Reactive extrusion composition, method for enhancing mechanical mechanisms of PLA / p (3HP) blends, and PLA / p (3HP) blends prepared therefrom
By performing interfacial coupling reaction during the extrusion process and using chain extenders and reactive compatibilizers to form PLA-g-P(3HP) copolymer, the problem of low mechanical properties of PLA/P(3HP) blends is solved. Its tensile strength and elongation at break are significantly improved, and excellent mechanical properties and biodegradability are achieved.
Patent Information
- Application Number
- CN202480002151.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-01-15
- Filing Date
- 2024-01-18
- Publication Date
- 2024-11-26
AI Technical Summary
PLA/P(3HP) blends have problems with low elongation and impact resistance in terms of mechanical properties, and existing blending methods are difficult to effectively improve their physical properties.
By using the reactive extrusion composition to perform an interfacial coupling reaction during the extrusion process, PLA-g-P(3HP) copolymer is formed, increasing the interfacial coupling reaction efficiency, forming a smaller dispersed phase and a denser network structure, thereby Improve impact resistance and improve interface bond strength by selecting suitable chain extenders and reactive compatibilizers.
The tensile strength and elongation of the PLA/P (3HP) blend are significantly improved, and its mechanical properties are improved while maintaining biodegradability.
Smart Images

Figure CN119032134A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a reactive extrusion composition, a method for enhancing the mechanical properties of a PLA / P(3HP) blend, and a PLA / P(3HP) blend having enhanced mechanical properties made therefrom. Background Art
[0002] In recent years, due to the increase in the amount of polymer waste, environmental pollution problems have become increasingly prominent, and therefore, research on biodegradable polymers has been actively carried out. PLA (polylactic acid) is a general biodegradable polymer that has excellent thermal processability, mechanical properties, chemical resistance and economic feasibility, and can therefore replace other existing petrochemical products, but due to its rigid molecular structure, it has the disadvantages of low elongation and impact resistance. Therefore, it has been considered to enhance the physical properties of PLA by modifying it with a plasticizer or copolymerizing or blending it with a highly flexible polymer.
[0003] When copolymerizing or blending with PLA, P(3HP) can be considered. P(3HP) is a biodegradable polymer with good flexibility and low thermal stability, but when blended with PLA, the low thermal stability of P(3HP) and the low elongation and impact strength of PLA can complement each other.
[0004] However, even when a blending method is used, it is important to apply conditions that can reduce the dispersed phase size between the resins to be mixed, increase the adhesive strength of the resin interface, and enhance the physical properties (such as mechanical and optical properties) of the blend. Summary of the invention
[0005] Technical issues
[0006] An object of the present application is to provide a PLA / P(3HP) blend with enhanced mechanical properties.
[0007] Another object of the present application is to provide a method for enhancing the mechanical properties (eg, elongation) of resin blends.
[0008] The above-mentioned objects and other objects of the present application can be solved by the present application, which will be described in detail below.
[0009] Technical Solution
[0010] According to a specific embodiment related to the present application, a reactive extrusion composition, a method for enhancing the mechanical properties of a blend of PLA (polylactic acid) and P(3HP) (poly(3-hydroxypropionate)) and a PLA / P(3HP) blend having enhanced mechanical properties prepared therefrom are provided.
[0011] The inventor of the present application has extensively studied the blend of PLA and P (3HP) with enhanced physical properties (e.g., mechanical properties, such as tensile strength, elongation, etc.) and biodegradability, and has completed the invention of the present application. Specifically, in the large-scale production of the blend, reactive extrusion can be used to form PLA-gP (3HP) copolymers through interfacial coupling reaction during extrusion, wherein PLA-gP (3HP) copolymers can be used as a compatibilizer to reduce the interfacial tension between the two phases. When the efficiency of this interfacial coupling reaction becomes high, a network structure with a smaller and denser distribution of the dispersed phase can be formed, making the impact energy easier to propagate and dissipate in the entire matrix, thereby improving impact resistance. In addition, as the amount of the PLA-gP (3HP) copolymer interface produced increases, tensile strength increases, and elongation at break can also be improved. On the other hand, when PLA and P (3HP) are simply blended, the interfacial adhesion between the two phases is low. Therefore, when a force is applied, the force acts on the weak part of the interface, thereby easily causing fracture.
[0012] Hereinafter, in order to improve the problems of the prior art and achieve the technical purpose of the present application, a reactive extrusion composition of predetermined components, a reactive extrusion method carried out under specific conditions, and a PLA / P(3HP) blend produced therefrom will be described in more detail.
[0013] In one embodiment related to the present application, the present application relates to a reactive extrusion composition. By this description, the reactive extrusion composition is intended for reactive extrusion and may be a composition comprising the components described below. Alternatively, the reactive extrusion composition may refer to a composition that satisfies a predetermined complex viscosity when heated (e.g., heated at a temperature range of 150 to 300° C.). For example, a reactive extrusion composition is provided, comprising 100 parts by weight of a resin component containing PLA and P (3HP); 0.2 to 15 parts by weight of an epoxy-containing chain extender; and 0.2 to 15 parts by weight of a reactive compatibilizer, wherein the reactive compatibilizer comprises an epoxy group and a vinyl group.
[0014] The composition includes predetermined components in addition to PLA and P(3HP) to enhance the interfacial coupling reaction between two phases, ie, PLA (polylactic acid) and P(3HP) (poly(3-hydroxypropionate)).
[0015] According to a specific embodiment of the present application, the reactive extrusion composition includes a resin component containing PLA and P(3HP); a reactive compatibilizer; and a chain extender. In a blend of PLA and P(3HP), when the reactive compatibilizer and the chain extender are mixed / reacted together, a synergistic effect is generated, thereby improving the extrusion mixing performance (for example, the size of the dispersed phase is small, which can improve the mixing performance), and the coupling reaction efficiency between the resin interfaces can be increased.
[0016] In an exemplary embodiment, the resin component in the reactive extrusion composition can include 30 to 95% by weight of PLA and 5 to 70% by weight of P (3HP). Specifically, the content of PLA in the resin component can be, for example, 35% by weight or more, 40% by weight or more, 45% by weight or more, 50% by weight or more, 55% by weight or more, 60% by weight or more, 65% by weight or more, 70% by weight or more, 75% by weight or more, 80% by weight or more, 85% by weight or more, 90% by weight or more. And the upper limit of its content can be, for example, 90% by weight or less, 85% by weight or less, 80% by weight or less, 75% by weight or less, 70% by weight or less, 65% by weight or less, 60% by weight or less, 55% by weight or less. Based on 100% by weight of the resin component, P (3HP) can be included in the remaining content except the above-mentioned PLA content. Within the above-mentioned content range, the low thermal stability of P (3HP) and the low elongation and impact strength of PLA can complement each other.
[0017] In an exemplary embodiment, the PLA in the resin component can be used in excess relative to P(3HP). That is, relatively excessive PLA is a continuous phase, and a relatively small amount of P(3HP) is a dispersed phase. For example, the resin component can contain 70 to 90% by weight of PLA, and the remainder can be occupied by P(3HP). Specifically, the PLA content of the resin component can be more than 75% by weight, more than 80% by weight, or more than 85% by weight, and the upper limit of the content can be, for example, less than 85% by weight, less than 80% by weight, or less than 75% by weight. At this time, based on 100% by weight of the resin component, P(3HP) can be included in the resin component in an amount other than the above-mentioned PLA content.
[0018] The molecular weight of the resin component may be controlled at a level that can ensure tensile strength and improved elongation at break, which will be described below.
[0019] In an exemplary embodiment, the weight average molecular weight of PLA may be in the range of 50,000 to 400,000. Specifically, the weight average molecular weight of PLA may be, for example, 60,000 or more, 80,000 or more, 100,000 or more, 120,000 or more, 140,000 or more, 150,000 or more, or 170,000 or more, and, for example, 350,000 or less, 320,000 or less, 300,000 or less, 250,000 or less, 230,000 or less, or 200,000 or less. If the weight average molecular weight of PLA is too low, mechanical properties may be reduced, and if the weight average molecular weight of PLA is too large, processability may be reduced.
[0020] In an exemplary embodiment, the weight average molecular weight of P(3HP) may be, for example, in the range of 2,000 or more to 200,000 or less. Specifically, the weight average molecular weight of P(3HP) may be, for example, 5,000 or more, 7,000 or more, 10,000 or more, 13,000 or more, 15,000 or more, or 20,000 or more, and, for example, 150,000 or less, 130,000 or less, 100,000 or less, 80,000 or less, 70,000 or less, 50,000 or less, 40,000 or less, or 30,000 or less. If the weight average molecular weight of P(3HP) is too low, mechanical properties may be reduced, and if the weight average molecular weight of P(3HP) is too large, processing properties may be reduced.
[0021] In an exemplary embodiment, P(3HP) may have a lower molecular weight than PLA. In a specific embodiment of the present application, when PLA is in excess relative to P(3HP), P(3HP) may have a lower molecular weight than PLA. Specifically, the inventors of the present application have found through experiments that: the chain extender described below selectively reacts with the P(3HP) phase rather than the PLA phase (i.e., the chain extender has a higher reactivity with P(3HP)); the chain extender selectively reacts with the dispersed phase P(3HP) dispersed in the continuous phase PLA, thereby increasing its molecular weight and viscosity; through the chain extension reaction of P(3HP), the viscosity difference between the high molecular weight PLA and the low molecular weight P(3HP) is reduced, thereby improving the extrusion mixing performance (for example, due to the improved mixing efficiency, the dispersed phase P3HP is less broken), and the improvement of the extrusion mixing performance promotes the coupling reaction with the reactive compatibilizer at the interface between PLA and P(3HP), thereby improving the compatibility between P(3HP) and PLA (for example, the dispersed phase size is reduced) and the interfacial adhesion, and improving the tensile properties. At this time, the relatively high reactivity between the chain extender and P(3HP) is due to the higher affinity between the two components in terms of chemical structure.
[0022] The type and / or content of the reactive compatibilizer and chain extender included in the composition together with the resin component may be determined to a level capable of improving the interfacial coupling reaction between PLA and P(3HP) and achieving the technical purpose of the present application.
[0023] In the present application, the chain extender can be a component in the PLA / P(3HP) blend, that is, in the state where PLA and P(3HP) are mixed, that selectively extends the P(3HP) chain. For P(3HP) that selectively reacts with the chain extender, its viscosity and molecular weight increase, which can reduce the viscosity difference between high molecular weight PLA and low molecular weight P(3HP), and can also improve extrusion kneading efficiency and mechanical properties.
[0024] The type of chain extender is not particularly limited as long as it does not hinder the achievement of the technical purpose of the present application. For example, epoxy compounds, acid anhydride compounds or oxazoline compounds can be used as chain extenders.
[0025] For example, epoxy compounds may contain or the functional groups of the units derived therefrom, the anhydride compounds may contain such as or the functional groups of the units derived therefrom, the oxazoline compounds may contain such as Or the functional group of the unit derived therefrom.
[0026] In an exemplary embodiment, as a chain extender, a chain extender containing at least one reactive functional group (e.g., epoxy (glycidyl)) can be used. In this case, the chain extender can include, for example, 2 or more reactive functional groups, specifically 2 to 15 functional groups. Such chain extenders can include, but are not limited to, poly (alkyl glycol) diglycidyl ether (e.g., poly (ethylene glycol) diglycidyl ether, poly (propylene glycol) diglycidyl ether, etc.), trimethylolpropane triglycidyl ether, 1,4-butanediol diglycidyl ether, etc.
[0027] In an exemplary embodiment, the weight average molecular weight of the chain extender may be 200 g / mol or more and 10,000 g / mol or less.
[0028] In an exemplary embodiment, the reactive extrusion composition may include 0.2 to 15 parts by weight of a chain extender based on 100 parts by weight of the above-mentioned resin component. Specifically, the content of the chain extender may be less than 10 parts by weight or less than 5 parts by weight based on 100 parts by weight of the resin component, and its lower limit may be more than 0.5 parts by weight, more than 1.0 parts by weight, more than 1.5 parts by weight, or more than 2.0 parts by weight. If the content is lower than the above range, the physical property improvement effect is small, and if the content exceeds the above range, the physical properties may be deteriorated due to unreacted chain extender. In view of this, the chain extender may be included in the composition at 0.2 to 5 parts by weight based on 100 parts by weight of the resin component.
[0029] In addition, the reactive extrusion composition may include 1.0 to 15 parts by weight of a chain extender based on 100 parts by weight of the PLA resin. Specifically, the content of the chain extender may be 10 parts by weight or less or 5 parts by weight or less based on 100 parts by weight of the PLA resin, and the lower limit thereof may be 1.2 parts by weight or more, 1.3 parts by weight or more, 1.5 parts by weight or more, or 2.0 parts by weight or more.
[0030] The reactive compatibilizer may contain a reactive functional group capable of reacting with the chain end groups (e.g., -OH or -COOH) of the polyester polymers PLA and P(3HP). The reactive functional group contained in the reactive compatibilizer may include at least one selected from, for example, epoxy, isocyanate, isocyanurate, etc. Examples of reactive compatibilizers containing epoxy groups include compatibilized products such as Joncryl ADR, examples of reactive compatibilizers containing isocyanate groups include polyhexamethylene diisocyanate, etc., and examples of reactive compatibilizers containing isocyanurate groups include triglycidyl isocyanurate, etc.
[0031] The reactive compatibilizer can include, for example, 1 to 30 or 3 to 30 reactive functional groups.
[0032] The above-mentioned reactive compatibilizers may include a vinyl group in addition to the reactive functional group.
[0033] In an exemplary embodiment, the reactive compatibilizer may include an epoxy group, that is, it may be an epoxy-containing reactive compatibilizer. Further, the reactive compatibilizer may contain an epoxy group and a vinyl group, that is, it may be a polymer containing an epoxy group and a vinyl group. Since the reactive compatibilizer contains both an epoxy group and a vinyl group, the reaction efficiency and the storage stability of the raw material can be improved.
[0034] The molecular weight of the reactive compatibilizer can be determined by considering the affinity solubility of the polymer and the rate of penetration into the PLA phase. For example, the weight average molecular weight of the reactive compatibilizer can be in the range of 1,000 g / mol to 15,000 g / mol, 3,000 g / mol to 13,000 g / mol, 5,000 g / mol to 10,000 g / mol.
[0035] Epoxy equivalent weight is the number of reactive epoxy functional groups, which is related to the number of PLA and P3HP polymers bonded to the reactive compatibilizer. For example, the reactive compatibilizer can meet an epoxy equivalent of 200 g / eq or more and 600 g / eq or less, 250 g / eq or more and 550 g / eq or less, 300 g / eq or more and 500 g / eq or less, or 350 g / eq or more and 485 g / eq or less. If the epoxy equivalent exceeds the above range, the effect of using the compatibilizer may be small, and if the epoxy equivalent is below the above range, it may become too hard while forming a cross-linked polymer structure.
[0036] Vinyl equivalent weight is the number of reactive vinyl functional groups, wherein vinyl is related to the number of PLA and P3HP polymers bonded to the reactive compatibilizer. For example, the reactive compatibilizer can meet a vinyl equivalent weight of more than 100 g / eq and less than 1000 g / eq, more than 120 g / eq and less than 900 g / eq, more than 140 g / eq and less than 800 g / eq, more than 170 g / eq and less than 700 g / eq, or more than 190 g / eq and less than 500 g / eq. If the vinyl equivalent exceeds the above range, the effect of using the compatibilizer may be less, and if the vinyl equivalent is lower than the above range, it may become too hard due to an increase in the degree of crosslinking.
[0037] In an exemplary embodiment, based on 100 parts by weight of resin components, the reactive extrusion composition may include 0.2 to 15 parts by weight of reactive compatibilizer. Specifically, based on 100 parts by weight of resin components, the content of reactive compatibilizer may be less than 10 parts by weight, or less than 5 parts by weight, and its lower limit may be more than 0.3 parts by weight, more than 0.5 parts by weight, more than 0.6 parts by weight, or more than 1.0 parts by weight. If the content of reactive compatibilizer is lower than the above range, it is difficult to expect the compatibility improvement effect, and if the content of reactive compatibilizer exceeds the above range, the mechanical properties of the blended material may deteriorate. Taking this into account, based on 100 parts by weight of resin components, the content range of reactive compatibilizer in the composition may be 0.2 to 5 parts by weight.
[0038] In addition, the reactive extrusion composition may contain 1.5 to 15 parts by weight of a reactive compatibilizer based on 100 parts by weight of the PLA resin. Specifically, based on 100 parts by weight of the PLA resin, the content of the reactive compatibilizer may be 10 parts by weight or less, 5 parts by weight or less, and its lower limit may be 1.7 parts by weight or more, 1.8 parts by weight or more, or 2.0 parts by weight or more.
[0039] The reactive extrusion composition may also contain additives. The additives may be, for example, antioxidants and / or lubricants.
[0040] The lubricant is a component that can assist the extrudate flow and reduce the extrusion load. The specific type of the lubricant is not particularly limited. For example, the lubricant may include at least one selected from a higher fatty acid having a carbon number of 10 to 20 and a salt thereof. For example, stearic acid, zinc stearate, etc. can be used as a lubricant.
[0041] In an exemplary embodiment, the reactive extrusion composition may include a lubricant in an amount ranging from 0.1 to 5 parts by weight, 0.2 to 3 parts by weight, or 0.4 to 2 parts by weight based on 100 parts by weight of the resin component. If the content of the lubricant is lower than the above range, it is difficult to expect the effect of adding the lubricant. If the content of the lubricant exceeds the above range, the physical properties (impact resistance, heat resistance, transparency) of the resin may deteriorate.
[0042] The type of antioxidant is also not particularly limited. For example, products such as Irganox 1010 or Irgafos 168 may be used.
[0043] The content of the antioxidant can be appropriately adjusted to a level that does not affect the technical purpose of the present application. For example, based on 100 parts by weight of the resin component, the reactive extrusion composition can include an antioxidant in an amount ranging from 0.1 to 5 parts by weight, 0.2 to 3 parts by weight, or 0.5 to 2 parts by weight.
[0044] In an exemplary embodiment, the reactive extrusion composition may satisfy a complex viscosity of 2,000 Pa.s or more at 185°C, 0.5% strain, and 0.3 rad / s. Specifically, the complex viscosity of the composition may be 2500 Pa.s or more, 3000 Pa.s or more, 3500 Pa.s or more, 4000 Pa.s or more, 4500 Pa.s or more, 5000 Pa.s or more, 5500 Pa.s or more, 6000 Pa.s or more, 6500 Pa.s or more, 7000 Pa.s or more, 7500 Pa.s or more, or 8000 Pa.s or more. And, its upper limit may be, for example, 25000 Pa.s or less, 20000 Pa.s or less, 15000 Pa.s or less, 10000 Pa.s or less, specifically 9000 Pa.s or less or 8000 Pa.s or less. The composition satisfying the above range is advantageous for providing a blended product having excellent extrusion processability and excellent mechanical properties.
[0045] In another embodiment related to the present application, the present application is directed to an extrusion process for enhancing the mechanical properties of a blend of PLA and P(3HP).
[0046] In a specific embodiment related to the present application, the extrusion method can be a reactive extrusion method. Specifically, the method can be a method comprising reacting a composition containing a compatibilizer and a chain extender in addition to PLA and P(3HP) under predetermined conditions to increase the interfacial coupling reaction between the two phases (i.e., PLA and P(3HP)). Therefore, the extrusion mixing performance can be improved (for example, the small size of the dispersed phase can improve the mixing performance), and the efficiency of the PLA / P(3HP) interfacial coupling reaction can be improved.
[0047] For example, an extrusion method for producing a PLA / P(3HP) blend is provided, the method comprising the following steps: feeding a reactive extrusion composition comprising a resin component containing PLA and P(3HP), a chain extender and a reactive compatibilizer into an extruder having a stirring shaft rotating at 250 rpm or more at a flow rate of 2.0 g / min or more and 7.0 g / min or less within a temperature range of 110° C. or more and 200° C. or less, wherein the reactive extrusion composition comprises 0.2 to 15 parts by weight of the chain extender and 0.2 to 15 parts by weight of the reactive compatibilizer based on 100 parts by weight of the resin component.
[0048] The method may include the step of feeding a reactive extrusion composition including a resin component comprising PLA and P(3HP), a reactive compatibilizer, and a chain extender into an extruder controlled under predetermined conditions.
[0049] The contents of PLA and P(3HP), weight average molecular weight, type and / or content of reactive compatibilizer and chain extender, and type and / or content of additives contained in the resin component of the extrusion composition are the same as those described above for the reactive extrusion composition.
[0050] The process of the present application can be carried out under controlled conditions such that the blends produced from the reactive extrusion composition have excellent mechanical properties (eg, increased elongation).
[0051] Specifically, the method may include the following steps: feeding the reactive extrusion composition into an extruder having a stirring shaft rotating at 250 rpm or more at a flow rate of 2.0 to 7.0 g / min at a temperature range of 110 to 200° C. Experiments have confirmed that when the reactive extrusion conditions are controlled as described above, excellent mechanical properties (e.g., elongation) can be imparted to the blend of PLA and P(3HP).
[0052] In an exemplary embodiment, the extruder can be controlled so that there is a temperature gradient in the conveying direction of the reactive extrusion composition in the extruder. Here, the conveying direction refers to the direction in which the reactive extrusion composition fed into the feed inlet of the extruder moves to the discharge outlet of the extruder.
[0053] The method of imparting the temperature gradient within the extruder is not particularly limited, and a device such as a known sensor may be used.
[0054] In a specific embodiment of the present application, the method may be a method comprising dividing the extruder into at least three zones in the conveying direction, and giving a temperature gradient of low temperature → high temperature → low temperature or low temperature → high temperature → medium temperature to each zone in each conveying direction (the direction from the feed inlet to the discharge outlet). In this case, the corresponding zones may be referred to as the first zone, the second zone, and the third zone in the conveying direction (the direction from the feed inlet to the discharge outlet).
[0055] For example, the method can be a method of imparting a temperature gradient by controlling the temperature of the reactive extrusion composition feed inlet side of the extruder within the range of 120°C to 165°C, controlling the temperature of the reactive extrusion composition discharge outlet side of the extruder within the range of 135°C to 180°C, and controlling the temperature between the feed inlet side and the discharge outlet side within the range of 170°C to 200°C. The feed inlet side can be referred to as the first zone, the discharge outlet side can be referred to as the third zone, and the zone between the first zone and the third zone (i.e., between the feed inlet side and the discharge outlet side) can be referred to as the second zone. It has been experimentally confirmed that when the reactive extrusion conditions are controlled as described above, it is more conducive to imparting excellent mechanical properties (e.g., elongation) to the blend of PLA and P (3HP).
[0056] In an exemplary embodiment, the method may be a method of imparting a temperature gradient such that the temperature of the second zone is higher than the temperatures of the first zone and the third zone.
[0057] In an exemplary embodiment, the method may be a method of imparting a temperature gradient such that the temperature of the first zone is higher than the temperature of the third zone.
[0058] In an exemplary embodiment, the method may be a method of applying a temperature gradient such that the temperature of the third zone is higher than the temperature of the first zone.
[0059] In an exemplary embodiment, at least one of the first zone, the second zone, and the third zone can be divided into at least two zones according to temperature. For example, the first zone can be divided into zone 1-1 and zone 1-2 from the composition feed inlet side to the discharge outlet side, and the third zone can be divided into zone 3-1 and zone 3-2 from the composition feed inlet side to the discharge outlet side. At this time, zone 1-1 and zone 1-2 can be controlled to be the temperature range of zone 1 (120°C to 165°C), and the temperature of zone 1-2 can be higher than the temperature of zone 1-1. In addition, zone 3-1 and zone 3-2 can be controlled within the temperature range of the above-mentioned zone 3 (135°C to 180°C), and the temperature of zone 3-1 can be higher than the temperature of zone 3-2.
[0060] In an exemplary embodiment, the rotation speed of the extruder shaft may be 300 rpm or more, 350 rpm or more, or 400 rpm or more, and its upper limit may be, for example, 500 rpm or less, 450 rpm or less, 400 rpm or less, or 350 rpm or less. It has been experimentally confirmed that when the reactive extrusion conditions are controlled as described above, it is more conducive to imparting excellent mechanical properties (e.g., elongation) to the blend of PLA and P (3HP).
[0061] In one exemplary embodiment, the extruder may include rotor blades.
[0062] In an exemplary embodiment, the speed of the reactive extrusion composition feeding or moving in the extruder can be 2.0 to 7.0g / min. For example, the flow rate of the reactive extrusion composition can be more than 2.5g / min, more than 3.0g / min, more than 3.5g / min, more than 4.0g / min, more than 4.5g / min or more than 5.0g / min, and its upper limit can be, for example, less than 6.5g / min, less than 6.0g / min, less than 5.5g / min, less than 5.0g / min, less than 4.5g / min or less than 4.0g / min. It has been experimentally confirmed that when the reactive extrusion conditions are controlled as described above, it is more conducive to giving excellent mechanical properties (such as elongation) to the blend of PLA and P (3HP).
[0063] In a specific embodiment of the present application, the method can be a method of feeding the reactive extrusion composition into an extruder having a stirring shaft rotating at 250 to 350 rpm at a flow rate of 4.5 to 5.5 g / min. It has been experimentally confirmed that when the reactive extrusion conditions are controlled as described above, a higher elongation can be imparted to the blend of PLA and P(3HP).
[0064] In an exemplary embodiment, the residence time of the reactive extruded composition in the extruder can be in the range of 220 to 300 seconds (sec). If the residence time is longer than the above time, the polymer may decompose and the molecular weight may decrease. If the residence time is shorter than the above time, the reaction may not occur sufficiently, so the molecular weight may decrease. The reduction in molecular weight leads to a reduction in mechanical properties (e.g., tensile strength and elongation).
[0065] In another exemplary embodiment related to the present application, the present application relates to a blend of PLA and P(3HP) having excellent mechanical properties. The blend of PLA and P(3HP) used herein may be referred to as a PLA / P(3HP) blend.
[0066] For example, a PLA / P(3HP) blend prepared by reactive extrusion is provided, wherein a PLA-gP(3HP) copolymer is present at the interface of PLA and P(3HP), and the blend has a tensile strength of more than 25 MPa and an elongation at break of more than 20%. At this time, the tensile strength and elongation at break can be measured according to ASTM D882, and the stretching speed can be measured under the condition of 30-50% / min (stretching speed of 30-50% of the initial sample length per minute).
[0067] Specifically, the tensile strength of the PLA / P(3HP) blend can be, for example, more than 30 MPa, more than 35 MPa, more than 40 MPa, more than 45 MPa, or more than 50 MPa, and the upper limit can be, for example, less than 70 MPa, less than 65 MPa, less than 60 MPa, less than 55 MPa, less than 50 MPa, less than 45 MPa, less than 40 MPa, or less than 35 MPa.
[0068] Specifically, the elongation at break of the PLA / P(3HP) blend may be, for example, 20% or more, 30% or more, 40% or more, 50% or more, 60% or more, more specifically 70% or more, 80% or more, 90% or more, 100% or more, 110% or more, 120% or more, 130% or more, 140% or more, 150% or more, 160% or more, 170% or more, 180% or more, 190% or more, 200% or more, 210% or more, 220% or more, 230% or more, 240% or more, or 250% or more. And, its upper limit may be, for example, 600% or less, 550% or less, 500% or less, 450% or less, 400% or less, 350% or less, 300% or less, 250% or less, or 200% or less. The PLA-gP(3HP) copolymer present at the interface is entangled with the polymers in the PLA phase and the P(3HP) phase, resulting in increased interfacial adhesion, so that when an external force (elongation) is applied, the resistance at the interface can be increased (high elongation). On the other hand, the lack of entanglement caused by the PLA-gP(3HP) copolymer in the PLA phase and the P(3HP) phase leads to the formation of voids at the interface, which can easily tear the blended product (low elongation).
[0069] The blend has excellent mechanical properties, such as tensile strength and elongation, while being environmentally friendly, which makes it useful as a material for daily necessities such as biodegradable films and biodegradable injection containers.
[0070] In another exemplary embodiment related to the present application, the present application is directed to an article comprising the above blend.
[0071] Specifically, the article can be an injection product or a film. The injection product can be manufactured, for example, in the form of a container. The film can be manufactured to have a thickness of, for example, about 1 mm or less, 0.5 mm or less, 0.3 mm or less, or 0.1 mm or less.
[0072] Beneficial Effects
[0073] According to the specific implementation of the present application, the PLA / P (3HP) blend not only has environmentally friendly characteristics such as biodegradability, but also has excellent extrusion processability and mechanical properties (such as tensile strength, elongation, etc.). BRIEF DESCRIPTION OF THE DRAWINGS
[0074] FIG. 1 is a diagram of Example 1 ( Figure 1a ) and Comparative Example 1 ( Figure 1b ). Specifically, each film was placed on a black background to observe its transparency. Compared with Example 1, the film of Comparative Example 1 had wrinkles and thus had poor transparency. This is because the extrusion kneading efficiency and processability of the extruded composition of the comparative example were poor.
[0075] Figure 2 It is a comparison chart of complex viscosity between Example 1-2 and Comparative Example 1-2. DETAILED DESCRIPTION
[0076] The following will describe the effects and functions of the present invention in more detail in conjunction with specific embodiments of the present invention. However, these embodiments are only for illustrative purposes and are not intended to limit the scope of the present invention in any way.
[0077] Preparation Example 1
[0078] A composition containing the following ingredients was prepared.
[0079] PLA: NatureWorks 2003D (molecular weight: 170,000)
[0080] P(3HP): P(3HP) manufactured by LG Chemical Co., Ltd. (molecular weight: 30,000)
[0081] Chain extenders: PEGDE (polyethylene glycol diglycidyl ether, Sigma-Aldrich), TMPTE (trimethylolpropane triglycidyl ether, Sigma-Aldrich) (both are compounds containing epoxy groups and having a weight average molecular weight of 200 to 10,000 g / mol)
[0082] Reactive compatibilizer: ADR-4400 (BASF) (compound containing epoxy and vinyl groups, epoxy equivalent weight of 485 g / eq, weight average molecular weight of 1,000 to 15,000 g / mol)
[0083] Lubricant: Zn-St (zinc stearate)
[0084] Antioxidant: Irganox 1010 and Irgafos 168 mixed in a weight ratio of 5:5
[0085] Examples 1 to 4 and Comparative Examples 1 to 5
[0086] A mixture having the composition shown in Table 1 below, which is the composition of Preparation Example 1, was reactively extruded using a co-rotating twin-screw extruder (BA11 extruder from Bautech) (diameter (D) = 11 mm, length (L) / diameter (D) = 40)), and the mechanical properties of the blend obtained under the reactive extrusion conditions were evaluated using an extruder simulator (Ludovic v7).
[0087] Specifically, the flow rate in the extruder is adjusted to a range of 4.5 to 5.5 g / min, and the rotation speed of the extruder is adjusted to 400 rpm. In addition, the extruder has a temperature gradient so that the average temperature of multiple zones in the order of the conveying direction (i.e., from the feed inlet side to the discharge outlet side) is 140°C, 170°C, 185°C and 165°C. Under the above conditions, the residence time of the composition in the extruder is 220 to 300 seconds (sec). Regarding the evaluation of tensile strength and elongation at break, the sample reactively extruded from the extruder is pressed with a hot press at 170°C to produce a sample having a thickness of about 0.15 mm.
[0088] [Table 1]
[0089]
[0090]
[0091] Examples 5 to 7 and Comparative Examples 6 to 9
[0092] The mixture having the composition shown in Table 2 below as the composition of Preparation Example 1 was reactively extruded using a Bautech BA11 extruder (diameter (D) = 11 mm, length (L) / diameter (D) = 40), and the mechanical properties of the blend obtained under the reactive extrusion conditions were evaluated using an extruder simulator (Ludovic v7).
[0093] Specifically, the flow rate in the extruder was adjusted to a range of 4.5 to 5.5 g / min, and the rotation speed of the extruder was adjusted as listed in Table 2 below. In addition, the extruder has a temperature gradient so that the average temperature of multiple zones sequentially located in the conveying direction (i.e., from the feed inlet side to the discharge outlet side) is 120° C., 160° C., 185° C., 175° C., and 145° C. Under the above conditions, the residence time of the composition in the extruder is 220 to 300 seconds (sec). Regarding the evaluation of tensile strength and elongation at break, the sample reactively extruded from the extruder was pressed with a hot press at 170° C. to produce a sample having a thickness of about 0.15 mm (sample length 80 mm, width 6 mm).
[0094] [Table 2]
[0095]
[0096]
[0097] evaluate
[0098] The physical properties of Examples and Comparative Examples were measured as follows, and the results are listed in Table 3 below.
[0099] (1) Complex viscosity: The complex viscosity of the PLA / P(3HP) reactive extrusion composition was measured using a DISCOVERY hybrid rheometer DHR-3 (TA Instruments). When loading the sample, a parallel plate with a diameter of 25.0 mm was used, and the gap was set to 1.0 mm. At this time, the complex viscosity was measured in a dynamic strain frequency sweep mode at 185°C, 0.5% strain, and a frequency of 0.3 rad / s to 500 rad / s.
[0100] (2) Tensile strength: measured using a UTM (universal testing machine) according to ASTM D882. The length and width of the sample are as specified in the ASTM D882 standard, and a stretching speed of 40% / min (40% of the initial sample length is stretched per minute) is applied at room temperature (e.g., about 15-35° C., without heating or cooling).
[0101] (3) Elongation at break: measured using a UTM (universal testing machine) according to ASTM D882. The length and width of the sample are as specified in the ASTM D882 standard, and a stretching speed of 40% / min (40% of the initial sample length is stretched per minute) is applied at room temperature (e.g., about 15-35° C., without heating or cooling).
[0102] [Table 3]
[0103]
[0104]
[0105] It was confirmed that in Examples 1 to 7, the increase in tensile elongation was large.
[0106] In contrast, even in the case of a PLA / P(3HP) blend, it can be seen that if neither a reactive compatibilizer nor a chain extender is used during reactive extrusion, the elongation at room temperature is poor (Comparative Examples 1, 2, 8, 9). In addition, when PLA is extruded alone, it can be seen that if neither a reactive compatibilizer nor a chain extender is used, the elongation is poor (Comparative Examples 3, 6). When a reactive emulsifier is used alone, it can be seen that although the viscosity increase is large, the elongation improvement effect is small (Comparative Example 4). In addition, when a chain extender is used alone, it can be confirmed that the reactivity between the chain extender and PLA is low and the viscosity increase is small (Comparative Example 5). Moreover, it was confirmed that even if PLH is extruded alone, the elongation is poor (Comparative Example 7).
Claims
1. A reactive extrusion composition comprising: 100 parts by weight of a resin component containing PLA and P(3HP); 0.2 to 15 parts by weight of a chain extender containing an epoxy group; and 0.2 to 15 parts by weight of a reactive compatibilizer, Wherein, the reactive compatibilizer contains epoxy group and vinyl group.
2. The reactive extrusion composition according to claim 1, wherein: The weight average molecular weight of the PLA is greater than the weight average molecular weight of P(3HP).
3. The reactive extrusion composition of claim 1, wherein: The reactive compatibilizer has an epoxy equivalent of 200 g / eq or more and 600 g / eq or less.
4. The reactive extrusion composition of claim 1, wherein: The reactive compatibilizer has a weight average molecular weight of 1,000 g / mol or more and 15,000 g / mol or less.
5. The reactive extrusion composition of claim 1, wherein: The weight average molecular weight of the PLA is 50,000 or more and 400,000 or less.
6. The reactive extrusion composition of claim 1, wherein: The weight average molecular weight of the P(3HP) is 2,000 or more and 200,000 or less.
7. The reactive extrusion composition of claim 1, wherein: The resin component contains 30 to 95 wt % of PLA and 5 to 70 wt % of P(3HP).
8. The reactive extrusion composition of claim 1, wherein: The chain extender contains an epoxy group and has a weight average molecular weight of 200 g / mol or more and 10,000 g / mol or less.
9. The reactive extrusion composition of claim 1, wherein: The reactive extrusion composition further comprises a lubricant, and The lubricant is a higher fatty acid having 10 to 20 carbon atoms and a salt thereof.
10. The reactive extrusion composition of claim 1, wherein: The reactive extrusion composition also includes an antioxidant.
11. The reactive extrusion composition of claim 1, wherein: The complex viscosity at 185° C., 0.5% strain and 0.3 rad / s is 2,000 Pa.s or more.
12. An extrusion method for producing a PLA / P(3HP) blend, the method comprising feeding a reactive extrusion composition comprising resin components of PLA and P(3HP), a chain extender and a reactive compatibilizer into an extruder having a stirring shaft rotating at 250 rpm or more at a flow rate of 2.0 g / min or more and 7.0 g / min or less within a temperature range of 110° C. or more and 200° C. or less, in, The reactive extrusion composition includes 0.2 to 15 parts by weight of a chain extender and 0.2 to 15 parts by weight of a reactive compatibilizer, based on 100 parts by weight of the resin component.
13. The extrusion method for producing a PLA / P(3HP) blend according to claim 12, wherein: The extruder has a temperature gradient in a conveying direction of the reactive extrusion composition in the extruder (wherein the conveying direction refers to a direction in which the reactive extrusion composition fed into a feed inlet of the extruder moves to a discharge outlet of the extruder).
14. The extrusion method for producing a PLA / P(3HP) blend according to claim 13, wherein: The temperature of the first zone on the reactive extrusion composition feed inlet side of the extruder is controlled to be above 120° C. and below 165° C., The temperature of the third zone on the reactive extrusion composition discharge outlet side of the extruder is controlled to be above 135° C. and below 180° C., The temperature of the second zone between the feed inlet side and the discharge outlet side is controlled to be above 170° C. and below 200° C., and A temperature gradient is applied such that the temperature of the second zone is higher than the temperatures of the first zone and the third zone.
15. The extrusion method for producing a PLA / P(3HP) blend according to claim 12, wherein: The residence time of the reactive extrusion composition in the extruder is 220 seconds (sec) or more and 300 seconds (sec) or less.
16. The extrusion method for making a PLA / P(3HP) blend according to claim 12, wherein: The reactive extrusion composition is fed at a flow rate of 4.5 g / min or more and 5.5 g / min or less into an extruder having a stirring shaft rotating at 250 rpm or more and 350 rpm or less.
17. The extrusion method for making a PLA / P(3HP) blend according to claim 12, wherein: The reactive extrusion composition contains 1.5 to 15 parts by weight of a reactive compatibilizer and 1.0 to 15 parts by weight of a chain extender based on 100 parts by weight of the PLA resin.
18. A PLA / P(3HP) blend, which is a blend of PLA and P(3HP) produced by reactive extrusion, in, PLA-gP(3HP) copolymer is present at the interface of PLA and P(3HP), and The tensile strength of the blend is greater than 25 MPa, and the elongation at break is greater than 20% (provided that the tensile strength and the elongation at break are measured in accordance with ASTM D882).