Online repairing method for belt conveyor roller
Through the online repair method, the complex disassembly and replacement process of belt conveyor drum after wear is solved, local repair of the drum is achieved, production downtime and spare parts requirements are reduced, and management efficiency and safety are improved.
Patent Information
- Application Number
- CN202411418472.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-11-29
AI Technical Summary
The existing belt conveyor drum needs to be replaced after wear, resulting in bulky and difficult disassembly, reverse transportation, lifting and replacement processes, causing production shutdowns and safety hazards, and inconvenient spare parts management, resulting in high failure rate and difficult inventory management.
By using the online repair method, the area to be repaired on the surface of the drum is analyzed, divided into arc surfaces along the axial direction, cleaned and polished, coated belt glue, bonded and pounded to repair, local repair of the drum surface is achieved, and disassembled and replaced. process.
It realizes online maintenance of rollers, reduces production downtime, reduces spare parts demand, improves construction site management efficiency, reduces safety hazards, and is suitable for the repair of a variety of shaft-shaped equipment.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of belt conveyor roller repair, and relates to an online repair method for a belt conveyor roller. Background Art
[0002] The belt conveyor has many rollers, such as the head and tail rollers, redirecting rollers, tensioning rollers, counterweight rollers, etc. These rollers have different functions, but the common feature is that the surfaces of these rollers are in direct contact with the belts. The belt needs to transport minerals and needs to rotate. With the occurrence of rolling friction, the wear-resistant rubber layer on the surface of the roller will be worn; in this case, a better roller is needed, otherwise further wear will cause the surface iron layer inside the roller to be damaged. If the iron layer is broken, the roller will in turn damage the conveyor belt, causing the conveyor belt to be torn or damaged.
[0003] When the wear-resistant rubber layer on the surface of the drum is worn, it is necessary to organize relevant personnel to replace the drum of the belt conveyor. The usual replacement method is to transport the same drum spare parts that can replace the damaged drum to the vicinity of the replaced drum one day in advance. Since the belt conveyor is generally inside the belt corridor of the factory, there is generally no crane or electric hoist inside; since the drum is heavy, taking the redirection drum with a diameter of 400mm and a length of 1200mm as an example, at least 4-6 maintenance personnel are required to replace the drum. With the help of the corresponding hand hoist, the fixing bolts on the left and right sides of the damaged drum are first removed, and then a hoist is used to lift a part of the loosened conveyor belt, and the damaged drum is lifted out with other hoists (this process is difficult to operate, limited by space, limited by the weight of the replaced drum, and limited by the strength of the personnel). Then install the prepared drum again. The process of replacing the redirection drum, including the advance preparation work, takes about 14 hours. During these 14 hours, the machine cannot be started for production, because generally mines do not have spare belt conveyors for belts, and basically the mid-transport belts are unique. The disassembled rollers need to be transported back, and then the damaged rollers need to be returned to the factory for lagging repair. Summary of the invention
[0004] The present application provides an online repair method for a belt conveyor roller, which is a method for realizing online repair when the surfaces of various rollers of the belt conveyor or the surfaces of shaft-shaped parts are worn.
[0005] In order to achieve the above technical purpose, the technical solution adopted by the present application is: an online repair method for a belt conveyor roller, comprising the following steps:
[0006] Analyze the area to be repaired on the drum surface, and divide the drum surface along the axial direction, the division method is: each division surface is an arc surface, the corresponding angle is 45 degrees to 90 degrees, and the length of each division surface is equal to the length of the drum; the area to be repaired on the drum surface exists in one of the division surfaces or multiple division surfaces;
[0007] Clean the area on the drum surface to be repaired;
[0008] Apply conveyor belt glue to the area to be repaired on the surface of the roller, and cover the area to be repaired with a surface for repair;
[0009] Hammering the bonding surface between the surface to be repaired and the area to be repaired on the drum surface;
[0010] Repeat the above process to complete the repair of all the areas to be repaired on the drum surface.
[0011] As an improved technical solution of the present application, cleaning the area on the drum surface to be repaired includes: polishing the area on the drum surface to be repaired, and cleaning the area on the drum surface to be repaired with a non-aqueous cleaning agent.
[0012] As an improved technical solution of the present application, coating the conveyor belt glue on the area to be repaired on the surface of the roller includes first applying a first layer of conveyor belt glue and thinning it to 0.1±0.025mm with a scraper, and then baking it so that the first layer of conveyor belt glue is 65%-80% dry; applying a second layer of conveyor belt glue and thinning it again to 0.1±0.025mm, and baking it so that the second layer of conveyor belt glue is 65%-80% dry.
[0013] As an improved technical solution of the present application, each repair process includes standing still after completion, and each standing still time is no less than 40 minutes.
[0014] As an improved technical solution of the present application, the bonding surface between the surface to be repaired and the area to be repaired on the drum surface is hammered to control the drying degree of the conveyor belt glue to be within 95%.
[0015] Beneficial Effects
[0016] The repair method of the present application can perform online repairs without removing the roller on the belt conveyor, which not only solves the problems of the roller being heavy and difficult to disassemble, transport, hoist, and replace, but also facilitates direct repairs during the construction process. Repairing directly on the belt conveyor can effectively avoid long-term shutdowns of a process or a system, and can effectively reduce costs and increase efficiency for the enterprise. At the same time, the repair method can perform intermittent repairs, shutting down the machine for repairs during peak hours every day, and then performing repairs in small quantities and multiple times. However, the repairs need to be done in advance to reduce the need for maintenance personnel to work for a long time in the event of a problem, thereby reducing safety hazards.
[0017] After the repair method is properly utilized, rollers with low failure rates can be left as spares or with fewer spares. This effectively solves the problem of spare parts quantity and inventory, thereby achieving further improvement in construction site management.
[0018] Through online partial repair, we can reasonably utilize the principle of repairing the old and reusing the waste, and make rational use of many replaced or excess belt top layers.
[0019] In summary, the online repair method of the present application has a wide range of applications and can be applied to the online maintenance of roller-shaped or shaft-shaped equipment. For example, the side surface of a roller, that is, a cylinder, can be repaired by this method for other spare parts or equipment, such as round shafts, square shafts, or other planes, thereby achieving surface treatment. DETAILED DESCRIPTION
[0020] The technical solution of the present application is described in detail below in conjunction with embodiments.
[0021] The drum is heavy and inconvenient to replace, and it is also inconvenient to transport spare parts up and down. The drum replaced by the user needs to be returned to the factory for repair with rubber. Depending on the size of the drum, the repair cost is high. At the same time, if the drum is damaged and needs to be replaced, it will cause at least 12 hours of shutdown of at least one system. In addition, since the drum to be handled is heavy, there are certain safety hazards during maintenance and treatment. Once damaged, maintenance personnel generally need to work continuously, which also affects safety.
[0022] To this end, the present application provides an online repair method for a belt conveyor roller, comprising the following steps:
[0023] Analyze the area on the drum surface to be repaired, and divide the drum surface in the axial direction. The division method is: each division surface is an arc-shaped surface, the corresponding angle is 45 degrees to 90 degrees, and the length of each division surface is equal to the length of the drum; the area on the drum surface to be repaired exists in one or more of the division surfaces. The purpose of division is to ensure that the area on the drum surface to be repaired is located in as few division surfaces as possible, while ensuring that the effect of the division surface does not affect the online operation of the drum. An example is: division by length in the axial direction: for example, the drum diameter is 800mm and the length is 1400mm. The cutting needs to be carried out in the direction of the central axis, and the arc size is 200mm and the length is 14000mm.
[0024] Clean the area on the drum surface to be repaired: Cleaning the area on the drum surface to be repaired includes: grinding the area on the drum surface to be repaired, and using a non-aqueous cleaning agent to clean the area on the drum surface to be repaired. In order to avoid bulging, detachment, and internal aging of the belt in the later stage, the cleaning agent must be a non-aqueous cleaning agent, such as gasoline and acetone (water will leave water residue on the contact surface of the covered surface). After cleaning with the cleaning agent, the dust and other debris on the surface to be bonded can be removed as little as possible, and grinding is to better remove the previous residue.
[0025] Apply the conveyor belt glue to the area to be repaired on the surface of the roller, and cover the surface to be repaired at the location to be repaired. Including: first apply the first layer of conveyor belt glue, and use a scraper to thin it to 0.1±0.025mm, and then bake it to make the first layer of conveyor belt glue dry to 65%-80%; apply the second layer of conveyor belt glue, and thin it again to 0.1±0.025mm, and bake it to make the second layer of conveyor belt glue dry to 65%-80%. This dryness is about 65%-80%, preferably 65%-75%. Because there are two layers of glue with a dryness of 65%-80%, the glue has the greatest adhesion in this case; but if it is completely dry, the viscosity of the conveyor belt glue will be significantly weakened.
[0026] The bonding surface between the repaired surface and the area to be repaired on the drum surface is hammered; the hammering time between the repaired surface and the area to be repaired on the drum surface is controlled when the conveyor belt glue is dried to within 95%. When the two surfaces cover each other, this coverage needs to be strictly marked in advance, and the size is adjusted so that the error of the bonded surface basically does not exceed 1.5mm. After covering and bonding, the entire surface needs to be knocked with a rubber hammer to make the bonded surfaces fit very well, and there must be no air and dust. The knocking process needs to be relatively fast, mainly depending on the ambient temperature. The higher the temperature, the faster it needs to be to prevent the glue from drying and curing to 95%, so that the bonding is more solid.
[0027] Repeat the above process to complete the repair of all the areas to be repaired on the drum surface.
[0028] As an improved technical solution of the present application, each repair also includes standing still, and each standing time is not less than 40 minutes. The purpose is that after covering and bonding, the glue dryness is about 65%-80%. Although after knocking and hammering, the entire repaired surface is pressed with a heavy object, and then it is left to stand. After this covering, the inside of the bonding surface is not ventilated, and the upper and lower parts are covered and squeezed. It takes time for the glue to dry naturally, not to mention this state. After drying, the glue has a certain amount of heat and needs to wait for natural cooling. Therefore, the normal standing time is not less than 40 minutes, and then the equipment can be removed and the machine can be tested.
[0029] The technical solution of this application is applicable to the repair of the rubber wear-resistant layer on the surface of the roller, and is also applicable to the repair of the damage / wear on the surface of the roller or other shaft-like parts. In the repair process of different objects: the repair path is the same, the difference is the selection of the repair surface used for repair, and the connection method between the repair surface and the area to be repaired is different. If the area to be repaired is metal, the repair surface and the area to be repaired can be glued or welded.
[0030] Example 1
[0031] Since the drum is a hollow drum, its surface is generally made of 6 / 8mm iron sheet, and the iron sheet drum is welded to the drum drive shaft. There is a rubber wear-resistant layer on the surface of the iron sheet drum. After the rubber wear-resistant layer is worn, it needs to be repaired as soon as possible, otherwise it will continue to wear and wear through the iron sheet on the surface of the drum. In this case, the drum needs to remove all the iron sheet drums on the surface, then re-roll them, and then re-weld them. Moreover, after the iron sheet drum is worn through, since the strength of the metal is greater than the conveyor belt of the belt conveyor, it will also cause wear or tear of the conveyor belt of the belt conveyor. And after the wear-resistant layer on the surface of the transmission drum is worn, since the iron parts will be worn very brightly by the conveyor belt, it will also cause the belt conveyor to slip. Therefore, the wear-resistant layer on the surface of the drum needs to be handled in time.
[0032] An online repair method for a belt conveyor roller can be used to repair various belt conveyor roller surfaces such as wear-resistant layers that are worn, and can also be used to repair damaged locations on the surfaces of other shaft-like parts.
[0033] The specific on-site construction process of this repair method is as follows:
[0034] 1. For belt conveyors that need to be repaired, power off and put up signs, and set up warning signs near rollers that need to be operated.
[0035] 2. Preparation of the surface for repair: The method of repairing and reusing waste was used on site. The thickest layer of rubber on the surface of the conveyor belt was peeled off from the excess short conveyor belt that could not be effectively used when replacing the conveyor belt, and used as the surface for repair.
[0036] 3. Analyze the area on the drum surface to be repaired, and divide the drum surface in the axial direction. The division method is: each division surface is an arc surface, the corresponding angle is 45 degrees to 90 degrees, and the length of each division surface is equal to the length of the drum; and ensure that the area on the drum surface to be repaired is located in one or more of the division surfaces. Specifically: the on-site construction personnel divide the drum surface into multiple blocks according to the size of the drum to be repaired. This embodiment takes the example of dividing it into 4 blocks. Each division surface is horizontal (axial), not the kind that goes around the drum (non-radial direction). For example, the circumference of the drum is 800mm and the length is 1400mm. The cutting needs to be carried out in the direction of the central axis. The arc length is 200mm, and the length of the division surface is 14000mm. This is convenient for operation.
[0037] The purpose is ①, better operation, too wide is inconvenient to work, too narrow is low repair efficiency, the width varies according to different people; ②, due to the different sizes of the drum, the repair time is different, but the belt conveyor will not have a spare line for the mine, so when production is needed, it is limited to consider starting the machine. Take the site as an example: the crushing section is not started for 3 hours in the morning and 2.5 hours in the afternoon. Therefore, this block is divided according to the amount of work that can be done, and it is necessary to ensure that a small block needs to be repaired before starting the machine, and the corresponding tools are evacuated.
[0038] 4. Clean the area on the drum surface to be repaired: first clean the stones bonded to the drum surface, then clean the wear-resistant layer on the drum surface accordingly, and grind it with a polisher (the wear of the wear-resistant layer is different in different positions, some wear-resistant layers are thicker, and some have been completely worn out).
[0039] 5. After polishing, the surface to be repaired needs to be cleaned with a volatile, water-free cleaning agent such as acetone, gasoline, etc. The back of the bonded conveyor belt surface also needs to be cleaned (the repair method of this embodiment is to use conveyor belt cold glue to bond the conveyor belt surface to the drum surface). The purpose is to ensure that there is no dust on the conveyor belt surface and the drum surface during bonding, and to prevent the bonding from falling off later.
[0040] 6. Apply the conveyor belt glue to the area to be repaired on the surface of the roller, and cover the surface for repair in the area to be repaired, including: after cleaning, wait for the two bonding surfaces (the surface of the area to be repaired and the surface for repair) to dry, first apply a layer of conveyor belt glue (the conveyor belt glue in this embodiment is model: Sai Tiepai, manufacturer: Changzhou Nature Chemical Co., Ltd.), and use a scraper to scrape it thin to 0.1±0.25mm, and then bake it quickly to dry the conveyor belt glue to 65%-80%; then apply glue to the two bonding surfaces again, bake and dry to 65%-80%. The second application of glue is because the first application is not so uniform, and there may be pores in some places; so the second application, and only 2 times, because after the thick application, the gap between the two bonding surfaces is larger, which may have a certain impact on the stability of the structure.
[0041] 7. Beat the adhesive surface of the repaired surface and the roller surface to be repaired, including: bonding the adhesive surface of the conveyor belt (the repaired surface) and the roller adhesive surface (the surface of the area to be repaired); then use a rubber hammer to beat the bonding surfaces one by one, and the entire surface needs to be beaten. The purpose is to expel the air and excess conveyor belt glue inside the bonding surface, so that the bonding is tighter and stronger. If the beating is not performed, the air will cause air bulging on the bonding surface in the later stage. The time for beating the adhesive surface of the repaired surface and the roller surface to be repaired should be controlled within 95% of the drying of the conveyor belt glue; the beating speed mainly depends on the ambient temperature. The higher the temperature, the faster it needs to be to prevent the glue from drying and curing to 95%, so that the bonding is more firm.
[0042] 8. After each repair is completed, it also includes a static rest, and each static rest time is not less than 40 minutes. Specifically: after the first piece is repaired, due to the limited space exposed by the online repair of the worn part, it is necessary to rotate the roller to expose the second piece to be repaired. The piece that has just been bonded can be pressed by the conveyor belt. The purpose is 1. It is more difficult to enter the air after being pressed, etc. 2. After the bonding and knocking, it is necessary to wait for the glue to completely dry and bond. It is collectively called maintenance, which takes about 40 minutes. Then start repeating the second, third, and fourth pieces.
[0043] 9. After the fourth block is finished, it is also necessary to reserve maintenance time of at least 40 minutes. Then you can start the machine normally. Of course, if time does not allow, such as on-site, after repairing one block, turn out the second block after the leak, and then evacuate the personnel. Then wait for the maintenance time to end. Then repeat the operation next time.
Claims
1. An online repair method for a belt conveyor roller, characterized in that: The steps include: Analyze the area to be repaired on the drum surface, and divide the drum surface along the axial direction, the division method is: each division surface is an arc surface, the corresponding angle is 45 degrees to 90 degrees, and the length of each division surface is equal to the length of the drum; the area to be repaired on the drum surface exists in one of the division surfaces or multiple division surfaces; Clean the area on the drum surface to be repaired; Apply conveyor belt glue to the area to be repaired on the surface of the roller, and cover the area to be repaired with a surface for repair; Hammering the bonding surface between the surface to be repaired and the area to be repaired on the drum surface; Repeat the above process to complete the repair of all the areas to be repaired on the drum surface.
2. The online repair method for a belt conveyor roller according to claim 1, characterized in that: Cleaning the area on the drum surface to be repaired includes: grinding the area on the drum surface to be repaired, and cleaning the area on the drum surface to be repaired with a non-aqueous cleaning agent.
3. The online repair method for a belt conveyor roller according to claim 1, characterized in that: Applying the conveyor belt glue to the area to be repaired on the surface of the roller includes first applying a first layer of conveyor belt glue and thinning it to 0.1±0.025mm with a scraper, and then baking it to make the first layer of conveyor belt glue dry to 65%-80%; applying a second layer of conveyor belt glue and thinning it again to 0.1±0.025mm, and baking it to make the second layer of conveyor belt glue dry to 65%-80%.
4. The online repair method for a belt conveyor roller according to claim 1, characterized in that: After each repair is completed, it also includes a rest period, and each rest period lasts no less than 40 minutes.
5. The online repair method for a belt conveyor roller according to claim 1, characterized in that: The hammering process of the bonding surface between the surface to be repaired and the area to be repaired on the drum surface is controlled so that the degree of drying of the conveyor belt glue is within 95%.