Positive electrode active material for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery

By using a lithium composite oxide mixture containing Ni as the positive electrode active substance in a nonaqueous electrolyte secondary battery, the problem of taking into account both the capacity and the charge and discharge cycle characteristics is solved, and high capacity and stability are improved.

CN119032436APending Publication Date: 2024-11-26PANASONIC ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380021873.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-25
Filing Date
2023-02-21
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

While improving capacity, the existing nonaqueous electrolyte secondary batteries are difficult to take into account the reduction of charge and discharge cycle characteristics.

Method used

The lithium composite oxide containing Ni is used as the positive electrode active material, and the mixture of the first positive electrode active material and the second positive electrode active material is used as the positive electrode active material, and the mole ratio of Ni of the first positive electrode active material is 80% or more, Mn The ratio is 1% or less, and the ratio of Ni of the second positive electrode active material is within the range of ±3%. A peak of NiO was observed in the mixture, and X-ray diffraction was used to suppress the reduction of charge and discharge cycle characteristics.

Benefits of technology

The battery is high-capacity and the reduction of charge and discharge cycle characteristics are achieved, and the battery charge and discharge stability and capacity retention rate are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004993084620000131
    Figure BDA0004993084620000131
  • Figure HDA0004993084630000011
    Figure HDA0004993084630000011
Patent Text Reader

Abstract

The positive electrode active material for a non-aqueous electrolyte secondary battery is characterized by comprising a mixture of a first positive electrode active material, which is a lithium composite oxide containing Ni, and a second positive electrode active material, the ratio (A1) of the number of moles of Ni relative to the total number of moles of metal elements other than Li being 80% or more, and the ratio (A2) of the number of moles of Ni relative to the total number of moles of metal elements other than Li being 80% or more. The ratio (A2) of the number of moles of Mn relative to the total number of moles of metal elements other than Li is 1% or less, the second positive electrode active material is a Ni-containing lithium composite oxide, and the ratio (B1) of the number of moles of Ni relative to the total number of moles of metal elements other than Li is within the range of + / -3% of the ratio (A1); the ratio (B2) of the number of moles of Mn to the total number of moles of metal elements other than Li is 3% or more, and a peak of NiO is observed in X-ray diffraction measurement of the mixture.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a positive electrode active material for a nonaqueous electrolyte secondary battery and a nonaqueous electrolyte secondary battery. Background Art

[0002] In recent years, nonaqueous electrolyte secondary batteries have been widely used as high-output, high-energy-density secondary batteries that include a positive electrode, a negative electrode, and a nonaqueous electrolyte and that perform charge and discharge by transferring lithium ions or the like between the positive electrode and the negative electrode.

[0003] For example, Patent Document 1 discloses a non-aqueous electrolyte secondary battery that uses a lithium composite oxide as a positive electrode active material, wherein the lithium composite oxide is composed of a granular lithium composite oxide containing at least lithium, nickel, cobalt, manganese and tantalum as constituent elements and a layer of nickel oxide formed on the surface of the lithium composite oxide.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2016-110924 Summary of the invention

[0007] However, along with the high capacity of non-aqueous electrolyte secondary batteries, the high capacity of positive electrode active materials is required. As a method for high capacity of positive electrode active materials, it is conceivable to use a lithium composite oxide containing Ni that increases the ratio of the molar number of Ni relative to the total molar number of metal elements other than lithium. However, if the ratio of the above-mentioned Ni becomes high, the charge-discharge cycle characteristics are reduced, and it is therefore difficult to achieve a balance between high capacity and suppression of the reduction of charge-discharge cycle characteristics.

[0008] Therefore, an object of the present invention is to provide a positive electrode active material for a nonaqueous electrolyte secondary battery that can achieve both high battery capacity and suppression of degradation in charge and discharge cycle characteristics, and a nonaqueous electrolyte secondary battery having the same.

[0009] A positive electrode active material for a non-aqueous electrolyte secondary battery as one embodiment of the present invention is characterized in that it has a mixture of a first positive electrode active material and a second positive electrode active material, wherein the first positive electrode active material is a lithium composite oxide containing Ni, the ratio (A1) of the molar number of Ni relative to the total molar number of metal elements excluding Li is 80% or more, and the ratio (A2) of the molar number of Mn relative to the total molar number of metal elements excluding Li is 1% or less, and the second positive electrode active material is a lithium composite oxide containing Ni, the ratio (B1) of the molar number of Ni relative to the total molar number of metal elements excluding Li is in the range of ±3% of the above ratio (A1), and the ratio (B2) of the molar number of Mn relative to the total molar number of metal elements excluding Li is 3% or more, and in the X-ray diffraction measurement of the above mixture, a NiO peak is observed.

[0010] A nonaqueous electrolyte secondary battery as one embodiment of the present invention is characterized by comprising a positive electrode, a negative electrode, and a nonaqueous electrolyte, wherein the positive electrode contains the positive electrode active material for a nonaqueous electrolyte secondary battery.

[0011] According to one embodiment of the present invention, a positive electrode active material for a nonaqueous electrolyte secondary battery that can achieve both high battery capacity and reduced charge-discharge cycle characteristics, and a nonaqueous electrolyte secondary battery including the positive electrode active material can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 It is a cross-sectional view of a nonaqueous electrolyte secondary battery as an example of the embodiment. DETAILED DESCRIPTION

[0013] The drawings referred to in the description of the embodiments are schematic drawings, and the dimensional ratios of the components depicted in the drawings may differ from the actual ones.

[0014] Figure 1 It is a schematic cross-sectional view of a secondary battery as an example of an embodiment. Figure 1The secondary battery 10 shown has a wound electrode body 14 in which a positive electrode 11 and a negative electrode 12 are wound with a separator 13 interposed therebetween, a non-aqueous electrolyte, insulating plates 18 and 19 respectively arranged above and below the electrode body 14, and a battery case 15 for accommodating the above components. The battery case 15 includes a shell body 16 in a cylindrical shape with a bottom and a sealing body 17 for sealing the opening of the shell body 16. It should be noted that other forms of electrode bodies such as a laminated electrode body in which a positive electrode and a negative electrode are alternately laminated with a separator interposed therebetween may be used instead of the wound electrode body 14. In addition, as the battery case 15, examples may include cylindrical, square, coin-shaped, button-shaped, and other metal shells, resin shells formed by laminating resin sheets (so-called laminated type), and the like.

[0015] The non-aqueous electrolyte includes, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. The non-aqueous solvent may be, for example, esters, ethers, nitriles, amides, and mixed solvents of two or more thereof. The non-aqueous solvent may contain a halogen substitute in which at least a portion of the hydrogen of these solvents is replaced by a halogen atom such as fluorine. The electrolyte salt may be, for example, a lithium salt such as LiPF6. It should be noted that the electrolyte is not limited to a liquid electrolyte, and may also be a solid electrolyte using a gel-like polymer or the like.

[0016] The outer shell body 16 is, for example, a metal container in a cylindrical shape with a bottom. A gasket 28 is provided between the outer shell body 16 and the sealing body 17 to ensure the airtightness inside the battery. The outer shell body 16 has a protrusion 22 formed by, for example, a part of the side portion protruding inward to support the sealing body 17. The protrusion 22 is preferably formed in an annular shape along the circumferential direction of the outer shell body 16, and supports the sealing body 17 with its upper surface.

[0017] The sealing body 17 has a structure in which a filter 23, a lower valve body 24, an insulating member 25, an upper valve body 26 and a cap 27 are stacked in order from the electrode body 14 side. The components constituting the sealing body 17 have, for example, a disc shape or a ring shape, and the components except the insulating member 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective central portions, and an insulating member 25 is sandwiched between their respective peripheral portions. When the internal pressure of the secondary battery 10 rises due to heat caused by an internal short circuit, for example, the lower valve body 24 is deformed and broken in a manner that pushes the upper valve body 26 toward the cap 27 side, thereby blocking the current path between the lower valve body 24 and the upper valve body 26. When the internal pressure rises further, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.

[0018] Figure 1In the secondary battery 10 shown, the positive electrode lead 20 attached to the positive electrode 11 passes through the through hole of the insulating plate 18 and extends to the sealing body 17 side, and the negative electrode lead 21 attached to the negative electrode 12 passes through the outside of the insulating plate 19 and extends to the bottom side of the outer shell body 16. The positive electrode lead 20 is connected to the lower surface of the filter 23 as the bottom plate of the sealing body 17 by welding or the like, and the cap 27 as the top plate of the sealing body 17 electrically connected to the filter 23 becomes the positive terminal. The negative electrode lead 21 is connected to the bottom inner surface of the outer shell body 16 by welding or the like, and the outer shell body 16 becomes the negative terminal.

[0019] Hereinafter, the positive electrode 11 , the negative electrode 12 , and the separator 13 will be described in detail.

[0020] [positive electrode]

[0021] The positive electrode 11 includes a positive electrode current collector and a positive electrode mixture layer disposed on the positive electrode current collector. It should be noted that the positive electrode mixture layer is preferably disposed on both surfaces of the positive electrode current collector.

[0022] The positive electrode current collector may be made of a foil of a metal such as aluminum or aluminum alloy that is stable in the potential range of the positive electrode, or a film having the metal disposed on the surface. The positive electrode current collector has a thickness of, for example, about 10 μm to 100 μm.

[0023] The positive electrode mixture layer includes a positive electrode active material. The positive electrode active material includes a mixture of a first positive electrode active material and a second positive electrode active material. From the perspective of bonding the positive electrode active materials to ensure the mechanical strength of the positive electrode mixture layer, the positive electrode mixture layer is suitable for including a binding material. In addition, from the perspective of being able to improve the conductivity of the positive electrode mixture layer, the layer is suitable for including a conductive material.

[0024] For example, a positive electrode mixture slurry containing a positive electrode active material, a binder, a conductive material, etc. is prepared, the positive electrode mixture slurry is applied to a positive electrode current collector, the coating is dried, and then the coating is rolled to produce a positive electrode.

[0025] The first positive electrode active material is a nickel-containing lithium composite oxide. The ratio (A1) of the molar number of Ni to the total molar number of metal elements excluding Li is 80% or more, and the ratio (A2) of the molar number of Mn to the total molar number of metal elements excluding Li is 1% or less. Regarding the ratio (A1) of the molar number of Ni, from the aspect of increasing the capacity of the battery, it is preferably 85% or more. In addition, the ratio (A2) of the molar number of Mn may also be 0%. In addition, regarding the nickel-containing lithium composite oxide of the first positive electrode active material, from the aspect of suppressing the deterioration of charge-discharge cycle characteristics, it preferably contains Co, and particularly preferably the ratio (A3) of the molar number of Co to the total molar number of metal elements excluding Li is 3% or more. The upper limit of the ratio (A3) of the molar number of Co may also be 10% or less, for example.

[0026] The nickel-containing lithium composite oxide of the first positive electrode active material is preferably, for example, a nickel-containing lithium composite oxide represented by the following general formula (1).

[0027] Li z Ni 1-x-y Co x M y O2 (1)

[0028] In the formula, x, y, and z preferably satisfy 0 < x ≤ 0.10, 0 < y ≤ 0.05, 0.85 ≤ 1 - x - y ≤ 0.95, and 0.960 ≤ z ≤ 0.983. In addition, M in the formula is preferably at least one element selected from Mn, Al, W, Nb, Mg, Ti, and Mo, and more preferably Al.

[0029] The second positive electrode active material is a nickel-containing lithium composite oxide. The ratio (B1) of the molar number of Ni to the total molar number of metal elements excluding Li is in the range of ±3% of the ratio (A1) of the molar number of Ni to the total molar number of metal elements excluding Li of the first positive electrode active material. For example, if the ratio (A1) of the molar number of Ni in the first positive electrode active material is 90%, then the ratio (B1) of the molar number of Ni in the second positive electrode active material is in the range of 87% to 93%. In addition, in the second positive electrode active material, regarding the ratio (B2) of the molar number of Mn to the total molar number of metal elements excluding Li, from the aspect of suppressing the deterioration of charge-discharge cycle characteristics, it is 3% or more, preferably 3% or more and 10% or less. In addition, in the second positive electrode active material, the ratio (B3) of the molar number of Co to the total molar number of metal elements excluding Li is preferably 1 mol% or less, and more preferably 0 mol%.

[0030] The Ni-containing lithium composite oxide of the second positive electrode active material is preferably, for example, the Ni-containing lithium composite oxide represented by the following general formula (2).

[0031] Li z Ni 1-x-y Mn x M y O2 (2)

[0032] In the formula, x, y, and z preferably satisfy 0 < x ≤ 0.10, 0 < y ≤ 0.08, 0.82 ≤ 1 - x - y ≤ 0.98, and 0.974 ≤ z ≤ 1.004. In addition, M in the formula is preferably at least one element selected from Al, W, Nb, Mg, Ti, and Mo, and more preferably Al.

[0033] The composition of the Ni-containing lithium composite oxide is measured by inductively coupled plasma (ICP) optical emission spectrometry.

[0034] When performing X-ray diffraction measurement on the mixture of the first positive electrode active material and the second positive electrode active material, a peak of NiO is observed in the X-ray diffraction pattern. It should be noted that in the X-ray diffraction measurement using CuKα radiation, a peak of NiO is observed around 2θ = 43.0°. Here, the mixture is composed of the first positive electrode active material and the second positive electrode active material, and is not composed of a substance obtained by mixing these positive electrode active materials with NiO powder. Therefore, the peak of NiO observed by the X-ray diffraction measurement of the mixture is a peak of NiO formed in the crystal structure of at least any one of the first positive electrode active material and the second positive electrode active material. It should be noted that in view of the manufacturing method of the mixture of the first positive electrode active material and the second positive electrode active material described below, it is speculated that NiO is mainly formed in the crystal structure of the first positive electrode active material.

[0035] In the mixture where a NiO peak is observed by X-ray diffraction measurement, since NiO is incorporated into the crystal structure, Ni exists in the crystal 2+ , and therefore it is speculated that when Li detaches from the positive electrode active material constituting the mixture, Ni 2+The valence of changes, thereby performing charge compensation. Based on this point, when the battery is charged, the release of O from the positive electrode active material can be prevented, so it can be considered that the instability of the crystal structure of the positive electrode active material is suppressed, thereby suppressing the reduction in the charge and discharge cycle characteristics of the battery. In addition, since the ratio (A1, B1) of the molar number of Ni relative to the total molar number of metal elements excluding Li is high, the first positive electrode active material and the second positive electrode active material constituting the mixture can achieve a high capacity of the battery. Therefore, by using a mixture of the first positive electrode active material and the second positive electrode active material of this embodiment as the positive electrode active material, it is possible to achieve a balance between a high capacity of the battery and suppression of a reduction in the charge and discharge cycle characteristics.

[0036] The measurement conditions of X-ray diffraction are as follows.

[0037] Radiation source: Cu Kα1 (wavelength )

[0038] Detector: PSD (LYNX EYE)

[0039] X-ray output power: 40kV×40mA

[0040] Goniometer radius: 250mm

[0041] Operating axis: 2θ / θ

[0042] Measurement method: Continuous

[0043] Counting unit: CPS

[0044] Scanning speed: 0.03° / sec

[0045] Start angle: 10°, End angle: 100°

[0046] The mass ratio of NiO contained in the mixture is preferably in the range of 0-4% or more and 0.8% or less. When the mass ratio of NiO is within the above range, the reduction of the charge-discharge cycle characteristics can be further suppressed compared with the case outside the above range. The mass ratio of NiO contained in the mixture can be calculated based on the peak intensity (cts) and half-value width (deg) of the (104) surface of the mixture and the (200) surface of NiO obtained by X-ray diffraction measurement of the mixture according to the following formula.

[0047] Mass ratio of NiO (%) = (Peak intensity of NiO × Half value width of NiO) / (Peak intensity of mixture × Half value width of mixture) × 100

[0048] The content of the second positive electrode active material is preferably 1% by mass or more and 10% by mass or less relative to the mass of the first positive electrode active material, and more preferably 2% by mass or more and 5% by mass or less. If the content of the second positive electrode active material is within the range of 1% by mass or more and 10% by mass or less, compared with the case where it is greater than 10% by mass, there is a situation where the reduction in charge and discharge cycle characteristics can be further suppressed. It should be noted that the content of the mixture of the first positive electrode active material and the second positive electrode active material contained in the positive electrode mixture layer is preferably 80% by mass or more relative to the total mass of the positive electrode mixture layer, and more preferably 90% by mass or more.

[0049] The average particle size of the first positive electrode active material and the second positive electrode active material is, for example, 1 μm to 30 μm. The average particle size is a volume average particle size measured by laser diffraction, which means a median particle size at which the volume cumulative value in the particle size distribution reaches 50%.

[0050] An example of a method for producing the first positive electrode active material and the second positive electrode active material will be described.

[0051] Prepare a first precursor oxide for obtaining a first positive electrode active material and a second precursor oxide for obtaining a second positive electrode active material. The first precursor oxide is an oxide in which the ratio of the molar number of Ni relative to the total molar number of metal elements in the oxide is 80% or more, and the ratio of the molar number of Mn relative to the total molar number of metal elements in the oxide is 1% or less. The first precursor oxide may contain Co, Al, etc. as needed. In addition, the second precursor oxide is an oxide in which the ratio of the molar number of Ni relative to the total molar number of metal elements in the oxide is in the range of ±3% of the ratio of the molar number of Ni relative to the total molar number of metal elements in the first precursor oxide, and the ratio of the molar number of Mn relative to the total molar number of metal elements in the second precursor oxide is 3% or more. The second precursor oxide may contain Al, etc. as needed. These precursor oxides can be manufactured by a known method, for example, by calcining a composite hydroxide containing Ni obtained by a coprecipitation method at a specified temperature and time.

[0052] Thereafter, the first precursor oxide, the second precursor oxide, and a Li source such as lithium hydroxide and lithium carbonate are mixed, and the mixture is calcined in an oxygen atmosphere. As mentioned above, if the second positive electrode active material becomes more, the charge and discharge cycle characteristics of the battery will be affected, so the mixing amount of the second precursor oxide is preferably 1% by mass or more and 10% by mass or less relative to the mass of the first precursor oxide, and more preferably 2% by mass or more and 5% by mass or less. The calcination temperature of the mixture can be, for example, in the range of 600°C to 800°C. The calcination time of the mixture can be, for example, in the range of 1 hour to 24 hours.

[0053] By using this method, a mixture of the present embodiment can be obtained. The mechanism of forming NiO in the mixture is not fully understood, but it can be inferred to be the following mechanism. Usually, Li is added in excess relative to the metal amount of the precursor oxide in consideration of the generation of lithium side reactions, etc. Therefore, from the viewpoint of charge compensation, the Ni valence of the first positive electrode active material is greater than 3 valences, and a portion of the Ni in the second positive electrode active material exists in a 2-valent form due to the presence of 4-valent Mn. However, during calcination, since the first positive electrode active material and the second positive electrode active material respectively make the Ni valence close to the stable 3 valences, Li and O are pulled out of the first positive electrode active material and move to the adjacent second positive electrode active material. Since the structure of the first positive electrode active material lacking Li and O becomes unstable, a NiO phase is generated. The formation of this NiO is a specific reaction that may occur only when the first precursor oxide, the second precursor oxide, and the Li source having the same Ni ratio (within the range of ±3%) are calcined together. It should be noted that, although the NiO phase is mainly formed in the first positive electrode active material according to the mechanism presumed as described above, it is also considered that reactions other than the above mechanism occur and the NiO phase may also be formed in the second positive electrode active material.

[0054] As the conductive material contained in the positive electrode mixture layer, carbon materials such as carbon black, acetylene black, Ketjen black, and graphite can be exemplified. They can be used alone or in combination of two or more. The content of the conductive material in the positive electrode mixture layer is preferably, for example, 0.5% by mass or more and 4% by mass or less, more preferably 0.5% by mass or more and 1.5% by mass or less.

[0055] As the binding material contained in the positive electrode mixture layer, fluororesins such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide resins, acrylic resins, polyolefin resins, styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC) or its salt, polyacrylic acid (PAA) or its salt (PAA-Na, PAA-K, etc., can also be partially neutralized salts), polyethylene oxide (PEO), polyvinyl alcohol (PVA), etc. can be cited. They can be used alone or in combination with more than two kinds. The content of the binding material in the positive electrode mixture layer is, for example, preferably 0.5% by mass or more and 4% by mass or less, more preferably 0.5% by mass or more and 1.5% by mass or less.

[0056] [negative electrode]

[0057] The negative electrode 12 includes, for example, a negative electrode current collector and a negative electrode mixture layer formed on the current collector. The negative electrode current collector may be a foil of a metal such as copper that is stable within the potential range of the negative electrode, or a film having the metal disposed on the surface. The negative electrode mixture layer includes, for example, a negative electrode active material and a binding material. For example, a negative electrode mixture slurry including a negative electrode active material, a binding material, etc. is prepared, the negative electrode mixture slurry is applied to the negative electrode current collector, and after the coating is dried, the coating is rolled, thereby making the negative electrode.

[0058] Negative electrode active material is not particularly limited as long as it can occlude and release lithium ions, for example, lithium alloys such as metallic lithium, lithium-aluminum alloy, lithium-lead alloy, lithium-silicon alloy, lithium-tin alloy, carbon materials such as graphite, coke, organic matter calcined bodies, SnO2, SnO, TiO2 and other metal oxides etc. can be cited. They can be single 1 kind, and can also be used in combination of two or more kinds.

[0059] As the binder contained in the negative electrode mixture layer, fluorine resin, PAN, polyimide resin, acrylic resin, polyolefin resin, SBR, CMC or its salt, PAA or its salt, PEO, PVA, etc. can be cited as in the case of the positive electrode. It should be noted that the negative electrode mixture layer can contain a conductive material as in the case of the positive electrode.

[0060] [Spacer]

[0061] For example, a porous sheet having ion permeability and insulation can be used as the spacer 13. Specific examples of the porous sheet include microporous films, woven fabrics, nonwoven fabrics, etc. The spacer 13 is made of, for example, polyolefins such as polyethylene and polypropylene, cellulose, etc. The spacer 13 can also be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as polyolefin. In addition, the spacer 13 can be a multilayer spacer including a polyethylene layer and a polypropylene layer, and can also have a surface layer including an aromatic polyamide resin or a surface layer including an inorganic filler.

[0062] Example

[0063] Hereinafter, the present invention will be further described using examples; however, the present invention is not limited to these examples.

[0064] <Example 1>

[0065] [Synthesis of positive electrode active material]

[0066] As the first precursor oxide, Ni 0.90 Co 0.05 Al 0.05 O2 represented composite oxide, Ni as the second precursor oxide 0.90 Al 0.05 Mn 0.05The composite oxide represented by O2 and lithium hydroxide are mixed so that the molar ratio is 1:0.05:1.05. The mixture is calcined at 720°C for 20 hours under an oxygen gas flow to obtain a mixture of a composite oxide containing lithium derived from the first precursor oxide (the first positive electrode active material) and a composite oxide containing lithium derived from the second precursor oxide (the second positive electrode active material).

[0067] The obtained mixture was subjected to X-ray diffraction measurement, and as a result, a peak of NiO as a divalent oxide was observed. In addition, the mass ratio of NiO in the mixture was calculated based on the peak intensity and half-value width of the (104) surface of the mixture and the (200) surface of NiO obtained by X-ray diffraction measurement, and the result was 0.58%.

[0068] [Production of positive electrode]

[0069] The above mixture, acetylene black and polyvinylidene fluoride were mixed at a mass ratio of 100:1:1, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added to prepare a positive electrode mixture slurry. The slurry was coated on both sides of a positive electrode collector made of aluminum foil, and after the coating was dried, it was rolled using a calendering roller, thereby obtaining a positive electrode having a positive electrode mixture layer formed on both sides of the positive electrode collector.

[0070] [Production of negative electrode]

[0071] Artificial graphite, CMC and SBR were mixed at a mass ratio of 100:1:1, and an appropriate amount of water was added to prepare a negative electrode mixture slurry. The slurry was applied to both sides of a negative electrode collector made of copper foil, and after the coating was dried, it was rolled using a rolling roller to obtain a negative electrode having a negative electrode mixture layer formed on both sides of the negative electrode collector.

[0072] [Preparation of non-aqueous electrolyte]

[0073] In a mixed solvent of ethylene carbonate (EC), ethyl methyl carbonate (MEC), and dimethyl carbonate in a volume ratio of 3:3:4, LiPF6 was dissolved at a concentration of 1.2 mol / L, thereby obtaining a non-aqueous electrolyte.

[0074] [Fabrication of non-aqueous electrolyte secondary battery]

[0075] The positive electrode lead is installed on the positive electrode produced above, and the negative electrode lead is installed on the negative electrode produced above. A spacer is arranged between the two poles and wound in a spiral shape, thereby producing a wound electrode body. The electrode body is inserted into the shell body, the lead on the negative electrode side is welded to the bottom of the shell body, and the lead on the positive electrode side is welded to the sealing body. After injecting a non-aqueous electrolyte into the shell body, the open end of the shell body is riveted to the sealing body through a gasket. It is set as a non-aqueous electrolyte secondary battery.

[0076] <Example 2>

[0077] In addition to using Ni as the first precursor oxide 0.90 Co 0.05 Al 0.05 O2 represented composite oxide, Ni as the second precursor oxide 0.90 Al 0.05 Mn 0.05 A mixture was prepared in the same manner as in Example 1 except that the composite oxide represented by O2 and lithium hydroxide were mixed so as to have a molar ratio of 1:0.02:1.02. A nonaqueous electrolyte secondary battery was prepared in the same manner as in Example 1 using the mixture.

[0078] The mixture obtained in Example 2 was subjected to X-ray diffraction measurement. As a result, a peak of NiO was observed, and the mass ratio of NiO in the mixture was 0.51%.

[0079] <Example 3>

[0080] In addition to using Ni 0.90 Mn 0.10 A mixture was prepared in the same manner as in Example 1 except that the composite oxide represented by O2 was used as the second precursor oxide. A nonaqueous electrolyte secondary battery was prepared in the same manner as in Example 1 using the mixture.

[0081] The mixture obtained in Example 3 was subjected to X-ray diffraction measurement. As a result, a peak of NiO was observed, and the mass ratio of NiO in the mixture was 0.61%.

[0082] <Example 4>

[0083] In addition to using Ni 0.88 Al 0.04 Mn 0.04 A mixture was prepared in the same manner as in Example 1 except that the composite oxide represented by O2 was used as the second precursor oxide. A nonaqueous electrolyte secondary battery was prepared in the same manner as in Example 1 using the mixture.

[0084] The mixture obtained in Example 4 was subjected to X-ray diffraction measurement. As a result, a peak of NiO was observed, and the mass ratio of NiO in the mixture was 0.57%.

[0085] <Example 5>

[0086] In addition to using Ni 0.92 Al 0.03 Mn 0.03A mixture was prepared in the same manner as in Example 1 except that the composite oxide represented by O2 was used as the second precursor oxide. A nonaqueous electrolyte secondary battery was prepared in the same manner as in Example 1 using the mixture.

[0087] The mixture obtained in Example 5 was subjected to X-ray diffraction measurement. As a result, a peak of NiO was observed, and the mass ratio of NiO in the mixture was 0.58%.

[0088] <Comparative Example 1>

[0089] A mixture was prepared in the same manner as in Example 1 except that the second precursor oxide was not used. A nonaqueous electrolyte secondary battery was prepared in the same manner as in Example 1 using the mixture.

[0090] The mixture obtained in Comparative Example 1 was subjected to X-ray diffraction measurement. As a result, no peak of NiO was observed.

[0091] <Comparative Example 2>

[0092] In addition to using Ni 0.82 Al 0.08 Mn 0.10 A mixture was prepared in the same manner as in Example 1 except that the composite oxide represented by O2 was used as the second precursor oxide. A nonaqueous electrolyte secondary battery was prepared in the same manner as in Example 1 using the mixture.

[0093] The mixture obtained in Comparative Example 2 was subjected to X-ray diffraction measurement. As a result, no NiO peak was observed.

[0094] <Comparative Example 3>

[0095] In addition to using Ni 0.95 Al 0.02 Mn 0.03 A mixture was prepared in the same manner as in Example 1 except that the composite oxide represented by O2 was used as the second precursor oxide. A nonaqueous electrolyte secondary battery was prepared in the same manner as in Example 1 using the mixture.

[0096] The mixture obtained in Comparative Example 3 was subjected to X-ray diffraction measurement. As a result, no peak of NiO was observed.

[0097] [Charge and discharge test]

[0098] The non-aqueous electrolyte secondary battery of each embodiment and each comparative example was charged at a constant current of 0.2C under a temperature environment of 25°C until the battery voltage reached 4.2V, and then charged at a constant voltage of 4.2V until the current value reached 0.02C. Thereafter, constant current discharge was performed at a constant current of 0.2C until the battery voltage reached 2.5V. The discharge capacity at this time was set as the initial discharge capacity. Thereafter, 500 cycles of the above-mentioned charge and discharge cycles were performed, and the capacity retention rate was calculated using the following formula.

[0099] Capacity retention rate (%) = (discharge capacity at the 500th cycle / initial discharge capacity) × 100

[0100] The results of the initial discharge capacity and the capacity retention rate in each example and each comparative example are summarized in Table 1. These results are expressed as relative values ​​with the result of Comparative Example 1 as a reference (100).

[0101] [Table 1]

[0102]

[0103] Compared with Comparative Example 1, Examples 1 to 5 have the same or higher initial discharge capacity and higher capacity retention rates. Therefore, by using the following mixture as the positive electrode active material, a high discharge capacity can be exhibited as in Comparative Example 1, and a decrease in charge and discharge cycle characteristics can be suppressed compared with Comparative Example 1. The mixture is a mixture of a first positive electrode active material and a second positive electrode active material, wherein the ratio (A1) of the molar number of Ni relative to the total molar number of metal elements excluding Li is 80% or more, and the ratio (A2) of the molar number of Mn relative to the total molar number of metal elements excluding Li is 1% or less, and the ratio (B1) of the molar number of Ni relative to the total molar number of metal elements excluding Li in the second positive electrode active material is in the range of ±3% of the ratio (A1), and the ratio (B2) of the molar number of Mn relative to the total molar number of metal elements excluding Li is 3% or more, and in the X-ray diffraction measurement, a peak of NiO can be observed.

[0104] In addition, in the embodiment, a mixture of the first positive electrode active material and the second positive electrode active material is used as the positive electrode active material, the first positive electrode active material uses Co, and the second positive electrode active material suppresses the use of Co. That is, by using a positive electrode active material that suppresses the use of Co, the use of a positive electrode active material using Co can be reduced, so it is also better than Comparative Example 1 in terms of material cost.

[0105] Description of Reference Numerals

[0106] 10 secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 15 battery case, 16 case body, 17 sealing body, 18, 19 insulating plates, 20 positive electrode lead, 21 negative electrode lead, 22 protrusion, 23 filter, 24 lower valve body, 25 insulating member, 26 upper valve body, 27 cap, 28 gasket.

Claims

1. A positive electrode active material for a non-aqueous electrolyte secondary battery, It has a mixture of a first positive electrode active material and a second positive electrode active material, The first positive electrode active material is a lithium composite oxide containing Ni, wherein a ratio A1 of the number of moles of Ni relative to the total number of moles of metal elements excluding Li is 80% or more, and a ratio A2 of the number of moles of Mn relative to the total number of moles of metal elements excluding Li is 1% or less, The second positive electrode active material is a lithium composite oxide containing Ni, a ratio B1 of the molar number of Ni relative to the total molar number of metal elements excluding Li is within the range of ±3% of the ratio A1, and a ratio B2 of the molar number of Mn relative to the total molar number of metal elements excluding Li is 3% or more, In the X-ray diffraction measurement of the mixture, a peak of NiO was observed.

2. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein In the first positive electrode active material, a ratio A3 of the number of moles of Co relative to the total number of moles of metal elements excluding Li is greater than 1%. In the second positive electrode active material, a ratio B3 of the number of moles of Co to the total number of moles of metal elements excluding Li is 1% or less.

3. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein The content of the second positive electrode active material is in a range of 1 mass % to 10 mass % based on the mass of the first positive electrode active material.

4. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 3, wherein The content of the second positive electrode active material is in a range of 2 mass % or more and 5 mass % or less relative to the mass of the first positive electrode active material.

5. A non-aqueous electrolyte secondary battery, It includes a positive electrode, a negative electrode and a non-aqueous electrolyte. The positive electrode comprises the positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 4.