Monodisperse core-shell microspheres and preparation method thereof

By combining microfluidic technology with enzyme crosslinking methods to prepare monodisperse core-shell microspheres, the problems of complex preparation and low efficiency in existing technologies have been solved, and highly monodisperse core-shell microspheres with consistent performance have been achieved, which are suitable for a variety of application scenarios.

CN119034632AActive Publication Date: 2024-11-29ZHENGZHOU UNIV

Patent Information

Application Number
CN202411444565.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-11-29
Estimated Expiration
2044-10-16

AI Technical Summary

Technical Problem

Existing microfluidic techniques for preparing core-shell microspheres are complex, inefficient, and difficult to prepare monodisperse core-shell microspheres. Furthermore, during the encapsulation process, there is a tendency for unencapsulated or encapsulated cores to occur.

Method used

Monodisperse microspheres were formed by microfluidic technology using a dispersed phase liquid containing biodegradable polymers. Then, a hydrogel layer was coated on the surface of the microspheres through enzymatic crosslinking methods combining dopamine self-polymerization, electrostatic adsorption, and chemical grafting with horseradish peroxidase to form monodisperse core-shell microspheres.

Benefits of technology

This invention achieves highly monodisperse, consistent-performance core-shell microspheres, simplifies the operation process, improves preparation efficiency, and enhances the stability and application stability of the microspheres. These microspheres are suitable for applications such as drug delivery, cell adhesion and cell delivery, medical aesthetic filling, scaffold materials, and joint lubrication.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005087359330000011
    Figure HDA0005087359330000011
  • Figure HDA0005087359330000012
    Figure HDA0005087359330000012
  • Figure HDA0005087359330000021
    Figure HDA0005087359330000021
Patent Text Reader

Abstract

The invention relates to the technical field of materials, in particular to a monodisperse core-shell microsphere and a preparation method thereof. The method comprises the following steps: S1, forming a monodisperse degradable polymer microsphere by adopting a dispersion phase liquid containing a degradable polymer through a microfluidic process or an emulsification method; s2, the surfaces of the degradable polymer microspheres are subjected to one or more of dopamine auto-polymerization, electrostatic adsorption and chemical grafting, horseradish peroxidase is combined, under the catalytic action of the horseradish peroxidase, the degradable polymer microspheres and a hydrogel material are subjected to cross-linking coating, and monodisperse core-shell microspheres with a hydrogel layer are obtained; the hydrogel material is a hydrogel system which can be initiated by enzyme to be crosslinked, such as hydroxyphenylpropionic acid hydrogel, fibroin or hyaluronic acid hydrogel. The highly-monodispersed degradable core-shell microsphere material can be obtained through the method, and the method is simple in technological operation and beneficial to wide popularization and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of materials, and in particular to monodisperse core-shell microspheres and a preparation method thereof. Background Art

[0002] Core-shell microspheres are tiny particles consisting of a core and a shell. The core-shell structure is usually made of different materials, which can integrate the properties of the two materials, giving it properties that cannot be achieved by a single material of the core and shell. The properties of core-shell microsphere composites make them very suitable for pharmaceutical and biomedical applications, including cell encapsulation, cell research, targeted drug delivery, controlled drug release, medical and aesthetic filling, cell delivery, scaffold materials, food industry, catalysis and environmental monitoring. At present, a wide range of technologies have been used to prepare core-shell microsphere materials. Common preparation methods include coaxial nozzle extrusion, microfluidics, solvent evaporation and self-assembly. However, it is often difficult to prepare monodisperse core-shell microspheres with existing technologies. In addition, due to the presence of hydrogel, the hydrophobic microspheres have better cell adhesion ability, and cells can spread better on the surface of the microspheres.

[0003] Microfluidics is a technology that controls the mixing and flow of complex fluids at a microscopic scale. Droplets are produced through tiny channels, and the immiscible continuous and dispersed phases flow in their respective microchannels using the driving force of volume (such as a syringe pump) or pressure (such as a pressure vessel). At the intersection of the microchannels, the continuous phase and the dispersed phase are squeezed or sheared, causing the interface to become unstable and break, thereby forming dispersed droplets; then, the droplets are converted into core-shell microspheres by solidification, gelation, cross-linking, etc. The method of preparing core-shell microspheres using microfluidics combines microfluidics and particle preparation technology, and can be used to prepare microsphere particles with controlled particle size, shape, shell thickness, and core-shell structure. The preparation of core-shell microspheres by microfluidics belongs to an emerging field that combines microfluidics with particle preparation technology. It achieves precise control of the shape, particle size, and core-shell structure of microsphere particles through precise fluid manipulation and chemical reactions on a microfluidic platform. This technology has broad application prospects, especially in the fields of drug delivery, bioanalysis, and materials science, providing a higher level of controllability and customization for the research and application of microsphere materials.

[0004] However, the existing microfluidic technology for preparing core-shell microspheres mostly adopts the double emulsion method. Among them, biocompatible microspheres such as PLLA are generally prepared by the double emulsion method. In the encapsulation process, it is easy to have unencapsulated or encapsulated multiple cores. The existing double emulsion method for preparing microsphere structures is complex and inefficient, and usually requires the use of three or more injection pumps to simultaneously control the flow rate, and to observe the generation of microspheres by connecting a microscope. The operation is relatively complicated and the process is difficult to control. Summary of the invention

[0005] In view of this, the present invention provides a monodisperse core-shell microsphere and a preparation method thereof. The method of the present invention can obtain a highly monodisperse degradable core-shell microsphere material, and the process operation is simple, which is conducive to wide promotion and application.

[0006] The present invention provides a method for preparing monodisperse core-shell microspheres, comprising the following steps:

[0007] S1. Using a dispersed phase liquid containing a degradable polymer to form monodisperse degradable polymer microspheres through a microfluidic process or an emulsification method;

[0008] S2. The surface of the degradable polymer microspheres is treated with one or more of dopamine self-polymerization, electrostatic adsorption and chemical grafting, combined with horseradish peroxidase, and under the catalysis of the horseradish peroxidase, the degradable polymer microspheres are cross-linked and coated with a hydrogel material to obtain monodisperse core-shell microspheres with a hydrogel layer; the hydrogel material is a hydrogel system that can be cross-linked by enzymes, such as hydroxyphenylpropionic acid hydrogel, silk fibroin or hyaluronic acid hydrogel.

[0009] In some embodiments of the present invention, the particle size of the degradable polymer microspheres is 10 to 1000 μm, 30 to 250 μm, preferably 40 to 200 μm, and more preferably 50 to 180 μm.

[0010] In some embodiments of the present invention, the degradable polymer is at least one of PLA, PLGA, PCL, and PGA, preferably PLA.

[0011] In some embodiments of the present invention, the microfluidic process in step S1 includes:

[0012] Injecting an oily dispersed phase liquid containing a degradable polymer into the inner phase channel of the coaxial microfluidic chip, injecting an aqueous continuous phase liquid into the outer phase channel, collecting degradable polymer droplets at the outlet of the inner phase channel, removing the solvent of the oily dispersed phase liquid, preferably washing with water and freeze-drying, to obtain monodisperse degradable polymer microspheres;

[0013] The emulsification method in step S1 includes: stirring and emulsifying an oily dispersed phase liquid containing a degradable polymer and an aqueous continuous phase liquid to form a degradable polymer liquid, removing the solvent of the oily dispersed phase liquid, preferably washing with water and freeze-drying to obtain monodisperse degradable polymer microspheres.

[0014] In some embodiments of the present invention, in step S1, the coaxial microfluidic chip is a glass capillary chip or a PDMS chip; a coaxial collecting channel is provided at the outlet end of the inner phase channel, and the straight-line distance between the inlet of the collecting channel and the outlet of the inner phase channel is 30 to 1000 μm, preferably 50 to 500 μm.

[0015] In some embodiments of the present invention, in step S1, the aqueous continuous phase liquid is a PVA aqueous solution, and the flow rate can be adjusted to 1-100 ml / h, such as 10-50 ml / h, preferably 20-40 mL / h, by a syringe pump.

[0016] In some embodiments of the present invention, in step S1, the solvent of the oily dispersed phase liquid is at least one of dichloromethane, chloroform, ethyl acetate, acetone and tetrahydrofuran, preferably dichloromethane; the flow rate of the oily dispersed phase liquid is 0.1 to 50 ml / h, preferably 1 to 5 mL / h.

[0017] In some embodiments of the present invention, step S2 includes:

[0018] The degradable polymer microspheres are immersed in a dopamine solution and then immersed in a horseradish peroxidase solution to allow the dopamine to self-polymerize and bind to the horseradish peroxidase to obtain microspheres with horseradish peroxidase on the surface;

[0019] The microspheres with horseradish peroxidase on the surface are mixed with hydrogel materials and cross-linked to obtain monodisperse core-shell microspheres with hydrogel layers.

[0020] In some embodiments of the present invention, in step S2, the concentration of the dopamine solution is 0.1 to 5 mg / mL, and the concentration of the horseradish peroxidase solution is 0.01 to 1 mg / mL, preferably 0.01 to 0.1 mg / mL;

[0021] The cross-linking reaction time is 0.1 to 5 minutes, and water is added to terminate the reaction to prevent excessive cross-linking.

[0022] The present invention provides a monodisperse core-shell microsphere, which is obtained according to the preparation method described above. The surface of the monodisperse core-shell microsphere is smooth and can be used for drug delivery, cell adhesion and cell delivery carriers, medical and aesthetic filling materials, scaffold materials, bone and joint lubrication and catalyst preparation.

[0023] The present invention mainly combines microfluidic technology with enzyme crosslinking to prepare degradable polymer microspheres with core-shell structure, so that the formed core-shell microsphere samples show excellent consistency and stability in performance and function, and the process operation is simple. First, the present invention adopts microfluidic technology combined with enzyme crosslinking to achieve highly monodisperse core-shell microsphere samples. In this preparation process, by accurately controlling the fluid mixing and reaction process in the microfluidic system, it is ensured that the size and shape of each microsphere are very close, thereby achieving a highly uniform core-shell microsphere sample. This monodispersity makes the performance and function between the microspheres highly consistent, and enhances the application stability of the microspheres. Secondly, the obtained highly monodisperse core-shell microsphere sample has excellent stability and anti-aggregation performance. Because the size and shape of each microsphere are very close, the microspheres in the sample are not easy to stick together, thereby maintaining the independence and stability of the microspheres. This is very important for some applications, especially when it is necessary to maintain the dispersed state of the microspheres, highly monodisperse samples are more advantageous.

[0024] In addition, compared with the high cost and low efficiency of the traditional double emulsion preparation method, the present invention is simple to operate by preparing degradable polymer microspheres only through microfluidic technology, and then a hydrogel layer can be formed on the surface of the microspheres by in situ enzyme crosslinking, thereby realizing the construction of core-shell microspheres. The embodiment of the present invention prepares monodisperse core-shell microsphere samples by combining microfluidic technology with enzyme crosslinking, which can achieve more precise control. This microfluidic technology can accurately control experimental conditions and reaction parameters, thereby ensuring that the preparation process of microspheres is more reliable and more repeatable. This precise control helps to improve the quality of the product, and in some applications that require high consistency and accuracy, highly monodisperse microsphere samples are more popular. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0026] Figure 1 A device design diagram for preparing a capillary microfluidic chip provided in an embodiment of the present application; (a) is the chip design part, and (b) is the actual chip;

[0027] Figure 2 The structure diagram and physical diagram of the microfluidic system in the embodiment of the present application; (a) is the schematic diagram of the structure of the microfluidic system, and (b) is the physical system;

[0028] Figure 3Schematic diagram of the structure of the microfluidic system in the preparation method of Example 1 of the present application; (a) is the main dimension marking part, and (b) is the actual object and spacing schematic part;

[0029] Figure 4 This is an optical microscope image of the PLLA microspheres obtained in Example 1 of the present application;

[0030] Figure 5 This is an optical microscope image of the PLLA-GelHPA core-shell microspheres of Example 2 of the present application;

[0031] Figure 6 The particle size of PLLA microspheres under different spacing conditions in Example 3 of the present application;

[0032] Figure 7 The particle size of PLLA microspheres under different water phase flow rate conditions in Example 4 of the present application;

[0033] Figure 8 The particle size of PLLA microspheres under different oil phase flow rate conditions in Example 5 of the present application;

[0034] Fig. 9 This is the particle size distribution diagram of PLLA microspheres obtained in Example 1 of the present application;

[0035] Fig.10 This is the particle size distribution diagram of PLLA-GelHPA core-shell microspheres of Example 2 of the present application;

[0036] Fig.11 This is a SEM image of PLLA microspheres obtained in Example 1 of the present application;

[0037] Fig.12 This is the SEM image of PLLA-GelHPA core-shell microspheres of Example 2 of the present application;

[0038] Fig.13 This is the element distribution diagram of the PLLA microspheres obtained in Example 1 of the present application;

[0039] Fig.14 This is the element distribution diagram of the PLLA-GelHPA core-shell microspheres of Example 2 of the present application;

[0040] Fig.15 The infrared spectra of the PLLA microspheres of Example 1 and the PLLA-GelHPA core-shell microspheres of Example 2;

[0041] Fig.16 It is a fluorescence image of the GelHPA hydrogel coating on the surface of the PLLA-GelHPA core-shell microspheres of Example 2;

[0042] Fig.17 The PLLA microsphere suspension of Example 1 is removed;

[0043] Fig.18 The PLLA-GelHPA core-shell microsphere suspension of Example 2 is removed;

[0044] Fig.19 The friction coefficient diagram of the PLLA microspheres of Example 1 and the PLLA-GelHPA core-shell microspheres of Example 2;

[0045] Fig. 20 This is a picture of the grinding disc of PLLA-GelHPA core-shell microspheres of Example 2;

[0046] Fig.21 This is the live and dead image of stem cells on PLLA microspheres in Example 1;

[0047] Fig. 22 Live and dead images of stem cells seeded on PLLA-GelHPA core-shell microspheres of Example 2;

[0048] Fig.23 This is a staining image of the PLLA microsphere cell culture of Example 1;

[0049] Fig.24 This is a staining image of the PLLA-GelHPA core-shell microsphere cell culture in Example 2. DETAILED DESCRIPTION

[0050] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the technical scheme of the present invention is now described in detail below in conjunction with specific embodiments. The described embodiments are only a part of the embodiments of the present invention, rather than all of the embodiments.

[0051] The present invention provides a method for preparing monodisperse core-shell microspheres, comprising the following steps:

[0052] S1. Using a dispersed phase liquid containing a degradable polymer to form monodisperse degradable polymer microspheres through a microfluidic process or an emulsification method;

[0053] S2. The surface of the degradable polymer microspheres is subjected to one or more of dopamine self-polymerization, electrostatic adsorption and chemical grafting, combined with horseradish peroxidase, and under the catalysis of the horseradish peroxidase, the degradable polymer microspheres are cross-linked and coated with a hydrogel material to obtain monodisperse core-shell microspheres with a hydrogel layer; the hydrogel material is a hydrogel system that can be cross-linked by an enzyme, such as hydroxyphenylpropionic acid hydrogel, silk fibroin or hyaluronic acid hydrogel.

[0054] The method of the present invention can obtain highly monodisperse degradable core-shell microsphere materials, and the process operation is simple and convenient for precise control.

[0055] See also Figure 1 The capillary microfluidic chip device of the present invention first designs a coaxial glass capillary microfluidic chip by Solidworks; the present invention can also adopt other material chips with similar principles, such as polydimethylsiloxane (PDMS) chips, etc. In a specific embodiment of the present invention, the main components of the capillary microfluidic chip device are a glass slide, a plurality of capillaries and a dispensing needle. First, a circular capillary (outer diameter 1mm) can be fixed on a glass slide by ultraviolet glue, and the interior of the capillary is mainly an external phase channel; then, two cylindrical capillaries (inner diameter / outer diameter: 0.5mm / 0.8mm) are pulled by an igniter to gradually become thinner, and then the tip of the capillary is polished to the required diameter with sandpaper. Under a microscope, two tapered glass capillaries are respectively inserted into the left and right sides of the outer circular glass tube so that their tapered mouths are opposite; the interiors of the two capillaries correspond to the internal phase channel and the collection channel respectively. By observation and adjustment, ensure that the positions of the two capillaries are adjusted to be coaxial, and gradually fine-tune the axial distance between them to 200 μm; it can also be adjusted between 30 and 1000 μm, preferably 50 and 500 μm, for example, 50, 100, 300, 400, 500 μm, etc.

[0056] The embodiment of the present invention can cut two grooves on both sides of the plastic end of a dispensing needle so that it can be embedded in the contact between the outer circular tube and the incident circular tube, and finally fix the needle at the connection between the left tapered capillary and the outer circular capillary, and seal the remaining tube opening. A section of silicone hose is connected to the other end of the incident tapered capillary, and a syringe is connected through the needle, and the dispersed phase liquid can be injected from the capillary; the silicone hose and the needle can be connected at the dispensing needle, and the continuous phase liquid can be injected. Furthermore, glue is used to bond the hose and the capillary at the connection to fix it and prevent leakage; after the glue solidifies, a coaxial capillary microfluidic chip can be obtained.

[0057] See also Figure 2 , Figure 2 The structure diagram and physical picture of the microfluidic system of the embodiment of the present invention. This microfluidic system mainly forms droplets, and consists of two parts: a preparation device and a collection device. The preparation device includes a microfluidic chip and a syringe pump, and the collection device is mainly a beaker for holding the collected liquid. The embodiment of the present invention can fix the microfluidic chip on a beaker, and the inlet end is connected to the syringe pump through a silicone hose; by adjusting the relevant parameters of the syringe pump, the flow rate of the dispersed phase and the continuous phase can be accurately controlled.

[0058] In some specific embodiments, the phase solution in the microfluidic chip flows through a circular capillary with a smaller diameter, which can be called an incident tube, and the caliber of the incident tube can be 50-150 μm; the droplets are formed in another capillary, which is called a collecting tube, and can also be connected to a beaker containing the collected liquid. The caliber of the collecting tube can be 200-300 μm; the spacing range between the incident tube and the collecting tube is as described above. In the above embodiments, the glass capillary is a hydrophilic material, and no treatment is required when preparing water-in-oil droplets (such as PLLA droplets). The hydrophilicity of the capillary itself can be used to generate water-in-oil droplets; it can also be subjected to hydrophilic treatment to improve the hydrophilicity of the capillary so that the water-in-oil droplets are better generated.

[0059] The embodiment of the present invention configures an oil phase solution containing a degradable polymer, which is an oily dispersed phase liquid. The degradable polymer is mainly polylactic acid (PLA), including poly L-lactide (PLLA, poly L-lactic acid), dextrorotatory polylactic acid (PDLA), polylactic acid-glycolic acid copolymer (PLGA, polyvinyl lactide), PGA (polyglycolide) and polycaprolactone (PCL) at least one, preferably polylactic acid, such as PLLA. Among them, the PLLA molecular weight is further preferably 15901-16135. In addition, the solvent of the oily dispersed phase liquid may be at least one of dichloromethane, chloroform, ethyl acetate, acetone and tetrahydrofuran, preferably dichloromethane. For example, degradable polymer powders such as PLLA are dissolved in dichloromethane (DCM) and prepared into a 4-10% (w / v) oil phase solution, preferably with a concentration of 5% (w / v).

[0060] At the same time, the embodiment of the present invention prepares an aqueous continuous phase liquid, which is also called an aqueous phase solution, mainly a polyvinyl alcohol (PVA) aqueous solution, and the aqueous phase (PVA) concentration can be 1-3% (w / v), preferably 1% (w / v). In addition, the collection liquid in the above-mentioned collecting device is preferably a 0.5% (w / v) PVA aqueous solution. The polymers described in the embodiments of the present invention can all be commercially available products, wherein the PVA alcoholysis degree can be 87.0-89.0% (mol / mol).

[0061] In the step S1 of the embodiment of the present invention, monodisperse degradable polymer microspheres are prepared, specifically, an oily dispersed phase liquid containing a degradable polymer is injected into the inner phase channel of the coaxial microfluidic chip, and an aqueous continuous phase liquid is injected into the outer phase channel, and degradable polymer droplets are obtained in a collection tube at the outlet end of the inner phase channel, which can be collected in a beaker with the collection liquid. Afterwards, the solvent of the oily dispersed phase liquid is removed, and the microspheres are obtained after washing with water and freeze-drying.

[0062] Microfluidics is an advanced technology that can control the mixing and flow rate of complex fluids at a microscopic scale. Although the core-shell microparticles prepared by microfluidics have controllable morphology, the system structure is often complex and the thickness of the shell is difficult to control. Droplet microfluidics is a universal tool for making almost all types of particles. The convection flow pattern inside the droplets is conducive to mixing, and the components in the droplets are separated to avoid contamination and mutual interference. Therefore, since the emergence of droplet microfluidics, it has been widely studied and applied in theory and practice. Droplet microfluidics can produce precisely calibrated droplets in a repeatable and designable manner. In addition, individual droplet reactors can operate independently, facilitating biochemical reactions and chip laboratory applications.

[0063] In the process of generating degradable polymer droplets in the embodiment of the present invention, the aqueous phase solution is adjusted by a syringe pump to adjust the flow rate, which can be 1 to 100 ml / h, such as further 10 to 50 ml / h, preferably 20 to 40 mL / h, and further 30 mL / h. The oily dispersed phase liquid is also adjusted by another syringe pump, and the flow rate can be 0.1 to 50 ml / h, specifically 1 to 5 ml / h, preferably 2 to 4 mL / h, and further 2 mL / h. The degradable polymer droplets collected in the beaker are preferably stirred at room temperature for 24 hours to volatilize dichloromethane. The obtained degradable polymer microspheres are washed with a large amount of water (generally deionized water in the laboratory) and freeze-dried for storage; the degradable polymer microspheres have uniform particle size, are in a monodisperse state, and may have a porous structure; their particle size can be 30 to 250 μm, preferably 40 to 200 μm, more preferably 50 to 180 μm, and further 80 to 120 μm, etc., and also have a certain hydrophobicity.

[0064] After obtaining monodisperse degradable polymer microspheres, the embodiment of the present invention directly immerses them into a dopamine solution of a certain concentration, and the adhesion of dopamine on the surface of the microspheres can be achieved. Then, the microspheres with dopamine on the surface are immersed in a horseradish peroxidase (HRP) solution of a certain concentration and left for a certain period of time. Among them, dopamine is oxidized and self-polymerized under weak alkaline conditions (using a buffer solution or NaOH for regulation, generally pH = 8.5) to form polydopamine, and the o-quinone group on polydopamine can be covalently bonded to the amino group on the HRP enzyme, so that the HRP enzyme can be fixed on the surface of the microspheres to achieve covalent bonding between polydopamine and the enzyme, and obtain microspheres with horseradish peroxidase on the surface.

[0065] In the embodiment of the present invention, the microspheres with horseradish peroxidase on the surface are then washed with water, and then hydrogen peroxide and a hydrogel material solution are added to carry out a cross-linking reaction; the hydrogel material is a hydrogel system that can be cross-linked by enzymes, such as hydroxyphenylpropionic acid gelatin, silk fibroin or hyaluronic acid, and further is hydroxyphenylpropionic acid gelatin (GelHPA). Horseradish peroxidase (HRP) is reacted with hydrogen peroxide (H2 O 2 , hydrogen peroxide), it can efficiently catalyze the free radical coupling of phenol and aniline derivatives. Taking GelHPA as an example, under the catalysis of horseradish peroxidase, the p-hydroxyphenylpropionic acid group on GelHPA is activated, and the presence of enzymes on the surface of polymer microspheres such as PLLA makes it possible for only the surface of the microspheres to cross-link to form the GelHPA hydrogel coating layer (shell layer). Similarly, silk itself contains enzyme-crosslinkable groups, or HPA can be grafted onto silk protein and hyaluronic acid hydrogel materials to achieve better enzyme cross-linking effects.

[0066] In a specific embodiment of the present invention, the concentration of the dopamine solution can be 0.1-5 mg / mL, preferably 1-5 mg / mL, and further 2-3 mg / mL; when soaking, it is preferred to select an equal amount (50 mg) of microspheres to be soaked in a certain volume (3 ml) of dopamine solution. The concentration of the horseradish peroxidase solution can be 0.01-1 mg / mL, such as 0.01-0.1 mg / mL, preferably 0.02-0.05 mg / mL, and soak for 24 hours [soaking for a shorter time can also play a role]. GelHPA solution is usually a gelatin hydrogel of parahydroxyphenylpropionic acid (HPA), and its concentration is 20% by mass volume. The temperature range of the cross-linking reaction is generally 25-30°C, and it is easy to gel at a lower temperature; the time of the cross-linking reaction is preferably 0.1-5 minutes, and further 0.5-2.5 minutes, such as 1 minute, 2 minutes, 3 minutes, etc., and it is easy to form a mass if the time is too long. In order to avoid the phenomenon of excessive cross-linking of the hydrogel layer and the formation of agglomerates, it is preferred to add 1 ml of water to terminate the reaction after 2 minutes of reaction, and monodisperse core-shell microspheres with a uniform hydrogel layer on the surface can be obtained. The hydrogel shell in the embodiment of the present invention is mainly formed by in situ enzyme cross-linking. The enzyme cross-linking can control the cross-linking degree of the hydrogel by the concentration of hydrogen peroxide, the concentration of enzyme and the concentration of hydrogel, so as to obtain hydrogel shell layers of different thicknesses.

[0067] The present invention provides a monodisperse core-shell microsphere, which is obtained according to the preparation method described above. The surface of the monodisperse core-shell microsphere is smooth and can be used for drug delivery, cell adhesion and cell delivery carriers, medical and aesthetic filling materials, scaffold materials, bone and joint lubrication and catalyst preparation, etc.

[0068] In a specific embodiment of the present invention, the monodisperse core-shell microspheres are core-shell structures, having the characteristics of uniform particle size and single encapsulation; the core is a PLLA microsphere, the shell layer covering the core is a hydrogel layer, and further a GelHPA hydrogel layer (which can be recorded as PLLA-GelHPA core-shell microspheres), and the shell thickness is controllable (estimated to be approximately between 0.1 and 100 microns).

[0069] Among them, PLLA is a polymer, and PLLA microspheres have certain rigidity and hardness, which can play a supporting role under heavy load and protect the microspheres from being destroyed. PLLA microspheres can provide mechanical support for articular cartilage, and have good biocompatibility and degradability. After a period of time, they can be gradually degraded into lactic acid in the body and metabolized and discharged. Hydrogel microspheres are low in strength and fragile, but hydrogels have viscoelasticity, and when the outside world applies force to the microspheres, they have a certain wear resistance. In osteoarthritis, smooth hydrogels can effectively improve the lubrication properties of cartilage in the affected parts, reduce friction, reduce wear, and extend the service life of joints, thereby improving the quality of life of patients with osteoarthritis. However, due to the erosion of osteoarthritis, the lubrication properties of cartilage in the affected part usually decrease significantly. The presence of the hydrogel layer of the core-shell microspheres described in the embodiment of the present invention can play a certain lubricating role. Therefore, the core-shell microspheres with a hydrogel layer can not only play a wear-resistant role, but also play a supporting role due to the presence of the PLLA kernel.

[0070] Furthermore, PLLA is a hydrophobic material that easily sticks to the wall of the gun tip. GelHPA hydrogel is hydrophilic and has a cell adhesion site RGD. The hydrogel shell of the core-shell microspheres described in the embodiment of the present invention can enhance the compatibility of the hydrophobic microspheres with the water environment, and prevent direct contact between the hydrophobic cores and between the hydrophobic cores and the needle or container wall. The suspension stability of the microspheres that are not coated with hydrogel in water is low, and clogging problems may occur during the injection process. The hydrogel layer on the surface of the PLLA-GelHPA core-shell microspheres has a sequence that promotes cell adhesion, which is beneficial to cell adhesion, making cells more willing to adhere to the surface of the core-shell microspheres for spreading and proliferation, which is particularly beneficial for applications in cell analysis research and other aspects.

[0071] In addition, the shell and core materials of the monodisperse core-shell microspheres have a wide range of options. PLLA material can be replaced by PLGA, PLA, and GelHPA can be replaced by silk fibroin, hyaluronic acid hydrogel; due to the controllability of microfluidics and other technologies, core-shell microspheres of different sizes can be prepared.

[0072] The embodiment of the present invention mainly combines microfluidic technology with enzyme cross-linking, which can realize the preparation of monodisperse core-shell microspheres, is simple to operate, and reduces the cost of the core-shell microsphere preparation device; and the core-shell microspheres such as PLLA-GelHPA have good monodispersity, better hydrophilicity and biocompatibility, etc.

[0073] In order to better illustrate the present invention, the following examples are further illustrated. In the examples, all raw reagents and materials are commercially available, and the experimental methods without specific experimental conditions are conventional methods and conditions known in the art. The molecular weight of PLLA is 15901-16135, and the intrinsic viscosity is 0.47. The alcoholysis degree of PVA is 87.0-89.0% (mol / mol).

[0074] Example 1

[0075] See also Figure 3 , Figure 3 This is a schematic diagram of the structure of the microfluidic system in the preparation method of Example 1 of the present application. The diameter of the oil phase inlet of the incident tube (the inner phase flows through a circular capillary with a smaller diameter) is 500 μm, and the outer phase channel has a water phase inlet with a diameter of 1000 μm; the diameter of the droplet outlet of the collecting tube (coaxial capillary) is 500 μm, and the droplet generation is between the incident tube outlet and the collecting tube inlet (with a diameter of 250 μm), and the spacing between them is adjustable.

[0076] The preparation of monodisperse biodegradable microspheres is as follows:

[0077] (a) Oil phase solution: PLLA powder was dissolved in dichloromethane (DCM) to prepare a 5% (w / v) solution;

[0078] (b) Aqueous phase solution: PVA aqueous solution (1%, w / v);

[0079] (c) Collecting solution: 0.5% (w / v) PVA aqueous solution.

[0080] (d) During the droplet generation process, the water phase flow rate is 30 ml / h and the oil phase flow rate is 2 ml / h (the flow rates are adjusted by injection pumps, respectively). The distance between the outlet of the injection tube and the inlet of the collection tube is 200 μm, and the PLLA droplets are formed in the collection tube. Afterwards, the PLLA droplets collected in the beaker (containing the collection liquid) are stirred at room temperature for 24 hours to evaporate the dichloromethane. The obtained PLLA microspheres are washed with a large amount of deionized water and freeze-dried for storage.

[0081] See also Figure 4 , Figure 4 The optical microscope image of PLLA microspheres prepared by capillary microfluidic chip shows that the obtained PLLA microspheres have the characteristics of uniform particle size and monodispersity.

[0082] Example 2

[0083] The GelHPA hydrogel shell is formed by in situ enzyme crosslinking to obtain monodisperse core-shell microspheres. First, 50 mg of the PLLA microspheres prepared in Example 1 were directly immersed in a 2 mg / ml dopamine solution (3 ml). After 2 hours at room temperature, dopamine adhered to the surface of the microspheres. Then, the microspheres with dopamine on the surface were immersed in a 0.04 mg / ml HRP enzyme solution for 24 hours to achieve the binding of polydopamine to the enzyme. Subsequently, the obtained microspheres were washed three times with deionized water and 100 μl HRP was added. 2 O 2 (concentration 10 mM) and 200 μl of 20% GelHPA solution were cross-linked at 25-30° C. to form a GelHPA hydrogel layer. After two minutes of reaction, 1 ml of deionized water was added to terminate the reaction to obtain monodisperse core-shell microspheres with a uniform hydrogel layer on the surface.

[0084] See also Figure 5 , Figure 5 This is an optical microscope image of PLLA-GelHPA core-shell microspheres prepared by enzyme crosslinking. As can be seen from the figure, there is a transparent and uniform GelHPA hydrogel layer on the surface of the opaque PLLA microspheres.

[0085] Example 3

[0086] Compared with Example 1, the distance between the incident tube and the collecting tube in Example 1(d) is adjusted to 50, 400 and 1000 μm. Figure 6 , Figure 6 is the size of PLLA microspheres under different conditions of the distance between the incident tube and the collection tube.

[0087] It can be seen that when other parameters remain unchanged, the larger the distance between the incident port and the collecting port, the larger the particle size of the microsphere. When the corresponding distances are 50, 200, 400 and 1000 μm, the diameters of the obtained microspheres are approximately 48, 100, 170 and 230 μm. Based on this, PLLA microspheres with a size of 100 μm were selected for subsequent gel layer preparation.

[0088] Example 4

[0089] Compared with Example 1, the aqueous phase flow rate in Example 1(d) was adjusted to 20, 40 and 50 ml / h. Figure 7 , Figure 7 The particle size of PLLA microspheres at different water phase flow rates. It can be seen that the larger the water phase flow rate, the smaller the particle size of the microspheres, which decreases from about 140μm to about 30μm.

[0090] Example 5

[0091] Compared with Example 1, the oil phase flow rate in Example 1(d) was adjusted to 3 and 4 ml / h. Figure 8 , Figure 8 The diameter of PLLA microspheres at different oil phase flow rates. It can be seen that the larger the oil phase flow rate, the larger the diameter of the microspheres, which can reach more than 130 μm.

[0092] In addition, characterization tests were performed on Example 1 and Example 2, and the results are as follows.

[0093] See also Fig. 9 , Fig. 9 The particle size of the PLLA microspheres is statistically analyzed in Example 1. It can be seen that the particle size of the microspheres is distributed around 100 μm, and has the characteristics of uniform particle size and monodispersity.

[0094] See also Fig.10 , Fig.10 The particle size of the PLLA-GelHPA microspheres is calculated in Example 2. Due to the presence of a layer of hydrogel on the surface, the particle size of the PLLA-GelHPA core-shell microspheres is slightly larger than that of the PLLA microspheres, with the diameter increasing from the original 102 μm to about 108 μm, and also having the characteristic of uniform size distribution.

[0095] See also Fig.11 , Fig.11 The surface morphology of the freeze-dried PLLA microspheres characterized by scanning electron microscopy (SEM) in Example 1. The surface morphology of the PLLA microspheres is porous, which is due to the surface pores formed when the dichloromethane evaporates during the curing process.

[0096] See also Fig.12 , Fig.12 The surface morphology of the freeze-dried PLLA-GelHPA microspheres characterized by SEM in Example 2. As can be seen from the figure, the PLLA-GelHPA core-shell microspheres are smooth on the surface due to the presence of the gel layer.

[0097] The porous structure can be used for drug encapsulation, thereby achieving drug loading and sustained release. By encapsulating the hydrophobic drug in the polymer core and then encapsulating it in the hydrogel layer, sustained release of the drug can be achieved. Therefore, core-shell microspheres with a hydrogel layer can achieve a sustained release effect to a greater extent.

[0098] See also Fig.13 , Fig.13 Elemental analysis of the freeze-dried PLLA microspheres characterized by X-ray energy dispersive spectroscopy (EDS) in Example 1. As can be seen from the figure, the PLLA microspheres are composed of C and O elements.

[0099] See also Fig.14 , Fig.14 Elemental analysis of freeze-dried PLLA-GelHPA microspheres characterized by EDS in Example 2. N element was found in PLLA-GelHPA, which also proved the successful formation of the hydrogel layer on the surface of PLLA-GelHPA microspheres.

[0100] See also Fig.15 , Fig.15 The infrared spectra of PLLA microspheres and PLLA-GelHPA microspheres are shown in Figure 2. -1 The characteristic peak at 3200cm is due to the ester group. -1 The broad peaks on the left and right are OH stretching vibrations at 1604 cm -1 The characteristic peaks at are due to the asymmetric stretching vibration of the COO of the hydrogel. These features qualitatively indicate the presence of the GelHPA hydrogel shell on the PLLA microspheres. Therefore, by comparing the infrared results, the successful formation of the GelHPA hydrogel layer can be confirmed.

[0101] See also Fig.16 , Fig.16 This is a fluorescence image of the GelHPA hydrogel coating on the surface of the PLLA-GelHPA core-shell microspheres; fluorescence can be seen in the fluorescently labeled GelHPA using laser confocal microscopy (grafting and photography are common methods). The carboxyl group of GelHPA can combine with Rhodamine 123 to form GelHPA grafted with Rhodamine 123. Rhodamine 123 emits green light under the action of confocal laser. Using a confocal microscope to observe the prepared PLLA-GelHPA microspheres under the green light channel, it can be seen that there is a green outline on the surface of the microspheres, and the PLLA microspheres are surrounded by a fluorescent layer, which is the GelHPA gel coating.

[0102] Example 6

[0103] See also Fig.17 , use a 1ml pipette to absorb the PLLA microsphere suspension, eject the microspheres from the tip of the pipette, and observe the aggregation of the microspheres on the pipette tip wall. It can be seen that the hydrophobic PLLA microspheres are prone to self-aggregation, the microspheres not coated with hydrogel are ejected unevenly from the pipette tip, and some microspheres will aggregate and adhere to the inner wall of the pipette tip.

[0104] See also Fig.18, the PLLA-GelHPA core-shell microspheres were sucked into the 1ml pipette tip. Under the action of injection force, the polylactic acid microspheres wrapped by the hydrogel were smoothly discharged from the tip, and there was no residue inside the tip. The core-shell microspheres with hydrogel shells have high suspension stability and can maintain good injectability even at high volume fractions, which is conducive to implanting a large number of microspheres into small volume tissues.

[0105] Example 7

[0106] See also Fig.19 The lubrication performance of the microspheres was measured in a linear reciprocating mode using a friction and wear tester (UMT-5, Bruker Nano Inc, Germany) (detected by a third-party testing platform). The physiological state of the joint was simulated by sliding the upper sample along the lower sample surface. All samples were prepared in PBS suspension and added to the contact surface as a lubricant between the upper and lower samples. It can be observed that compared with the PLLA microspheres with a larger friction coefficient, the friction coefficient COF value of the core-shell microspheres is somewhat reduced, indicating that the core-shell microspheres have a certain lubrication effect while the hydrogel layer has a ball bearing effect.

[0107] Core-shell microspheres have certain advantages in the treatment of osteoarthritis, starting from the hydrogel shell and polymer core. The shell hydrogel effectively reduces the surface roughness, giving the core-shell microspheres the ability to reduce friction and wear. The core polymer is used to load drugs, and the thickness of the hydrogel shell is adjusted to control the drug release cycle. The core and shell of the core-shell microspheres can be regulated to fine-tune their biochemical and biomechanical properties to meet the needs of various tissues.

[0108] See also Fig. 20 , observe the depth and width of the wear scar on the steel disk (from left to right: PBS group, PLLA microsphere group and PLLA-GelPHA core-shell microsphere group). According to the surface morphology of the worn surface of the steel disk, it can be seen that the wear scar of the PLLA-GelHPA core-shell microsphere is lighter in color, indicating that the presence of the hydrogel coating reduces the wear effect of the microspheres on the substrate.

[0109] Example 8

[0110] See also Fig.21 (Green represents live cells, red represents dead cells). By culturing stem cells on PLLA microspheres, live-dead staining was performed on the third day of culture to observe the growth of cells on the microspheres (culture and staining are well known to industry technicians). As can be seen from the figure, the cells on the surface of the PLLA microspheres are basically alive.

[0111] See also Fig. 22, by culturing stem cells on PLLA-GelHPA core-shell microspheres, the growth of cells on the microspheres was observed. There were more cells on the surface of the core-shell microspheres, which is because GelHPA hydrogel, as a natural polymer material, has better biocompatibility.

[0112] See also Fig.23 On the third day of cell culture, the cytoskeleton and nucleus were stained to observe the spreading of cells on the surface of PLLA microsphere samples. The cells showed a certain degree of adhesion and spreading on the surface of PLLA microspheres, which was caused by the hydrophobicity of PLLA microspheres.

[0113] See also Fig.24 , the core skeleton of the PLLA-GelHPA core-shell microspheres cultured for three days was stained, and it can be observed that the cells on the surface of the core-shell microspheres basically wrapped all the microspheres, and cell clusters appeared. This is because the GelHPA hydrogel has a cell adhesion site RGD, so more cells adhere and spread on the surface of the core-shell microspheres.

[0114] Example 9

[0115] Monodisperse degradable microspheres were prepared according to the steps of Example 1;

[0116] Furthermore, monodisperse core-shell microspheres were obtained according to the steps of Example 2, except that the reaction time was changed to five minutes, and the thickness of the hydrogel shell layer in the obtained monodisperse core-shell microspheres was increased to 5 μm.

[0117] It can be seen from the above examples that the core-shell microspheres of the embodiment of the present invention have the characteristics of uniform particle size and monodispersity, and due to the presence of hydrogel, the surface is smooth and has high suspension stability. Even at high volume fractions, it can maintain good injectability, and it also has a lubricating effect, which reduces the wear of the microspheres on the substrate and has good biocompatibility. In particular, the GelHPA hydrogel has a cell adhesion site RGD, which is beneficial to cell survival. The hydrogel shell in the embodiment of the present invention is mainly formed by in situ enzyme crosslinking. Enzyme crosslinking can control the crosslinking degree of the hydrogel by reaction time, hydrogen peroxide concentration, enzyme concentration and hydrogel concentration, so as to obtain hydrogel shell layers of different thicknesses; it can be used for drug delivery, cell adhesion and cell delivery carriers, medical and aesthetic filling materials, scaffold materials, bone joint lubrication and catalyst preparation, etc., and has good application prospects.

[0118] The above examples are only used to illustrate the technical features and implementation process of the present invention, rather than to limit the technical solution of the present invention. It should be pointed out that for ordinary technicians in this field, the present invention can still be modified or replaced by equivalents, and modifications or replacements that do not deviate from the principles of the present invention are all covered by the protection of the present invention.

Claims

1. A method for preparing monodisperse core-shell microspheres, characterized in that: The following steps are involved: S1. Using a dispersed phase liquid containing a degradable polymer to form monodisperse degradable polymer microspheres through a microfluidic process or an emulsification method; S2. The surface of the degradable polymer microspheres is treated with one or more of dopamine self-polymerization, electrostatic adsorption and chemical grafting, combined with horseradish peroxidase, and under the catalysis of the horseradish peroxidase, the degradable polymer microspheres are cross-linked and coated with a hydrogel material to obtain monodisperse core-shell microspheres with a hydrogel layer; the hydrogel material is a hydrogel system that can be cross-linked by enzymes, such as hydroxyphenylpropionic acid hydrogel, silk fibroin or hyaluronic acid hydrogel.

2. The preparation method according to claim 1, characterized in that: The particle size of the degradable polymer microspheres is 10 to 1000 μm, and may be 30 to 250 μm, preferably 40 to 200 μm, and more preferably 50 to 180 μm.

3. The preparation method according to claim 1, characterized in that: The degradable polymer is at least one of PLA, PLGA, PCL and PGA, preferably PLA.

4. The preparation method according to any one of claims 1 to 3, characterized in that The microfluidic process in step S1 includes: Injecting an oily dispersed phase liquid containing a degradable polymer into the inner phase channel of the coaxial microfluidic chip, injecting an aqueous continuous phase liquid into the outer phase channel, collecting degradable polymer droplets at the outlet of the inner phase channel, removing the solvent of the oily dispersed phase liquid, preferably washing with water and freeze-drying, to obtain monodisperse degradable polymer microspheres; The emulsification method in step S1 includes: stirring and emulsifying an oily dispersed phase liquid containing a degradable polymer and an aqueous continuous phase liquid to form a degradable polymer liquid, removing the solvent of the oily dispersed phase liquid, preferably washing with water and freeze-drying to obtain monodisperse degradable polymer microspheres.

5. The preparation method according to claim 4, characterized in that: In step S1, the coaxial microfluidic chip is a glass capillary chip or a PDMS chip; a coaxial collecting channel is provided at the outlet of the inner phase channel, and the straight-line distance between the inlet of the collecting channel and the outlet of the inner phase channel is 30 to 1000 μm, preferably 50 to 500 μm.

6. The preparation method according to claim 5, characterized in that: In step S1, the aqueous continuous phase liquid is a PVA aqueous solution, and the flow rate can be adjusted to 1-100 mL / h, such as 10-50 mL / h, preferably 20-40 mL / h, by a syringe pump.

7. The preparation method according to claim 6, characterized in that: In the step S1, the solvent of the oily dispersed phase liquid is at least one of dichloromethane, chloroform, ethyl acetate, acetone and tetrahydrofuran, preferably dichloromethane; the flow rate of the oily dispersed phase liquid is 0.1 to 50 mL / h, preferably 1 to 5 mL / h.

8. The preparation method according to any one of claims 1 to 3, characterized in that: The step S2 comprises: The degradable polymer microspheres are immersed in a dopamine solution and then immersed in a horseradish peroxidase solution to allow the dopamine to self-polymerize and bind to the horseradish peroxidase to obtain microspheres with horseradish peroxidase on the surface; The microspheres with horseradish peroxidase on the surface are mixed with hydrogel materials and cross-linked to obtain monodisperse core-shell microspheres with hydrogel layers.

9. The preparation method according to claim 8, characterized in that: In step S2, the concentration of the dopamine solution is 0.1 to 5 mg / mL, and the concentration of the horseradish peroxidase solution is 0.01 to 1 mg / mL, preferably 0.01 to 0.1 mg / mL; The cross-linking reaction time is 0.1 to 5 minutes, and water is added to terminate the reaction to prevent excessive cross-linking.

10. A monodisperse core-shell microsphere, characterized in that: The monodisperse core-shell microspheres obtained by the preparation method according to any one of claims 1 to 9 have a smooth surface and can be used for drug delivery, cell adhesion and cell delivery carriers, medical and aesthetic filling materials, scaffold materials, bone and joint lubrication, and catalyst preparation.

Citation Information

Patent Citations

  • Magnetic / functionalized SiO2 composite microsphere immobilized enzyme and preparation method thereof

    CN101613694A

  • Functional nano-particle compound cross-linking microsphere powder as well as preparation method and application thereof

    CN102908960A

  • Preparation of uniform microparticles with inner pore structures and dimple structures on the surface by using a microfluidic device

    KR1020120080267A

  • System and method for computing medical data

    KR102821475B1

  • Method and system of producing hydrogel microspheres

    US20230143252A1

Cited By

  • Procedure for obtaining a granulated microparticle material, granulated microparticle material and use thereof for the storage and release of cellular components

    ES3055176A1