Resin composition and multilayer laminated film
By using specific resin compositions and layer structures, the problems of insufficient recyclability and bonding strength of the laminated film in the prior art are solved, and firmer resin layer bonding and better packaging material performance are achieved.
Patent Information
- Application Number
- CN202380034656.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-22
- Filing Date
- 2023-04-21
- Publication Date
- 2024-11-26
AI Technical Summary
The conventional laminated film for packaging materials is difficult to improve function and physical properties while maintaining recyclability, and the bonding force of the resin composition is insufficient, resulting in unsolid bonding between the resin layers.
Resin compositions using specific modified ethylene-α-olefin copolymers, unmodified ethylene-α-olefin copolymer resins and unmodified ethylene-α-olefin copolymer elastomers are combined with specific layer structures to form more Strong multi-layer laminated film.
A firmer bonding between different resin layers is achieved, the overall performance and recovery of the laminated film are improved, and the bonding force of the resin composition and the strength and gas barrier properties of the multi-layer laminated film are enhanced.
Smart Images

Figure BDA0005089128430000161
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition and a multi-layer laminate film. Background Art
[0002] Laminated films used for packaging materials are conventionally produced by laminating a resin composition having adhesive properties, a resin outer layer having excellent mechanical properties such as tensile strength, a resin intermediate layer such as a polyamide resin and an ethylene-vinyl alcohol copolymer having excellent barrier properties, and a resin inner layer having excellent heat sealability.
[0003] As the resin used for the inner layer, low-density polyethylene is widely used. In addition, as the resin used for the outer layer, polyethylene terephthalate, polypropylene, etc. are widely used. That is, by making various combinations of the outer layer, the inner layer, and the intermediate layer, it is possible to give the laminated film and even the packaging material excellent functions and physical properties.
[0004] On the other hand, there is a growing demand for packaging materials to reduce their environmental impact, and more specifically, for packaging materials to be more easily recyclable. However, since laminated films used in packaging materials are manufactured by combining various resins to give them excellent functions and properties, recycling is difficult.
[0005] Therefore, a laminated film produced with fewer types of resins is required. As such a laminated film, a stretched polyolefin film has attracted attention, and a stretched polyethylene film is a representative example.
[0006] Since stretched polyethylene films are superior to unstretched polyethylene films in mechanical properties such as tensile strength, various studies have been conducted on the use of stretched polyethylene films in laminated films for packaging materials that do not contain polyethylene terephthalate, polypropylene, etc. In conjunction with such studies, various studies have been conducted on resin compositions for bonding polyethylene and barrier resins in a multilayer stretched polyethylene film containing polyethylene as outer and inner layers and containing a barrier resin as an intermediate layer.
[0007] For example, Patent Document 1 discloses the use of a bonding polyethylene composition having specified physical properties containing a specified modified ethylene-α-olefin copolymer, a specified unmodified ethylene-α-olefin copolymer resin, a specified unmodified ethylene-α-olefin copolymer elastomer and a thickener to obtain a laminated film containing a stretched polyethylene film.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Laid-Open No. 9-249779 Summary of the invention
[0011] Problems to be solved by the invention
[0012] However, in recent years, there is a need not only to improve the functions and properties of laminated films for packaging materials while maintaining easy recycling, but also to have a resin composition with bonding properties, for example, it is necessary to be able to more firmly bond the resins forming the layers of the multilayer laminated film. As such demands increase, the bonding strength of the bonding polyethylene composition described in Patent Document 1 also needs to be improved.
[0013] The present invention provides a resin composition capable of bonding a plurality of resin layers formed of different resins more firmly than conventional resin compositions. In addition, the present invention also provides a multilayer laminated film capable of bonding resin layers formed of different resins more firmly than conventional resin compositions.
[0014] Technical solutions to solve problems
[0015] The inventors of the present invention conducted research under this situation and found that the above-mentioned problems can be solved by a resin composition containing a specific modified ethylene-α-olefin copolymer, a specific unmodified ethylene-α-olefin copolymer resin [B], a specific unmodified ethylene-α-olefin copolymer elastomer [C], and a multilayer laminated film with a specific layer structure including a layer containing the resin composition, thereby completing the present invention.
[0016] That is, the present invention relates to the following [1] to
[13] .
[0017] [1] A resin composition comprising:
[0018] [I] A modified ethylene-α-olefin copolymer [A] obtained by modifying a copolymer of ethylene and an α-olefin having 3 to 20 carbon atoms with an unsaturated carboxylic acid or a derivative thereof, wherein the modified ethylene-α-olefin copolymer [A] satisfies the following (i) and (ii),
[0019] (i) Density 0.860 g / cm 3 Above and less than 0.900g / cm 3 range,
[0020] (ii) the grafting amount is 0.01 to 5% by mass;
[0021] [II] an unmodified ethylene-α-olefin copolymer resin [B] having a melting point of 121° C. or less; and
[0022] [III] unmodified ethylene-α-olefin copolymer elastomer [C],
[0023] The melt flow rate (ASTM D 1238, 190°C, load 2.16 kg) of the resin composition is in the range of 0.1 to 50 g / 10 minutes.
[0024] The graft amount of the unsaturated carboxylic acid or its derivative is in the range of 0.01 to 1.0 mass % based on 100 mass % of the entire resin composition.
[0025] [2] The resin composition according to [1], wherein the density of the unmodified ethylene-α-olefin copolymer resin [B] is 0.900 g / cm 3 above,
[0026] The density of the unmodified ethylene-α-olefin copolymer elastomer [C] is less than 0.900 g / cm 3 .
[0027] [3] The resin composition according to [1] or [2], wherein the melting point of the resin composition is 119° C. or less.
[0028] [4] The resin composition according to any one of [1] to [3], wherein the density of the unmodified ethylene-α-olefin copolymer resin [B] is less than 0.930 g / cm 3 .
[0029] [5] The resin composition according to any one of [1] to [4], wherein the density of the unmodified ethylene-α-olefin copolymer resin [B] is 0.915 g / cm 3 the following.
[0030] [6] The resin composition according to any one of [1] to [4], wherein the density of the resin composition is 0.875 to 0.920 g / cm 3 .
[0031] [7] A multi-layer laminate film, characterized in that:
[0032] The multilayer laminated film is a laminated body of three or more layers in which the following layers are laminated in sequence,
[0033] polyolefin layer [I];
[0034] A bonding layer [II] comprising the resin composition described in any one of [1] to [6]; and
[0035] A polyamide resin layer [III], an ethylene-vinyl alcohol copolymer layer [IV] or a mixed layer of a polyamide resin and an ethylene-vinyl alcohol copolymer [V].
[0036] [8] The multilayer laminated film according to [7], wherein the polyolefin is polyethylene or polypropylene.
[0037] [9] The multilayer laminated film according to [7], wherein the multilayer laminated film is stretched in at least one axial direction.
[0038]
[10] The multilayer laminated film according to [9], wherein the multilayer laminated film is stretched at a stretching ratio of 1.5 to 10 times in at least one axial direction.
[0039]
[11] The multilayer laminated film according to [7], wherein the multilayer laminated film is biaxially stretched.
[0040]
[12] The multilayer laminated film according to
[11] , wherein the multilayer laminated film is biaxially stretched at a stretching ratio of 1.5 to 10 times in each axial direction.
[0041]
[13] The multilayer laminated film according to [7], wherein the bonding layer [II] and
[0042] The total thickness of the polyamide resin layer [III], the ethylene-vinyl alcohol copolymer layer [IV] or the mixed layer of polyamide resin and ethylene-vinyl alcohol copolymer [V] is not more than 12% of the total thickness of the laminate.
[0043] Effects of the Invention
[0044] According to the present invention, a resin composition capable of bonding a plurality of resin layers formed of different resins more firmly than conventional resin compositions can be provided. In addition, the present invention also provides a multilayer laminated film capable of bonding resin layers formed of different resins more firmly than conventional resin compositions. DETAILED DESCRIPTION
[0045] In the present invention, unless otherwise specified, the description of "XX or more and YY or less" and "XX to YY" indicating a numerical range means a numerical range including the lower limit and the upper limit as endpoints.
[0046] Furthermore, when a numerical range is described in stages, the upper limit and the lower limit of each numerical range can be arbitrarily combined.
[0047] The resin composition of the present invention and the multilayer laminated film obtained by using the composition will be described in detail below.
[0048] <Modified ethylene-α-olefin copolymer [A]>
[0049] The modified ethylene-α-olefin copolymer [A] used in the present invention is obtained by modifying a copolymer [A'] of ethylene and an α-olefin having 3 to 20 carbon atoms with an unsaturated carboxylic acid or a derivative thereof, and specifically can be obtained by graft modification.
[0050] (Unmodified ethylene-α-olefin copolymer [A'])
[0051] The copolymer [A'] of ethylene and an α-olefin having 3 to 20 carbon atoms (hereinafter also referred to as unmodified ethylene-α-olefin copolymer [A']) as an unmodified polymer is a copolymer obtained by copolymerizing monomers containing ethylene and an α-olefin having 3 to 20 carbon atoms.
[0052] Examples of α-olefins having 3 to 20 carbon atoms include propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and 1-decene. Among them, α-olefins having 3 to 10 carbon atoms are preferred, and propylene, 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene are more preferred. These α-olefins may be used alone or in combination of two or more.
[0053] The density of the unmodified ethylene-α-olefin copolymer [A'] is usually 0.860 to 0.930 g / cm 3 , preferably 0.860~0.900g / cm 3 , more preferably 0.860 to 0.895 g / cm 3 , particularly preferably 0.860 to 0.890 g / cm 3 within the range.
[0054] The ethylene-α-olefin copolymer [A'] used in the present invention may contain structural units derived from other monomers in addition to the structural units derived from ethylene and α-olefin within a range not impairing its properties.
[0055] Examples of such structural units derived from other monomers include structural units derived from linear non-conjugated dienes such as 1,4-hexadiene, 1,6-octadiene, 2-methyl-1,5-hexadiene, 6-methyl-1,5-heptadiene, and 7-methyl-1,6-octadiene; structural units derived from cyclic non-conjugated dienes such as cyclohexadiene, dicyclopentadiene, methyltetrahydroindene, 5-vinylnorbornene, 5-ethylidene-2-norbornene, 5-methylene-2-norbornene, 5-isopropylidene-2-norbornene, and 6-chloromethyl-5-isopropenyl-2-norbornene; and structural units derived from diene compounds such as 2,3-diisopropylidene-5-norbornene, 2-ethylidene-3-isopropylidene-5-norbornene, and 2-propenyl-2,2-norbornadiene. These other monomers may be used alone or in combination of two or more.
[0056] The content of the structural unit derived from the above-mentioned other monomers is usually 10 mol% or less, preferably 0 to 5 mol%.
[0057] The method for producing the ethylene-α-olefin copolymer [A'] is not particularly limited, and the copolymer can be produced by a conventionally known method using a catalyst such as a Ti-based catalyst, a vanadium (V)-based catalyst, or a Zr-based catalyst.
[0058] The density of the modified ethylene-α-olefin copolymer [A] used in the present invention is 0.860 g / cm 3 Above, 0.930g / cm 3 The following range, preferably 0.860 g / cm 3 Above, 0.900g / cm 3 The following range, more preferably 0.860 g / cm 3 Above and less than 0.900g / cm 3 , further preferably at 0.860 g / cm 3 Above, 0.895g / cm 3 Below, particularly preferably at 0.860 g / cm 3 Above, 0.890g / cm 3 By using the modified ethylene-α-olefin copolymer [A] in such a range, a resin composition having improved bonding strength can be obtained.
[0059] The melt flow rate (MFR; ASTM D 1238, 190°C, load 2.16 kg) of the modified ethylene-α-olefin copolymer [A] is preferably in the range of 0.5 to 10 g / 10 min, more preferably 1 to 5 g / 10 min.
[0060] The graft amount of the unsaturated carboxylic acid or its derivative in the modified ethylene-α-olefin copolymer [A] is in the range of 0.01 to 5% by mass, preferably in the range of 0.1 to 3% by mass, and more preferably in the range of 0.3 to 1% by mass, relative to 100% by mass of the modified ethylene-α-olefin copolymer [A]. By using the modified ethylene-α-olefin copolymer [A] in such a range, a resin composition having improved bonding strength can be obtained.
[0061] Examples of the unsaturated carboxylic acid grafted to the unmodified ethylene-α-olefin copolymer [A'] include acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, and the like. Examples of the derivatives of the unsaturated carboxylic acid include unsaturated carboxylic acid anhydrides, unsaturated carboxylic acid esters, unsaturated carboxylic acid amides, unsaturated carboxylic acid imides, and unsaturated carboxylic acid metal salts. Specific examples of the unsaturated carboxylic acid derivatives include maleic anhydride, nadic anhydride TD (nadic anhydride TD), and nadic anhydride TD (nadic anhydride TD). anhydride: nadic anhydride), itaconic anhydride, citraconic anhydride; methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, glycidyl acrylate, monoethyl maleate, diethyl maleate, monomethyl fumarate, dimethyl fumarate, monomethyl itaconate, diethyl itaconate; acrylamide, methacrylamide, maleic acid monoamide, maleic acid diamide, maleic acid-N-monoethylamide, maleic acid-N,N-diethylamide, maleic acid-N-monobutylamide, maleic acid-N,N-dibutylamide, fumaric acid monoamide, fumaric acid diamide, fumaric acid-N-monobutylamide, fumaric acid-N,N-dibutylamide; maleimide, N-butylmaleimide, N-phenylmaleimide; sodium acrylate, sodium methacrylate, potassium acrylate, potassium methacrylate, etc. Among these unsaturated carboxylic acids or derivatives thereof, maleic anhydride and nadic anhydride TD are preferred, and maleic anhydride is more preferred.
[0062] The method for producing the modified ethylene-α-olefin copolymer [A] using the above-mentioned unsaturated carboxylic acid or its derivative (grafting monomer) and the unmodified ethylene-α-olefin copolymer [A'] as raw materials is not particularly limited.
[0063] As a method for producing the modified ethylene-α-olefin copolymer [A], there are, for example, a melt modification method in which an unmodified ethylene-α-olefin copolymer [A'] is melted in an extruder, a grafting monomer is added to the melt, and graft modification (graft copolymerization) is performed; and a solution modification method in which an unmodified ethylene-α-olefin copolymer [A'] is dissolved in a solvent, and a grafting monomer is added to the resulting solution to perform graft modification. Among these, the melt modification method is preferred.
[0064] In any manufacturing method, in order to make the graft monomer graft copolymerize efficiently, it is preferred to react in the presence of a free radical initiator. There is no particular limitation on the free radical initiator, as long as it can achieve graft modification of the unsaturated carboxylic acid or its derivative as the graft monomer, and examples thereof include organic peroxides, organic peresters, azo compounds, and the like. Examples of the free radical initiator include organic peroxides such as benzoyl peroxide, dichlorobenzoyl peroxide, diisopropylbenzene peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxyisopropyl)benzene, and lauroyl peroxide; organic peresters such as tert-butyl peracetate, 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, tert-butyl perbenzoate, tert-butyl perphenylacetate, tert-butyl perisobutyrate, tert-butyl persecanoate, tert-butyl perpivalate, isopropyl perpivalate, and tert-butyl perdiethylacetate; and azo compounds such as azoisobutyronitrile and dimethyl azoisobutyrate. Among them, organic peroxides and organic peresters are preferred, and dialkyl peroxides such as dicumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(peroxybenzoate)-3-hexyne, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, and 1,4-bis(tert-butylperoxyisopropyl)benzene are more preferred.
[0065] The radical initiator is usually used in a ratio of 0.001 to 1 part by mass based on 100 parts by mass of the unmodified ethylene-α-olefin copolymer [A']. In the above-mentioned graft modification process, other monomers such as styrene may coexist as graft monomers.
[0066] <Unmodified ethylene-α-olefin copolymer resin [B]>
[0067] The unmodified ethylene-α-olefin copolymer resin [B] used in the present invention is a copolymer resin obtained by copolymerizing a monomer containing ethylene and an α-olefin having 3 to 20 carbon atoms.
[0068] The content of structural units derived from ethylene (ethylene content) in the unmodified ethylene-α-olefin copolymer resin [B] is 70 mol% or more, preferably 75 to 99 mol%.
[0069] Examples of the α-olefins include propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and 1-decene. Among them, propylene, 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene are preferred. These α-olefins may be used alone or in combination of two or more.
[0070] The melting point of the unmodified ethylene-α-olefin copolymer resin [B] is 121° C. or lower, preferably 120° C. or lower, and more preferably 119° C. or lower. The lower limit of the melting point is not particularly limited, but may be 80° C. or higher, for example.
[0071] When the melting point of the copolymer resin [B] is below 121°C, for example, after the layer made of the resin composition of the present invention is stretched, the copolymer resin [B] is more easily melted, so that the stress remaining at the interface between the layer made of the resin composition and the object to be bonded is reduced, thereby increasing the resistance to peeling, and making it possible to bond the layer made of the resin composition to the object to be bonded more firmly. It should be noted that the above melting point is the temperature of the peak position detected on the highest temperature side of the endothermic curve measured by a differential scanning calorimeter (DSC).
[0072] The density of the unmodified ethylene-α-olefin copolymer resin [B] is preferably less than 0.930 g / cm 3 , more preferably 0.915 g / cm 3 The lower limit of the density is not limited, but may be, for example, 0.900 g / cm 3 above.
[0073] When the density of the copolymer resin [B] is less than 0.930 g / cm 3 When the resin composition of the present invention is used, for example, a multilayer laminated film including a layer obtained from the resin composition of the present invention can be made soft. Therefore, the stress when attempting to peel the layer obtained from the resin composition of the present invention contained in the multilayer laminated film from other layers is dispersed, and the layer obtained from the resin composition of the present invention and other layers (for example, an intermediate layer having excellent barrier properties) in the multilayer laminated film can be more firmly bonded.
[0074] The melt flow rate (MFR; ASTM D 1238, 190°C, load 2.16 kg) of the unmodified ethylene-α-olefin copolymer resin [B] is preferably in the range of 0.5 to 10 g / 10 min, more preferably 1 to 5 g / 10 min.
[0075] The unmodified ethylene-α-olefin copolymer resin [B] can be produced by a conventionally known method using a catalyst such as a titanium (Ti)-based catalyst or a zirconium (Zr)-based catalyst.
[0076] <Unmodified ethylene-α-olefin copolymer elastomer [C]>
[0077] The unmodified ethylene-α-olefin copolymer elastomer [C] used in the present invention is a copolymer of ethylene and an α-olefin having 3 to 20 carbon atoms, and its density is usually less than 0.900 g / cm 3 , preferably at 0.860 g / cm 3Above and below 0.900g / cm 3 , more preferably 0.860 to 0.895 g / cm 3 In the range of 0.860 to 0.890 g / cm 3 within the range.
[0078] The unmodified ethylene-α-olefin copolymer elastomer [C] preferably has a melt flow rate (MFR; ASTM D 1238, 190°C, load 2.16 kg) of 1 to 12 g / 10 min, more preferably 2 to 6 g / 10 min.
[0079] Specific examples and preferred examples of the α-olefin having 3 to 20 carbon atoms are the same as those in the case of the unmodified ethylene-α-olefin copolymer [A'].
[0080] The ethylene-α-olefin copolymer elastomer [C] used in the present invention may further contain structural units derived from other monomers in addition to the structural units derived from ethylene and α-olefins within a range that does not impair its properties. Specific examples of other monomers and the preferred range of the content of the structural units derived from other monomers are the same as those in the case of the unmodified ethylene-α-olefin copolymer [A'].
[0081] The method for producing the ethylene-α-olefin copolymer elastomer [C] is not particularly limited, but it can be produced by a conventionally known method using a catalyst such as a Ti-based catalyst, a vanadium (V)-based catalyst, or a Zr-based catalyst.
[0082] <Resin composition>
[0083] The melt flow rate (ASTM D 1238, 190°C, load 2.16 kg) of the resin composition of the present invention is in the range of 0.1 to 50 g / 10 minutes, preferably 0.2 to 10 g / 10 minutes, and more preferably 0.5 to 5 g / 10 minutes. Since the melt flow rate of the resin composition is in the above range, the resin composition has excellent moldability.
[0084] The graft amount of the unsaturated carboxylic acid or its derivative is in the range of 0.01 to 1.0% by weight, preferably in the range of 0.1 to 0.8% by weight, relative to 100% by weight of the entire resin composition of the present invention. Within such a range of the graft amount, a resin composition having improved bonding strength can be obtained.
[0085] The melting point of the resin composition of the present invention is preferably 119° C. or lower, more preferably 100 to 119° C., and further preferably 100 to 110° C. A resin composition having such a melting point can more easily and firmly bond a plurality of resin layers made of different resins than conventional resin compositions.
[0086] The density of the resin composition of the present invention is preferably 0.875 to 0.920 g / cm 3 , more preferably 0.880 to 0.910 g / cm 3 When the density of the resin composition of the present invention is 0.920 g / cm 3 When the above conditions are met, for example, a multilayer laminated film including a layer formed by the resin composition of the present invention tends to become soft, and when the layer formed by the resin composition of the present invention is peeled off from the multilayer laminated film, the stress tends to be dispersed, so that the resin layers constituting the laminated film can be more firmly bonded to each other.
[0087] In the resin composition of the present invention, the mass ratio ([A]+[C]) / [B] of the modified ethylene-α-olefin copolymer [A] and the unmodified ethylene-α-olefin copolymer elastomer [C] to the unmodified ethylene-α-olefin copolymer resin [B] is preferably 95 / 5 to 50 / 50, more preferably 90 / 10 to 60 / 40, further preferably 85 / 15 to 70 / 30, and particularly preferably 85 / 15 to 75 / 25.
[0088] In the resin composition of the present invention, the mass ratio ([A] / [C]) of the modified ethylene-α-olefin copolymer [A] to the unmodified ethylene-α-olefin copolymer elastomer [C] is preferably 50 / 50 to 30 / 70, more preferably 40 / 60 to 25 / 65.
[0089] The resin composition of the present invention may further contain additives and polymers other than [A] to [C] within the range that does not impair the purpose of the present invention. Examples of the additives include tackifiers, heat stabilizers, weather stabilizers, antistatic agents, nucleating agents, pigments, dyes, waxes, etc. Examples of the polymers include polyolefins other than [A] to [C], polyester resins, polyamide resins, etc.
[0090] The resin composition of the present invention exhibits high bonding strength to polyolefins such as polyethylene and polypropylene, polyamide resins, and ethylene-vinyl alcohol copolymers.
[0091] <Preparation of resin composition>
[0092] The resin composition of the present invention is obtained by mixing the above-mentioned components using, for example, a Henschel mixer, a V-type blender, a ribbon blender, a drum blender, etc., and melt-kneading the obtained mixture using, for example, a single-screw extruder, a twin-screw extruder, a kneader, a Banbury mixer, etc. The resin composition can also be formed into a granular form by further subjecting the obtained melt-kneaded product to a granulation step, or by pulverizing a mass obtained by cooling the melt-kneaded product.
[0093] <Multilayer Laminated Film>
[0094] The multilayer laminated film of the present invention is a laminate of three or more layers in which the following layers are laminated in sequence: a polyolefin layer [I] made of polyolefin; a bonding layer [II] made of (prepared from) the resin composition of the present invention obtained as described above; a polyamide resin layer [III], an ethylene-vinyl alcohol copolymer layer [IV] or a mixed layer [V] of a polyamide resin and an ethylene-vinyl alcohol copolymer.
[0095] Examples of the polyolefin forming the polyolefin layer [I] include homopolymers of α-olefins such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and 1-decene, or copolymers made from any two or more of these α-olefins. Among them, polyethylene and polypropylene are preferred, and polyethylene is more preferred.
[0096] The polyethylene may be linear or branched, preferably linear. In addition, the polyethylene may be high-density polyethylene or low-density polyethylene, but preferably low-density polyethylene. That is, the polyethylene is more preferably linear low-density polyethylene.
[0097] Among them, high-density polyethylene refers to polyethylene with a density higher than 0.940g / cm 3 Low-density polyethylene refers to polyethylene with a density of 0.940 g / cm 3 The following polyethylene.
[0098] As the polyamide resin forming the polyamide resin layer [III] and the polyamide resin contained in the mixed layer [V], for example, nylon 6, nylon 66, nylon 610, nylon 12, nylon 11, MXD nylon, amorphous nylon, terephthalic acid / adipic acid / hexamethylenediamine copolymer, etc. are preferably used.
[0099] As the ethylene-vinyl alcohol copolymer forming the ethylene-vinyl alcohol copolymer layer [IV] and the ethylene-vinyl alcohol copolymer contained in the mixed layer [V], a copolymer having a structural unit content derived from ethylene (ethylene content) of 20 to 50 mol% is preferably used. Such an ethylene-vinyl alcohol copolymer can be prepared by saponifying an ethylene-vinyl acetate copolymer.
[0100] From the viewpoint of excellent physical properties of the film after recovery, the total thickness of the bonding layer [II], the polyamide resin layer [III], the ethylene-vinyl alcohol copolymer layer [IV] or the mixed layer [V] of the polyamide resin and the ethylene-vinyl alcohol copolymer in the multilayer laminated film of the present invention is preferably less than 12% of the total thickness of the laminate, and more preferably less than 10% of the total thickness of the laminate.
[0101] In the multilayer laminated film of the present invention, the total thickness of the bonding layer [II], the polyamide resin layer [III], the ethylene-vinyl alcohol copolymer layer [IV] or the mixed layer of the polyamide resin and the ethylene-vinyl alcohol copolymer [V] is usually at least 1% of the total thickness of the laminate.
[0102] Examples of the layer structure of the multilayer laminated film of the present invention include the following layer structures.
[0103] (1) Three-layer laminated film of polyolefin layer [I] / adhesive layer [II] / polyamide resin layer [III]
[0104] (2) Three-layer laminated film of polyolefin layer [I] / bonding layer [II] / ethylene-vinyl alcohol copolymer layer [IV]
[0105] (3) Three-layer laminated film of polyolefin layer [I] / bonding layer [II] / mixed layer of polyamide resin and ethylene-vinyl alcohol copolymer [V]
[0106] (4) Four-layer laminated film of polyolefin layer [I] / adhesive layer [II] / polyamide resin layer [III] / ethylene-vinyl alcohol copolymer layer [IV]
[0107] (5) Four-layer laminated film of polyolefin layer [I] / bonding layer [II] / ethylene-vinyl alcohol copolymer layer [IV] / polyamide resin layer [III]
[0108] (6) Four-layer laminated film of polyolefin layer [I] / bonding layer [II] / mixed layer of polyamide resin and ethylene-vinyl alcohol copolymer [V] / polyamide resin layer [III]
[0109] (7) Four-layer laminated film of polyolefin layer [I] / bonding layer [II] / mixed layer of polyamide resin and ethylene-vinyl alcohol copolymer [V] / ethylene-vinyl alcohol copolymer layer [IV]
[0110] (8) Five-layer laminated film of polyolefin layer [I] / adhesive layer [II] / polyamide resin layer [III] / adhesive layer [II] / polyolefin layer [I]
[0111] (9) Five-layer laminated film of polyolefin layer [I] / adhesive layer [II] / ethylene-vinyl alcohol copolymer layer [IV] / adhesive layer [II] / polyolefin layer [I]
[0112] (10) Five-layer laminated film of polyolefin layer [I] / adhesive layer [II] / mixed layer of polyamide resin and ethylene-vinyl alcohol copolymer [V] / adhesive layer [II] / polyolefin layer [I]
[0113] (11) Four-layer laminated film of polyolefin layer [I] / bonding layer [II] / ethylene-vinyl alcohol copolymer layer [IV] / bonding layer [II]
[0114] (12) Four-layer laminated film of polyolefin layer [I] / bonding layer [II] / polyamide resin layer [III] / bonding layer [II]
[0115] The multilayer laminated film of the present invention, such as a three-layer laminated film, can be produced by laminating, for example, a polyolefin layer [I], a bonding layer [II], a polyamide resin layer [III], an ethylene-vinyl alcohol copolymer layer [IV] or a mixed layer [V] of a polyamide resin and an ethylene-vinyl alcohol copolymer in a molten state.
[0116] The multilayer laminated film of the present invention can be produced, for example, by a method of co-extrusion molding the resins forming the respective layers.
[0117] The multilayer laminated film of the present invention can be obtained by setting the molding speed to, for example, 20 m / min or more, preferably to a high speed of 20 to 150 m / min, when performing the above-mentioned coextrusion molding or T-die casting molding, thereby showing high bonding strength.
[0118] The multilayer laminated film of the present invention may be in an unstretched state after being formed, or may be in a state after being stretched in at least one axial direction, preferably in two axial directions. When the multilayer laminated film contains a polyamide resin layer [III], it is preferably used after being stretched. In addition, when the multilayer laminated film contains an ethylene-vinyl alcohol copolymer layer [IV], it can be used in both an unstretched state and a stretched state. A high-strength film can be obtained by stretching, so when the film needs high strength, a stretched multilayer laminated film is preferably used. Usually, when the film is stretched, the bonding force of the bonding layer is greatly reduced, but even if the multilayer laminated film of the present invention is stretched, the bonding force is not greatly reduced, and the bonding force is sufficiently high. When the multilayer laminated film is stretched, the stretching is preferably carried out at a stretching ratio of 1.5 to 10 times, preferably 1.5 to 6 times, in one axial direction. In addition, in the case of biaxial stretching, it is preferably stretched at a stretching ratio of 1.5 to 10 times, preferably 1.5 to 6 times, in two axial directions (each axial direction).
[0119] The stretching conditions for manufacturing a multilayer laminated film as a shrink film are that the stretching temperature is usually 70 to 130°C, and the stretching ratio (film longitudinal direction × film width direction) is usually 2×2 to 5×5 times. The thickness of the film manufactured under this condition is usually 10 to 200 μm. Such a film can be heat-shrunk in length or width by usually 5% to 50% between 70 and 130°C, for example.
[0120] The resin composition of the present invention exhibits excellent bonding strength relative to other resins (eg, ethylene-vinyl alcohol copolymer).
[0121] Furthermore, the multilayer laminated film of the present invention exhibits excellent bonding strength even when stretched, and is excellent in strength and gas barrier properties.
[0122] Therefore, the multilayer laminated film of the present invention can be suitably used, for example, in the form of a shrink film for packaging general foods and for packaging meat such as ham.
[0123] Example
[0124] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.
[0125] The polymers and the like used in Examples and Comparative Examples are shown below.
[0126] [Modified ethylene-α-olefin copolymer (A)]
[0127] As the modified ethylene-α-olefin copolymer (A), the following was used.
[0128] Maleic anhydride modified ethylene-1-butene copolymer (A-1)
[0129] MFR (190°C, load 2.16 kg) = 2.4 g / 10 min, density = 0.885 g / cm 3 , maleic anhydride grafting amount = 0.5 mass %.
[0130] Maleic anhydride modified ethylene-1-hexene copolymer (A-2)
[0131] MFR (190°C, load 2.16 kg) = 4.0 g / 10 min, density = 0.920 g / cm 3 , maleic anhydride grafting amount = 2.0 mass %.
[0132] [Ethylene-α-olefin copolymer resin (B)]
[0133] As the ethylene-α-olefin copolymer resin (B), the following products were used.
[0134] Ethylene-1-butene copolymer resin (B-1)
[0135] MFR (190°C, load 2.16 kg) = 2.6 g / 10 min, density = 0.918 g / cm 3 , melting point = 119°C
[0136] Ethylene-1-hexene copolymer resin (B-2)
[0137] MFR (190°C, load 2.16 kg) = 2.0 g / 10 min, density = 0.913 g / cm 3 , melting point = 113°C
[0138] Ethylene-1-butene copolymer resin (B-3)
[0139] MFR (190°C, load 2.16 kg) = 2.0 g / 10 min, density = 0.918 g / cm 3 , melting point = 122°C
[0140] [Ethylene-α-olefin copolymer elastomer (C)]
[0141] As the ethylene-α-olefin copolymer elastomer (C), the following was used.
[0142] Ethylene-propylene copolymer elastomer (C-1)
[0143] MFR (190°C, load 2.16 kg) = 3.0 g / 10 min, density = 0.869 g / cm 3
[0144] Ethylene-1-butene copolymer elastomer (C-2)
[0145] MFR (190°C, load 2.16 kg) = 3.6 g / 10 min, density = 0.885 g / cm 3
[0146] The physical properties of the polymers and resin compositions used in Examples and Comparative Examples were measured by the following methods.
[0147] [Measurement methods of physical properties]
[0148] <Melt Flow Rate (MFR)>
[0149] The MFR was measured in accordance with ASTM D1238 at a temperature of 190° C. and a load of 2.16 kg.
[0150] <density>
[0151] The density was measured according to ASTM D1505 (density gradient tube method).
[0152] <Grafting Amount (Amount of Structural Units Derived from Maleic Anhydride)>
[0153] The characteristic peak 1790 cm-1 derived from maleic anhydride was analyzed by infrared absorption analysis. ﹣1 The intensity of the grafted structure was measured, and the grafted amount (the amount of structural units derived from maleic anhydride) was quantified using a pre-made calibration curve.
[0154] <Melting point>
[0155] The melting point of the ethylene-α-olefin copolymer resin (B) was measured by differential scanning calorimetry (DSC) according to the following method.
[0156] About 5 mg of a sample was sealed in an aluminum bowl, and the temperature was raised from room temperature to 200°C at a rate of 10°C / min using DSCRDC220 manufactured by Seiko Instruments. After keeping the temperature at 200°C for 5 minutes, the temperature was lowered from 200°C to -100°C at a rate of 10°C / min, and after further keeping the temperature at -100°C for 5 minutes, the temperature was raised to 200°C at a rate of 10°C / min. The melting point was determined from the endothermic curve in this case.
[0157] It should be noted that the melting point is the temperature at the peak position of the endothermic curve measured by DSC. In addition, when a plurality of characteristic peaks are detected during the measurement, the peak temperature detected on the highest temperature side is defined as the melting point.
[0158] [Example 1]
[0159] <Manufacturing of resin composition>
[0160] Maleic anhydride-modified ethylene-1-butene copolymer (A-1): 30% by mass,
[0161] Ethylene-1-butene copolymer resin (B-1): 20% by mass,
[0162] Ethylene-propylene copolymer elastomer (C-1): 20% by mass, and
[0163] Ethylene-1-butene copolymer elastomer (C-2): 30 mass%
[0164] The mixture was melt-kneaded using a single screw extruder at 200°C to obtain a resin composition (1). The obtained resin composition had an MFR of 2.8 g / 10 min and a density of 0.888 g / cm 3 , the maleic anhydride grafting amount is 0.15 mass %.
[0165] <Manufacturing of Laminated Body>
[0166] An ethylene-vinyl alcohol copolymer (EVOH: EVAL J171B manufactured by Kuraray Co., Ltd., MFR (190°C, load 2.16 kg) = 1.7 g / 10 min, ethylene content = 32 mol%), the above resin composition (1) and a linear low-density polyethylene (PE: Ult-Zex 2021L manufactured by Primen Polymer Co., Ltd., MFR (190°C, load 2.16 kg) = 2.0 g / 10 min, density = 0.920 g / cm 3 ), three types of 5-layer co-extruded cast films were formed under the following conditions.
[0167] <Molding conditions>
[0168] Molding device: die head diameter Extruder (for PE layer)
[0169] Set temperature: 220℃
[0170] Die head diameter Extruder (for resin composition (1) layer)
[0171] Set temperature: 220℃
[0172] Die head diameter Extruder (for EVOH layer)
[0173] Set temperature: 220℃
[0174] Forming speed: 20m / min
[0175] Under the above conditions, the film layer composition and the thickness of each layer are PE (outer layer) / resin composition (1) / EVOH (middle layer) / resin composition (1) / PE (inner layer) = 30 / 15 / 10 / 15 / 30 μm.
[0176] The five-layer film obtained as described above was heated at 110° C. for 1 minute using a stretching apparatus manufactured by Bruckner, and then stretched 3 times in the MD direction at the same temperature to prepare a stretched film.
[0177] In addition, under the same conditions as above, a five-layer film having a film layer composition and layer thickness of PE (outer layer) / resin composition (1) / EVOH (middle layer) / resin composition (1) / PE (inner layer) = 60 / 30 / 20 / 30 / 60 μm was heated at 110°C for 1 minute using a stretching device manufactured by Bruckner, and then stretched 4.5 times in the MD direction at the same temperature to prepare a stretched film.
[0178] After the obtained stretched film was stored at room temperature for 1 week, it was cut into 15 mm wide pieces and subjected to T-type peeling at a peeling speed of 300 mm / min to obtain the interlayer adhesion (peel strength) between the resin composition layer (1) on the inner layer side and the EVOH layer. The physical properties of the obtained resin composition and stretched film are shown in Table 1.
[0179] [Example 2]
[0180] A resin composition was produced in the same manner as in Example 1 except that the mixing formulation was changed to that shown in Table 1, and a stretched film was produced in the same manner as in Example 1.
[0181] Table 1 shows the physical properties of the obtained resin composition and stretched film.
[0182] [Comparative Example 1]
[0183] A resin composition was produced in the same manner as in Example 1 except that the mixing formulation was changed to that shown in Table 1, and a stretched film was produced in the same manner as in Example 1.
[0184] Table 1 shows the physical properties of the obtained resin composition and stretched film.
[0185] [Comparative Example 2]
[0186] A resin composition was produced in the same manner as in Example 1 except that the mixing formulation was changed to that shown in Table 1, and a stretched film was produced in the same manner as in Example 1.
[0187] Table 1 shows the physical properties of the obtained resin composition and stretched film.
[0188] [Table 1]
[0189]
Claims
1. A resin composition, characterized in that contain: [I] A modified ethylene-α-olefin copolymer [A] obtained by modifying a copolymer of ethylene and an α-olefin having 3 to 20 carbon atoms with an unsaturated carboxylic acid or a derivative thereof, wherein the modified ethylene-α-olefin copolymer [A] satisfies the following (i) and (ii), (i) Density 0.860 g / cm 3 Above and less than 0.900g / cm 3 range, (ii) the grafting amount is 0.01 to 5% by mass; [II] an unmodified ethylene-α-olefin copolymer resin [B] having a melting point of 121° C. or less; and [III] an unmodified ethylene-α-olefin copolymer elastomer [C], The melt flow rate (ASTM D 1238, 190°C, load 2.16 kg) of the resin composition is in the range of 0.1 to 50 g / 10 minutes. The graft amount of the unsaturated carboxylic acid or its derivative is in the range of 0.01 to 1.0 mass % based on 100 mass % of the entire resin composition.
2. The resin composition according to claim 1, characterized in that The density of the unmodified ethylene-α-olefin copolymer resin [B] is 0.900 g / cm 3 above, The density of the unmodified ethylene-α-olefin copolymer elastomer [C] is less than 0.900 g / cm 3 .
3. The resin composition according to claim 1 or 2, characterized in that The melting point of the resin composition is below 119°C.
4. The resin composition according to claim 1 or 2, characterized in that The density of the unmodified ethylene-α-olefin copolymer resin [B] is less than 0.930 g / cm 3 .
5. The resin composition according to claim 1 or 2, characterized in that The density of the unmodified ethylene-α-olefin copolymer resin [B] is 0.915 g / cm 3 the following.
6. The resin composition according to claim 1 or 2, characterized in that The density of the resin composition is 0.875-0.920 g / cm 3 .
7. A multi-layer laminate film, characterized in that The multilayer laminated film is a laminated body of three or more layers in which the following layers are laminated in sequence, polyolefin layer [I]; A bonding layer [II] comprising the resin composition according to claim 1 or 2; and A polyamide resin layer [III], an ethylene-vinyl alcohol copolymer layer [IV] or a mixed layer of a polyamide resin and an ethylene-vinyl alcohol copolymer [V].
8. The multi-layer laminated film according to claim 7, wherein: The polyolefin is polyethylene or polypropylene.
9. The multi-layer laminated film according to claim 7, wherein: The multi-layer laminate film is stretched in at least one axial direction.
10. The multi-layer laminated film according to claim 9, wherein The multi-layer laminated film is stretched at a stretching ratio of 1.5 to 10 times in at least one axial direction.
11. The multi-layer laminated film according to claim 7, wherein: The multi-layer laminated film is biaxially stretched.
12. The multi-layer laminated film according to claim 11, wherein The multi-layer laminated film is biaxially stretched at a stretching ratio of 1.5 to 10 times in each axial direction.
13. The multi-layer laminated film according to claim 7, wherein: Bonding layer [II] and The total thickness of the polyamide resin layer [III], the ethylene-vinyl alcohol copolymer layer [IV] or the mixed layer of polyamide resin and ethylene-vinyl alcohol copolymer [V] is not more than 12% of the total thickness of the laminate.
Citation Information
Patent Citations
Adhesive polyethylene composition and multilayer laminated film prepared by using the same
JP1997249779A