Nonaqueous electrolyte secondary battery
By using specific non-aggregated particles and secondary particles in a nonaqueous electrolyte secondary battery and adjusting the electrolyte composition, the problem that batteries in the prior art are difficult to take into account both high capacity and cycle characteristics, and high capacity and excellent Storage and cycle characteristics battery performance.
Patent Information
- Application Number
- CN202380027046.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-23
- Filing Date
- 2023-03-03
- Publication Date
- 2024-11-26
AI Technical Summary
The existing non-aqueous electrolyte secondary batteries are difficult to take into account high capacity, storage characteristics and cycle characteristics during power storage purposes. Especially when non-condensed particles are used as the positive electrode active substance, the reduction in filling properties leads to a decrease in battery capacity, and it is difficult for the mixture to take into account high capacity. and good cycle characteristics.
Use specific non-aggregated particles and secondary particles as the positive electrode active substances, and increase the content of non-aggregated particles in the positive electrode mixture layer, adjust the ratio of cyclic carbonate to chain carbonate in the non-aqueous electrolyte to ensure the electrolyte flow path and permeability to improve circulation and storage characteristics.
It achieves high capacity, excellent storage characteristics and cycle characteristics, improves the overall performance of the battery, ensures the high filling density and good cycle stability of the battery.
Smart Images

Figure CN119032446A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a nonaqueous electrolyte secondary battery. Background Art
[0002] In recent years, with the popularity of non-aqueous electrolyte secondary batteries in vehicle-mounted applications and power storage applications, non-aqueous electrolyte secondary batteries with high capacity and excellent cycle characteristics are required. Because the positive electrode has a great influence on the battery characteristics including battery capacity and cycle characteristics, a lot of research has been done on the positive electrode. For example, Patent Document 1 discloses a non-aqueous electrolyte secondary battery, which uses single crystal particles as non-agglomerated particles and / or secondary particles formed by agglomeration of multiple primary particles as positive electrode active materials. Patent Document 1 describes the effect of improving the cycle characteristics of the battery.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2020-53386 Summary of the invention
[0006] However, in power storage applications, in addition to cycle characteristics, high capacity and storage characteristics are also required. Patent document 1 does not study storage characteristics. In addition, the research results of the inventors show that when non-agglomerated particles are used as positive electrode active materials, although the cycle characteristics are improved, the battery capacity is reduced due to the reduced filling property of the positive electrode active material. It is also found that even when a mixture of non-agglomerated particles and secondary particles is used, it may not be possible to take into account both high capacity and good cycle characteristics. The invention described in patent document 1 has not studied batteries with high capacity, improved storage characteristics and cycle characteristics, and there is still room for improvement.
[0007] An object of the present invention is to provide a nonaqueous electrolyte secondary battery having a high capacity and excellent storage characteristics and cycle characteristics.
[0008] A non-aqueous electrolyte secondary battery in one embodiment of the present invention is characterized in that it comprises a positive electrode, a negative electrode, and a non-aqueous electrolyte, wherein the non-aqueous electrolyte contains a cyclic carbonate and a chain carbonate in a volume ratio of 3:7 to 6:4, and the positive electrode has a positive electrode core material and a positive electrode mixture layer formed on the surface of the positive electrode core material, the positive electrode mixture layer comprising: first lithium metal composite oxide particles, which are non-agglomerated particles with a volume-based median diameter of 2 to 10 μm; second lithium metal composite oxide particles, which are aggregated from primary particles with an average particle diameter of 50 nm to 2 μm, and are secondary particles with a volume-based median diameter of 10 to 30 μm, and when the positive electrode mixture layer is divided into two equal parts in the thickness direction and defined as a first region and a second region in sequence from the surface side of the positive electrode, the content of the first lithium metal composite oxide particles in the positive electrode mixture layer is more in the first region than in the second region.
[0009] According to one embodiment of the present invention, a nonaqueous electrolyte secondary battery having a high capacity and excellent storage characteristics and cycle characteristics can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 It is a cross-sectional view of a nonaqueous electrolyte secondary battery as an example of the embodiment.
[0011] Figure 2 It is a cross-sectional view of a positive electrode as an example of an embodiment. DETAILED DESCRIPTION
[0012] As mentioned above, it is an important issue to obtain a non-aqueous electrolyte secondary battery with high capacity, excellent storage characteristics and cycle characteristics. The inventors have made a intensive study to solve this problem and found that by using specific non-agglomerated particles and specific secondary particles as positive electrode active materials, increasing the content (mass) of non-agglomerated particles on the surface side relative to the core material side of the positive electrode mixture layer, and making the ratio of cyclic carbonate to chain carbonate in the non-aqueous electrolyte within a specific range, a non-aqueous electrolyte secondary battery that solves the above-mentioned problems can be obtained.
[0013] In a non-aqueous electrolyte, by increasing the ratio of cyclic carbonate to chain carbonate, the decomposition of the non-aqueous electrolyte during charge and discharge is suppressed, and the storage characteristics are improved. However, if the ratio of cyclic carbonate increases, the viscosity of the non-aqueous electrolyte increases, which hinders the penetration of the non-aqueous electrolyte in the positive electrode mixture layer, and the cycle characteristics are easily reduced. Here, by making the content of non-agglomerated particles in the positive electrode mixture layer satisfy the first area on the surface side of the positive electrode mixture layer>the second area on the core material side, the flow path of the non-aqueous electrolyte can be ensured, and the cycle characteristics can be improved. High capacity can also be achieved by using specific non-agglomerated particles and specific secondary particles. Although the filling property of the positive electrode active material is reduced by using non-agglomerated particles, by using secondary particles in combination, particle cracking occurs in the compression process of the positive electrode, and the filling density of the active material becomes higher.
[0014] Hereinafter, an example of an embodiment of a positive electrode for a nonaqueous electrolyte secondary battery and a nonaqueous electrolyte secondary battery using the positive electrode of the present invention will be described in detail with reference to the drawings. It is assumed from the outset that a plurality of embodiments and modifications described below may be selectively combined.
[0015] Hereinafter, a cylindrical battery in which a wound electrode body 14 is contained in an outer can 16 having a bottomed cylindrical shape is exemplified, but the outer body of the battery is not limited to a cylindrical outer can, and may be, for example, a rectangular outer can (rectangular battery) or a coin-shaped outer can (coin-shaped battery), or an outer body composed of a laminate including a metal layer and a resin layer (laminated battery). In addition, the electrode body may also be a laminated electrode body in which a plurality of positive electrodes and a plurality of negative electrodes are alternately laminated via a separator.
[0016] Figure 1 FIG. 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery 10 as an example of an embodiment. Figure 1 As shown, the non-aqueous electrolyte secondary battery 10 comprises: a wound electrode body 14; a non-aqueous electrolyte; and an outer can 16 for containing the electrode body 14 and the non-aqueous electrolyte. The electrode body 14 comprises a positive electrode 11, a negative electrode 12, and a separator 13, and has a wound structure in which the positive electrode 11 and the negative electrode 12 are wound in a spiral shape with the separator 13 interposed therebetween. The outer can 16 is a metal container in the shape of a bottomed cylindrical body with an opening on one side in the axial direction, and the opening of the outer can 16 is sealed by a sealing body 17. For the sake of convenience in the following description, the sealing body 17 side of the battery is taken as the upper side, and the bottom side of the outer can 16 is taken as the lower side.
[0017] The positive electrode 11, the negative electrode 12 and the separator 13 constituting the electrode body 14 are all strip-shaped long bodies, which are alternately stacked in the radial direction of the electrode body 14 by being wound into a spiral shape. In order to prevent the precipitation of lithium, the negative electrode 12 is formed to be one circle larger than the positive electrode 11. That is, the negative electrode 12 is formed longer in the longitudinal direction and the width direction (lateral width direction) than the positive electrode 11. The two separators 13 are formed to be at least one circle larger than the positive electrode 11, for example, arranged in a manner of sandwiching the positive electrode 11. The electrode body 14 includes: a positive electrode lead 20 connected to the positive electrode 11 by welding or the like; and a negative electrode lead 21 connected to the negative electrode 12 by welding or the like.
[0018] Insulating plates 18 and 19 are disposed above and below the electrode body 14, respectively. Figure 1 In the example shown, the positive electrode lead 20 extends to the sealing body 17 side through the through hole of the insulating plate 18, and the negative electrode lead 21 extends to the bottom side of the outer can 16 through the outside of the insulating plate 19. The positive electrode lead 20 is connected to the lower surface of the internal terminal plate 23 of the sealing body 17 by welding or the like, and the top plate of the sealing body 17, that is, the cap 27 electrically connected to the internal terminal plate 23, serves as the positive terminal. The negative electrode lead 21 is connected to the inner surface of the bottom of the outer can 16 by welding or the like, and the outer can 16 serves as the negative terminal.
[0019] A gasket 28 is provided between the outer can 16 and the sealing body 17 to ensure the airtightness inside the battery. A groove portion 22 is formed in the outer can 16, with a part of the side portion bulging inward to support the sealing body 17. Preferably, the groove portion 22 is formed in an annular shape along the circumference of the outer can 16, and the sealing body 17 is supported by its upper surface. The sealing body 17 is fixed to the upper part of the outer can 16 through the groove portion 22 and the open end of the outer can 16 riveted to the sealing body 17.
[0020] The sealing body 17 has a structure in which an internal terminal plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26 and a cap 27 are stacked in order from the electrode body 14 side. The components constituting the sealing body 17 have, for example, a disc shape or a ring shape, and the components except the insulating member 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected at their respective central portions, and the insulating member 25 is interposed between their respective peripheral portions. If the internal pressure of the battery rises due to abnormal heat release, the lower valve body 24 is deformed and broken in a manner that pushes the upper valve body 26 to the side of the cap 27, thereby cutting off the current path between the lower valve body 24 and the upper valve body 26. In addition, if the internal pressure rises, the upper valve body 26 breaks, and the gas is discharged from the opening of the cap 27.
[0021] Hereinafter, the positive electrode 11 , the negative electrode 12 , the separator 13 , and the non-aqueous electrolyte, particularly the positive electrode 11 and the non-aqueous electrolyte, will be described in detail.
[0022] [positive electrode]
[0023] The positive electrode 11 includes a positive electrode core material 30 and a positive electrode mixture layer 31 formed on the surface of the positive electrode core material 30. For the positive electrode core material 30, a foil of a metal such as aluminum or aluminum alloy that is stable in the potential range of the positive electrode 11, a thin film of the metal disposed on the surface layer, etc. can be used. An example of the positive electrode core material 30 is a foil of aluminum or aluminum alloy with a thickness of 10 to 20 μm. The positive electrode mixture layer 31 includes a positive electrode active material, a conductive agent, and a binder, and is preferably formed on both sides of the positive electrode core material 30. The thickness of the positive electrode mixture layer 31 is, for example, 30 to 100 μm on one side of the positive electrode core material 30. The positive electrode 11 can be manufactured, for example, by coating a positive electrode mixture slurry containing a positive electrode active material, a conductive agent, and a binder on the positive electrode core material 30, drying the coating, and then compressing the positive electrode mixture layer 31 to form the positive electrode mixture layer 31 on both sides of the positive electrode core material 30.
[0024] Examples of the conductive agent contained in the positive electrode mixture layer 31 include carbon materials such as carbon black, acetylene black, Ketjen black, graphite, carbon nanotubes, carbon nanofibers, and graphene. The content of the conductive agent is, for example, 0.01 to 10 parts by mass, preferably 0.05 to 5 parts by mass, relative to 100 parts by mass of the positive electrode active material.
[0025] As the binder contained in the positive electrode mixture layer 31, fluorine-containing resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide, acrylic resin, polyolefin, etc. can be exemplified. In addition, these resins can also be used in combination with carboxymethyl cellulose (CMC) or its salt, polyethylene oxide (PEO), etc. The content of the binder is, for example, 0.1 to 10 parts by mass, preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of the positive electrode active material.
[0026] In the positive electrode mixture layer 31, as a positive electrode active material, a granular lithium metal composite oxide is included. The lithium metal composite oxide is a composite oxide containing metal elements such as Co, Mn, Ni, and Al in addition to Li. The metal elements constituting the lithium metal composite oxide are, for example, at least one selected from Mg, Al, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, Y, Zr, Sn, Sb, W, Pb, and Bi. Among them, it is preferred to contain at least one selected from Co, Ni, and Mn. As an example of a suitable composite oxide, a lithium metal composite oxide containing Ni, Co, and Mn and a lithium metal composite oxide containing Ni, Co, and Al can be listed.
[0027] The positive electrode mixture layer 31 contains two kinds of lithium metal composite oxide particles. In addition, when the positive electrode mixture layer 31 is divided into two equal parts in the thickness direction and defined as the first region 31a and the second region 31b in order from the surface side of the positive electrode 11, the materials contained in the first region 31a and the second region 31b are different from each other. In this embodiment, when the types of lithium metal composite oxide particles contained in the first region 31a and the second region 31b are different, and when each region contains two kinds of lithium metal composite oxide particles, their mass ratios are different. On the other hand, the types and contents of the conductive agent and the binder may be the same or different in the first region 31a and the second region 31b.
[0028] The positive electrode mixture layer 31 contains: first lithium metal composite oxide particles, which are non-agglomerated particles; and second lithium metal composite oxide particles, which are secondary particles formed by agglomeration of primary particles having an average particle size of 50 nm to 2 μm. The positive electrode mixture layer 31 may contain only the first and second lithium metal composite oxide particles as positive electrode active materials, or may contain third lithium metal composite oxide particles within a range that does not impair the purpose of the present invention. As an example of the third lithium metal composite oxide particles, composite oxide particles that do not satisfy the particle size conditions described below may be cited.
[0029] The volume-based median diameter (hereinafter sometimes referred to as "D50") of the first lithium metal composite oxide particles is 2 to 10 μm, preferably 3 to 8 μm. The D50 of the second lithium metal composite oxide particles is 10 to 30 μm, preferably 12 to 20 μm. D50 means the particle size at which the accumulation of frequencies from the smaller particle size reaches 50% in the volume-based particle size distribution. The particle size distribution of the lithium metal composite oxide particles is measured using a laser diffraction particle size distribution measuring device (e.g., MT3000II manufactured by MicrotracBEL Co., Ltd.) using water as the dispersion medium.
[0030] The first lithium metal composite oxide particles are particles without grain boundaries inside, for example, single crystal primary particles. The crystallinity of the lithium metal composite oxide particles can be confirmed using a scanning ion microscope. However, among the first lithium metal composite oxide particles synthesized by the production method described below, for example, there are cases where particles include 5 or less primary particles.
[0031] The second lithium metal composite oxide particles are secondary particles formed by agglomeration of primary particles having an average particle size of 50 nm to 2 μm, preferably 500 nm to 2 μm. There are grain boundaries of primary particles in the second lithium metal composite oxide particles. The primary particles can be confirmed by observing the second lithium metal composite oxide particles with a scanning electron microscope (SEM). In addition, even when the second lithium metal composite oxide particles are subjected to strong forces such as during pulverization after synthesis and during preparation of positive electrode mixture slurry, multiple primary particles are still bonded to each other with a strength that does not disperse.
[0032] The average particle size of the primary particles constituting the second lithium metal composite oxide particles is obtained by analyzing the SEM image of the particle cross section. For example, the positive electrode 11 is buried in a resin, a cross section is made by cross section polishing (CP), and the cross section is photographed by SEM. From the SEM image, 30 primary particles are randomly selected to observe the grain boundary, and the diameter of the circumscribed circle of each of the 30 primary particles is obtained, and the average value thereof is taken as the average particle size.
[0033] Each lithium metal composite oxide particle can be synthesized by the method described in the examples described below. The first lithium metal composite oxide particle can be synthesized by, for example, increasing the pH of the alkaline aqueous solution used when synthesizing a precursor (metal composite hydroxide) containing Ni, Co, Mn, Al, etc., and / or increasing the calcination temperature of the precursor, compared to the case of synthesizing the second lithium metal composite oxide particle. An example of a preferred pH of the alkaline aqueous solution is 10 to 11, and an example of a preferred calcination temperature is 950 to 1100°C. When synthesizing the second lithium metal composite oxide particle, for example, an alkaline aqueous solution with a pH of 9 to 10 is used, and the calcination temperature is below 950°C.
[0034] Each lithium metal composite oxide particle is composed of, for example, a lithium metal composite oxide having a hexagonal crystal structure belonging to the space group R-3m, preferably LiNi x Co y Mn z O2 (0.3<x<0.6, x+y+z=1), or LiNi x Co y Al z O2 (0.8<x<0.95, x+y+z=1) is the main component. Here, the so-called main component means the component with the largest mass among the components constituting the lithium metal composite oxide particles. In addition, the composition of each lithium metal composite oxide particle may be the same or different.
[0035] The positive electrode mixture layer 31 contains the first and second lithium metal composite oxide particles as described above, but the materials contained in the first region 31a and the second region 31b are different from each other. The content of the first lithium metal composite oxide particles in the positive electrode mixture layer 31 is not uniform, and is greater in the first region 31a than in the second region 31b.
[0036] The first lithium metal composite oxide particles are less likely to crack during the manufacturing process of the positive electrode 11 than the second lithium metal composite oxide particles, so a large amount of the first lithium metal composite oxide particles is present in the first region 31a, which is the surface side of the positive electrode mixture layer 31, thereby ensuring a flow path for the electrolyte in the first region 31a. In this case, it is considered that the permeability of the electrolyte to the second region 31b is good, and the cycle characteristics are improved.
[0037] In addition, it is preferred that the ratio of the mass of the first lithium metal composite oxide particles to the mass of the positive electrode active material in the first region 31a is higher than the ratio of the mass of the first lithium metal composite oxide particles to the mass of the positive electrode active material in the second region 31b. The content of the positive electrode active material may be different in the first region 31a and the second region 31b, but is preferably substantially the same. The content of the positive electrode active material is, for example, 90 to 99.9% by mass, preferably 95 to 99% by mass, relative to the mass of the positive electrode mixture layer 31.
[0038] The first region 31a may substantially contain only the first lithium metal composite oxide particles as the positive electrode active material. In addition, the first lithium metal composite oxide particles may, for example, be contained only in the first region 31a and not exist in the second region 31b. When the second lithium metal composite oxide particles exist in the first region 31a, the mass ratio of the composite oxide particles in the first region 31a is preferably the first lithium metal composite oxide particles> the second lithium metal composite oxide particles.
[0039] In addition, the content of the second lithium metal composite oxide particles is greater in the second region 31b than in the first region 31a. Preferably, the ratio of the mass of the second lithium metal composite oxide particles in the second region 31b to the mass of the positive electrode active material is higher than the ratio of the mass of the second lithium metal composite oxide particles in the first region 31a to the mass of the positive electrode active material.
[0040] The second lithium metal composite oxide particles can be filled more per unit volume than the first lithium metal composite oxide particles, so the use of the second lithium metal composite oxide particles can make the positive electrode mixture layer 31 high-density, which contributes to the high capacity of the battery. The second lithium metal composite oxide particles can be present in large quantities on the positive electrode core material 30 side, which has little effect on the permeability of the electrolyte, so that good cycle characteristics can be maintained while achieving high capacity.
[0041] The second region 31b may substantially contain only the second lithium metal composite oxide particles as the positive electrode active material. In addition, the second lithium metal composite oxide particles may, for example, be contained only in the second region 31b and not exist in the first region 31a. When the first lithium metal composite oxide particles exist in the second region 31b, the mass ratio of the composite oxide particles in the second region 31b is preferably such that the first lithium metal composite oxide particles are less than the second lithium metal composite oxide particles.
[0042] As described above, the first region 31a may contain first and second lithium metal composite oxide particles. In this case, the preferred mass ratio of the first lithium metal composite oxide particles to the second lithium metal composite oxide particles in the first region 31a is 60:40 to 90:10, and more preferably 65:35 to 80:20. If the mass ratio of each composite oxide particle is within this range, high capacity and excellent cycle characteristics can be easily achieved.
[0043] In the second region 31b, the content of the first and second lithium metal composite oxide particles can also be made the same, but it is preferred that the first lithium metal composite oxide particles are less than the second lithium metal composite oxide particles, or only the second lithium metal composite oxide particles are used as the positive electrode active material. When the second region 31b contains the first lithium metal composite oxide particles, the mass ratio of the first lithium metal composite oxide particles to the second lithium metal composite oxide particles in the second region 31b is 10:90 to 40:60, and more preferably 20:80 to 35:65. If the mass ratio of each composite oxide particle is within this range, it is easy to achieve both high capacity and excellent cycle characteristics.
[0044] [negative electrode]
[0045] The negative electrode 12 includes a negative electrode core material and a negative electrode mixture layer formed on the surface of the negative electrode core material. The negative electrode core material can be made of a foil of a metal such as copper or copper alloy that is stable in the potential range of the negative electrode 12, or a thin film of the metal arranged on the surface. An example of a negative electrode core material is a foil of copper or copper alloy having a thickness of 5 to 15 μm. The negative electrode mixture layer includes a negative electrode active material and a binder, and is preferably formed on both sides of the negative electrode core material. The thickness of the negative electrode mixture layer is, for example, 30 to 100 μm on one side of the negative electrode core material. The negative electrode 12 can be manufactured by coating a negative electrode mixture slurry containing a negative electrode active material, a binder, etc. on the negative electrode core material, and after drying the coating, compressing it to form the negative electrode mixture layer on both sides of the negative electrode core material.
[0046] In the negative electrode mixture layer, as the negative electrode active material, a carbon-based active material that reversibly occludes and releases lithium ions is included. Preferred carbon-based active materials are natural graphites such as flaky graphite, blocky graphite, and earthy graphite, and graphites such as artificial graphites such as blocky artificial graphite (MAG) and graphitized mesophase carbon microbeads (MCMB). In addition, in the negative electrode active material, a Si-based active material composed of at least one of Si and a Si-containing compound can also be used, and a carbon-based active material and a Si-based active material can also be used in combination.
[0047] The binder included in the negative electrode mixture layer can use fluororesins such as PTFE and PVdF, PAN, polyimide, acrylic resin, polyolefin, styrene-butadiene rubber (SBR), etc. In addition, the negative electrode mixture layer may also contain CMC or its salt, polyacrylic acid (PAA) or its salt, polyvinyl alcohol (PVA), etc. The content of the binder is, for example, 0.1 to 10 parts by mass, preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of the negative electrode active material. In addition, conductive agents such as carbon black, acetylene black, and Ketjen black may also be added to the negative electrode mixture layer.
[0048] [Spacer]
[0049] The spacer 13 may be a porous sheet having ion permeability and insulation. Specific examples of the porous sheet include microporous films, woven fabrics, nonwoven fabrics, etc. The material of the spacer is preferably polyolefins such as polyethylene and polypropylene, cellulose, etc. The spacer 13 may be a single-layer structure or a laminated structure. In addition, a resin layer with high heat resistance such as aramid resin may be formed on the surface of the spacer 13.
[0050] A filler layer containing an inorganic filler may also be formed at the interface between the separator 13 and at least one of the positive electrode 11 and the negative electrode 12. Examples of the inorganic filler include oxides of metals such as Ti, Al, Si, and Mg, and phosphate compounds. The filler layer can be formed by applying a slurry containing the filler on the surface of the positive electrode 11, the negative electrode 12, or the separator 13.
[0051] [Non-aqueous electrolyte]
[0052] The non-aqueous electrolyte contains a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. The non-aqueous solvent of the non-aqueous electrolyte contains cyclic carbonate and chain carbonate in a volume ratio of 3:7 to 6:4. In this way, it is possible to take into account both storage characteristics and cycle characteristics. Examples of cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate. Examples of chain carbonates include dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and isopropyl methyl carbonate.
[0053] The nonaqueous electrolyte solution can also contain the nonaqueous solvents beyond the cyclic carbonate and the linear carbonate. The total of the content of the cyclic carbonate and the linear carbonate in the nonaqueous solvent is preferably more than 80 volume %, more preferably more than 90 volumes with respect to the total volume of the nonaqueous solvent. The nonaqueous solvent can also only be composed of cyclic carbonate and the linear carbonate.
[0054] As the nonaqueous solvent beyond cyclic carbonate and chain carbonate, can enumerate the amides of nitrile, dimethylformamide etc. of esters, ethers, acetonitrile etc. beyond carbonate.Nonaqueous solvent can also contain the halogen substitution body that at least a portion of the hydrogen of these solvents is replaced with the halogen atom of fluorine etc.As the halogen substitution body, can enumerate the fluorinated chain carboxylic acid esters of fluorinated cyclic carbonate, fluorinated chain carbonate, methyl fluoropropionate (FMP) etc. etc.
[0055] Examples of esters other than carbonates include cyclic carboxylic acid esters such as γ-butyrolactone (GBL) and γ-pentylpropyl (GVL), and chain carboxylic acid esters such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate.
[0056] Ethers include cyclic ethers and chain ethers. Examples of cyclic ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, and crown ethers. Examples of the chain ethers include 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, methyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.
[0057] The electrolyte salt is preferably a lithium salt. Examples of lithium salts include LiBF4, LiClO4, LiPF6, LiAsF6, LiSbF6, LiAlCl4, LiSCN, LiCF3SO3, LiCF3CO2, Li(P(C2O4)F4), LiPF 6-x (C n F 2n+1 ) x (1<x<6, n is 1 or 2), LiB 10 Cl 10, LiCl, LiBr, LiI, lithium chloroborane, lithium lower aliphatic carboxylate, Li2B4O7, borate such as Li(B(C2O4)F2), LiN(SO2CF3)2, LiN(C1F 2l+1 SO2)(C m F 2m+1 SO2) {l, m is an integer greater than 0} and the like. The lithium salt may be used alone or in combination. Among them, LiPF6 is preferably used from the viewpoint of ionic conductivity, electrochemical stability, etc. The concentration of the lithium salt is, for example, 0.8 to 2.6 mol / L.
[0058] Example
[0059] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.
[0060] <Example 1>
[0061] [Synthesis of First Lithium Metal Composite Oxide Particles]
[0062] Nickel sulfate, cobalt sulfate, and manganese sulfate are mixed in a predetermined ratio and uniformly mixed in an alkaline aqueous solution with a pH of 10 to 11 to prepare a precursor. Next, the precursor is mixed with lithium carbonate, calcined at a temperature of 1000° C. for 15 hours, and then pulverized to obtain first lithium metal composite oxide particles as non-agglomerated particles. The composition and D50 of the particles are as follows.
[0063] Composition: LiNi 0.5 Co 0.2 Mn 0.3 O2
[0064] D50: 4.5μm
[0065] [Synthesis of Second Lithium Metal Composite Oxide Particles]
[0066] The pH of the alkaline aqueous solution was changed to 9-10, and the calcination temperature was changed to 900° C., and the second lithium metal composite oxide particles as secondary particles formed by agglomeration of primary particles were obtained in the same manner as the first lithium metal composite oxide particles. The composition of the particles, the average particle size of the primary particles, and the D50 of the secondary particles are as follows.
[0067] Composition: LiNi 0.5 Co 0.2 Mn 0.3 O2
[0068] Average particle size of primary particles: 1.6 μm
[0069] D50 of secondary particles (second lithium metal composite oxide particles): 14.1 μm
[0070] [Production of positive electrode]
[0071] The first lithium metal composite oxide particles, acetylene black (AB), and polyvinylidene fluoride (PVdF) were mixed in a mass ratio of 98:1:1, and N-methyl-2-pyrrolidone (NMP) was added as a dispersion medium in an appropriate amount to prepare a first positive electrode mixture slurry with a solid content concentration of 70% by mass. In addition, the second lithium metal composite oxide particles were used instead of the first lithium metal composite oxide particles, and the second positive electrode mixture slurry was prepared in the same manner as the first positive electrode mixture slurry. Then, the second positive electrode mixture slurry was applied on both sides of the positive electrode core material composed of aluminum foil, and then the first positive electrode mixture slurry was applied on the coating film of the second positive electrode mixture slurry, and the coating film was dried and compressed (linear pressure 3000N / m), and then cut into a specified electrode size to prepare a positive electrode with a positive electrode mixture layer formed on both sides of the positive electrode core material. The coating amount of the first positive electrode mixture slurry and the second positive electrode mixture slurry was the same value.
[0072] [Production of negative electrode]
[0073] As the negative electrode active material, 95 parts by mass of graphite powder and 5 parts by mass of SiO x A mixture of Si-containing compounds represented by . 100 parts by mass of negative electrode active material, 1 part by mass of sodium carboxymethyl cellulose (CMC-Na) and water are mixed, and 1.2 parts by mass of a dispersion of styrene-butadiene rubber (SBR) are further mixed to prepare a negative electrode mixture slurry. Next, the negative electrode mixture slurry is applied on both sides of a negative electrode core material composed of copper foil, and after drying and compressing the coating film, it is cut into a specified electrode size to produce a negative electrode having a negative electrode mixture layer formed on both sides of the negative electrode core material.
[0074] [Preparation of non-aqueous electrolyte]
[0075] A mixed solvent was prepared by mixing ethylene carbonate (EC) and dimethyl carbonate (DMC) at a volume ratio of 6:4 (25° C.). 5 parts by mass of vinylene carbonate (VC) was added to 100 parts by mass of the mixed solvent to dissolve LiPF6 to a concentration of 1 mol / L, thereby preparing a non-aqueous electrolyte.
[0076] [Battery production]
[0077] Lead terminals are installed on the positive electrode and the negative electrode respectively, and the positive electrode and the negative electrode are wound into a spiral shape through a spacer to produce a wound electrode body. The electrode body is housed in an outer can with a bottom cylindrical shape, and welded to the bottom inner surface of the outer can of the negative electrode lead, and the positive electrode lead is welded to the internal terminal plate of the sealing body. Thereafter, the non-aqueous electrolyte is injected into the outer can, and the opening edge of the outer can is riveted and fixed to the sealing body to produce a cylindrical secondary battery with a battery capacity of 2500mAh.
[0078] <Example 2>
[0079] In the preparation of the nonaqueous electrolyte solution, a positive electrode and a nonaqueous electrolyte secondary battery were prepared in the same manner as in Example 1 except that a mixed solvent was prepared by mixing EC:DMC at a volume ratio of 5:5 (25° C.).
[0080] <Example 3>
[0081] A positive electrode and a nonaqueous electrolyte secondary battery were prepared in the same manner as in Example 1 except that a mixed solvent was prepared by mixing EC:DMC at a volume ratio of 4:6 (25° C.).
[0082] <Example 4>
[0083] In the preparation of the nonaqueous electrolyte solution, a positive electrode and a nonaqueous electrolyte secondary battery were prepared in the same manner as in Example 1 except that a mixed solvent was prepared by mixing EC:DMC at a volume ratio of 3:7 (25° C.).
[0084] <Comparative Example 1>
[0085] In the production of the positive electrode, the first positive electrode mixture slurry is applied on both sides of the positive electrode core material, and the first positive electrode mixture slurry is again applied on the coating film of the first positive electrode mixture slurry. In the preparation of the non-aqueous electrolyte, EC:DMC is mixed in a volume ratio of 5:5 (25°C) to prepare a mixed solvent. Otherwise, the positive electrode and non-aqueous electrolyte secondary battery are produced in the same manner as in Example 1.
[0086] <Comparative Example 2>
[0087] In the production of the positive electrode, after the first positive electrode mixture slurry is applied on both sides of the positive electrode core material, the second positive electrode mixture slurry is applied on the coating film of the first positive electrode mixture slurry. In the preparation of the non-aqueous electrolyte, EC:DMC is mixed in a volume ratio of 5:5 (25°C) to prepare a mixed solvent. Otherwise, the positive electrode and non-aqueous electrolyte secondary battery are produced in the same manner as in Example 1.
[0088] <Comparative Example 3>
[0089] In the production of the positive electrode, the second positive electrode mixture slurry is applied on both sides of the positive electrode core material, and the second positive electrode mixture slurry is again applied on the coating film of the second positive electrode mixture slurry. In the preparation of the non-aqueous electrolyte, EC:DMC is mixed in a volume ratio of 5:5 (25°C) to prepare a mixed solvent. Otherwise, the positive electrode and non-aqueous electrolyte secondary battery are produced in the same manner as in Example 1.
[0090] <Comparative Example 4>
[0091] In the preparation of the nonaqueous electrolyte solution, a positive electrode and a nonaqueous electrolyte secondary battery were prepared in the same manner as in Example 1 except that a mixed solvent was prepared by mixing EC:DMC at a volume ratio of 2:8 (25° C.).
[0092] <Comparative Example 5>
[0093] In the preparation of the nonaqueous electrolyte solution, a positive electrode and a nonaqueous electrolyte secondary battery were prepared in the same manner as in Example 1 except that a mixed solvent was prepared by mixing EC:DMC at a volume ratio of 7:3 (25° C.).
[0094] The positive electrodes and batteries of Examples and Comparative Examples were evaluated by the following methods. The evaluation results are shown in Table 1.
[0095] [Positive electrode mixture layer density (packing density)]
[0096] The thickness and mass of the positive electrode were measured, and the density of the positive electrode mixture layer was calculated.
[0097] [Storage characteristics]
[0098] At a temperature of 25°C, the battery is charged at a constant current of 0.2It until the battery voltage reaches 4.2V. Then, the battery is charged at a constant voltage of 4.2V until the current reaches 0.05It. Next, the battery is discharged at a constant current of 0.2It until the battery voltage reaches 2.5V, and the initial discharge capacity is measured. Thereafter, the battery is charged at a constant current of 0.2It until the battery voltage reaches 4.2V, and then, the battery is charged at a constant voltage of 4.2V until the current reaches 0.05It. The battery in this state is left to stand at a temperature of 55°C for 60 days. Next, after cooling to 25°C, the battery is charged at a constant current of 0.2It at a temperature of 25°C until the battery voltage reaches 4.2V. Then, the battery is charged at a constant voltage of 4.2V until the current reaches 0.05It. Next, the battery is discharged at a constant current of 0.2It until the battery voltage reaches 2.5V, and the discharge capacity after storage is measured. The storage characteristics are calculated using the following formula. Also, It(A) = rated capacity (Ah) / 1(h).
[0099] Storage characteristics (%) = (discharge capacity after storage / initial discharge capacity) × 100
[0100] [Cycle characteristics (capacity retention rate)]
[0101] At a temperature of 45°C, the battery was charged at a constant current of 0.2 It until the battery voltage reached 4.2 V. The battery was then charged at a constant voltage of 4.2 V until the current reached 0.05 It. Thereafter, the battery was discharged at a constant current of 0.2 It until the battery voltage reached 2.5 V. This charge and discharge was performed for 300 cycles, and the capacity retention rate was calculated by the following formula.
[0102] Capacity retention rate (%) = (discharge capacity at the 300th cycle / discharge capacity at the 1st cycle) × 100
[0103] [Table 1]
[0104]
[0105] As shown in Table 1, the battery of the embodiment has excellent storage characteristics and cycle characteristics. In addition, the battery of the embodiment has a high filling density of the positive electrode active material, which can achieve a high capacity of the battery. On the other hand, the battery of the comparative example has at least one of the storage characteristics, capacity retention rate and filling density is low. Therefore, it can be seen that by using specific non-agglomerated particles and specific secondary particles as the positive electrode active material, and making the content of non-agglomerated particles more on the surface side than on the core material side of the positive electrode mixture layer, and making the ratio of cyclic carbonates and chain carbonates in the non-aqueous electrolyte within a specific range, a non-aqueous electrolyte secondary battery with high capacity and taking into account both storage characteristics and cycle characteristics can be obtained.
[0106] Also have, by improving the concentration of electrolyte salt, replace the ratio that improves cyclic carbonate with respect to linear carbonate, because the viscosity of nonaqueous electrolytic solution rises, so also can bring into play the same effect with present embodiment.For example, by making the concentration of electrolyte salt be 1.8~2.6 mol / L, no matter the mixing ratio of nonaqueous solvent, all can make the cycle characteristic of battery improve.
[0107] Explanation of symbols
[0108] 10 non-aqueous electrolyte secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 16 outer can, 17 sealing body, 18, 19 insulating plate, 20 positive electrode lead, 21 negative electrode lead, 22 groove portion, 23 internal terminal plate, 24 lower valve body, 25 insulating member, 26 upper valve body, 27 cap, 28 gasket, 30 positive electrode core material, 31 positive electrode mixture layer, 31a first region, 31b second region
Claims
1. A non-aqueous electrolyte secondary battery comprising a positive electrode, a negative electrode and a non-aqueous electrolyte solution, wherein: The non-aqueous electrolyte contains a cyclic carbonate and a chain carbonate as a non-aqueous solvent in a volume ratio of 3:7 to 6:
4. The positive electrode comprises a positive electrode core material and a positive electrode mixture layer formed on a surface of the positive electrode core material. The positive electrode mixture layer comprises: first lithium metal composite oxide particles, the first lithium metal composite oxide particles are non-agglomerated particles with a volume-based median diameter of 2 to 10 μm; second lithium metal composite oxide particles, the second lithium metal composite oxide particles are aggregated from primary particles with an average particle diameter of 50 nm to 2 μm, and secondary particles with a volume-based median diameter of 10 to 30 μm, When the positive electrode mixture layer is divided into two equal parts in the thickness direction and defined as a first region and a second region in order from the surface side of the positive electrode, the content of the first lithium metal composite oxide particles in the positive electrode mixture layer is greater in the first region than in the second region.
2. The nonaqueous electrolyte secondary battery according to claim 1, wherein The total content of the cyclic carbonate and the chain carbonate in the non-aqueous solvent is 80% by volume or more relative to the total volume of the non-aqueous solvent.