Method for preparing lanthanum-based super-nitrogen polymer

The lanthanum metal samples were prepared by magnetron sputtering or vacuum evaporation, and the lanthanum-based supernitrogen polymer LaN8 was successfully synthesized by using high-pressure nitrogen and infrared laser heating technology, solving the limitation of lanthanum and nitrogen compounds in the prior art to low nitrogen content and The problem of simple configuration achieves high energy density material preparation and demonstrates good repeatability.

CN119038501AActive Publication Date: 2024-11-29JILIN UNIVERSITY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411162998.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

It is difficult to synthesize lanthanum-based supernitrogen polymers with excellent energy properties under lower pressures, and the compounds of lanthanum and nitrogen are limited to compounds with low nitrogen atom content and simple configuration.

Method used

Magneto-controlled sputtering or vacuum evaporation is used to prepare lanthanum metal samples, high-pressure gas loading device is loaded with high-pressure nitrogen, and the anvil device is reached through diamond to achieve the target pressure, combined with an infrared laser to perform in-situ laser heating, and lanthanum-based supernitrogen polymerization is prepared LaN8 and quenched under pressure to 22 GPa.

Benefits of technology

The synthesis of a high nitrogen ratio lanthanum-based supernitrogen polymer under low pressure has a covalent single bond structure with a high energy-containing content, has potential as a high energy storage material, and the method has good repeatability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038501A_ABST
    Figure CN119038501A_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing a lanthanum-based super-nitrogen polymer, and belongs to the technical field of preparation of high-energetic materials. Lanthanum and nitrogen are placed in a diamond anvil cell through magnetron sputtering or vacuum evaporation and a high-pressure gas loading technology to be subjected to laser heating for direct reaction, and a brand new lanthanum-based super-nitrogen polymer LaN8 is synthesized under million atmospheric pressure. The lanthanum-based super-nitrogen polymer phase prepared by the invention has a cage-like N8 polymerization unit different from a known multi-nitrogen structure. The material has the longest nitrogen-nitrogen bond length in all multi-nitrogen polymers, and is a potential high-energy-density material. The research opens up a brand-new and promising way for discovering a novel super nitride with a unique nitrogen structure through a high-temperature and high-pressure experimental means.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-energy material preparation, and particularly relates to a method for preparing a lanthanum-based super nitrogen polymer material. Background Art

[0002] The conversion process of nitrogen molecules with triple bonds to single-bond polymeric nitrogen has been a research hotspot for decades. The mutual conversion between the two is usually accompanied by extremely significant energy changes, which have a series of potential application values, such as energy storage, propellants and high explosives. Combined with high temperature and high pressure synthesis technology, it is now possible to create a variety of solid nitrogen single-bond polymer structures such as cg-N, LP-N, HLP-N, BP-N, etc. However, the synthesis of these polymers still requires pressures higher than one million atmospheres. In order to reduce the synthesis pressure and increase the stable pressure range of the product. "Chemical pre-compression" as an important method has been widely used in a large number of high-pressure polymer synthesis experiments. Theoretical studies have shown that this method can stabilize various forms of polymer networks at lower pressures. For example, with pseudobenzene "N 6 "Molecular K 2 N 6 , with pentadiazole anion "N 5- "CsN 5 , ZnN with one-dimensional infinite “[N]” chain 4 and has an armchair-like "N 6 "Ring WN 6 These results demonstrate that the type of metal has a significant effect on the bonding pattern between two adjacent nitrogen atoms. Metal lanthanum (La) has abundant valence electrons and is an important element for synthesizing new compounds. In particular, lanthanum can react with hydrogen to generate high-temperature superconductors LaH 10 It has caused quite a stir, but the La-N compounds predicted or synthesized so far are limited to compounds with low nitrogen content and simple nitrogen configuration. Therefore, the search for a metal lanthanum nitrogen compound with a high ratio has been in a blank stage. This type of compound not only has excellent physical and chemical properties and potential application value, but can also provide technical guidance for the subsequent research of other transition metal and rare earth metal nitrides. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a new method for preparing metal polymer nitrogen materials with excellent energy properties by simple purely physical means.

[0004] The method uses magnetron sputtering or vacuum evaporation to prepare a metal sample La, and uses a high-pressure gas loading system (Gas Loading System, hereinafter referred to as GLS) to load high-pressure nitrogen, uses a diamond anvil cell (hereinafter referred to as DAC) to reach the target pressure, and uses an infrared laser to perform in-situ laser heating on the sample at the target pressure, thereby preparing a lanthanum-based super nitrogen polymer LaN 8 . It is then quenched under pressure to 22 GPa. This method has good reproducibility.

[0005] The specific technical solutions of the present invention are as follows:

[0006] A method for preparing a lanthanum-based super nitrogen polymer comprises the following steps: firstly, preparing an initial metal La film on a diamond surface by a magnetron sputtering method or a vacuum evaporation method; then, using a GLS system, loading high-purity nitrogen gas at a pressure of 180 MPa and encapsulating it; then, using a DAC, slowly pressurizing the loaded nitrogen gas and the La film to 110 GPa; then, using a 1070 nm infrared laser, uniformly performing high-pressure in-situ laser heating on the sample, the heating time being maintained for 3 to 5 minutes, and the heating temperature being 2000 K; then, turning off the laser for rapid annealing, and obtaining LaN with a lanthanum: nitrogen ratio of 1:8. 8 Material.

[0007] Preferably, the thickness of the initial metal La film is 1-2 microns, which is 1 / 4 of the size of the diamond anvil surface.

[0008] Preferably, the purity of the high-purity nitrogen is 99.999%.

[0009] Preferably, the pressurization rate of the slow pressurization to 110 GPa is 30 GPa / day; and the annealing rate of the rapid annealing is 1000° C. / second.

[0010] Preferably, the experimental method has good repeatability.

[0011] Beneficial effects:

[0012] The present invention first uses magnetron sputtering or vacuum evaporation to prepare a thinner metal sample layer, which is conducive to the complete reaction and testing of the sample. GLS can provide sufficient nitrogen for the reaction, which is conducive to the synthesis of metal nitrides with a high nitrogen ratio. The sample prepared by the present invention has nitrogen atoms in the structure constructed as a polymer network in the form of covalent single bonds. Its average nitrogen-nitrogen bond length exceeds all currently disclosed nitrides, has a high energy content, and can be used as a high energy storage material. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1It is the X-ray diffraction spectrum of the initial sample in Example 1 at a pressure of 97 GPa before the reaction.

[0014] Figure 2 These are microscopic photographs of the raw materials before reaction and the products after reaction in two groups of DACs used in Example 2, which have the same conditions except the volume of the raw materials.

[0015] Figure 3 This is the X-ray diffraction spectrum of Example 3 at a pressure of 110 GPa after the reaction.

[0016] Figure 4 The product P4 / n LaN prepared in Example 3 8 of the crystal structure.

[0017] Figure 5 The product LaN prepared in Example 3 8 Volume versus pressure curve.

[0018] Figure 6 The product LaN prepared in Example 3 8 Comparison of the average bond length of and other nitrides. DETAILED DESCRIPTION

[0019] The present invention is now described in more detail with reference to the following examples. Unless otherwise specified, all reagents used are commercially available products and are not further purified.

[0020] Example 1 Preparation of initial reaction product

[0021] First of all, whether the magnetron sputtering method or the vacuum evaporation method is used, it is necessary to use a 5mm×5mm×50μm W metal sheet to make a mask before preparing the sample, and pre-press the mask to 30GPa through the DAC device. Then, according to the target sample size, a corresponding hole is punched in the center of the indentation using a laser puncher, and the sheet is placed in the center of the diamond. Use vacuum seal (magnetron sputtering) or AB glue (vacuum evaporation) to fix the sheet as a mask. If the magnetron sputtering method is used, the lanthanum target (purity 99.9%) must first be loaded into the magnetron sputtering device and sputtered onto the diamond substrate covering the mask by direct current under an argon atmosphere of 0.5Pa. The sputtering time is 12 minutes. If the sample is thin, the sputtering time can be appropriately increased. It is worth noting that a 3-5 minute pre-sputtering is required before the formal sputtering to remove the oxide on the surface of the target material. If the vacuum evaporation method is used, the diamond substrate covered with the mask needs to be suspended upside down in the evaporation equipment, and an appropriate amount of metal La powder is filled in the lower molybdenum boat. Then the current is gradually increased to 30 amperes. When the molybdenum boat lights up, it means that the sample has been evaporated. At this time, the current can be turned off and the substrate can be taken out. After the metal film is prepared, the entire DAC device is placed in the GLS system, loaded with high-pressure nitrogen (180MPa), and then the DAC device is taken out and slowly increased to the target pressure of 110GPa. During the pressurization period, the purity of the initial sample is calibrated by X-ray diffraction. Figure 1 shown.

[0022] Example 2 Preparation of lanthanum-based super nitrogen polymer

[0023] The preparation of lanthanum-based super nitrogen polymers requires the support of a symmetrical DAC, which can easily achieve laser heating and sample synthesis under millions of atmospheres. This experiment uses two sets of Boheler-type diamonds with a standard DAC device. The two sets of experiments only differ in the initial sample size, and the rest of the experimental conditions are the same. The diamond standard pressure method is used to determine the pressure on the sample during the pressure loading process. The sample is pressurized to 110 GPa slowly (30 GPa / day) to minimize the pressure gradient inside it. Subsequently, a micro-focused infrared laser is used to uniformly laser heat the entire sample. The heating time is 3-5 minutes and the temperature is 2000K. After the heating is completed, the laser is quickly turned off to quench to room temperature. Photos of the sample cavity before and after laser heating are shown in the figure. Figure 2 shown.

[0024] Example 3 Structural Characterization of Lanthanum-Based Super Nitrogen Polymer

[0025] After the sample reaction is complete, the crystal structure properties of the sample can be characterized by (synchrotron radiation) X-ray diffraction. Figure 3This is the X-ray diffraction spectrum of the sample collected at the BL15U1 beamline of the synchrotron radiation source. In the figure, it can be seen that in addition to the peaks of the reactant La and the metal seal W, there are a large number of newly generated unknown X-ray diffraction signals (later identified as the target product LaN 8 Combined with theoretical calculation methods, it was determined that the new product is lanthanum-based super nitrogen polymer LaN 8 The nitrogen atoms are arranged in a cage-like pattern, and the three-dimensional structure is as follows: Figure 4 . Figure 5 The relationship between the sample volume and pressure of the new samples in the two groups of DAC. Even if the initial sample volume is different, the physical properties of the product are still highly consistent. This shows that the method has excellent repeatability. The pressure relief quenching experiment on the sample shows that the sample can be stabilized to a pressure of 22GPa, which is lower than the 46GPa of traditional polymerized nitrogen. This further confirms that the introduction of metal atoms plays a vital role in the synthesis and stabilization of the polymerized nitrogen structure. By calculating the average nitrogen-nitrogen bond length of the structure, Figure 6 It can be seen that the bond length of nitrogen atoms in this structure is longer than that of almost all other polymeric nitrides. This indicates that the nitrogen atoms in this structure will release more energy during the transformation from single bonds to triple bonds, and have the potential to be used as high-energy materials.

Claims

1. A method for preparing a lanthanum-based super nitrogen polymer, firstly, using a magnetron sputtering method or a vacuum evaporation method to prepare an initial metal La film on a diamond surface, and then using a high-pressure gas loading device to load high-purity nitrogen at a pressure of 180MPa and encapsulate; subsequently, using a DAC to slowly pressurize the loaded nitrogen and La film to 110GPa, and then using a 1070nm infrared laser to uniformly perform high-pressure in-situ laser heating on the sample, the heating time is maintained for 3 to 5 minutes, the heating temperature is 2000K, and then the laser is turned off for rapid annealing to obtain a LaN8 material with a lanthanum: nitrogen ratio of 1:

8.

2. A method for preparing a lanthanum-based super nitrogen polymer according to claim 1, characterized in that: The thickness of the initial metal La film is 1 to 2 microns, which is 1 / 4 of the size of the diamond anvil surface.

3. A method for preparing a lanthanum-based super nitrogen polymer according to claim 1, characterized in that: The purity of the high-purity nitrogen is 99.999%.

4. A method for preparing a lanthanum-based super nitrogen polymer according to claim 1, characterized in that: The pressurization rate of the slow pressurization to 110 GPa is 30 GPa / day; and the annealing rate of the rapid annealing is 1000° C. / second.

Citation Information

Patent Citations

  • Method for preparing ternary La0. 75+xCe0. 25-xH10 high-temperature superconductor at high pressure

    CN115893316A

  • Lanthanide metal hydride and preparation method thereof

    CN116873866A

  • Method for synthesizing quaternary lanthanum cerium yttrium hydride superconductor

    CN118448105A

  • High-temperature superconducting hydride and method for production thereof