Catalyst, and preparation method and application of composite catalyst
By using titanium silicon molecular sieve to support V2O5 and metal oxide or carbonate composite catalyst in methylbutenol isomerization, the problems of limited types of catalysts and low conversion rate are solved, and the efficient preparation of isoprenol is achieved. The service life of the catalyst is extended through resurrection and the preparation process is simplified.
Patent Information
- Application Number
- CN202411201126.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, the types of catalysts for isomerization of isopentenol are limited, with low conversion and selectivity, and the catalyst preparation is complex, with short service life, and requires frequent coating and high-temperature calcination.
Using a composite catalyst supported by titanium silicon molecular sieve with V2O5 and metal oxide or metal carbonate, prepared by drying and calcining, it is used for catalysis of methyl butenol, improve conversion and selectivity, and provide a resurrection method to extend service life .
It improves the conversion rate and selectivity of methyl butenol to isopentyl alcohol, simplifies the catalyst preparation process, extends the service life of the catalyst, and restores activity through resurrection, reducing production costs.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to a catalyst, a preparation method of a composite catalyst and application thereof. Background Art
[0002] Isopentenol (3-methyl-2-butene-1-ol) is an important fine chemical intermediate, mainly used in citral, a flavor and fragrance product, vitamin E and vitamin A in medicine, and pyrethroid insecticides, a highly effective and low-toxic pesticide. At present, the methods for synthesizing isopentenol in industry mainly include the isoprene method, the methylbutenol (2-methyl-3-butene-2-ol) isomerization method, and the Prince method.
[0003] The methylbutenol isomerization method has attracted wide attention due to its advantages of cheap and readily available raw materials, mild reaction conditions, simple purification steps and easy large-scale production. Common catalysts for this reaction include metal esters, metal salts and metal oxides.
[0004] For example, Japanese patent JP57045121 and US patent US3925485 use vanadate compounds as isomerization catalysts, and the conversion rate is within the range of 25-30%. However, vanadate is easily hydrolyzed in water to produce vanadic acid, which causes dehydration of raw materials and products and reduces the reaction selectivity. Chinese patent CN105967978A uses vanadium oxides or vanadium metal salts as catalysts, and the single-pass conversion rate is less than 30%. It is mentioned that it can be used in a continuous cycle, but the operation mode is intermittent, and the reaction liquid needs to be cooled and filtered after the reaction reaches equilibrium, and then the reaction liquid is added. At the same time, the low single-pass conversion rate means that subsequent distillation is required, and a large amount of raw materials need to be It needs to be recycled, has high energy consumption and low production efficiency; Chinese patent CN111167471A uses a ceramic corrugated plate coated with a composite oxide containing vanadium, titanium, manganese, iron, molybdenum, etc. as a catalyst, and achieves a higher yield and purity of isopentenol through continuous production in a distillation tower, but the preparation of the catalyst involves spray drying and high-temperature calcination at 700~1000℃, and the preparation process is relatively complicated. In addition, when this type of catalyst is used, metal oxygen-containing acid esters will be generated on the surface, which are easily dissolved by the product into the bottom of the kettle, causing the loss of the catalyst. When the coating layer is consumed to the point where the catalytic activity is reduced or coking is generated during use, it needs to be coated again, and the operation method is cumbersome. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the defect in the prior art that there are few types of catalysts that can be applied to the isomerization process of methylbutenol (2-methyl-3-butene-2-ol) to prepare isopentenol (3-methyl-2-butene-1-ol), and to provide a catalyst, a preparation method of a composite catalyst and application thereof. The catalyst structure of the present invention is completely new, and when the composite catalyst of the present invention is used in the reaction of preparing isopentenol from methylbutenol, the reaction conversion rate and selectivity are better.
[0006] The present invention solves the above technical problems through the following technical solutions.
[0007] The present invention provides a catalyst, which comprises titanium silicon molecular sieve, V2O5 and a metal compound, wherein the titanium silicon molecular sieve is loaded with the V2O5 and the metal compound;
[0008] Wherein, the metal compound is a metal oxide and / or a metal carbonate; the metal in the metal oxide is selected from one or more metal elements in the main group II and the lanthanide series; the metal in the metal carbonate is selected from one or more metal elements in the main group II and the lanthanide series;
[0009] The molar ratio of vanadium in the V2O5 to the metal in the metal compound is (20-50):1; the ratio of the sum of the molar numbers of the metal in the metal compound and the vanadium in the V2O5 to the mass of the titanium silicon molecular sieve is (0.05-2) mol: (0.5-20) kg.
[0010] In the present invention, preferably, the catalyst is a catalyst for methylbutenol and / or methylbutynol.
[0011] Here, the catalyst functions, for example, in the form of an active ingredient.
[0012] In the present invention, preferably, the specific surface area of the titanium silicate molecular sieve is 100-500m 2 / g, for example 380m 2 / g, 214m 2 / g or 486m 2 / g.
[0013] In the present invention, preferably, the silicon-titanium ratio of the titanium silicon molecular sieve is 15-40, such as 30.
[0014] In the present invention, preferably, the structure of the titanium silicalite molecular sieve is MFI, MEL or MWW.
[0015] Wherein, when the structure of the titanium silicalite molecular sieve is MFI, preferably, the model of the titanium silicalite molecular sieve is TS-1.
[0016] Wherein, when the structure of the titanium silicate molecular sieve is MEL, preferably, the model of the titanium silicate molecular sieve is TS-2.
[0017] Wherein, when the structure of the titanium silicate molecular sieve is MWW, preferably, the model of the titanium silicate molecular sieve is Ti-MWW.
[0018] In the present invention, the metal oxide is, for example, MgO and / or La2O3.
[0019] In the present invention, the metal carbonate is, for example, one or more of CaCO3, SrCO3 and BaCO3.
[0020] In the present invention, preferably, the molar ratio of vanadium in the V2O5 to the metal in the metal compound is (20-35):1, for example (33.5:1), (20.6:1) or (20.2:1).
[0021] In the present invention, preferably, the ratio of the sum of the molar numbers of the metal in the metal compound and the vanadium in the V2O5 to the mass of the titanium silicon molecular sieve is (0.01-1) mol: (0.5-20) kg, more preferably, (0.01-1) mol: (0.5-2) kg, for example 0.23 mol: 0.97 kg.
[0022] In a specific embodiment of the present invention, the catalyst is a catalyst of any of the following schemes:
[0023] Scheme 1: The catalyst comprises titanium silicon molecular sieve, V2O5 and MgO, the model of the titanium silicon molecular sieve is TS-1, the titanium silicon molecular sieve is loaded with the V2O5 and the MgO, wherein the molar ratio of V in the V2O5 to Mg in the MgO is 33.5:1; the ratio of the sum of the molar numbers of V in the V2O5 and Mg in the MgO to the mass of the titanium silicon molecular sieve is 0.23 mol:0.97 kg;
[0024] Scheme 2: The catalyst includes titanium silicon molecular sieve, V2O5, MgO and La2O3, the model of the titanium silicon molecular sieve is TS-1, and the titanium silicon molecular sieve is loaded with the V2O5, the MgO and the La2O3, wherein the ratio of the molar number of V in the V2O5 to the sum of the molar numbers of Mg in the MgO and the La in the La2O3 is 20.6:1; the ratio of the sum of the molar numbers of V in the V2O5, the Mg in the MgO and the La in the La2O3 to the mass of the titanium silicon molecular sieve is 0.23 mol:0.97 k;
[0025] Scheme 3: The catalyst includes titanium silicon molecular sieve, V2O5, MgO and La2O3, the model of the titanium silicon molecular sieve is TS-2, and the titanium silicon molecular sieve is loaded with the V2O5, the MgO and the La2O3, wherein the ratio of the molar number of V in the V2O5 to the sum of the molar numbers of Mg in the MgO and the La in the La2O3 is 20.6:1; the ratio of the sum of the molar numbers of V in the V2O5, the Mg in the MgO and the La in the La2O3 to the mass of the titanium silicon molecular sieve is 0.23 mol: 0.97 kg;
[0026] Scheme 4: The catalyst includes titanium silicon molecular sieve, V2O5, MgO and La2O3, the model of the titanium silicon molecular sieve is Ti-MWW, and the titanium silicon molecular sieve is loaded with the V2O5, the MgO and the La2O3, wherein the ratio of the molar number of V in the V2O5 to the sum of the molar numbers of Mg in the MgO and the La in the La2O3 is 20.6:1; the ratio of the sum of the molar numbers of V in the V2O5, the Mg in the MgO and the La in the La2O3 to the mass of the titanium silicon molecular sieve is 0.23 mol: 0.97 kg;
[0027] Scheme 5: The catalyst includes titanium silicon molecular sieve, V2O5, SrCO3 and La2O3, the model of the titanium silicon molecular sieve is TS-1, and the titanium silicon molecular sieve is loaded with the V2O5, the SrCO3 and the La2O3, wherein the ratio of the molar number of V in the V2O5 to the sum of the molar numbers of Sr in the SrCO3 and the La in the La2O3 is 20.6:1; the ratio of the sum of the molar numbers of V in the V2O5, the Sr in the SrCO3 and the La in the La2O3 to the mass of the titanium silicon molecular sieve is 0.23 mol: 0.97 kg;
[0028] Option 6: The catalyst includes titanium silicalite, V2O5, BaCO3 and La2O3, the model of the titanium silicalite is TS-1, and the titanium silicalite is loaded with the V2O5, the BaCO3 and the La2O3, wherein the ratio of the molar number of V in the V2O5 to the sum of the molar numbers of Ba in the BaCO3 and the La in the La2O3 is 20.2:1; the ratio of the sum of the molar numbers of V in the V2O5, the Ba in the BaCO3 and the La in the La2O3 to the mass of the titanium silicalite is 0.23 mol:0.97 kg.
[0029] The present invention also provides a catalyst, the raw materials of which include a mixed solution and titanium silicon molecular sieve;
[0030] The mixed solution comprises water, a soluble metal salt and a soluble vanadium salt, wherein the metal in the soluble metal salt is selected from one or more metals in the main group II and the lanthanide series;
[0031] In the mixed solution, the total molar concentration of the metal cations in the soluble metal salt and the vanadium ions in the soluble vanadium salt is 0.05-2 mol / L;
[0032] In the mixed solution, the molar ratio of vanadium ions in the soluble vanadium salt to metal cations in the soluble metal salt is (20-50):1;
[0033] The mass ratio of the mixed solution to the titanium silicon molecular sieve is 1:(0.5-20).
[0034] In the present invention, preferably, the catalyst is a catalyst for methylbutenol and / or methylbutynol.
[0035] Here, the catalyst functions, for example, in the form of an active ingredient.
[0036] In the present invention, preferably, the raw materials of the catalyst consist of a mixed solution and titanium silicon molecular sieve.
[0037] In the present invention, preferably, the specific surface area of the titanium silicate molecular sieve is 100-500m 2 / g, for example 380m 2 / g, 214m 2 / g or 486m 2 / g.
[0038] In the present invention, preferably, the silicon-titanium ratio of the titanium silicon molecular sieve is 15-40, such as 30.
[0039] In the present invention, preferably, the structure of the titanium silicalite molecular sieve is MFI, MEL or MWW.
[0040] Wherein, when the structure of the titanium silicalite molecular sieve is MFI, preferably, the model of the titanium silicalite molecular sieve is TS-1.
[0041] Wherein, when the structure of the titanium silicate molecular sieve is MEL, preferably, the model of the titanium silicate molecular sieve is TS-2.
[0042] Wherein, when the structure of the titanium silicate molecular sieve is MWW, preferably, the model of the titanium silicate molecular sieve is Ti-MWW.
[0043] In the present invention, the metal of Group II is, for example, one or more of Mg, Ca, Sr and Ba.
[0044] In the present invention, the lanthanide metal is La, for example.
[0045] In the present invention, preferably, the anions in the soluble metal salt are selected from one or more of nitrate ions, acetate ions and chloride ions.
[0046] In the present invention, preferably, the soluble metal salt is selected from one or more of magnesium acetate, lanthanum nitrate, strontium acetate and barium acetate.
[0047] In the present invention, preferably, the anion in the soluble vanadium salt is selected from one or more of oxalate oxide ion, acetylacetonate oxide ion and dichloride oxide ion.
[0048] In the present invention, preferably, the soluble vanadium salt is selected from one or more of vanadyl oxalate, vanadyl acetylacetonate and vanadyl dichloride.
[0049] In the present invention, preferably, the valence state of the vanadium ions in the soluble vanadium salt is +2, +3, +4 or +5.
[0050] In the present invention, preferably, in the mixed solution, the total molar concentration of the metal cations in the soluble metal salt and the vanadium ions in the soluble vanadium salt is 0.1-1 mol / L, for example, 0.23 mol / L.
[0051] In the present invention, preferably, in the mixed solution, the molar ratio of vanadium ions in the soluble vanadium salt to metal cations in the soluble metal salt is (20-35):1, for example (33.5:1), (20.6:1) or (20.2:1).
[0052] In the present invention, preferably, the mass ratio of the mixed solution to the titanium silicon molecular sieve is 1:(0.5-1.5), for example, 1:1.04.
[0053] In the present invention, preferably, the catalyst is prepared according to the following method: drying and calcining a mixture, wherein the mixture comprises the mixed solution and the titanium silicon molecular sieve.
[0054] Preferably, the drying temperature is 60-200°C, such as 80°C or 150°C.
[0055] Preferably, the drying time is 4-48 hours, such as 6 hours or 2 hours.
[0056] Preferably, the calcination temperature is 300-600°C, such as 450°C or 550°C.
[0057] Preferably, the calcination time is 1-5 h, such as 2 h.
[0058] The calcination is performed in a muffle furnace, for example.
[0059] In a specific embodiment of the present invention, the catalyst is a catalyst of any of the following schemes:
[0060] Scheme 1: The raw materials include a mixed solution and titanium silicalite; the mixed solution includes vanadium oxalate and magnesium acetate; in the mixed solution, the total molar concentration of vanadium ions in the vanadium oxalate and magnesium ions in the magnesium acetate is 0.23 mol / L; in the mixed solution, the molar ratio of vanadium ions in the vanadium oxalate and magnesium ions in the magnesium acetate is 33.5:1; the model of the titanium silicalite is TS-1; the mass ratio of the mixed solution to the titanium silicalite is 1:1.04; the raw materials are dried at 80°C for 6 hours, and then calcined at 450°C for 2 hours;
[0061] Scheme 2: Its raw materials include a mixed solution and titanium silicon molecular sieve; the mixed solution includes vanadyl oxalate, magnesium acetate and lanthanum nitrate; in the mixed solution, the total molar concentration of vanadium ions in the vanadyl oxalate, magnesium ions in the magnesium acetate and lanthanum ions in the lanthanum nitrate is 0.23 mol / L; in the mixed solution, the ratio of the molar number of vanadium ions in the vanadyl oxalate to the molar number of magnesium ions in the magnesium acetate and the molar number of lanthanum ions in the lanthanum nitrate is 20.6:1; the model of the titanium silicon molecular sieve is TS-1; the mass ratio of the mixed solution to the titanium silicon molecular sieve is 1:1.04; the raw material is dried at 80°C for 6h, and then calcined at 450°C for 2h;
[0062] Scheme 3: Its raw materials include a mixed solution and titanium silicon molecular sieve; the mixed solution includes vanadyl oxalate, magnesium acetate and lanthanum nitrate; in the mixed solution, the total molar concentration of vanadium ions in the vanadyl oxalate, magnesium ions in the magnesium acetate and lanthanum ions in the lanthanum nitrate is 0.23 mol / L; in the mixed solution, the ratio of the molar number of vanadium ions in the vanadyl oxalate to the molar number of magnesium ions in the magnesium acetate and the molar number of lanthanum ions in the lanthanum nitrate is 20.6:1; the model of the titanium silicon molecular sieve is TS-1; the mass ratio of the mixed solution to the titanium silicon molecular sieve is 1:1.04; the raw materials are dried at 150°C for 2h, and then calcined at 550°C for 2h;
[0063] Scheme 4: Its raw materials include a mixed solution and titanium silicon molecular sieve; the mixed solution includes vanadyl oxalate, magnesium acetate and lanthanum nitrate; in the mixed solution, the total molar concentration of vanadium ions in the vanadyl oxalate, magnesium ions in the magnesium acetate and lanthanum ions in the lanthanum nitrate is 0.23 mol / L; in the mixed solution, the ratio of the molar number of vanadium ions in the vanadyl oxalate to the molar number of magnesium ions in the magnesium acetate and the molar number of lanthanum ions in the lanthanum nitrate is 20.6:1; the model of the titanium silicon molecular sieve is TS-2; the mass ratio of the mixed solution to the titanium silicon molecular sieve is 1:1.04; the raw material is dried at 80°C for 6h, and then calcined at 450°C for 2h;
[0064] Scheme 5: Its raw materials include a mixed solution and titanium silicon molecular sieve; the mixed solution includes vanadyl oxalate, magnesium acetate and lanthanum nitrate; in the mixed solution, the total molar concentration of vanadium ions in the vanadyl oxalate, magnesium ions in the magnesium acetate and lanthanum ions in the lanthanum nitrate is 0.23 mol / L; in the mixed solution, the ratio of the molar number of vanadium ions in the vanadyl oxalate to the molar number of magnesium ions in the magnesium acetate and the molar number of lanthanum ions in the lanthanum nitrate is 20.6:1; the model of the titanium silicon molecular sieve is Ti-MWW; the mass ratio of the mixed solution to the titanium silicon molecular sieve is 1:1.04; the raw materials are dried at 80°C for 6h, and then calcined at 450°C for 2h;
[0065] Scheme 6: Its raw materials include a mixed solution and titanium silicon molecular sieve; the mixed solution includes vanadyl oxalate, strontium acetate and lanthanum nitrate; in the mixed solution, the total molar concentration of vanadium ions in the vanadyl oxalate, strontium ions in the strontium acetate and lanthanum ions in the lanthanum nitrate is 0.23 mol / L; in the mixed solution, the ratio of the molar number of vanadium ions in the vanadyl oxalate to the molar number of strontium ions in the strontium acetate and the molar number of lanthanum ions in the lanthanum nitrate is 20.6:1; the model of the titanium silicon molecular sieve is Ti-MWW; the mass ratio of the mixed solution to the titanium silicon molecular sieve is 1:1.04; the raw materials are dried at 80°C for 6h, and then calcined at 450°C for 2h;
[0066] Scheme 7: The raw materials include a mixed solution and titanium silicalite; the mixed solution includes vanadium oxalate, barium acetate and lanthanum nitrate; in the mixed solution, the total molar concentration of vanadium ions in the vanadium oxalate, barium ions in the barium acetate and lanthanum ions in the lanthanum nitrate is 0.23 mol / L; in the mixed solution, the ratio of the molar number of vanadium ions in the vanadium oxalate to the molar number of barium ions in the barium acetate and the molar number of lanthanum ions in the lanthanum nitrate is 20.6:1; the model of the titanium silicalite is Ti-MWW; the mass ratio of the mixed solution to the titanium silicalite is 1:1.04; the raw materials are dried at 80°C for 6 hours, and then calcined at 450°C for 2 hours.
[0067] The present invention also provides a composite catalyst, the components of which include the catalyst and a carrier as described above.
[0068] In the present invention, preferably, the composite catalyst is a catalyst for methylbutenol and / or methylbutynol.
[0069] In the present invention, the composite catalyst exists in the form of filler, for example.
[0070] In the present invention, preferably, the carrier comprises titanium dioxide.
[0071] In the present invention, preferably, the components further include oxides of metal elements in bentonite, such as silicon dioxide and / or aluminum oxide.
[0072] In the present invention, preferably, the components further include oxides of metal elements in the titanium sol, such as titanium dioxide.
[0073] In the present invention, preferably, the components further include oxides of metal elements in the silica sol, such as silicon dioxide.
[0074] In the present invention, preferably, the composite catalyst is prepared according to the following method, which specifically comprises the following steps:
[0075] a) mixing 10-40 parts of the catalyst, 100 parts of the titanium dioxide, 1-10 parts of a plasticizer, 1-10 parts of a binder and 10-50 parts of water to make mud;
[0076] b) kneading the above mud materials for 10-200 minutes;
[0077] c) sealing and aging the kneaded clay for 5-48 hours;
[0078] d) vacuum slurry the above aged clay for 2-4 times, with the vacuum degree of -0.08~-0.1mPa;
[0079] e) putting the clay material after kneading into an extruder for extrusion molding, and extruding the clay material at an extrusion pressure of 3-8 mPa;
[0080] f) drying the wet embryo after extrusion at a temperature of 100 to 120° C. for a drying time of 5 to 15 hours;
[0081] g) roasting the dried embryo at a temperature of 400-600° C. for 2-6 hours.
[0082] The plasticizer is generally a conventional plasticizer in the art, for example, the plasticizer is a mixture of polyethylene oxide and hydroxypropyl methylcellulose in a mass ratio of 1:1.
[0083] The adhesive is generally a conventional adhesive in the art, for example, the adhesive is a mixture of bentonite and titanium sol in a mass ratio of 1:2.
[0084] The present invention also provides a method for reviving the composite catalyst as described above, and the operation includes soaking in an aqueous solution of an inorganic acid, washing with water until neutrality, and drying.
[0085] In the present invention, the composite catalyst is generally a deactivated composite catalyst, for example, a composite catalyst whose conversion rate drops below 90% when used to catalyze the reaction of preparing isopentenol with methylbutenol as a raw material or preparing isopentenal with methylbutynol as a raw material.
[0086] In the present invention, preferably, the inorganic acid is one or more of sulfuric acid, nitric acid, hydrochloric acid and hydrofluoric acid.
[0087] In the present invention, preferably, the mass fraction of the solute in the aqueous solution of the inorganic acid is greater than 10%, for example 50%.
[0088] In one embodiment of the present invention, the aqueous solution of the inorganic acid is a 50% by mass aqueous solution of sulfuric acid.
[0089] In the present invention, preferably, the amount of the aqueous solution of the inorganic acid used is 1-5 times, for example, 2 times, the weight of the composite catalyst.
[0090] The present invention also provides an application of the above catalyst or the above composite catalyst in the reaction of preparing isopentenol with methylbutynol as a raw material or preparing isopentenal with methylbutynol as a raw material.
[0091] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0092] The reagents and raw materials used in the present invention are commercially available.
[0093] The positive and progressive effects of the present invention are:
[0094] The body of the composite catalyst provided by the present invention has certain mechanical strength, can be processed into filler, has a greater thickness of active components, has a longer service life than coated catalysts, and has a simple method for reviving after the activity decreases.
[0095] The resurrection method of the composite catalyst provided by the present invention only requires immersion in inorganic acid to corrode the surface of the deactivated catalyst, so that the surface deactivated catalyst is peeled off, and then washed with water to neutrality and dried to restore the activity of the composite catalyst without re-coating or molding. DETAILED DESCRIPTION
[0096] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0097] The raw material information involved in the examples and comparative examples of the present invention is shown in Table 1:
[0098] Table 1
[0099]
[0100] Example 1
[0101] Weigh 30.99g of vanadyl oxalate and 0.85g of magnesium acetate and dissolve them in 900g of water to prepare a mixed solution. The silicon-titanium ratio is 30 and the specific surface area is 380m 2 / g titanium silicalite molecular sieve (model TS-1), the mixed solution was impregnated onto 970g TS-1 by equal volume impregnation method, and the obtained solid was dried at 80°C for 6h. The dried powder was placed in a muffle furnace and calcined at 450°C for 2h to obtain catalyst A.
[0102] Among them, vanadyl oxalate is converted into V2O5, magnesium acetate is converted into MgO, and catalyst A is a titanium silicon molecular sieve loaded with V2O5 and MgO.
[0103] Example 2
[0104] Weigh 30.99g of vanadyl oxalate, 0.85g of magnesium acetate and 1.62g of lanthanum nitrate and dissolve them in 900g of water to prepare a mixed solution. The silicon-titanium ratio is 30 and the specific surface area is 380m 2 / g titanium silicalite molecular sieve (model TS-1), the mixed solution was impregnated onto 970g TS-1 by equal volume impregnation method, and the obtained solid was dried at 80°C for 6h. The dried powder was placed in a muffle furnace and calcined at 450°C for 2h to obtain catalyst B.
[0105] Among them, vanadyl oxalate is converted into V2O5, magnesium acetate is converted into MgO, and lanthanum nitrate is converted into La2O3. Catalyst B is a titanium silicon molecular sieve loaded with V2O5, MgO and La2O3.
[0106] Example 3
[0107] Weigh 30.99g of vanadyl oxalate, 0.85g of magnesium acetate and 1.62g of lanthanum nitrate and dissolve them in 900g of water to prepare a mixed solution. The silicon-titanium ratio is 30 and the specific surface area is 380m 2 / g titanium silicalite molecular sieve (model TS-1), the mixed solution was impregnated onto 970g TS-1 by equal volume impregnation method, and the obtained solid was dried at 150°C for 2h. The dried powder was placed in a muffle furnace and calcined at 550°C for 2h to obtain catalyst C.
[0108] Among them, vanadyl oxalate is converted into V2O5, magnesium acetate is converted into MgO, and lanthanum nitrate is converted into La2O3. Catalyst C is a titanium silicalite molecular sieve loaded with V2O5, MgO and La2O3.
[0109] Example 4
[0110] Weigh 30.99g of vanadyl oxalate, 0.85g of magnesium acetate and 1.62g of lanthanum nitrate and dissolve them in 900g of water to prepare a mixed solution. The silicon-titanium ratio is 30 and the specific surface area is 214m 2 / g titanium silicalite molecular sieve (model TS-2), the mixed solution was impregnated onto 970g TS-2 by equal volume impregnation method, and the obtained solid was dried at 80°C for 6h. The dried powder was placed in a muffle furnace and calcined at 450°C for 2h to obtain catalyst D.
[0111] Among them, vanadyl oxalate is converted into V2O5, magnesium acetate is converted into MgO, and lanthanum nitrate is converted into La2O3. Catalyst D is a titanium silicon molecular sieve loaded with V2O5, MgO and La2O3.
[0112] Example 5
[0113] Weigh 30.99g of vanadyl oxalate, 0.85g of magnesium acetate and 1.62g of lanthanum nitrate and dissolve them in 900g of water to prepare a mixed solution. The silicon-titanium ratio is 30 and the specific surface area is 486m 2 / g titanium silicon molecular sieve (model: Ti-MWW), the mixed solution was impregnated onto 970g Ti-MWW by equal volume impregnation method, and the obtained solid was dried at 80°C for 6h. The dried powder was placed in a muffle furnace and calcined at 450°C for 2h to obtain catalyst E.
[0114] Among them, vanadyl oxalate is converted into V2O5, magnesium acetate is converted into MgO, and lanthanum nitrate is converted into La2O3. Catalyst E is a titanium silicalite molecular sieve loaded with V2O5, MgO and La2O3.
[0115] Example 6
[0116] Weigh 30.99g of vanadyl oxalate, 1.23g of strontium acetate and 1.62g of lanthanum nitrate and dissolve them in 900g of water to prepare a mixed solution. The silicon-titanium ratio is 30 and the specific surface area is 380m 2 / g titanium silicalite molecular sieve (model TS-1), the mixed solution was impregnated onto 970g TS-1 by equal volume impregnation method, and the obtained solid was dried at 80°C for 6h. The dried powder was placed in a muffle furnace and calcined at 450°C for 2h to obtain catalyst F.
[0117] Among them, vanadyl oxalate is converted into V2O5, strontium acetate is converted into SrCO3, and lanthanum nitrate is converted into La2O3. Catalyst F is a titanium silicon molecular sieve loaded with V2O5, SrCO3 and La2O3.
[0118] Example 7
[0119] Weigh 30.99g of vanadyl oxalate, 1.57g of barium acetate and 1.62g of lanthanum nitrate and dissolve them in 900g of water to prepare a mixed solution. The silicon-titanium ratio is 30 and the specific surface area is 380m 2 / g titanium silicalite molecular sieve (model TS-1), the mixed solution was impregnated onto 970g TS-1 by equal volume impregnation method, and the obtained solid was dried at 80°C for 6h. The dried powder was placed in a muffle furnace and calcined at 450°C for 2h to obtain catalyst G.
[0120] Among them, vanadyl oxalate is converted into V2O5, barium acetate is converted into BaCO3, and lanthanum nitrate is converted into La2O3. Catalyst G is a titanium silicon molecular sieve loaded with V2O5, BaCO3 and La2O3.
[0121] Example 8
[0122] Take 1000g of catalyst A, 5000g of titanium dioxide, 250g of plasticizer (a mixture of polyethylene oxide and hydroxypropyl methylcellulose in a mass ratio of 1:1), 400g of binder (a mixture of bentonite and titanium sol in a mass ratio of 1:2), and 1500g of water, mix and make mud, knead for 60min and seal and age for 24h. The aged mud is smelted twice at -0.1mPa. The smelted mud is put into an extruder for molding, and the molding pressure is 5mPa. The wet embryo is dried at 100°C for 2h and then calcined at 450°C for 2h to obtain a composite catalyst, which is recorded as filler 1.
[0123] Example 9
[0124] The catalyst A in Example 8 is replaced by catalyst B, and the obtained composite catalyst is filler 2.
[0125] Example 10
[0126] The catalyst A in Example 8 is replaced by catalyst C, and the obtained composite catalyst is filler three.
[0127] Embodiment 11
[0128] The catalyst A in Example 8 is replaced by catalyst D, and the resulting composite catalyst is filler four.
[0129] Example 12
[0130] The catalyst A in Example 8 was replaced by catalyst E, and the obtained composite catalyst was filler five.
[0131] Embodiment 13
[0132] The catalyst A in Example 8 was replaced by catalyst F, and the obtained composite catalyst was filler six.
[0133] Embodiment 14
[0134] The catalyst A in Example 8 is replaced by catalyst G, and the obtained composite catalyst is filler seven.
[0135] Comparative Example 1
[0136] The operation method is the same as that of Example 8, except that catalyst A is not added when preparing the composite catalyst. The composite catalyst prepared in this way is comparative filler 1.
[0137] Comparative Example 2
[0138] The operation method is the same as that of Example 8, except that the catalyst is different. The preparation method of the catalyst is the same as the preparation method of catalyst A in Example 1 except that "no titanium silicon molecular sieve TS-1 is added". In addition, the composite catalyst is prepared in full accordance with the method of Example 8 to obtain comparative filler 2.
[0139] Comparative Example 3
[0140] The operation method is the same as that of Example 8, except that the catalyst is different. The preparation method of the catalyst is the same as the preparation method of catalyst A in Example 1 except that "no vanadyl oxalate is added". In addition, the composite catalyst is prepared in full accordance with the method of Example 9 to obtain comparative filler 3.
[0141] Comparative Example 4
[0142] The operation mode is the same as that of Example 8, except that the catalyst is different. The preparation method of the catalyst is the same as that of the preparation method of catalyst A in Example 1 except that the amount of vanadyl oxalate added is different, that is, "the amount of vanadyl oxalate added is 3.1 g" in this comparative example. In addition, the composite catalyst is prepared in full accordance with the method of Example 9 to obtain comparative filler 4.
[0143] Embodiment 15
[0144] Take 100g of catalyst A, 500g of titanium dioxide, 25g of binder (a mixture of bentonite and titanium sol in a mass ratio of 1:2), 16g of plasticizer (a mixture of polyethylene oxide and hydroxypropyl methylcellulose in a mass ratio of 1:1), and 1300g of water to mix to make a slurry. The slurry is coated on a cordierite honeycomb carrier, and the coating amount is 170 g / L (wherein, "g / L" refers to the mass of the coated slurry on each liter of the cordierite honeycomb carrier in g). After the coated cordierite carrier is dried at 100°C for 2h, it is calcined at 450°C for 2h to obtain a composite catalyst, which is recorded as comparative filler 5.
[0145] Effect Example 1
[0146] The fillers prepared in Examples 8 to 15 and Comparative Examples 1 to 4 were used to catalyze the reaction of preparing 3-methyl-2-butene-1-ol (isoprenol) from 2-methyl-3-butene-2-ol (methylbutenol). They were respectively filled into the reaction section of a distillation tower according to a theoretical plate number of 12. In the separation section under the reaction section, ordinary ceramic corrugated plate fillers with a theoretical plate number of 30 were filled. The reaction temperature in the distillation tower was controlled to be 150-155° C., the reaction pressure was 0.04-0.06 MPa, the tower top condensation temperature was 80° C., and isopentenol was started to be produced after 3 hours of equilibrium. The results are shown in Table 2.
[0147] Table 2
[0148]
[0149] As can be seen from Table 2, the catalysts prepared by Examples 1-7 of the present invention, and then the composite catalysts prepared by Examples 8-15, respectively, are used to catalyze the reaction of preparing 3-methyl-2-butene-1-ol (isopentenol) from 2-methyl-3-butene-2-ol (methylbutenol). Compared with the composite catalysts prepared by Comparative Examples 1 to 4, the conversion rate of methylbutenol is higher and the selectivity of the obtained isopentenol is also higher.
[0150] Example 16
[0151] The composite catalyst obtained in Example 8, i.e. filler one, is used to catalyze the reaction of preparing isopentenol from methylbutenol. After the conversion rate drops below 90%, the filler is taken out and soaked in 50% sulfuric acid with a mass fraction of twice the weight of the filler for 1 hour. The filler is fished out and washed with water until the pH value of the washing liquid is 6.8-7. After drying at 100°C for 2 hours, the revived filler one is obtained.
[0152] Comparative Example 5
[0153] The operation is the same as in Example 16, except that the acid used for soaking the filler is formic acid, and the filler is revived as compared to Example 16.
[0154] Comparative Example 6
[0155] The operation is the same as that of Example 16, except that the acid used for soaking the filler is 10% by mass hydrochloric acid, and a comparative resurrection filler 2 is obtained.
[0156] Comparative Example 7
[0157] The operation is the same as in Example 16, except that the amount of acid used to soak the filler is 0.5 times the weight of the filler, and a comparative resurrection filler three is obtained.
[0158] Comparative Example 8
[0159] The operation is the same as that of Example 16, except that after the soaking, the filler is washed with water until the pH value is 3-4, thereby obtaining a comparative resurrection filler 4.
[0160] Embodiment 17
[0161] The composite catalyst obtained in Example 15, i.e., comparative filler 6, was used to catalyze the reaction of preparing isopentenol from methylbutenol. After the conversion rate dropped below 90%, the filler was taken out and soaked in 50% sulfuric acid with a mass fraction of twice the weight of the filler for 1 hour. The filler was fished out and washed with water until the pH value of the washing liquid was 6.8-7. After drying at 100°C for 2 hours, the revived filler 5 was obtained.
[0162] Effect Example 2
[0163] The fillers prepared in Examples 16-17 and Comparative Examples 5-8 were used to catalyze the reaction of preparing 3-methyl-2-butene-1-ol (isoprenol) from 2-methyl-3-butene-2-ol (methylbutenol). They were respectively filled into the reaction section of a distillation tower according to a theoretical plate number of 12. In the separation section under the reaction section, ordinary ceramic corrugated plate fillers with a theoretical plate number of 30 were filled. The reaction temperature in the distillation tower was controlled to be 150-155°C, the reaction pressure to be 0.04-0.06MPa, the tower top condensation temperature to be 80°C, and isopentenol was started to be produced after 3 hours of equilibrium. The results are shown in Table 3.
[0164] Table 3
[0165]
[0166] As shown in Table 3, according to the resurrection method of Example 16 of the present invention, the composite catalyst after the conversion rate is reduced to below 90% is resurrected, and the resurrection filler 1 obtained is used to catalyze the reaction of preparing 3-methyl-2-butene-1-ol (isopentenol) from 2-methyl-3-butene-2-ol (methylbutenol). The conversion rate of methylbutenol is still high, higher than 98%, and the selectivity of the obtained isopentenol is also high, higher than 99%. When the comparative resurrection fillers 1, 2, 3, and 4 obtained by the resurrection method of Comparative Examples 5-8 are used to catalyze the reaction of preparing 3-methyl-2-butene-1-ol (isopentenol) from 2-methyl-3-butene-2-ol (methylbutenol), the conversion rate of methylbutenol is significantly lower than 92%, and the selectivity of the obtained isopentenol is significantly lower than 96.5%. Example 17, the composite catalyst (catalyst coated on a cordierite honeycomb carrier) after the conversion rate is reduced to below 90%, that is, the comparative filler 6, and the resurrected filler 5 obtained by the resurrection method of Example 16 of the present invention, the conversion rate of methyl butenol and the selectivity of the obtained isopentenol are both lower than 10%.
Claims
1. A catalyst, characterized in that It includes titanium silicon molecular sieve, V2O5 and metal compound, and the titanium silicon molecular sieve is loaded with the V2O5 and the metal compound; Wherein, the metal compound is a metal oxide and / or a metal carbonate; the metal in the metal oxide is selected from one or more metal elements in the main group II and the lanthanide series; the metal in the metal carbonate is selected from one or more metal elements in the main group II and the lanthanide series; The molar ratio of vanadium in the V2O5 to the metal in the metal compound is (20-50):1; the ratio of the sum of the molar numbers of the metal in the metal compound and the vanadium in the V2O5 to the mass of the titanium silicon molecular sieve is (0.05-2) mol: (0.5-20) kg.
2. The catalyst according to claim 1, characterized in that It meets one or more of the following conditions: (1) The catalyst is a catalyst for methylbutenol and / or methylbutynol; wherein the catalyst acts, for example, in the form of an active ingredient; (2) The specific surface area of the titanium silicate molecular sieve is 100-500m 2 / g, for example 380m 2 / g, 214m 2 / g or 486m 2 / g; (3) The silicon-titanium ratio of the titanium silicon molecular sieve is 15-40, for example 30; (4) The structure of the titanium silicalite molecular sieve is MFI, MEL or MWW; Wherein, when the structure of the titanium silicalite molecular sieve is MFI, preferably, the model of the titanium silicalite molecular sieve is TS-1; Wherein, when the structure of the titanium silicalite molecular sieve is MEL, preferably, the model of the titanium silicalite molecular sieve is TS-2; Wherein, when the structure of the titanium silicon molecular sieve is MWW, preferably, the model of the titanium silicon molecular sieve is Ti-MWW; (5) The metal oxide is MgO and / or La2O3; (6) The metal carbonate is one or more of CaCO3, SrCO3 and BaCO3; (7) The molar ratio of vanadium in the V2O5 to the metal in the metal compound is (20-35):1, for example (33.5:1), (20.6:1) or (20.2:1); (8) The ratio of the sum of the molar numbers of the metal in the metal compound and the vanadium in the V2O5 to the mass of the titanium silicon molecular sieve is (0.01-1) mol: (0.5-20) kg, more preferably, (0.01-1) mol: (0.5-2) kg, for example 0.23 mol: 0.97 kg.
3. The catalyst according to claim 1, characterized in that The catalyst is any one of the following catalysts: Scheme 1: The catalyst comprises titanium silicon molecular sieve, V2O5 and MgO, the model of the titanium silicon molecular sieve is TS-1, the titanium silicon molecular sieve is loaded with the V2O5 and the MgO, wherein the molar ratio of V in the V2O5 to Mg in the MgO is 33.5:1; the ratio of the sum of the molar numbers of V in the V2O5 and Mg in the MgO to the mass of the titanium silicon molecular sieve is 0.23 mol:0.97 kg; Scheme 2: The catalyst includes titanium silicon molecular sieve, V2O5, MgO and La2O3, the model of the titanium silicon molecular sieve is TS-1, and the titanium silicon molecular sieve is loaded with the V2O5, the MgO and the La2O3, wherein the ratio of the molar number of V in the V2O5 to the sum of the molar numbers of Mg in the MgO and the La in the La2O3 is 20.6:1; the ratio of the sum of the molar numbers of V in the V2O5, the Mg in the MgO and the La in the La2O3 to the mass of the titanium silicon molecular sieve is 0.23 mol:0.97 k; Scheme 3: The catalyst includes titanium silicon molecular sieve, V2O5, MgO and La2O3, the model of the titanium silicon molecular sieve is TS-2, and the titanium silicon molecular sieve is loaded with the V2O5, the MgO and the La2O3, wherein the ratio of the molar number of V in the V2O5 to the sum of the molar numbers of Mg in the MgO and the La in the La2O3 is 20.6:1; the ratio of the sum of the molar numbers of V in the V2O5, the Mg in the MgO and the La in the La2O3 to the mass of the titanium silicon molecular sieve is 0.23 mol: 0.97 kg; Scheme 4: The catalyst includes titanium silicon molecular sieve, V2O5, MgO and La2O3, the model of the titanium silicon molecular sieve is Ti-MWW, and the titanium silicon molecular sieve is loaded with the V2O5, the MgO and the La2O3, wherein the ratio of the molar number of V in the V2O5 to the sum of the molar numbers of Mg in the MgO and the La in the La2O3 is 20.6:1; the ratio of the sum of the molar numbers of V in the V2O5, the Mg in the MgO and the La in the La2O3 to the mass of the titanium silicon molecular sieve is 0.23 mol: 0.97 kg; Scheme 5: The catalyst includes titanium silicon molecular sieve, V2O5, SrCO3 and La2O3, the model of the titanium silicon molecular sieve is TS-1, and the titanium silicon molecular sieve is loaded with the V2O5, the SrCO3 and the La2O3, wherein the ratio of the molar number of V in the V2O5 to the sum of the molar numbers of Sr in the SrCO3 and the La in the La2O3 is 20.6:1; the ratio of the sum of the molar numbers of V in the V2O5, the Sr in the SrCO3 and the La in the La2O3 to the mass of the titanium silicon molecular sieve is 0.23 mol: 0.97 kg; Option 6: The catalyst includes titanium silicalite, V2O5, BaCO3 and La2O3, the model of the titanium silicalite is TS-1, and the titanium silicalite is loaded with the V2O5, the BaCO3 and the La2O3, wherein the ratio of the molar number of V in the V2O5 to the sum of the molar numbers of Ba in the BaCO3 and the La in the La2O3 is 20.2:1; the ratio of the sum of the molar numbers of V in the V2O5, the Ba in the BaCO3 and the La in the La2O3 to the mass of the titanium silicalite is 0.23 mol:0.97 kg.
4. A catalyst, characterized in that Its raw materials include mixed solution and titanium silicon molecular sieve; The mixed solution comprises water, a soluble metal salt and a soluble vanadium salt, wherein the metal in the soluble metal salt is selected from one or more metals in the main group II and the lanthanide series; In the mixed solution, the total molar concentration of the metal cations in the soluble metal salt and the vanadium ions in the soluble vanadium salt is 0.05-2 mol / L; In the mixed solution, the molar ratio of vanadium ions in the soluble vanadium salt to metal cations in the soluble metal salt is (20-50):1; The mass ratio of the mixed solution to the titanium silicon molecular sieve is 1:(0.5-20).
5. The catalyst according to claim 4, characterized in that It meets one or more of the following conditions: (1) The catalyst is a catalyst for methylbutenol and / or methylbutynol; wherein the catalyst acts, for example, in the form of an active ingredient; (2) The raw materials of the catalyst are composed of a mixed solution and titanium silicon molecular sieve; (3) The specific surface area of the titanium silicate molecular sieve is 100-500m 2 / g, for example 380m 2 / g, 214m 2 / g or 486m 2 / g; (4) The silicon-titanium ratio of the titanium silicon molecular sieve is 15-40, for example 30; (5) The structure of the titanium silicalite molecular sieve is MFI, MEL or MWW; Wherein, when the structure of the titanium silicalite molecular sieve is MFI, preferably, the model of the titanium silicalite molecular sieve is TS-1; Wherein, when the structure of the titanium silicalite molecular sieve is MEL, preferably, the model of the titanium silicalite molecular sieve is TS-2; Wherein, when the structure of the titanium silicon molecular sieve is MWW, preferably, the model of the titanium silicon molecular sieve is Ti-MWW; (6) The metal of Group II is one or more of Mg, Ca, Sr and Ba; (7) The lanthanide metal is La; (8) The anions in the soluble metal salt are selected from one or more of nitrate ions, acetate ions and chloride ions; (9) The soluble metal salt is selected from one or more of magnesium acetate, lanthanum nitrate, strontium acetate and barium acetate; (10) The anion in the soluble vanadium salt is selected from one or more of oxalate oxide ion, acetylacetonate oxide ion and dichloride oxide ion; (11) The soluble vanadium salt is selected from one or more of vanadyl oxalate, vanadyl acetylacetonate and vanadyl dichloride; (12) The valence state of the vanadium ion in the soluble vanadium salt is +2, +3, +4 or +5; (13) In the mixed solution, the total molar concentration of the metal cations in the soluble metal salt and the vanadium ions in the soluble vanadium salt is 0.1-1 mol / L, for example, 0.23 mol / L; (14) In the mixed solution, the molar ratio of vanadium ions in the soluble vanadium salt to metal cations in the soluble metal salt is (20-35):1, for example (33.5:1), (20.6:1) or (20.2:1); (15) The mass ratio of the mixed solution to the titanium silicalite molecular sieve is 1:(0.5-1.5), for example, 1:1.04; (16) The catalyst is prepared by the following method: drying and calcining a mixture, wherein the mixture comprises the mixed solution and the titanium silicon molecular sieve; Preferably, the drying temperature is 60-200°C, such as 80°C or 150°C; Preferably, the drying time is 4-48 hours, for example 6 hours or 2 hours; Preferably, the calcination temperature is 300-600°C, such as 450°C or 550°C; Preferably, the calcination time is 1-5 h, such as 2 h.
6. The catalyst according to claim 4, characterized in that The catalyst is any one of the following catalysts: Scheme 1: The raw materials include a mixed solution and titanium silicalite; the mixed solution includes vanadium oxalate and magnesium acetate; in the mixed solution, the total molar concentration of vanadium ions in the vanadium oxalate and magnesium ions in the magnesium acetate is 0.23 mol / L; in the mixed solution, the molar ratio of vanadium ions in the vanadium oxalate and magnesium ions in the magnesium acetate is 33.5:1; the model of the titanium silicalite is TS-1; the mass ratio of the mixed solution to the titanium silicalite is 1:1.04; the raw materials are dried at 80°C for 6 hours, and then calcined at 450°C for 2 hours; Scheme 2: Its raw materials include a mixed solution and titanium silicon molecular sieve; the mixed solution includes vanadyl oxalate, magnesium acetate and lanthanum nitrate; in the mixed solution, the total molar concentration of vanadium ions in the vanadyl oxalate, magnesium ions in the magnesium acetate and lanthanum ions in the lanthanum nitrate is 0.23 mol / L; in the mixed solution, the ratio of the molar number of vanadium ions in the vanadyl oxalate to the molar number of magnesium ions in the magnesium acetate and the molar number of lanthanum ions in the lanthanum nitrate is 20.6:1; the model of the titanium silicon molecular sieve is TS-1; the mass ratio of the mixed solution to the titanium silicon molecular sieve is 1:1.04; the raw material is dried at 80°C for 6h, and then calcined at 450°C for 2h; Scheme 3: Its raw materials include a mixed solution and titanium silicon molecular sieve; the mixed solution includes vanadyl oxalate, magnesium acetate and lanthanum nitrate; in the mixed solution, the total molar concentration of vanadium ions in the vanadyl oxalate, magnesium ions in the magnesium acetate and lanthanum ions in the lanthanum nitrate is 0.23 mol / L; in the mixed solution, the ratio of the molar number of vanadium ions in the vanadyl oxalate to the molar number of magnesium ions in the magnesium acetate and the molar number of lanthanum ions in the lanthanum nitrate is 20.6:1; the model of the titanium silicon molecular sieve is TS-1; the mass ratio of the mixed solution to the titanium silicon molecular sieve is 1:1.04; the raw materials are dried at 150°C for 2h, and then calcined at 550°C for 2h; Scheme 4: Its raw materials include a mixed solution and titanium silicon molecular sieve; the mixed solution includes vanadyl oxalate, magnesium acetate and lanthanum nitrate; in the mixed solution, the total molar concentration of vanadium ions in the vanadyl oxalate, magnesium ions in the magnesium acetate and lanthanum ions in the lanthanum nitrate is 0.23 mol / L; in the mixed solution, the ratio of the molar number of vanadium ions in the vanadyl oxalate to the molar number of magnesium ions in the magnesium acetate and the molar number of lanthanum ions in the lanthanum nitrate is 20.6:1; the model of the titanium silicon molecular sieve is TS-2; the mass ratio of the mixed solution to the titanium silicon molecular sieve is 1:1.04; the raw material is dried at 80°C for 6h, and then calcined at 450°C for 2h; Scheme 5: Its raw materials include a mixed solution and titanium silicon molecular sieve; the mixed solution includes vanadyl oxalate, magnesium acetate and lanthanum nitrate; in the mixed solution, the total molar concentration of vanadium ions in the vanadyl oxalate, magnesium ions in the magnesium acetate and lanthanum ions in the lanthanum nitrate is 0.23 mol / L; in the mixed solution, the ratio of the molar number of vanadium ions in the vanadyl oxalate to the molar number of magnesium ions in the magnesium acetate and the molar number of lanthanum ions in the lanthanum nitrate is 20.6:1; the model of the titanium silicon molecular sieve is Ti-MWW; the mass ratio of the mixed solution to the titanium silicon molecular sieve is 1:1.04; the raw materials are dried at 80°C for 6h, and then calcined at 450°C for 2h; Scheme 6: Its raw materials include a mixed solution and titanium silicon molecular sieve; the mixed solution includes vanadyl oxalate, strontium acetate and lanthanum nitrate; in the mixed solution, the total molar concentration of vanadium ions in the vanadyl oxalate, strontium ions in the strontium acetate and lanthanum ions in the lanthanum nitrate is 0.23 mol / L; in the mixed solution, the ratio of the molar number of vanadium ions in the vanadyl oxalate to the molar number of strontium ions in the strontium acetate and the molar number of lanthanum ions in the lanthanum nitrate is 20.6:1; the model of the titanium silicon molecular sieve is Ti-MWW; the mass ratio of the mixed solution to the titanium silicon molecular sieve is 1:1.04; the raw materials are dried at 80°C for 6h, and then calcined at 450°C for 2h; Scheme 7: The raw materials include a mixed solution and titanium silicalite; the mixed solution includes vanadium oxalate, barium acetate and lanthanum nitrate; in the mixed solution, the total molar concentration of vanadium ions in the vanadium oxalate, barium ions in the barium acetate and lanthanum ions in the lanthanum nitrate is 0.23 mol / L; in the mixed solution, the ratio of the molar number of vanadium ions in the vanadium oxalate to the molar number of barium ions in the barium acetate and the molar number of lanthanum ions in the lanthanum nitrate is 20.6:1; the model of the titanium silicalite is Ti-MWW; the mass ratio of the mixed solution to the titanium silicalite is 1:1.04; the raw materials are dried at 80°C for 6 hours, and then calcined at 450°C for 2 hours.
7. A composite catalyst, characterized in that Its components include the catalyst and carrier as described in any one of claims 1 to 6.
8. The composite catalyst according to claim 7, characterized in that It meets one or more of the following conditions: (1) The composite catalyst is a catalyst for methylbutenol and / or methylbutynol; (2) The composite catalyst is in the form of filler; (3) The carrier comprises titanium dioxide; (4) The components also include oxides of metal elements in bentonite, such as silicon dioxide and / or aluminum oxide; (5) The components also include oxides of metal elements in the titanium sol, such as titanium dioxide; (6) The components also include oxides of metal elements in the silica sol, such as silicon dioxide.
9. A method for resurrecting a composite catalyst as claimed in any one of claims 7 to 8, characterized in that: The operation includes soaking with an aqueous solution of an inorganic acid, washing with water until neutral and drying; Preferably, the inorganic acid is one or more of sulfuric acid, nitric acid, hydrochloric acid and hydrofluoric acid; Preferably, the mass fraction of the solute in the aqueous solution of the inorganic acid is greater than 10%, for example, 50%; Preferably, the amount of the aqueous solution of the inorganic acid is 1-5 times, for example, 2 times, the weight of the composite catalyst.
10. Use of the catalyst according to any one of claims 1 to 6 or the composite catalyst according to any one of claims 7 to 8 in the reaction of preparing isopentenol from methylbutenol as a raw material or preparing isopentenal from methylbutynol as a raw material.