Low adhesive high density cemented carbide for neutron shielding applications

By using low-adhesive high-density cemented carbide compositions, including ceramic hard phase and iron-chromium metal adhesive phase, the poor effect of neutron shielding materials in the prior art in a limited space and complex manufacturing is solved. The problem of high density, corrosion resistance and short radioactive half-life are achieved.

CN119032189APending Publication Date: 2024-11-26HYPERION MATERIALS & TECH (SWEDEN) AB
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380035775.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-01-30
Filing Date
2023-05-30
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to effectively shield neutron flux in a limited space, while avoiding material activation and the formation of harmful by-products, and the manufacturing process is complex, making it difficult to meet the needs of nuclear reactors.

Method used

The low-adhesive high-density cemented carbide composition is used, including ceramic hard phase and iron-chromium metal adhesive phase, and is manufactured through the sintering process to ensure that the material has high density, corrosion resistance and short radioactive half-life.

Benefits of technology

It realizes effective shielding of neutron flux in a limited space, avoids material activation and the formation of harmful by-products, simplifies the manufacturing process, and improves the corrosion resistance and oxidation resistance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention provides a low binder high density cemented carbide composition for neutron shielding, the low binder high density cemented carbide composition comprising: a ceramic hard phase comprised of tungsten carbide (WC), substoichiometric di-tungsten carbide (W2C), or a combination thereof; and a low weight iron (Fe)-chromium (Cr) based metal binder phase, the low weight iron (Fe)-chromium (Cr) based metal binder phase being about 0.02 wt% to about 2.75 wt% based on the total weight of the cemented carbide composition. A weight content of Cr of the Fe-Cr based metal binder phase may be from about 5% by weight to about 16% by weight based on a total weight of the Fe-Cr based metal binder phase. Related methods of making sintered low binder high density cemented carbide for neutron shielding are also provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to low binder high density cemented carbide compositions and related methods of making low binder high density cemented carbide for neutron shielding. Background Art

[0002] When designing any type of nuclear reactor, the first consideration is how to protect the reactor components from the neutron flux and gamma rays produced by the nuclear reactor during fission and fusion reactions. In terms of radiation shielding, an effective biological shield is generally required, which also includes other parts of the reactor, such as electronic systems. A prerequisite is that the shielding material should be tailored to provide protection against various high-energy radioactive radiation species (including, for example, short-range alpha particles, beta particles, gamma rays and neutrons). These conditions impose strict restrictions on the types of materials that can be used in the design phase of a nuclear reactor. It is also important that the material forming the shield itself has resistance to activation and will not be converted into other harmful radioactive isotopes when exposed to radiation. This means that materials containing large amounts of, for example, nickel (Ni) and cobalt (Co) cannot usually be used for this purpose because they pose an activation risk when exposed to radiation because they are unexpectedly eliminated from the environment due to their extremely long radioactive half-life.

[0003] Small modular fusion nuclear reactors and magnetic confinement reactors have become popular choices for the next generation of nuclear power plants. Essentially, small modular nuclear power plants have the potential to be safer and more efficient than the large nuclear power plants currently in use. The downside is that in the case of magnetic confinement fusion reactors, they rely on cryogenically cooled copper and / or high temperature superconductors (HTS) to generate the magnetic field. Therefore, the space between the plasma chamber and the cold conductors (copper / HTS) is quite limited. In both cases, these types of reactors pose challenges when considering the selection of radiation shielding materials, as the geometry of such reactors means that space is indeed quite limited. Therefore, the shielding material must logically be applied in thin layers while still maintaining neutron shielding capabilities.

[0004] The challenge is therefore to find an alternative shielding material that does not need to be applied in excessive thickness to achieve a satisfactory shielding effect. Furthermore, the material should also not form any harmful byproducts when exposed to the nuclear fusion process. It is therefore important that the material does not contain associated elements that can be transformed into harmful radionuclides, which would hinder the decommissioning and refueling phase of nuclear reactors at the end of their operating cycle. What is more, a core aspect is that it should also be possible to manufacture the material for this application using conventional technologies without the need for multiple cumbersome steps.

[0005] In this regard, the most attractive materials will be high-density materials and also have the ability to have high corrosion and oxidation resistance. It is therefore crucial that neutron shielding materials for nuclear applications exhibit high density in order to effectively suppress the neutron flux by capturing the neutron flux generated in nuclear reactors. In addition to this, they should also be made of elements with short radioactive half-lives in order to avoid complex decommissioning procedures at the end of the reactor's life and to avoid complex storage facilities for irradiated materials. Finally, as mentioned above, it is important that they should have corrosion and oxidation resistance since they are continuously exposed to the cooling medium during the operation of nuclear reactors.

[0006] It is noteworthy that the properties of cemented carbide mainly depend on the content of metal bonding phase and tungsten carbide (WC) grain size. For this reason, based on the gross weight of cemented carbide, typical WC-cobalt (Co) or WC-nickel (Ni) cemented carbide can contain Co or Ni of about 2 wt % to about 30 wt %, and WC grain size can be generally in the range of submicron to several microns. Bonding phases such as Co or Ni are conducive to promoting the increase of firm fracture toughness and strength, but at the same time, metal bonding phases can also undesirably reduce the corrosion resistance, wear resistance and hardness of cemented carbide. Thus, it is still a considerable trade-off to improve fracture toughness and strength at the expense of reducing corrosion resistance, wear resistance and hardness. More noteworthy is that, due to the different thermal expansion coefficients compared with WC, for example, cobalt can also cause unnecessary thermal stress, therefore logically limiting its application under high temperature and other harsh conditions. Therefore, in the process of constantly seeking to alleviate at least the above-mentioned problem solution, low binder cemented carbide has naturally caused more and more research attention and attempts. Growing evidence from the research conducted indicates that low-binder cemented carbides exhibit superior physical properties in this regard, such as strong wear resistance, enhanced corrosion resistance and improved hardness due to the small amount of metal binder contained. Therefore, over the years, this has triggered a growing interest in limiting the addition of too high a concentration of metal binder during the manufacturing stage of cemented carbides in order to ultimately improve their corrosion resistance.

[0007] International patent publication number WO2018206174A1 relates to a cemented carbide including an iron-chromium (Fe-Cr) metal binder for use in manufacturing cutting tools, wear-resistant parts, sealing rings, bushings, automotive parts, molds, or tools for handling radioactive materials, and the international patent publication is incorporated herein by reference in its entirety. However, in this case, the cemented carbide disclosed in WO2018206174A1 is not optimized for handling radioactive materials because the content of the metal binder exceeds 3% by weight, thereby reducing the final density of the material, thereby substantially hindering its neutron shielding potential and ability. In addition, WO2018206174A1 does not disclose the use of substoichiometric tungsten carbide such as W2C to increase the material density.

[0008]

[0006] Therefore, in view of the above, there is a need for low binder high density cemented carbide compositions that exhibit improved corrosion resistance and acceptable short radioactive half-life activity for use in neutron shielding in nuclear reactors. Summary of the invention

[0009] According to a first aspect, a low-binder high-density cemented carbide composition for neutron shielding in a nuclear reactor is provided, the cemented carbide composition comprising a ceramic hard phase and an iron (Fe)-chromium (Cr) metal binder phase. The weight of Cr can be about 5 wt % to about 16 wt % based on the total weight of the Fe-Cr metal binder phase.

[0010] Optionally, the weight of chromium is from about 10.5 wt % to about 16 wt % based on the total weight of the Fe-Cr based metal binder phase.

[0011] Optionally, the weight of chromium is from about 10.5 wt % to about 10.7 wt % based on the total weight of the Fe—Cr based metal binder phase.

[0012] Optionally, the cemented carbide composition may include about 0.02 wt % to about 2.75 wt % of a Fe—Cr based metal binder phase, based on the total weight of the cemented carbide composition.

[0013] Optionally, the cemented carbide composition comprises about 2.75 wt % of a Fe—Cr based metal binder phase, based on the total weight of the cemented carbide composition.

[0014] Optionally, the ceramic hard phase comprises tungsten carbide (WC), substoichiometric ditungsten carbide (W2C), or a combination thereof.

[0015] Optionally, the ceramic hard phase comprises WC.

[0016] Optionally, the ceramic hard phase comprises substoichiometric W2C.

[0017] Optionally, the ceramic hard phase comprises a combination of WC and substoichiometric W2C in a 1:1 ratio.

[0018] Optionally, the cemented carbide composition may include about 97.25 wt % to about 99.98 wt % of the ceramic hard phase, based on the total weight of the cemented carbide composition.

[0019] Optionally, the cemented carbide composition has a hardness of about 15.25 g / cm 3 to about 17 g / cm 3 The theoretical density.

[0020] Optionally, a cemented carbide composition having improved corrosion resistance is obtained.

[0021] Optionally, the Fe-Cr based metal binder phase is prepared by blending FeCr powder with Cr3C2 powder.

[0022] Optionally, the cemented carbide composition has a HV30 Vickers hardness in the range of about 2227 HV30 to about 2700 HV30 and a Palmqvist fracture toughness (K Ic ).

[0023] The present invention also provides a method for manufacturing a sintered low-binder high-density cemented carbide for neutron shielding in a nuclear reactor, the method comprising blending a powder mixture in a grinding liquid with an organic binder to form a slurry blend, the powder mixture comprising: a powder of a hard component forming a ceramic hard phase; and an iron (Fe)-chromium (Cr) metal binder phase, the iron (Fe)-chromium (Cr) metal binder phase comprising about 5 wt % to about 16 wt % of chromium based on the total weight of the Fe-Cr metal binder phase. Next, the formed slurry mixture is dried to form a powder mixture. Finally, the formed powder mixture is sintered to obtain a sintered low-binder high-density cemented carbide for neutron shielding.

[0024] Optionally, the weight of the chromium is about 10.5 wt % to about 16 wt % based on the total weight of the Fe—Cr based metal binder phase.

[0025] Optionally, the weight of the chromium is about 10.5 wt % to about 10.7 wt % based on the total weight of the Fe—Cr based metal binder phase.

[0026] Optionally, the cemented carbide may include about 0.02 wt % to about 2.75 wt % of a Fe—Cr based metal binder phase based on the total weight of the cemented carbide.

[0027] Optionally, the cemented carbide comprises about 2.75 wt % of a Fe—Cr based metal binder phase based on the total weight of the cemented carbide.

[0028] Optionally, the ceramic hard phase comprises tungsten carbide (WC), substoichiometric ditungsten carbide (W2C), or a combination thereof.

[0029] Optionally, the ceramic hard phase comprises WC.

[0030] Optionally, the ceramic hard phase comprises substoichiometric W2C.

[0031] Optionally, the ceramic hard phase comprises a combination of WC and substoichiometric W2C in a 1:1 ratio.

[0032] Optionally, the cemented carbide may comprise from about 97.25 wt % to about 99.98 wt % of a ceramic hard phase, based on the total weight of the cemented carbide.

[0033] Optionally, the cemented carbide has a mass of about 15.25 g / cm 3 to about 17 g / cm 3 The theoretical density.

[0034] Optionally, a cemented carbide having improved corrosion resistance is obtained.

[0035] Optionally, the Fe-Cr based metal binder phase is prepared by blending FeCr powder with Cr3C2 powder.

[0036] Optionally, the cemented carbide has a HV30 Vickers hardness in the range of about 2227 HV30 to about 2700 HV30 and a Palmqvist fracture toughness (K Ic ).

[0037] Optionally, drying the slurry blend comprises vacuum drying, air drying, freeze drying, or spray drying by atomization.

[0038] Optionally, sintering comprises hot pressing (HP), hot isostatic pressing (HIP) or spark plasma sintering (SPS).

[0039] Other systems, methods, features and advantages will be or will become apparent to one skilled in the art upon examination of the following drawings and detailed description. It is intended that all such other systems, methods, features and advantages be included within this specification, fall within the scope of the invention, and be protected by the appended claims. Nothing in this section shall be construed as limiting these claims. Other aspects and advantages are discussed below in conjunction with embodiments of the invention. It should be understood that the above general description and the following detailed description of the invention are merely exemplary and illustrative, and are intended to further illustrate the claimed invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] The accompanying drawings, which are included to provide a further understanding of the subject matter and are incorporated in and constitute a part of this specification, illustrate embodiments of the subject matter and together with the description serve to explain the principles of the invention.

[0041] Figure 1 is a flow chart showing various process steps for manufacturing low binder high density cemented carbide for neutron shielding according to an exemplary embodiment of the present invention. DETAILED DESCRIPTION

[0042] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the presently described invention belongs.

[0043] Where a numerical range is provided, such as a concentration range, a percentage range or a ratio range, it is understood that, unless the context clearly indicates otherwise, each intermediate value (to one tenth of the unit of the lower limit) between the upper and lower limits of the range and any other described or intermediate values ​​within the range are included in the described subject matter. These smaller upper and lower limits may be independently included in the smaller range, and such embodiments are also included in the described subject matter, subject to any explicitly excluded limits within the described range. Where the range includes one or two limits, ranges excluding one or both of those included limits are also included in the described subject matter.

[0044] The following definitions set forth the parameters of the described subject matter.

[0045] As used in the context of the present invention, the term "low binder high density cemented carbide" generally refers to a composite material consisting of a (I) ceramic hard phase embedded, anchored and cemented (i.e., thereby producing a Fe-Cr metal binder phase) by a (II) Fe-Cr metal binder matrix, the (I) ceramic hard phase generally consisting of tungsten carbide (WC), substoichiometric ditungsten carbide (W2C) or a mixture thereof, wherein the Fe-Cr metal binder is generally used in an amount of about 0.02 wt % to about 2.75 wt % based on the total weight of the cemented carbide. As used in the context of the present invention, the term "substoichiometric" refers to a ratio W / C significantly higher than 1. Ceramic hard phase powders and Fe-Cr metal binder phase powders can be processed into various microstructures that achieve different mechanical and physical properties. In addition, other components can be added to the composition to help control and further improve the properties achieved by the cemented carbide composition. By controlling various parameters, including grain size, Fe-Cr content, foreign matter (dotation) (such as alloy carbides) and carbon content, cemented carbide manufacturers can advantageously adjust and guide its performance according to specific unique applications. Cemented carbide is carefully designed to have both the physical best properties of ceramics such as high temperature resistance and high hardness, and the physical best properties of metals such as being able to withstand plastic deformation and provide good fracture toughness. The soft Fe-Cr metal binder of natural ductility is used to offset the brittle behavior unique to the ceramic hard phase, thereby improving and thereby enhancing its associated fracture toughness and durability. The ceramic hard phase of cemented carbide is generally composed of refractory carbides of metals, such as but not limited to the most typical tungsten, but can also be titanium, tantalum, chromium, vanadium, zirconium or any combination thereof. The ceramic hard phase can be in the form of any possible combination of the above-mentioned metals, and in a weight that is not inconsistent and incompatible with the purpose of the subject matter of the present invention. To qualify as a cemented carbide within the present invention, the cemented carbide generally has a ceramic hard phase comprised of at least about 97.25 wt. % to about 99.98 wt. %, based on the total weight of the cemented carbide.

[0046] As used in the context of the present invention, "weight %" refers to a weight percentage given as follows: (I) based on the total weight of a low-binder, high-density cemented carbide composition for neutron shielding in a nuclear reactor; (II) based on the total weight of a low-binder, high-density cemented carbide for neutron shielding in a nuclear reactor; or (III) based on the total weight of a Fe-Cr-based metal binder phase. When "weight %" is mentioned in the present invention or claims, it will also be explicitly mentioned whether it refers to a given weight percentage of (I), (II) or (III) in each given specific scenario.

[0047] As used in the context of the present invention, the term "D 50 " refers to the sampled particles smaller than the D50 The volume of the value is 50% and the sampled particles are larger than the D 50 The value of volume is the particle size at which 50% of the particles are present. 90 " refers to the sampled particles smaller than the D 90 The volume of the value is 90% and the sampled particles are larger than the D 90 The value is the particle size at which 10% of the volume is measured. 10 " refers to the sampled particles smaller than the D 10 The volume of the value is 10% and the sampled particles are larger than the D 10 The value is the particle size at which 90% of the volume is distributed. The width of the particle size distribution can be calculated by determining the span, which is given by the equation (D 90 -D 10 ) / D 50 The span gives an indication of how far the 10% and 90% points are from the normalized midpoint.

[0048] As used in the text of the present invention, the term "about" refers to ±5% of the numerical value of the number used in the claims and the text of the present invention. Thus, "about" can be used to provide flexibility to numerical range endpoints, wherein a given value can be "above" or "below" a given value. Thus, for example, a value of 50% may be intended to include ranges defined by ranges such as 47.5% to 52.25%, 47.5% to 52.5%, 47.75% to 50%, 50% to 52.5%, 48% to 48.5%, 48% to 48.75%, 48% to 49%, 48% to 49.5%, 48% to 49.75%, 48% to 50%, 48% to 50.25%, 48% to 50.5%, 48% to 50.75%, 48% to 51%, 48% to 51.5%, 48% to 51.75%, 48% to 52%, 48% to 52.25%, 48% to 52.5%, 48% to 48.75%, 25%~48.5%, 48.25%~48.75%, 48.25%~49%, 48.25%~49.5%, 48.25%~49.75%, 48.25%~50%, 48.25%~50.25%, 48.25%~50.5%, 48.25%~50.75%, 48.25%~51%, 48.25%~51.25%, 48.25%~51.5%, 48.25%~51.75%, 48.25%~52%, 48.25%~52.25%, 48.25%~52.5%, 48.5%~48.75%, 48.5%~49%, 4 8.5%~49.5%, 48.5%~49.75%, 48.5%~50%, 48.5%~50.25%, 48.5%~50.5%, 48.5%~50.75%, 48.5%~51%, 48.5%~51.25%, 48.5%~51.5%, 48.5%~51.75%, 48.5%~52%, 48.5%~52.25%, 48.5%~52.5%, 49%~49.25%, 49%~49.5%, 49%~49.75%, 49%~50%, 49%~50.25%, 49%~50.5%, 49%~50.75%, 49%~51%, 49%~51.25%, 49%~51.5%, 49%~51.75%, 49%~52%, 49%~52.25%, 49%~52.5%, 49.5%~49.75%, 49.5%~50%, 49.5%~50.25%, 49.5%~50.5%, 49.5%~50.75%, 49.5%~51%, 49.5%~51.5%, 49.5%~51.75%, 49.5%~52%, 49.5%~52.25%, 49.5%~52.5%, 49.75%~50%, 49.75%~50.25%, 49.75%~50.5%, 49.75%~50.75%, 49.75%~51%, 49.75%~51.25%, 49.75%~51.5%, 49.75%~51.75%, 49.75%~52%, 49.75%~52.25%, 49.75%~52.5%, 50%~50.25%, 50%~50.5%, 50%~50.75%, 50%~51%, 50%~51.25%, 50%~51.5%, 50%~52%, 50%~52.25%, 50%~52.5%, etc. .

[0049] As used in the context of the present invention, the term "sintering" refers to the process of heating under controlled pressure to minimize the surface area of ​​a particulate system, which is associated with the resulting bonding between adjacent small particles or granules and the subsequent shrinkage of the aggregated particles or granules. The particles are compacted and formed into a dense solid mass by heating under controlled pressure.

[0050] As used in the context of the present invention, the term "particle" refers to one or more discrete objects.

[0051] Throughout this specification, wherever used, the term "generally" has the meaning of "typically" or "closely" or "around or within the vicinity of...".

[0052] As used in the context of the present invention, the term "substantially" refers to the complete or nearly complete degree or extent of an action, characteristic, property, state, structure, item, or result.

[0053] As used herein, "spherical" means that the particles have a substantially "round" shape.

[0054] As used herein, the term "Palmqvist fracture toughness" means (K Ic ) refers to the ability of a material with a pre-crack to resist further fracture propagation when energy is absorbed.

[0055] As used herein, the term "HV30 Vickers hardness" (ie, 30 kgf applied load) is a measure of the resistance of a sample to localized plastic deformation, obtained by indenting a Vickers tip into the sample at 30 kgf.

[0056] As used herein, ISO 28079-2009 standard defines the method for measuring the fracture toughness and hardness of hard metal, cermet and cemented carbide at room temperature by indentation method. ISO 28079-2009 standard is applicable to the measurement of fracture toughness and hardness calculated by the diagonal length of the indentation produced by the corner using Vickers hardness indentation and crack, and is intended for carbides and carbonitrides (such as hard metal, cermet or cemented carbide) of metal bonding. The test procedure proposed in ISO28079-2009 standard is intended to be used at ambient temperature, but can be extended to higher or lower temperature by agreement. The test procedure proposed in ISO 28079-2009 standard is also intended to be used under normal laboratory air environment. They are usually not suitable for corrosive environments, such as in strong acid or seawater. The ISO 28079-2009 standard can be directly compared with the ASTM B771 standard, as disclosed in, for example, the "Comprehensive Hard Materials book", 2014, Elsevier Ltd. Page 312, which is incorporated herein by reference in its entirety. Therefore, it can be assumed that the fracture toughness and hardness measured using the ISO 28079-2009 standard are the same as the values ​​measured using the ASTM B771 standard.

[0057] As used in the context of the present invention, the term "corrosion" refers to the process of converting a metal into another chemical form such as an oxide, hydroxide, carbonate or sulfide. Corrosion refers to the process by which a material (i.e., usually a metal) is gradually destroyed by chemical and / or electrochemical reactions with its environment. In the most common usage of the term, corrosion refers to the electrochemical oxidation of a metal with an oxidant such as oxygen or sulfate in a reaction. Rusting, i.e., the formation of iron oxide, is a well-known example of an electrochemical corrosion process. This type of damage typically produces one or more oxides or one or more salts of the original metal. Corrosion can also occur in materials other than metals such as ceramics or polymers.

[0058] As used in the context of this specification, "physical vapor deposition (PVD)" refers to a variety of vacuum deposition methods that can be used to make thin films and coatings. PVD is characterized by a process in which the deposited material goes from a condensed phase to a vapor phase and then back to a thin film condensed phase. The most common PVD processes are sputtering and evaporation.

[0059] As used in the context of the present invention, "chemical vapor deposition (CVD)" refers to a process in which a substrate is exposed to one or more volatile precursors, which react and / or decompose on the substrate surface to produce a desired deposit. Typically, volatile byproducts are also produced, which are removed by the gas flow in the reaction chamber.

[0060] As used in the context of the present invention, the term "theoretical density" is defined as the maximum density that a material or component can achieve assuming that there are no voids or contaminants in the material. Theoretical density is calculated as follows:

[0061] ρ = (n × A) / (V × N), where

[0062] ρ is the density (g / cm 3 )

[0063] n is the number of atoms in each unit cell

[0064] A is the atomic weight (g / mol)

[0065] V is the volume of the unit cell (cm 3 / unit)

[0066] N is Avogadro's constant (6.023×10 23 mol -1 ).

[0067] Low binder high density cemented carbide compositions for neutron shielding

[0068] The present invention is based on the premise of providing a high-density cemented carbide composition and predicts that the weight of the low metal binder in the composition is generally about 0.02% by weight to about 2.75% by weight based on the gross weight of the cemented carbide composition. The present invention provides a low-binder high-density cemented carbide composition for neutron shielding in a nuclear reactor, which is composed of a ceramic hard phase and an iron (Fe)-chromium (Cr) metal binder phase. The binder phase is uniquely composed of elements with an acceptable good short radioactive half-life, and the half-life is, for example, about 44 days for Fe and about 27 days for Cr, which is contrasted with cobalt (Co) and nickel (Ni) that are traditionally used as metal binders in cemented carbide compositions. In addition, when Cr is added to the cemented carbide composition, improved corrosion resistance is obtained. Thus, the beneficial effect obtained is at least multifaceted. In fact, an environmentally friendly cemented carbide composition for neutron shielding in a nuclear reactor is manufactured, which exhibits low binder and high density and has improved corrosion resistance simultaneously, and the components constituting the cemented carbide composition have short radioactive half-life activity. However, the embodiments disclosed herein are not strictly limited to use only in neutron shielding in nuclear reactors. Importantly, they may also find compelling utility and be naturally implemented in conjunction with other systems that may generally require effective neutron shielding and suppression capabilities. This may include, for example: security scanners; industrial inspection systems; nuclear waste generated by, for example, defense, research and development (R&D) activities, utilities, or medical uses; and other nuclear energy-related applications that undesirably emit neutrons, such as nuclear waste recycling, neutron radiography (N-ray) devices using neutron imaging techniques, neutron generators used to eliminate neutrons scattered by building elements, such as those used in oil well logging and safety inspection systems, etc.

[0069] The ceramic hard phase of the cemented carbide composition for neutron shielding herein is most typically composed of tungsten carbide (WC), substoichiometric ditungsten carbide (W2C) or a combination thereof. In some instances, the ceramic hard phase of the cemented carbide composition can be alternatively composed of a carbide of at least one metal selected from the 4th, 5th or 6th group of the periodic table or any combination thereof. In certain specific embodiments, the ceramic hard phase can alternatively be composed of at least one of the carbides of tungsten, titanium, tantalum, vanadium, zirconium, chromium or any combination thereof. The ceramic hard phase comprising the above-mentioned metal carbides can be incorporated into them in a manner that is not inconsistent with the purpose of this subject matter and incompatible with any combination thereof.

[0070] The content of the ceramic hard phase can generally be about 97.25 wt % to about 99.98 wt % based on the total weight of the cemented carbide composition. In some examples, the content of the ceramic hard phase is about 97.50 wt % to about 99.98 wt % based on the total weight of the cemented carbide composition. In other examples, the content of the ceramic hard phase is about 97.75 wt % to about 99.98 wt % based on the total weight of the cemented carbide composition. In yet other examples, the content of the ceramic hard phase is about 98.00 wt % to about 99.98 wt % based on the total weight of the cemented carbide composition. In other examples, the content of the ceramic hard phase is about 98.25 wt % to about 99.98 wt % based on the total weight of the cemented carbide composition. In other examples, the content of the ceramic hard phase is about 98.50 wt % to about 99.98 wt % based on the total weight of the cemented carbide composition. In further other examples, the content of the ceramic hard phase is about 98.75 wt % to about 99.98 wt % based on the total weight of the cemented carbide composition. In still other examples, the content of the ceramic hard phase is about 99.00 wt % to about 99.98 wt % based on the total weight of the cemented carbide composition. In other embodiments, the content of the ceramic hard phase is about 99.25 wt % to about 99.98 wt % based on the total weight of the cemented carbide composition. In still other embodiments, the content of the ceramic hard phase is about 99.50 wt % to about 99.98 wt % based on the total weight of the cemented carbide composition. In still further other embodiments, the content of the ceramic hard phase is about 99.75 wt % to about 99.98 wt % based on the total weight of the cemented carbide composition.

[0071] The ceramic hard phase may also be present in an amount of about 97.25 wt % to about 97.50 wt %, about 97.50 wt % to about 97.75 wt %, about 97.50 wt % to about 98.00 wt %, about 97.25 wt % to about 97.75 wt %, about 97.25 wt % to about 98.00 wt %, about 97.25 wt % to about 98.25 wt %, about 97.25 wt % to about 98.50 wt %, about 97.25 wt % to about 98.75 wt %, about 97.25 wt % to about 99.00 wt %, about 97.7 ...%. %, about 98.00 wt % to about 98.25 wt %, about 97.75 wt % to about 98.25 wt %, about 98.25 wt % to about 98.50 wt %, about 98.50 wt % to about 98.75 wt %, about 98.25 wt % to about 98.75 wt %, about 98.75 wt % to about 99.00 wt %, about 99.00 wt % to about 99.25 wt %, about 98.25 wt % to about 99.25 wt %, about 98.75 wt % to about 99.25 wt %, about 98.75 wt % to about 99.50 wt %, or about 98.75 wt % to about 99.75 wt %.

[0072] Based on the total weight of the cemented carbide composition, the cemented carbide composition can generally include about 0.02% by weight to about 2.75% by weight of Fe-Cr metal binder phase. In some examples, based on the total weight of the cemented carbide composition, the cemented carbide composition includes about 0.10% by weight to about 2.75% by weight of Fe-Cr metal binder phase. In other examples, based on the total weight of the cemented carbide composition, the cemented carbide composition includes about 0.20% by weight to about 2.75% by weight of Fe-Cr metal binder phase. In other examples, based on the total weight of the cemented carbide composition, the cemented carbide composition includes about 0.25% by weight to about 2.75% by weight of Fe-Cr metal binder phase. In other examples, based on the total weight of the cemented carbide composition, the cemented carbide composition includes about 0.50% by weight to about 2.75% by weight of Fe-Cr metal binder phase. In other examples, based on the total weight of the cemented carbide composition, the cemented carbide composition includes about 0.75% by weight to about 2.75% by weight of Fe-Cr metal binder phase. In other embodiments, the cemented carbide composition comprises from about 1.00 wt % to about 2.75 wt % of a Fe-Cr metal binder phase, based on the total weight of the cemented carbide composition. In yet other embodiments, the cemented carbide composition comprises from about 1.25 wt % to about 2.75 wt % of a Fe-Cr metal binder phase, based on the total weight of the cemented carbide composition. In yet other embodiments, the cemented carbide composition comprises from about 1.50 wt % to about 2.75 wt % of a Fe-Cr metal binder phase, based on the total weight of the cemented carbide composition. In yet other embodiments, the cemented carbide composition comprises from about 1.75 wt % to about 2.75 wt % of a Fe-Cr metal binder phase, based on the total weight of the cemented carbide composition. In yet other embodiments, the cemented carbide composition comprises from about 2.00 wt % to about 2.75 wt % of a Fe-Cr metal binder phase, based on the total weight of the cemented carbide composition. In yet further other embodiments, the cemented carbide composition comprises from about 2.25 wt % to about 2.75 wt % of a Fe-Cr metal binder phase, based on the total weight of the cemented carbide composition. In still further other embodiments, the cemented carbide composition comprises from about 2.50 wt % to about 2.75 wt % of the Fe—Cr based metallic binder phase, based on the total weight of the cemented carbide composition.

[0073] The Fe—Cr-based metal binder phase may also be present in an amount by weight of about 0.02 wt % to about 0.10 wt %, about 0.10 wt % to about 0.20 wt %, about 0.20 wt % to about 0.25 wt %, about 0.02 wt % to about 0.20 wt %, about 0.02 wt % to about 0.25 wt %, about 0.02 wt % to about 0.50 wt %, about 0.02 wt % to about 0.75 wt %, about 0.25 wt % to about 0.50 wt %, about 0.25 wt % to about 0.75 wt %, about 0.50 wt % to about 0.75 wt %, about 0.75 wt % to about 1.00 wt %, about 1.00 wt % to about 1.25 wt %, or about 0.50 wt % to about 0.75 wt %. % to about 1.00 wt%, about 0.50 wt% to about 1.25 wt%, about 0.50 wt% to about 1.50 wt%, about 0.50 wt% to about 1.75 wt%, about 0.50 wt% to about 2.00 wt%, about 0.50 wt% to about 2.25 wt%, about 0.50 wt% to about 2.50 wt%, about 1.25 wt% to about 1.50 wt%, about 1.50 wt% to about 1.75 wt%, about 1.75 wt% to about 2.00 wt%, about 1.25 wt% to about 2.00 wt%, about 1.25 wt% to about 2.25 wt%, about 2.00 wt% to about 2.25 wt%, about 2.25 wt% to about 2.50 wt%, or about 2.00 wt% to about 2.50 wt%.

[0074] In certain specific embodiments, the cemented carbide composition may include about 2.75 wt % of the Fe—Cr based metal binder phase, based on the total weight of the cemented carbide composition.

[0075] The weight of Cr of the metal binder phase may generally be about 5 wt % to about 16 wt % based on the total weight of the Fe-Cr metal binder phase. In some examples, the weight of Cr of the metal binder phase is about 8 wt % to about 16 wt % based on the total weight of the Fe-Cr metal binder phase. In other examples, the weight of Cr of the metal binder phase is about 10 wt % to about 16 wt % based on the total weight of the Fe-Cr metal binder phase. In still other examples, the weight of Cr of the metal binder phase is about 12 wt % to about 16 wt % based on the total weight of the Fe-Cr metal binder phase. In still other examples, the weight of Cr of the metal binder phase is about 14 wt % to about 16 wt % based on the total weight of the Fe-Cr metal binder phase.

[0076] The weight content of Cr in the metal binder phase may also be about 5 wt % to about 6 wt %, about 5 wt % to about 7 wt %, about 5 wt % to about 8 wt %, about 5 wt % to about 9 wt %, about 5 wt % to about 10 wt %, about 8 wt % to about 9 wt %, about 8 wt % to about 10 wt %, about 8 wt % to about 11 wt %, about 8 wt % to about 12 wt %, about 8 wt % to about 13 wt %, about 10 wt % to about 12 wt %, about 10 wt % to about 13 wt %, about 10 wt % to about 14 wt %, about 10 wt % to about 15 wt %, about 12 wt % to about 13 wt %, about 12 wt % to about 14 wt %, or about 12 wt % to about 15 wt %, based on the total weight of the Fe—Cr-based metal binder phase.

[0077] In certain specific embodiments, the weight of Cr of the metallic binder phase is from about 10.5 wt % to about 16 wt % based on the total weight of the Fe—Cr based metallic binder phase.

[0078] In certain other specific embodiments, the weight of Cr of the metallic binder phase is from about 10.5 wt % to about 10.7 wt % based on the total weight of the Fe-Cr based metallic binder phase.

[0079] Grain growth inhibitors commonly known to those skilled in the art for inhibiting WC and substoichiometric W2C grain growth during processing, such as vanadium carbide (VC), chromium carbide (Cr3C2), tantalum carbide (TaC), titanium carbide (TiC) and zirconium carbide (ZrC) may be present in the cemented carbide composition for neutron shielding in any possible combination and in any weight not inconsistent with and incompatible with the purpose of the present subject matter.

[0080] The grain growth inhibitor may be present in an amount by weight based on the total weight of the cemented carbide composition of about 0.15 wt % to about 2.00 wt %, about 0.25 wt % to about 2.00 wt %, about 0.50 wt % to about 2.00 wt %, about 0.15 wt % to about 0.50 wt %, about 0.75 wt % to about 2.00 wt %, about 1.00 wt % to about 2.00 wt %, about 1.25 wt % to about 2.00 wt %, about 0.50 wt % to about 1.25 wt % to about 1.50 wt %, about 0.50 wt % to about 2.00 wt %. 0 wt % to about 1.50 wt %, about 0.50 wt % to about 1.75 wt %, about 0.75 wt % to about 1.25 wt %, about 1.00 wt % to about 1.25 wt %, about 1.00 wt % to about 1.50 wt %, about 1.25 wt % to about 1.50 wt %, about 1.25 wt % to about 1.75 wt %, about 1.25 wt % to about 2.00 wt %, about 1.50 wt % to about 2.00 wt %, or about 1.75 wt % to about 2.00 wt %.

[0081] The ceramic hard phase powder and Fe-Cr metal binder phase powder described in the text of the present invention may have any average particle size that is not incompatible with the purpose of the present invention. The ceramic hard phase powder and the Fe-Cr metal binder phase powder may generally exhibit, for example, an average particle size in the range of about 0.5 μm to about 30 μm. In some examples, the ceramic hard phase powder and the Fe-Cr metal binder phase powder have an average particle size in the range of about 1 μm to about 5 μm. In other examples, the ceramic hard phase powder and the Fe-Cr metal binder phase powder have an average particle size in the range of about 1 μm to about 10 μm. In other examples, the ceramic hard phase powder and the Fe-Cr metal binder phase powder have an average particle size in the range of about 1 μm to about 15 μm. In other examples, the ceramic hard phase powder and the Fe-Cr metal binder phase powder have an average particle size in the range of about 1 μm to about 20 μm. In a further example, the ceramic hard phase powder and the Fe-Cr metal binder phase powder have an average particle size in the range of about 1 μm to about 25 μm. In still other examples, the ceramic hard phase powder and the Fe—Cr based metal binder phase powder have an average particle size ranging from about 1 μm to about 30 μm.

[0082] The average particle size of the ceramic hard phase powder and the Fe-Cr-based metal binder phase powder may also be in the range of about 5 μm to about 10 μm, about 10 μm to about 15 μm, about 5 μm to about 15 μm, about 15 μm to about 20 μm, about 5 μm to about 20 μm, about 20 μm to about 25 μm, about 5 μm to about 25 μm, about 25 μm to about 30 μm, or about 5 μm to about 30 μm.

[0083] To determine the particle size, one of ordinary skill in the art can typically use dynamic digital image analysis (DIA), static laser light scattering (SLS) (also known as laser diffraction) or visual measurement by electron microscopy, a technique known as image analysis and light shielding. Each method covers a range of characteristic sizes that can be measured. These ranges overlap in part. However, the results of measuring the same sample may vary depending on the specific method used. A skilled person who wants to determine the particle size or particle size distribution will readily know how to generally perform and practice each of the methods described. Thus, the reader is referred to, for example: (i) "Comparison of Methods. Dynamic Digital Image Analysis, Laser Diffraction, Sieve Analysis", Retsch Technology and (ii) Kelly et al., "Graphical comparison of image analysis and laser diffraction particlesize analysis data obtained from the measurements of nonspherical particle systems", AAPS PharmSciTech. August 18, 2006, Volume 7 (3): 69 pages, for further understanding of the various procedures and methods, all of which are incorporated herein by reference in their entirety.

[0084] The cemented carbide compositions for neutron shielding described herein can generally exhibit a HV30 Vickers hardness value in the range of about 2227 HV30 to about 2700 HV30. In some examples, the HV30 Vickers hardness value ranges from about 2250 HV30 to about 2700 HV30. In other examples, the HV30 Vickers hardness value ranges from about 2275 HV30 to about 2700 HV30. In other other examples, the HV30 Vickers hardness value ranges from about 2300 HV30 to about 2700 HV30. In other other examples, the HV30 Vickers hardness value ranges from about 2325 HV30 to about 2700 HV30. In further other examples, the HV30 Vickers hardness value ranges from about 2350 HV30 to about 2700 HV30. In other embodiments, the HV30 Vickers hardness value ranges from about 2375 HV30 to about 2700 HV30. In still other embodiments, the HV30 Vickers hardness value ranges from about 2400 HV30 to about 2700 HV30. In still other embodiments, the HV30 Vickers hardness value ranges from about 2425 HV30 to about 2700 HV30. In still other embodiments, the HV30 Vickers hardness value ranges from about 2450 HV30 to about 2700 HV30. In still other embodiments, the HV30 Vickers hardness value ranges from about 2475 HV30 to about 2700 HV30. In still further other embodiments, the HV30 Vickers hardness value ranges from about 2500 HV30 to about 2700 HV30.

[0085] The HV30 Vickers hardness value can also be between about 2227 HV30 and about 2250 HV30, about 2250 HV30 and about 2275 HV30, about 2275 HV30 and about 2300 HV30, about 2227 HV30 and about 2300 HV30, about 2300 HV30 and about 2325 HV30, about 2325 HV30 and about 2350 HV30, about 2350 HV30 and about 2375 HV30, about 2375 HV30 and about 2400 HV30, about 2400 HV30 and about 2425 HV30, about 2400 HV30 and about 2450 HV30, about 2400 HV30 and about 2475 HV30, about 2400 HV30 and about 2500 HV30, about 2227 HV30 to about 2325 HV30, about 2227 HV30 to about 2350 HV30, about 2227 HV30 to about 2375 HV30, about 2227 HV30 to about 2400 HV30, about 2227 HV30 to about 2425 HV30, about 2227 HV30 to about 2450 HV30, about 2227 HV30 to about 2475 HV30, about 2227 HV30 to about 2500 HV30, about 2250 HV30 to about 2325 HV30, about 2250 HV30 to about 2350 HV30, about 2250 HV30 to about 2375 HV30, about 2250 HV30 to about 2400 HV30, about 2250 HV30 to about 2425 HV30, about 2250 HV30 to about 2450 HV30, about 2250 HV30 to about 2475 HV30, about 2250 HV30 to about 2500 HV30, about 2275 HV30 to about 2325 HV30, about 2275 HV30 to about 2350 HV30, about 2275 HV30 to about 2375 HV30, about 2275 HV30 to about 2400 HV30, about 2275 HV30 to about 2425 HV30, about 2275 HV30 to about 2450 HV30, about 2275 HV30 to about 2475 HV30, about 2275 HV30 to about 2500 HV30, about 2300 HV30 to about 2350 HV30, about 2300 HV30 to about 2375 HV30, about 2300 HV30 to about 2400 HV30, about 2300 HV30 to about 2425 HV30, about 2300 HV30 to about 2450 HV30, about 2300 HV30 to about 2475 HV30, about 2300 HV30 to about 2500 HV30, about 2325 HV30 to about 2375 HV30, about 2325 HV30 to about 2400 HV30, about 2325HV30 to about 2425 HV30, about 2325 HV30 to about 2450 HV30, about 2325 HV30 to about 2475 HV30, about 2325 HV30 to about 2500 HV30, about 2350 HV30 to about 2400 HV30, about 2350 HV30 to about 2425 HV30, about 2350 HV30 to about 2450 HV30, about 2350 HV30 to about 2475 HV30, or about 2350 HV30 to about 2500 HV30, about 2375 HV30 to about 2425 HV30, about 2375 HV30 to about 2450 HV30, about 2375 HV30 to about 2475 HV30, or about 2375 HV30 to about 2500 HV30.

[0086] The cemented carbide compositions for neutron shielding described herein may actually exhibit a Palmqvist fracture toughness (K Ic ) value. In some examples, the Palmqvist fracture toughness (K Ic ) values ​​range from about 6 MPa√m to about 7.6 MPa√m. In other examples, the Palmqvist fracture toughness (K Ic ) values ​​range from about 7 MPa√m to about 7.6 MPa√m.

[0087] Palmqvist fracture toughness (K Ic ) value may also range from about 5 MPa√m to about 6 MPa√m, about 5 MPa√m to about 7 MPa√m, or about 6 MPa√m to about 7 MPa√m.

[0088] Method for manufacturing sintered low-binder high-density cemented carbide for neutron shielding

[0089] By grinding the ceramic hard phase powder and the Fe-Cr metal binder phase powder for several hours (e.g., 8, 16, 32, 64 hours) under ambient conditions (i.e., in a ball mill, superfine pulverizer or planetary pulverizer at 25°C, 298.15 K and 101.325 kPa) to form a powder blend, the desired particle size of the cemented carbide composition can be produced. In some embodiments, as an alternative to the ball mill, superfine pulverizer or planetary pulverizer using physical blending equipment, ultrasonic mixing can be a suitable choice for the blending method. Thus, in this case, ultrasonic mixing uses sound energy to effectively process, for example, powders, pastes, liquids and combinations thereof under conditions of breakthrough speed, quality and repeatability. Powders of almost any size, material properties or morphology can be quickly and thoroughly mixed using, for example, an acoustic mixer. Acoustic processing is generally several orders of magnitude faster than conventional techniques. Here, the acoustic mixer may, for example, employ a 60 Hz motion, which then causes each particle to randomly collide with adjacent particles, change their paths, collide, and then collide again with other particles that behave in an equally chaotic manner. The main purpose of the grinding operation is to promote a good distribution of the Fe-Cr metal binder phase powder and a favorable wettability between the powder components. The grinding operation of the powder is essential to strengthen the physical integrity of the ground ceramic hard phase powder and the Fe-Cr metal binder phase powder, and in some cases, may also deagglomerate tungsten carbide (WC) or ditungsten carbide (W2C) crystals or crystals formed by their combination. An acceptable distribution of the Fe-Cr metal binder phase powder and a good quality of wettability between the powder components are basic parameters for obtaining a cemented carbide with excellent physical quality for neutron shielding. On the other hand, if the Fe-Cr metal binder phase powder distribution and wettability quality are poor, this results in the possibility of undesirable appearance of pores and cracks in the final sintered body, which is detrimental to the manufactured cemented carbide for neutron shielding. In some cases, the ceramic hard phase powder and the Fe-Cr based metal binder powder can be crushed or otherwise comminuted prior to the grinding operation.

[0090] As will be apparent to those skilled in the art, grinding is performed by first adding a grinding liquid to the powder to form a grinding powder slurry composition. The grinding liquid may be: water; an alcohol, such as but not limited to ethanol, methanol, isopropanol, butanol, cyclohexanol; an organic solvent, such as acetone or toluene; an alcohol mixture; a mixture of an alcohol and a solvent; or a similar composition. The properties of the grinding powder slurry composition depend, among other things, on the amount of grinding liquid added. Because the drying of the grinding powder slurry composition requires a lot of energy, the amount of grinding liquid used should be minimized to keep costs low. However, it is necessary to add enough grinding liquid to achieve an easily pumpable grinding powder slurry composition and to avoid system clogging. In addition, other compounds generally known to those skilled in the art can be added to the slurry, such as dispersants, pH regulators, and the like. Non-limiting examples of organic binders such as polyethylene glycol (PEG), paraffin, polyvinyl alcohol (PVA), long-chain fatty acids, waxes, or any combination thereof or similar components may be added to the grinding powder slurry composition before grinding, typically adding, for example, 15% by volume and 25% by volume of the total volume of the formed slurry (i.e., the total volume % composed of the various components). This is done primarily to facilitate the formation of a blend of ceramic hard phase and Fe-Cr based metal binder phase powders during the grinding operation.

[0091] Next, the ground powder slurry composition can be spray dried, freeze dried or vacuum dried and granulated to provide free-flowing powder aggregates that are generally spherical. As used in the context of the present invention, the term "free-flowing" refers to loosely packed cemented carbide powders that present pore spaces between each free-flowing particle of the cemented carbide powder, without any physical restrictions or obstacles that inhibit the free flow of the cemented carbide powder particles.

[0092] In the case of spray drying, the grinding powder slurry composition composed of ceramic hard phase powder mixed with organic liquid and Fe-Cr metal binder phase powder and organic binder can be atomized by a suitable nozzle in a drying tower, wherein small discrete droplets are instantaneously dried by hot gas streams such as nitrogen, argon or air streams flowing horizontally into the drying tower to form spherical powder agglomerates with free-flowing properties. As used herein, "atomization" refers to a process in which a large amount of liquid feed is converted into discrete droplets, thereby significantly increasing the surface area of ​​the feed liquid, thereby significantly increasing the achievable evaporation rate of a given solvent (i.e., grinding liquid). The atomization stage is intended to create optimal conditions for evaporating a given solvent from the grinding powder slurry composition. Nozzles and rotary atomizers are used to form sprays. The drying tower can be equipped with only one nozzle, or equipped with multiple such nozzles to form a mixed agglomerate of spherical ceramic hard phase powder and Fe-Cr metal binder phase powder with free-flowing properties.

[0093] The dried cemented carbide powder can be subjected to a pre-sintering temperature program to completely remove the organic binder, which is also referred to as depegging or dewaxing of the organic binder. A suitable temperature starting from 200°C to 450°C, starting from 200°C to 500°C, starting from 200°C to 550°C, starting from 200°C to 600°C, starting from 250°C to 450°C, starting from 250°C to 500°C, starting from 250°C to 550°C, starting from 250°C to 600°C, starting from 300°C to 450°C, starting from 300°C to 500°C, starting from 300°C to 550°C, or starting from 300°C to 600°C can be used to completely remove the organic binder. This can usually be carried out in a reactive H2 atmosphere, wherein the applied hydrogen (H2) flow rate is about 1000 liters / hour to about 10000 liters / hour, about 3000 liters / hour to about 10000 liters / hour, about 6000 liters / hour to about 10000 liters / hour or about 9000 liters / hour to about 10000 liters / hour. The temperature can usually be continuously increased at a rate of, for example, about 0.70°C / min. In some instances, after removing the organic binder, the temperature can be sequentially increased in series at a rate of about 2°C / min, and when a certain temperature range is reached, the rate becomes about 10°C / min, or again when a specific temperature range is reached, for example, at a rate of about 2°C / min to about 5°C / min. The above-mentioned temperature range of removal or dewaxing (i.e., debonding of the organic binder) can usually be reached after heating in a sintering furnace for about 60 minutes to about 90 minutes or about 60 minutes to about 7 hours. Thus, typically, the particular type of heating pattern selected is determined and carried out and for a particular period of time in a manner that imparts and thereby imparts the desired fully dewaxed phase transformation to the cemented carbide powder. Typically, the pre-sintering cycle for organic binder dewaxing can be carried out in a reactive (H2) atmosphere, in a vacuum, or in a non-reactive inert atmosphere such as nitrogen (N2) or argon (Ar).

[0094] Next, the cemented carbide powder is subsequently subjected to a consolidation process to ultimately form a high-density cemented carbide for neutron shielding. As used in the text of the present invention, the term "consolidation process" refers to any process including simultaneously (i) compacting (i.e., pressing) and (ii) consolidating (i.e., densifying, thereby sintering the material by heating) cemented carbide powder. In some instances, the consolidation process can be completed by hot pressing (HP) cemented carbide powder. HP is a relatively slow process, and compaction is usually uniaxial. Heating is completed simultaneously by components integrated in the press. In other instances, the consolidation process can be performed by hot isostatic pressing (HIP). HIP is also a relatively slow process, and compaction is isostatic, i.e., pressure is applied in 3 directions or axes. Heating is performed simultaneously by components integrated in the press. Therefore, HIP subjects cemented carbide powder to high temperature and isostatic gas pressure in, for example, a high-pressure vessel. The pressurized gas used can be, for example, argon. Inert gases such as argon are most commonly used so that the material subjected to HIP does not chemically react. The chamber is heated, resulting in an increase in pressure within the container. Pressure is applied to the cemented carbide powder from all three directions. Inert argon can generally apply a pressure of about 7,350psi (about 50.7 MPa) to about 45,000 psi (about 310 MPa), wherein about 15,000 psi (about 100 MPa) is generally the most commonly used pressure. In other examples, the consolidation process can be performed by spark plasma sintering (SPS). The main feature of SPS is that a pulsed direct current (DC) or alternating current (AC) current passes through the sintering mold. Unlike HP and HIP, in which heat is provided by an external heating element, heat is generated internally. This is conducive to achieving high heating and cooling rates (e.g., up to 1000 K / min). As a result, the sintering process is generally very fast, typically completed within a few minutes. The speed of the process ensures that it is possible to densify the cemented carbide powder to nanometer size or nanostructure while avoiding the roughening associated with standard densification techniques. In SPS, compaction is usually uniaxial, but with respect to stress state, isostatic stress state can be potentially reached due to the effect produced by the rigid sintering mold containing and wrapping cemented carbide powder. As mentioned above, heating is provided by subjecting the sintering mold to the electric current field of the sintering mold containing cemented carbide powder. SPS can be used as a tool to form functional gradient soft magnetic cemented carbide powder, and it helps to accelerate the development of magnetic materials. It is worth noting that, compared with more traditional consolidation methods, SPS improves the oxidation resistance and wear resistance of sintered cemented carbide. In other other examples, methods similar to this above-mentioned technology can be used for the consolidation process of cemented carbide powder, which is obvious to those of ordinary skill in the art.

[0095] The temperature applied for the aforementioned sintering and consolidation process may mainly be in the range of starting from 1300°C and ending at 1500°C, starting from 1300°C and ending at 1600°C, starting from 1300°C and ending at 1700°C, starting from 1300°C and ending at 1800°C, starting from 1400°C and ending at 1500°C, starting from 1400°C and ending at 1600°C, starting from 1400°C and ending at 1700°C, starting from 1400°C and ending at 1800°C, starting from 1500°C and ending at 1600°C, starting from 1500°C and ending at 1700°C, or starting from 1500°C and ending at 1800°C.

[0096] In the case of HIP, the cemented carbide powder can be HIPed, or, as an additional step, the sintered cemented carbide can be HIPed. In this case, the cemented carbide material will be pressed and typically vacuum sintered in a generally non-reactive inert atmosphere such as argon (Ar) or nitrogen (N2). Next, the sintered cemented carbide can be subjected to an additional HIP treatment step. This additional HIP step achieves the purpose of eliminating any pores that may be present in the sintered cemented carbide powder. During the vacuum sintering process, the temperature range applied can be, for example: starting from 1300°C and ending at 1500°C, starting from 1300°C and ending at 1600°C, starting from 1300°C and ending at 1700°C, starting from 1300°C and ending at 1800°C, starting from 1300°C and ending at 1900°C, starting from 1300°C and ending at 2000°C, starting from 1400°C and ending at 1500°C, starting from 1400°C and ending at 1600°C. starting at 1400°C and ending at 1700°C, starting at 1400°C and ending at 1800°C, starting at 1400°C and ending at 1900°C, starting at 1400°C and ending at 2000°C, starting at 1500°C and ending at 1600°C, starting at 1500°C and ending at 1700°C, starting at 1500°C and ending at 1800°C, starting at 1500°C and ending at 1900°C, or starting at 1500°C and ending at 2000°C.

[0097] Now turn to Figure 1 , which shows a flow chart illustrating the various process steps for manufacturing low binder high density cemented carbide for neutron shielding according to an exemplary embodiment of the subject matter. Figure 1It is shown that in step 100, the process starts with blending a powder mixture in a grinding liquid with an organic binder to form a slurry blend, the powder mixture comprising a powder of a hard component forming a ceramic hard phase and an iron (Fe)-chromium (Cr) metal binder phase, the iron (Fe)-chromium (Cr) metal binder phase comprising about 5 wt% to about 16 wt% chromium based on the total weight of the Fe-Cr metal binder phase, as described in paragraphs

[0081] to

[0082] . Next, in step 102, the formed slurry blend is dried by any of the methods described to obtain a powder blend, as described in paragraphs

[0083] to

[0084] . In step 105, a pre-sintering temperature program is performed, which thus completely removes any possible residual organic binder, thereby dewaxing and debonding the formed powder mixture, as described in paragraph

[0085] . The process finally ends in step 110, wherein the dewaxed powder blend is sintered by performing any of the consolidation methods previously described in paragraphs

[0086] to

[0088] to ultimately form a sintered high-density cemented carbide for neutron shielding, which consolidation method may include hot pressing (HP), hot isostatic pressing (HIP) or spark plasma sintering (SPS). However, it should be understood that sintering generally includes a process defined by debinding, solid state sintering, liquid phase sintering and finally cooling the sintered material to ambient conditions after the sintering operation is fully completed. A person of ordinary skill in the art will appreciate that the above steps in the consolidation process described in paragraphs

[0085] to

[0088] above can be performed together in the same consolidation equipment. Alternatively, a person of ordinary skill in the art will also appreciate that they can also be performed one after another in different consolidation equipment.

[0098] The theoretical density of the cemented carbide composition for neutron shielding described herein can generally be about 15.25 g / cm 3 to about 17 g / cm 3 In some examples, the theoretical density of the cemented carbide composition is about 15.50 g / cm 3 to about 17 g / cm 3 In other examples, the theoretical density of the cemented carbide composition is about 15.75 g / cm 3 to about 17 g / cm 3 In other examples, the theoretical density of the cemented carbide composition is about 16 g / cm 3 About 17g / cm 3 In yet other examples, the theoretical density of the cemented carbide composition is about 16.25 g / cm 3 About 17g / cm 3In still other examples, the theoretical density of the cemented carbide composition is about 16.50 g / cm 3 to about 17 g / cm 3 In yet other examples, the theoretical density of the cemented carbide composition is about 16.75 g / cm 3 to about 17 g / cm 3 within the range.

[0099] The cemented carbide composition may also have a hardness of about 15.25 g / cm 3 to about 15.50 g / cm 3 , about 15.50 g / cm 3 to about 15.75 g / cm 3 , about 15.75 g / cm 3 to about 16 g / cm 3 , about 15.25 g / cm 3 To about 15.75g / cm 3 , about 15.25 g / cm 3 to about 16 g / cm 3 , about 15.25g / cm 3 About 16.25g / cm 3 , about 16 g / cm 3 to about 16.25 g / cm 3 , about 16 g / cm 3 to about 16.50 g / cm 3 , about 16 g / cm 3 to about 16.75 g / cm 3 , about 16.25 g / cm 3 to about 16.50 g / cm 3 , about 16.25 g / cm 3 to about 16.75 g / cm 3 or about 16.50 g / cm 3 to about 16.75 g / cm 3 Theoretical density within the range.

[0100] Table 1 below shows the theoretical density in certain specific embodiments of the cemented carbide compositions A to E of the present application compared with the comparative sample F. Table 1 shows that when the weight of the metal binder phase is about 9% higher than 2.75 wt % based on the total weight of the cemented carbide composition (i.e., 3 wt % in the comparative sample H vs. 2.75 wt % in the application sample G), it is seen that the theoretical density increases from 15.21 g / cm 3 Reduced to 15.17 g / cm 3, which would then have a weakening and detrimental effect on the neutron shielding potential of comparative sample H. In other words, this means that in order to obtain the same neutron shielding effect and capability, the low-density cemented carbide sample would need to have a greater thickness than the high-density cemented carbide sample.

[0101]

[0102] Example

[0103] The following examples are put forward to provide those skilled in the art with a complete description and instructions of how to make and use the subject matter described, and are not intended to limit the scope of what the inventors regard as their disclosure, nor are they intended to represent that the experiments below are all or the only experiments performed. With respect to the numerical values ​​used, attempts have been made to ensure accuracy, but some experimental errors and deviations should be accounted for.

[0104] Example 1

[0105] High-density cemented carbide compositions having a ceramic hard phase and a low-weight iron (Fe)-chromium (Cr) metal binder phase exhibit superior corrosion resistance than comparative samples

[0106]

[0107] Table 2 shows that when the weight of the metal binder phase used is close to 3 wt% of the total weight of the cemented carbide composition (i.e., Comparative Samples E to F), Comparative Samples E and Comparative Samples F respectively exhibit (I) lower continuity and (II) poorer continuity of the passivation layer Cr3O2 on the metal binder surface. Therefore, in this case, Comparative Samples E and Comparative Samples F may exhibit lower corrosion resistance because the positive effect of the passivation layer Cr3O2 on the continuity of the metal binder surface is weakened. Although Comparative Sample D exhibits good continuity of the passivation layer (Cr3O2) on the metal binder surface when the weight of the metal binder phase is 3 wt%, this is advantageously attributed to the weight content of Cr being about 10.7 wt% based on the total weight of the Fe-Cr system metal binder phase.

[0108] Example 2

[0109] High density cemented carbide composites having a ceramic hard phase and a low weight iron (Fe)-chromium (Cr) metal binder phase exhibit strong hardness and fracture toughness

[0110]

[0111] Table 3 shows the compositions of samples W2C_Fe, WC_Fe1, WC_Fe2, WC_Fe3, WC_Fe4, WC_Fe5, and WC_Fe6, which contain Fe-Cr based metal binder in the weight range of 0.02 wt% to 2.75 wt%, WC in the weight range of 97.25 wt% to 99.98 wt%, and W2C in the weight range of 99.98 wt%.

[0112] As described in paragraph

[0056] of the present invention, the HV30 Vickers hardness and the Palmqvist fracture toughness (K Ic ). Three indentations were applied to each material at 30 kgf using a Vickers Limited device. The indentation diagonal and the length of cracks emerging from the indentation corner were measured using an optical microscope at a magnification of 500 times.

[0113] As shown in Table 3, the HV30 Vickers hardness values ​​obtained for samples W2C_Fe, WC_Fe1, WC_Fe2, WC_Fe3, WC_Fe4, WC_Fe5 and WC_Fe6 are in the range of 2227 HV30 to 2700 HV30. On the other hand, the Palmqvist fracture toughness (K Ic ) values ​​are in the range of 5 MPa√m to 7.6 MPa√m.

[0114] While the present invention has been described in conjunction with the embodiments thereof, those skilled in the art will appreciate that additions, deletions, modifications and substitutions not specifically described may be made without departing from the spirit and scope of the invention as defined in the appended claims.

[0115] Regarding the use of a large number of any plural and / or singular terms in this article, those skilled in the art are able to appropriately convert the plural to the singular and / or the singular to the plural according to the context and / or application. For clarity, various singular / plural conversions are not explicitly set forth herein.

[0116] The subject matter described herein sometimes shows different components contained in or connected to different other components.It should be understood that the architecture described in this way is only exemplary, and many other architectures that realize the same function can actually be completed.In a conceptual sense, any arrangement of components that realize the same function is effectively "associated" to achieve the desired function.Therefore, any two components combined to realize a specific function herein can be regarded as "associated" to each other to achieve the desired function, regardless of the architecture or intermediate components.Similarly, any two components so associated can also be regarded as "operably connected" or "operably coupled" to each other to achieve the desired function, and any two components that can be so associated can also be regarded as "operably coupled" to each other to achieve the desired function.Specific examples that can be operably coupled include but are not limited to physically matchable and / or physically interactive components, and / or wirelessly interactive and / or wirelessly interactive components, and / or logically interactive and / or logically interactive components.

[0117] In some cases, one or more components may be referred to herein as being "configured to," "configured to," "configurable to," "operable / operability," "adaptable / adaptable," "capable of," "compliant / conformant," etc. Those skilled in the art will recognize that such terminology (e.g., "configured to") can generally include active state components and / or inactive state components and / or standby state components unless the context requires otherwise.

[0118] Although particular aspects of the subject matter described herein have been shown and described, it will be apparent to those skilled in the art that changes and modifications may be made based on the claims herein without departing from the subject matter described herein and its broader aspects, and the appended claims will therefore cover within their scope all such changes and modifications within the true spirit and scope of the subject matter described herein. Those skilled in the art will understand that, in general, the terms used herein, particularly in the appended claims (e.g., the bodies of the appended claims), are generally intended to be "open" terms (e.g., the term "including" should be interpreted as "including but not limited to", the term "having" should be interpreted as "at least having", the term "including" should be interpreted as "including but not limited to", etc.).

[0119] Those skilled in the art will further understand that if a specific number of claim recitations is intended, such intent will be expressly recited in the claim, and in the absence of such a statement, such intent is absent. For example, as an aid to understanding, the following appended claims may contain the use of the introductory phrases "at least one" and "one or more" to introduce claim recitations. However, the use of such phrases should not be interpreted as implying that a claim recitation introduced by the indefinite article "a" or "an" limits any particular claim containing such introduced claim recitation to claims containing only one such statement, even when the same claim includes the introductory phrases "one or more" or "at least one" and an indefinite article such as "a" or "an" (e.g., "a" and / or "an" should typically be interpreted as meaning "at least one" or "one or more"); the same is true for the use of definite articles used to introduce claim recitations.

[0120] Furthermore, even if a specific number of an introduced claim statement is explicitly stated, those skilled in the art will recognize that such a statement should generally be interpreted to mean at least the stated number (e.g., a mere statement of "two statements," without other modifiers, generally means at least two statements, or more than two statements).

[0121] In addition, in those cases where a convention similar to "at least one of A, B, and C, etc." is used, generally such construction is intended that a person skilled in the art will understand the meaning of the convention (e.g., "a system having at least one of A, B, and C" will include but is not limited to systems having only A, only B, only C, A and B together, A and C together, B and C together, and / or A, B, and C together, etc.). In those cases where a convention similar to "at least one of A, B, or C, etc." is used, generally such construction is intended that a person skilled in the art will understand the meaning of the convention (e.g., "a system having at least one of A, B, or C" will include but is not limited to systems having only A, only B, only C, A and B together, A and C together, B and C together, and / or A, B, and C together, etc.). A person skilled in the art will further understand that transition words and / or phrases that typically indicate more than two alternative terms, whether in the specification, claims, or drawings, should be understood to contemplate the possibility of including one of the terms, any of the terms, or both of the terms, unless the context dictates otherwise. For example, the phrase "A or B" will generally be understood to include the possibilities of "A" or "B" or "A and B."

[0122] With respect to the appended claims, those skilled in the art will recognize that the operations described therein may generally be implemented in any order. Moreover, although various operational flows are presented in one or more sequences, it should be understood that the various operations may be implemented in other orders than those shown, or may be implemented simultaneously. Unless the context dictates otherwise, examples of such alternative orderings may include overlapping, interleaved, interrupted, reordered, incremental, preparatory, supplementary, simultaneous, reverse, or other variant orderings. Furthermore, unless the context dictates otherwise, terms such as "responsive to," "involving," or other past tense adjectives are generally not intended to exclude such variants.

[0123] Those skilled in the art will recognize that the specific exemplary processes and / or apparatus and / or techniques described above are representative of more general processes and / or apparatus and / or techniques set forth elsewhere herein, such as in the claims filed herewith and / or elsewhere in this application.

[0124] Although various aspects and embodiments have been disclosed herein, other aspects and embodiments will be apparent to those skilled in the art. The various aspects and embodiments disclosed herein are for illustrative purposes only and are not intended to be limiting, with the true scope and spirit being indicated by the following claims.

[0125] The exemplary embodiments described in the detailed description, drawings, and claims are not meant to be limiting. Other embodiments may be used, and other changes may be made, without departing from the spirit or scope of the subject matter presented here.

[0126] Where a range of values ​​is provided, it is understood that unless the context clearly indicates otherwise, each intervening value between the upper and lower limits of the range as small as one tenth of the unit of the lower limit or any other stated or intervening value within the range is also included within the scope of the present invention. The upper and lower limits of these smaller ranges that can be independently included in the smaller ranges are also included in the present invention, and any limit within the range is explicitly excluded. When the range includes one or two limits, the range excluding both included limits is also included in the present invention.

[0127] Those skilled in the art will recognize that, for the sake of conceptual clarity, the components (e.g., operations), devices, objects, and discussions accompanying them described herein are used as examples, and various configuration variations can be expected. Therefore, as used herein, the specific examples and accompanying discussions are intended to represent their more general categories. Generally, the use of any particular example is intended to represent its category, and the absence of a particular component (e.g., operation), device, and object should not be considered a limitation.

[0128] Additionally, for example, any sequence and / or timing of sequences of the systems and methods described herein are illustrative and should not be construed as being limiting in nature. Thus, it should be understood that process steps may be shown and described in a sequence or timing, but they are not necessarily limited to being performed in any particular sequence or order. For example, the steps in these processes or methods may generally be performed in a variety of different sequences and orders while still being within the scope of the present invention.

[0129] Finally, the application publications and / or patents discussed herein are provided solely for their disclosure prior to the filing date of the disclosure. Nothing herein should be construed as an admission that the disclosure is not entitled to antedate such publication by virtue of prior disclosure.

Claims

1. A high-density cemented carbide composition, comprising: Ceramic hard phase; and The iron (Fe)-chromium (Cr) metal binder phase comprises about 5 wt % to about 16 wt % of chromium based on the total weight of the Fe-Cr metal binder phase. 2 . The high-density cemented carbide composition according to claim 1 , wherein the weight of the chromium is about 10.5 wt % to about 16 wt % based on the total weight of the Fe—Cr based metal binder phase.

3. The high-density cemented carbide composition according to claim 2, wherein the weight of the chromium is about 10.5 wt% to about 10.7 wt% based on the total weight of the Fe-Cr system metal binder phase.

4. The high-density cemented carbide composition according to claim 1, wherein the cemented carbide composition comprises about 0.02 wt. % to about 2.75 wt. % of the Fe-Cr based metal binder phase based on the total weight of the cemented carbide composition. 5 . The high-density cemented carbide composition according to claim 4 , wherein the cemented carbide composition comprises about 2.75 wt % of the Fe—Cr-based metal binder phase based on the total weight of the cemented carbide composition.

6. The high-density cemented carbide composition of claim 1, wherein the ceramic hard phase comprises tungsten carbide (WC), substoichiometric ditungsten carbide (W2C), or a combination thereof.

7. The high-density cemented carbide composition according to claim 6, wherein the ceramic hard phase comprises WC.

8. The high density cemented carbide composition of claim 6, wherein the ceramic hard phase comprises substoichiometric W2C.

9. The high density cemented carbide composition of claim 6, wherein the ceramic hard phase comprises a combination of WC and substoichiometric W2C in a ratio of 1:

1.

10. The high density cemented carbide composition of claim 1, wherein the cemented carbide composition comprises about 97.25 wt% to about 99.98 wt% of the ceramic hard phase based on the total weight of the cemented carbide composition.

11. The high density cemented carbide composition of claim 1, wherein the cemented carbide composition has a density of about 15.25 g / cm 3 to about 17 g / cm 3 The theoretical density.

12. The high density cemented carbide composition according to claim 1, wherein a cemented carbide composition having improved corrosion resistance is obtained.

13. The high-density cemented carbide composition according to claim 1, wherein the Fe-Cr based metal binder phase is prepared by blending FeCr powder with Cr3C2 powder.

14. The high density cemented carbide composition according to claim 1, wherein the cemented carbide composition has a HV30 Vickers hardness in the range of about 2227 HV30 to about 2700 HV30 and a Palmqvist fracture toughness (K Ic ).

15. A method for manufacturing a sintered high-density cemented carbide, the method comprising: The powder mixture in the slurry is blended with an organic binder to form a slurry blend, wherein the powder mixture comprises: a powder of a hard component forming a ceramic hard phase; and an iron (Fe)-chromium (Cr)-based metal binder phase, wherein the iron (Fe)-chromium (Cr)-based metal binder phase comprises about 5 wt % to about 16 wt % of chromium based on the total weight of the Fe-Cr-based metal binder phase; drying the slurry blend to form a powder blend; and The powder blend is sintered to form a sintered high density cemented carbide. 16 . The method for manufacturing a sintered high-density cemented carbide according to claim 15 , wherein the weight of the chromium is about 10.5 wt % to about 16 wt % based on the total weight of the Fe—Cr system metal binder phase. 17 . The method for manufacturing a sintered high-density cemented carbide according to claim 16 , wherein the weight of the chromium is about 10.5 wt % to about 10.7 wt % based on the total weight of the Fe—Cr system metal binder phase.

18. The method for manufacturing a sintered high-density cemented carbide according to claim 15, wherein the cemented carbide comprises about 0.02 wt% to about 2.75 wt% of the Fe-Cr based metal binder phase based on the total weight of the cemented carbide.

19. The method for manufacturing a sintered high-density cemented carbide according to claim 18, wherein the cemented carbide comprises about 2.75 wt% of the Fe-Cr based metal binder phase based on the total weight of the cemented carbide.

20. The method for manufacturing a sintered high-density cemented carbide according to claim 15, wherein the ceramic hard phase comprises tungsten carbide (WC), substoichiometric ditungsten carbide (W2C), or a combination thereof.

21. The method for manufacturing a sintered high-density cemented carbide according to claim 20, wherein the ceramic hard phase comprises WC.

22. The method for manufacturing a sintered high-density cemented carbide according to claim 20, wherein the ceramic hard phase comprises substoichiometric W2C.

23. The method for manufacturing a sintered high-density cemented carbide according to claim 20, wherein the ceramic hard phase comprises a combination of WC and substoichiometric W2C in a ratio of 1:

1.

24. The method for manufacturing a sintered high-density cemented carbide according to claim 15, wherein the cemented carbide comprises about 97.25 wt% to about 99.98 wt% of the ceramic hard phase based on the total weight of the cemented carbide.

25. The method for manufacturing a sintered high-density cemented carbide according to claim 15, wherein the cemented carbide has a density of about 15.25 g / cm 3 to about 17 g / cm 3 The theoretical density.

26. The method for manufacturing a sintered high-density cemented carbide according to claim 15, wherein a cemented carbide having improved corrosion resistance is obtained.

27. The method for manufacturing a sintered high-density cemented carbide according to claim 15, wherein the Fe-Cr based metal binder phase is prepared by blending FeCr powder with Cr3C2 powder.

28. The method for manufacturing a sintered high-density cemented carbide according to claim 15, wherein the cemented carbide has a HV30 Vickers hardness in the range of about 2227 HV30 to about 2700 HV30 and a Palmqvist fracture toughness (K Ic ).

29. The method for manufacturing sintered high-density cemented carbide according to claim 15, wherein the drying the slurry blend comprises vacuum drying, air drying, freeze drying, or spray drying by atomization.

30. The method for manufacturing a sintered high-density cemented carbide according to claim 15, wherein the sintering comprises hot pressing (HP), hot isostatic pressing (HIP) or spark plasma sintering (SPS).

Citation Information

Cited By

  • Binding-phase-free hard alloy containing W2C and preparation method thereof

    CN122406066A