring stiffness tester manufactured by Toyo Seiki Co., Ltd. to measure the repulsive force. The measurement frequency is set to 50 Hz. The value (mN) of the repulsive force obtained in the measurement is used as the ring stiffness.
[0143] [Heat shrinkage (hot water heat shrinkage)]
[0144] The film was cut into a 10 cm × 10 cm square, immersed in hot water at 80°C ± 0.5°C for 10 seconds without load for heat shrinkage, then immersed in water at 25°C ± 0.5°C for 10 seconds, pulled out of the water, and the longitudinal and transverse dimensions of the film were measured, and the heat shrinkage rates were calculated according to the following formula 1. The direction with the largest heat shrinkage rate was taken as the main shrinkage direction (width direction).
[0145] Thermal shrinkage rate (%) = {(length before shrinkage - length after shrinkage) / length before shrinkage} × 100 Formula 1
[0146] [Heat seal strength]
[0147] According to JIS Z1707, the heat seal strength is measured. The specific steps are briefly shown. Use a heat sealer to seal one outermost layer and the other outermost layer of the film sample. The heat sealing conditions are set as follows: upper rod temperature 140°C, lower rod temperature 30°C, pressure 0.2MPa, time 2 seconds. The bonding samples are as follows: 10 samples are cut out in such a way that the sealing width becomes 15mm. The peel strength is measured using a tensile testing machine (manufactured by Shimadzu Corporation, Autograph AG-Xplus) at a tensile speed of 200mm / min. At this time, the peeling direction is as follows: Figure 3 The heat seal strength was determined as the average value of 10 tests and expressed as the strength per 15 mm (N / 15 mm).
[0148] [Heat sealing start temperature]
[0149] According to JIS Z1707, the heat seal start temperature is evaluated. The specific steps are briefly shown. Use a heat sealer to seal one outermost layer and the other outermost layer of the film sample. The heat sealing conditions are set as follows: lower rod temperature 30°C, pressure 0.2MPa, time 2 seconds, and the temperature of the upper rod is changed from 90°C to 160°C at intervals of 5°C to prepare bonding samples at each temperature. The bonding samples are as follows: for each upper rod temperature, 10 samples are cut out in such a way that the sealing width becomes 15mm. The peel strength is measured using a tensile testing machine (manufactured by Shimadzu Corporation, Autograph AG-Xplus) at a tensile speed of 200mm / min. At this time, the peeling direction is as follows: Figure 3 The heat seal strength was measured as the average of 10 tests and expressed as the strength per 15 mm (N / 15 mm). The heat seal temperature at which the heat seal strength began to reach 2 N / 15 mm or more was taken as the heat seal start temperature.
[0150] [Maximum thermal shrinkage stress]
[0151] A sample with a length of 200 mm in the main shrinkage direction (width direction) and a width of 20 mm (length direction) is cut out from the polyester film and measured using a strong elongation tester (TENSILON, a registered trademark of Orientec) with a heating furnace. The heating furnace is preheated to 90°C, and the chuck spacing is set to 100 mm. The air supply of the heating furnace is temporarily stopped, the door of the heating furnace is opened, and after the above sample is installed on the chuck, the door of the heating furnace is quickly closed and the air supply is started again. The heat shrinkage stress in the width direction when shrinking in 90°C hot air for 30 seconds is measured, and its maximum value is taken as the maximum heat shrinkage stress (MPa).
[0152] [Reversible thermal tolerance]
[0153] The film to be the sample is weighed in a T-zero pan or an aluminum pan (flat pan shape) at 5.0±0.2 mg using a temperature modulation differential scanning calorimeter (DSC) "DSC250" (manufactured by TA Instruments). The film is measured in the MDSC (registered trademark) heating mode only with an average heating rate of 2°C / min and a modulation period of 40 seconds to obtain a reverse heat flow. When the sample is sealed in the pan, in order to achieve good adhesion to the bottom of the pan, an overlapping film is used and punched into a circular shape (diameter 4.5 mm) with a punch. "Good adhesion to the bottom of the pan" refers to the following state: when the sample is sealed in the pan, there is no bend in the film sample in the pan, and there is no space between the films that are firmly pressed and overlapped with the cover. It should be noted that wrinkles can also enter the film before punching, but it is preferred to stretch the wrinkles in advance when punching the sample. In addition, the shape and size of the punched sample (punch) are not limited to the above, as long as the sample is stored in the bottom of the pan without bending.
[0154] From the obtained reverse heat flow, the reversible heat tolerance from 30° C. to 140° C. was calculated as shown in Formula 2 using the attached analysis software (Trios manufactured by TA Instruments).
[0155] Reversible thermal tolerance ΔCp=Cp1-Cp2 Formula 2
[0156] Cp1: Heat capacity at 140°C
[0157] Cp2: Heat capacity at 30°C
[0158] [Haze]
[0159] The haze was measured using a haze meter "500A" (manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K7136. The measurement was performed twice, and the average value was calculated.
[0160] [Anti-blocking properties]
[0161] According to ASTM D1893-67, the blocking value is measured. Cut the film sample into two pieces with a length of 150mm × width of 200mm, and overlap one side with the other side in a way that different sides overlap each other. The overlapping samples are clamped with a smooth glass plate (250mm square), and a weight of 20kg (5kg×4 pieces) is placed on top of it, and it is placed in a hot air oven set at 60℃±2℃ and left for 24 hours. Take out the film sample after placement and dry it for 1 hour in an environment of 23℃×humidity 65%. The dried sample is peeled off about 3cm from one end, and the sample is installed on the upper chuck of Autograph (AG-Xplus made by Shimadzu Corporation), and a rod (diameter 6mm) is installed on the lower chuck. The force when the rod peels off the sticking part at a speed (100m / minute) is measured. It should be noted that the rod and the peeling surface are horizontal, the measurement direction (the direction of the chuck movement) is the length direction of the film, and the measurement is performed twice, and the average value is calculated as the blocking value (unit: mN / 200mm). The obtained blocking value is evaluated according to the following criteria. It should be noted that the case where the sample is peeled off before the start of the measurement is recorded as an evaluation of ○, and the case where the sample is not peeled off by hand when installed in the chuck is recorded as an evaluation of ×.
[0162] Evaluation ○: Adhesion value 0 mN / 200 mm or more and less than 1000 mN / 200 mm
[0163] Evaluation ×: Adhesion value 1000mN / 200mm or more
[0164] [Suitability of installation]
[0165] The film was cut into 90 mm in the length direction and 250 mm in the width direction, placed on a plastic noodle container (long side 220 mm × short side 150 mm × height 50 mm) commercially available in convenience stores, and flowed on a conveyor belt set at a speed of 20 cm / second to evaluate the film's misalignment. It should be noted that as a prior preparation for flowing on the conveyor belt, the film was placed in a manner such that the length direction of the film was along the short side of the container, the end position of the film was marked on the container, and the initial position was recorded in advance. The distance that the film position after flowing on the conveyor belt deviated from the initial position was measured, and the evaluation was performed according to the following criteria.
[0166] Evaluation ○: Deviation distance is less than 1 cm
[0167] Rating ×: Deviation distance is greater than 1 cm
[0168] [Shrinkage finishing properties]
[0169] The film was cut out so that the length direction of the film (width with label) was 90 mm for a plastic noodle container (long side 220 mm×short side 150 mm×height 50 mm) commercially available at a convenience store, and two films were placed on the upper and lower sides of the container so that the main body and the lid of the container were fixed by the film, and the ends of the films were heat-sealed at 140°C. That is, at this time, the noodle container was covered with the heat-sealed ring-shaped film. At this time, the long sides of the noodle container were fixed by the ring-shaped film so that the shrinkage direction (width direction) of the film became the circumferential direction of the ring-shaped film, and the midpoint of the width direction of the ring-shaped film was aligned with the midpoint of the long side of the container. In addition, the relaxation amount of the ring-shaped film for the container was set to 25%. The package consisting of the noodle container and the ring-shaped label was heated and shrunk in hot air at a set temperature of 110°C in a hot air shrink tunnel (TORNADO2500 manufactured by Nippon Technology Solution Co., Ltd.), and the shrinkage finish was evaluated. The shrinkage finish was evaluated on two points: adhesion to the container and cracking of the heat-sealed portion.
[0170] (Sealing performance to container)
[0171] The close adhesion of the container was evaluated as follows: when the shrunk ring label was held by hand and lifted up together with the package, whether the container fell off the ring label was used as a criterion, and the evaluation was performed as follows.
[0172] Evaluation ○: The container is held without falling off the ring label.
[0173] Rating ×: The container fell off the ring label
[0174] (Peeling of heat-sealed portion)
[0175] Regarding the peeling of the heat seal, two heat-sealed portions were observed after the shrinkage was completed, and the peeling was judged according to the following criteria.
[0176] Evaluation ○: No peeling
[0177] Evaluation ×: Part or all of at least one heat-sealed portion was peeled off
[0178] <Synthesis of polyester raw materials>
[0179] [Synthesis of polyester raw material A]
[0180] In a polymerization device equipped with a stirrer, a distillation column and a pressure regulator, terephthalic acid and diols (ethylene glycol, neopentyl glycol, diethylene glycol) are added at a constant ratio (G / T: molar ratio of diol / terephthalic acid), and the esterification reaction is carried out at a reaction temperature of 240° C. and a reaction pressure of 0.35 MPa while successively removing water generated during the esterification.
[0181] Then, a constant amount of an ethylene glycol solution of an aluminum compound (basic aluminum acetate) and an ethylene glycol solution of a phosphorus compound (Irganox 1222) were added, and the temperature of the system was raised to 280°C within 1 hour. During this period, the pressure of the system was slowly reduced to 0.15 kPa, and the polycondensation reaction was carried out while the diols produced in the polycondensation reaction were removed in sequence while the system was maintained unchanged. When the predetermined stirring torque was reached, the reactor was purged with nitrogen to return to normal pressure, and the polyester resin was extracted from the polymerization device, water-cooled and solidified, and pelletized by a strand cutter to obtain a polyester raw material A. The composition of the monomer components of the polyester raw material A is shown in Table 1. In Table 1, the "acid component" column shows the content of each monomer component in 100 mol% of all acid components, and the "polyol component" column shows the content of each monomer component in 100 mol% of all polyol components. In Table 1, TPA is terephthalic acid, IPA is isophthalic acid, EG is ethylene glycol, BD is butanediol, NPG is neopentyl glycol, CHDM is cyclohexanedimethanol, DEG is diethylene glycol, and SA is sebacic acid.
[0182] [Synthesis of polyester raw materials B to E]
[0183] According to the same method as the polyester raw material A, polyester raw materials B to E having different monomer components were obtained as shown in Table 1. It should be noted that polyester raw material D was produced as follows: SiO2 (Sylysia 266 manufactured by FUJI SILYSIA CHEMICAL LTD.; average particle size 1.5 μm) was added as a lubricant to the polyester at a ratio of 7000 ppm. Each polyester raw material was preferably made into a small piece.
[0184] [Synthesis of polyester raw material F]
[0185] As the polyester raw material F, a mechanically recycled polyester raw material was prepared in the following procedure.
[0186] After washing away the remaining beverage and other foreign matters from the plastic bottle for beverages, the scales are crushed to obtain flakes. The obtained flakes are stirred and washed in the presence of a 3.5 wt % sodium hydroxide solution at a flake concentration of 10 wt %, 85° C., and 30 minutes. After alkali washing, the scales are taken out and washed with distilled water under stirring at a flake concentration of 10 wt %, 25° C., and 20 minutes. For this water washing, the distilled water is replaced and further repeated twice. After washing with water, the scales are dried, melted in an extruder, and the filters are changed to those with finer pore sizes twice in sequence, and fine foreign matters are further filtered out twice. The third time, a filter with a minimum pore size of 50 μm is used to filter out, and a polyester resin F with a characteristic viscosity of 0.69 dl / g and an isophthalic acid content of 3.0 mol% is obtained.
[0187] [Synthesis of polyester raw material G]
[0188] As the polyester raw material G, a chemically recycled polyester raw material was prepared in the following procedure.
[0189] The classified and collected / recycled plastic bottle caps are put into a wet grinder, and the mixture is circulated in the wet grinder to grind the plastic bottle caps, and the metal, sand, glass and other materials with high specific gravity are precipitated by a specific gravity separator connected to the grinder, and the scales are taken out from the upper layer. The scales are washed with pure water and centrifuged to form recovered scales.
[0190] 30 kg of the recovered flakes melted in an undried state were added to a preheated mixed solution of 150 kg of ethylene glycol and 150 g of zinc acetate dihydrate in an autoclave equipped with a stirrer, and fractions having a boiling point lower than that of ethylene glycol, such as water / acetic acid, were removed. Then, the mixture was reacted at a temperature of 195 to 200° C. for 4 hours using a reflux condenser.
[0191] After the reaction was completed, the temperature of the reactor contents was cooled to 97-98°C, and hot filtration was performed with a filter to remove suspended solids and precipitates. The filtrate after hot filtration was further cooled, and after confirming that the crude bis-2-hydroxyethyl terephthalate (BHET) was completely dissolved, it was passed through an activated carbon bed at 50-51°C, and then passed through an anion / cation exchange mixed bed for 30 minutes to perform pre-purification treatment.
[0192] The pre-purification treatment liquid is again put into the stirring autoclave and heated to distill the remaining ethylene glycol under normal pressure to obtain a molten liquid of concentrated BHET. The obtained molten liquid of concentrated BHET is stirred under a nitrogen atmosphere and cooled naturally, and then taken out from the autoclave to obtain fine flakes of concentrated BHET.
[0193] The flakes were heated and melted again at 130°C, and then fed to a thin film vacuum evaporator by a metering pump for evaporation and cooling to obtain purified BHET. The purified BHET was used as a raw material for melt polymerization to obtain a chemically recycled polyester resin G.
[0194] [Synthesis of Coating Polyester Resins H and I]
[0195] According to the same method as the polyester raw material A, coating polyester resins H and I having different monomer components were obtained as shown in Table 1. Each polyester raw material was appropriately formed into small pieces.
[0196] [Table 1]
[0197]
[0198] [Example 1]
[0199] Polyesters A, D, and F were mixed at a mass ratio of 80:8:12 and fed into an extruder. The mixed resin was melted at 280°C, extruded from a T-die, and rapidly cooled on a rotating metal roll whose surface temperature was cooled to 30°C to obtain an unstretched film with a thickness of about 250 μm.
[0200] An unstretched film is introduced into a longitudinal stretching machine in which a plurality of roller groups are continuously arranged, and longitudinal stretching is performed using the speed difference of the rollers. At this time, the rollers are set to low speed / medium-low speed / medium-high speed / high speed, and the longitudinal stretching interval is divided into three, and the film is longitudinally stretched. In the low-medium-low speed interval (first stretching zone) and the medium-low speed-medium-high speed interval (second stretching zone), the film is held on each roller by a roller in such a way that the film's passing line does not hug the roller but becomes a straight line. In the medium-high speed-high speed interval (third stretching zone), the film's passing line hugs the roller and becomes a cross. For the distance of the stretching interval, the roller configuration is adjusted so that it becomes 200mm in the first stretching zone and the second stretching zone, and 120mm in the third stretching zone. Regarding the temperature and ratio of each stretching zone, longitudinal stretching is performed in such a way that it becomes 1.6 times at 85°C in the first stretching zone, 1.7 times at 85°C in the second stretching zone, and 1.5 times at 90°C in the third stretching zone, and the total longitudinal stretching ratio is 4.1.
[0201] After that, the longitudinally stretched film was introduced into a heating furnace heated under far infrared rays for intermediate heat treatment. The temperature of the heating furnace was 130°C, and a 40% relaxation treatment was performed in the longitudinal direction by utilizing the speed difference between the rollers at the entrance and exit of the heating furnace.
[0202] The film after relaxation treatment is introduced into a transverse stretching machine (tenter), preheated to 130°C, and then Figure 2 , a section (relaxation zone) is set in the middle to restore the fixture pattern to a section parallel to the direction of travel and not stretched, and the lateral stretching is divided into 3 stages. Specifically, in the first stretching zone, the stretching is carried out to 1.5 times at a temperature of 100°C and a stretching speed of 30% / second, in the second stretching zone, the stretching is carried out to 1.6 times at a temperature of 95°C and a stretching speed of 30% / second (the ratio from the exit of the first stretching zone to the exit of the second stretching zone), and in the third stretching zone, the stretching is carried out to 1.7 times at a temperature of 93°C and a stretching speed of 15% / second. The total lateral stretching ratio is 4.1 times. Afterwards, heat treatment is carried out at 90°C in the final heat treatment zone.
[0203] Next, the film was introduced into a corona treatment machine, and the treatment temperature was set to 40° C. and the power was set to 0.3 kW, and the upper surface (F surface) of the film was subjected to corona treatment.
[0204] After that, the two edges of the film were cut and removed, and the film was wound into a roll with a width of 500 mm, thereby continuously manufacturing a film with a thickness of 25 μm over a predetermined length, thereby obtaining a film of Example 1. The manufacturing conditions of the film of Example 1 are shown in Table 2. The film of Example 1 was evaluated according to the above method. The evaluation results are shown in Table 3.
[0205] [Example 2]
[0206] In Example 1, various production conditions were changed as shown in Table 2, and the corona treatment was changed to coating. A film was obtained in the same manner as in Example 1. The film was coated according to the following method.
[0207] Polyester H and I were mixed at a ratio of 80:20, and dissolved in ethyl acetate by heating to prepare a coating solution. The coating solution was applied to the lower surface (B surface) of the film to a thickness of 2 μm to produce a film of Example 2. The production conditions of the film of Example 2 are shown in Table 2, and the evaluation results are shown in Table 3.
[0208] [Examples 3 to 7, Comparative Examples 1 to 4]
[0209] The films of Examples 3 to 7 and Comparative Examples 1 to 4 were produced as shown in Table 2. Table 3 shows the evaluation results of the films of Examples 3 to 7 and Comparative Examples 1 to 4.
[0210] [Table 2A]
[0211]
[0212] [Table 2B]
[0213]
[0214] [Table 3]
[0215]
[0216] The films of Examples 1 to 7 satisfy the conditions of the present invention and are all suitable as heat-shrinkable polyester films with labels.
[0217] In contrast, in Comparative Example 1, the heat seal strength was as low as 1, so the heat seal portion was peeled off in the evaluation of shrinkage finish. Therefore, the shrinkage finish could not be evaluated, and the shrinkage finish adhesion column in Table 3 was recorded as "-".
[0218] In Comparative Example 2, the ring stiffness was as low as 2 mN / 15 mm, so the film moved when flowing on the belt, and the mounting suitability was poor.
[0219] In Comparative Example 3, the heat shrinkage rate in the width direction was low, and therefore, the heat shrinkable polyester system was inferior in shrinkage finishing properties.
[0220] The wetting tension of Comparative Example 4 was too high, 57 mN / m, and thus the film had poor anti-blocking properties.
[0221] Industrial Applicability
[0222] Since the heat-shrinkable polyester film of the present invention has the above-mentioned properties, it can be suitably used for label applications and the like.
Claims
1. A heat-shrinkable polyester film, characterized in that: The main component is ethylene terephthalate and the following conditions (1) to (4) are satisfied. (1) The ring stiffness in the width direction is 6 mN / 25 mm or more and 200 mN / 25 mm or less, (2) the heat shrinkage in the width direction when shrunk in hot water at 80°C for 10 seconds is 20% or more and 70% or less, (3) When one side of the film is heat-sealed with the other side at a temperature of 140° C. and a pressure of 0.1 MPa for 1 second, the strength when peeled off in a shear test in the width direction is 20 N / 15 mm or more and 80 N / 15 mm or less, (4) The wetting tension of at least one outermost layer is 40 mN / m or more and 55 mN / m or less.
2. The heat-shrinkable polyester film according to claim 1, characterized in that The reversible heat capacity from 25° C. to 140° C. measured by a temperature modulation differential scanning calorimeter is 0.4 J / g·K or more and 1.4 J / g·K or less.
3. The heat-shrinkable polyester film according to any one of claims 1 or 2, characterized in that The oxygen atom abundance ratio on the thin film surface obtained from the peak of 285 to 290 eV in the C1s spectrum of X-ray photoelectron spectroscopy (ESCA) is 27% or more and 31% or less in at least one outermost layer.
4. The heat-shrinkable polyester film according to any one of claims 1 to 3, characterized in that The thickness is 20 μm or more and 50 μm or less.
5. The heat-shrinkable polyester film according to any one of claims 1 to 4, characterized in that The polyester constituting the film contains 1 mol % or more and 30 mol % or less of any one of isophthalic acid, neopentyl glycol, 1,4-cyclohexanedimethanol, butanediol, and diethylene glycol.
6. The heat-shrinkable polyester film according to any one of claims 1 to 5, characterized in that As a raw material constituting the film, a polyester raw material obtained by recycling PET bottles and subjecting them to mechanical and / or chemical recycling is used.
7. A label, characterized in that: It is a ring-shaped label in which at least a part of the heat-shrinkable polyester film according to any one of claims 1 to 6 is used, and the heat-shrinkable polyester film itself is bonded to each other or to other films, and the strength when the bonded part is peeled off in a shear test is 20N / 15mm or more and 80N / 15mm or less.
8. The label according to claim 7, characterized in that: The bonded portion is heat sealed.
9. A packaging body, characterized in that: Use the label according to any one of claims 7 and 8.