Starch-based hard carbon composite graphite negative electrode material and preparation method and application thereof
By esterified composite materials of starch and expanded graphite, combined with melamine crosslinking agent, the problems of structural damage and high crosslinking agent cost during high temperature carbonization are solved, and the starch-based with high lithium storage capacity and electrochemical stability are achieved Hard carbon composite graphite negative electrode material has excellent magnification and cycling performance.
Patent Information
- Application Number
- CN202411167638.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-23
AI Technical Summary
In the prior art, structural damage in the process of high-temperature carbonization leads to volume expansion, and the maleic anhydride crosslinking agent is costly and cannot improve the specific capacity of hard carbon in biomass, making it difficult to maintain the starch spherical morphology and improve the lithium storage performance.
A composite material of esterified starch and expanded graphite is used, through hydrothermal reaction and carbonization treatment, combined with melamine as a crosslinking agent, to form a starch-based hard carbon composite graphite negative electrode material to ensure the stability of the spherical structure and the uniform composite of graphite.
High lithium storage capacity, low volume change, excellent magnification and cycling performance are achieved, and additional active sites are provided through melamine doping, which improves the storage capacity and electrochemical stability of lithium ions.
Smart Images

Figure CN119038522A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery negative electrode materials, and in particular to a starch-based hard carbon composite graphite negative electrode material and a preparation method and application thereof. Background Art
[0002] Hard carbon is one of the most promising negative electrode materials for lithium-ion batteries because of its stable structure, excellent conductivity and easy processing. It also has excellent cycle performance at high current density and has become a popular choice for negative electrode materials for lithium-ion batteries. Starch is a low-cost, easily available, green and pollution-free biomass hard carbon that has been widely studied and applied. Among all biomass precursors, starch as a precursor has the highest degree of control over the microstructure, morphology and properties of the final hard carbon. Compared with other biomass precursors, starch exhibits an original natural spherical morphology, which makes it one of the most advantageous candidate materials for the preparation of spherical carbon materials. However, direct carbonization of starch easily leads to the rupture of the starch sphere morphology and low compaction density. Therefore, it is necessary to provide a means to maintain the starch sphere morphology and improve its lithium storage performance. During the heat treatment process, the introduction of the crosslinking agent promotes the effective connection of the aromatic units inside the starch. This highly crosslinked nanostructure not only keeps the final hard carbon in a good spherical morphology. The research and development of crosslinking agents has brought bright prospects for the application of starch in the negative electrode of lithium-ion batteries.
[0003] In the prior art, maleic anhydride is often used as a cross-linking agent. However, the raw material cost of maleic anhydride cross-linking agent is relatively high and it cannot improve the limited specific capacity of biomass hard carbon. In addition, directly using hard carbon as a lithium electron negative electrode material has the problem of the starch macromolecular structure being destroyed during the high-temperature carbonization process, resulting in volume expansion. Summary of the invention
[0004] The purpose of the present invention is to provide a starch-based hard carbon composite graphite negative electrode material and its preparation method and application in view of the above-mentioned deficiencies in the prior art. The material has good electronic conductivity, high lithium storage capacity, small volume change, large specific surface area, uniform particles, and excellent rate and cycle performance.
[0005] The invention discloses a method for preparing a starch-based hard carbon composite graphite negative electrode material. Expanded graphite and esterified starch are mixed and fully ground and then carbonized to obtain the starch-based hard carbon composite graphite negative electrode material.
[0006] Furthermore, the mass ratio of the expanded graphite to the esterified starch is 1:1-30.
[0007] Furthermore, the carbonization temperature is 900-1300° C., and the carbonization time is 1-8 hours.
[0008] Furthermore, the heating rate of carbonization is 1 to 10°C / min.
[0009] Furthermore, the preparation method of esterified starch is as follows: vacuum drying corn starch, and then hydrothermally reacting it with melamine to obtain esterified starch.
[0010] Furthermore, the mass ratio of corn starch to melamine is 4:1.
[0011] Furthermore, the hydrothermal reaction temperature is 50-150°C.
[0012] Furthermore, the expandable graphite is heated to 600° C. at a rate of 20 to 30° C. / min in a muffle furnace, kept at this temperature for 0.5 to 3 hours, and then cooled to obtain the expanded graphite.
[0013] A starch-based hard carbon composite graphite negative electrode material prepared by the above-mentioned preparation method.
[0014] An application of the starch-based hard carbon composite graphite negative electrode material as described above in a lithium battery.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] (1) The cross-linked spherical structure of esterified starch promotes the + The ML-1100 anode has a wide working potential (0–3 V vs Li / Li + ) and its capacitive properties can achieve high reversible capacity.
[0017] (2) The composite material prepared by the present invention has uniform particles, the spherical structure of corn starch remains stable and interconnected after esterification, and graphite is evenly compounded on the surface of the spherical structure;
[0018] The composite of graphite further enriches the lithium storage methods and capacity. When the voltage is lower than 0.25V, lithium ions begin to embed into the graphite layer, forming graphite interlayer compounds of different orders. There are three ways to store lithium in graphite materials: interlayer lithium storage, end face lithium storage and surface lithium storage. Among them, the graphite interlayer provides the main lithium storage space.
[0019] (3) The starch-based hard carbon and graphite composite material realizes the large-capacity storage of lithium ions through the synergistic effect of biomass hard carbon and graphite, and at the same time promotes the reaction kinetics. The starch-based hard carbon composite graphite negative electrode material prepared by the present invention has a wide potential window (relative to Li / Li + It exhibits a large lithium-ion storage capacity (423.7 mAh g) within 0–3 V. -1) and good charge / discharge rate. In addition, during the cycle test, the low polarization of the negative electrode and the minimal morphological structure change promoted its electrochemical stability, and the capacity retention rate was still above 90% after 100 cycles. This material has achieved a technological breakthrough in its high capacity and high rate performance in lithium-ion battery negative electrodes.
[0020] (4) The material has good electronic conduction, high lithium storage capacity, small volume change, large specific surface area, uniform particles, and excellent rate and cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is the SEM image of the starch-based hard carbon composite graphite negative electrode material prepared in Example 4.
[0022] Figure 2 These are XRD diagrams of starch-based hard carbon composite graphite negative electrode materials prepared in Example 1, Example 4, and Example 6.
[0023] Figure 3 The battery assembled with the starch-based hard carbon composite graphite negative electrode material prepared in Example 4 of the present invention was tested at a low current density of 25 mAg -1 The charge and discharge curve diagram below.
[0024] Figure 4 The battery assembled with the starch-based hard carbon composite graphite negative electrode material prepared in Example 4 of the present invention was charged at a low current density of 25 mAg -1 GCD performance graph below.
[0025] Figure 5 The battery assembled with the starch-based hard carbon composite graphite negative electrode material prepared in Examples 1-6 of the present invention was subjected to a current density of 0.1Ag. -1 The following cycle performance comparison chart.
[0026] Figure 6 The batteries assembled from the materials prepared in Comparative Examples 1-4 of the present invention were respectively subjected to a current density of 0.1Ag. -1 The cycle performance diagram below.
[0027] Figure 7 The batteries assembled from the materials prepared in Comparative Examples 1-4 of the present invention were respectively charged at a current density of 25 mAg -1 Comparison of the constant current intermittent titration (GITT) curves under lithiation and the calculated diffusion coefficient D during lithiation and delithiation processes.
[0028] Figure 8 The batteries assembled from the materials prepared in Example 3 of the present invention and Comparative Examples 2 and 4 were respectively subjected to a current density of 25m Ag. -1Comparison of the constant current intermittent titration (GITT) curves under lithiation and the calculated diffusion coefficient D during lithiation and delithiation processes.
[0029] Fig. 9 The battery assembled with the negative electrode materials prepared in Comparative Examples 2 and 5 of the present invention was subjected to a low current density of 25 mA g -1 The charge and discharge curve diagram below. DETAILED DESCRIPTION
[0030] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.
[0031] <Example 1>
[0032] S1. Pretreatment of starch-based raw materials: taking a certain amount of corn starch and putting it into a container, putting the container containing soluble starch into a vacuum drying oven at 50-100° C. for drying for 24 hours, then taking out the container, adding it into a reactor according to a starch to melamine mass ratio of 4:1, and performing dry powder hydrothermal treatment at 50-150° C. to obtain a precursor material, and then crushing it to obtain precursor particles, the precursor particle size is 40-500 mesh.
[0033] S2, composite graphite: heat the expandable graphite to 600°C in a muffle furnace at a rate of 20-30°C / min, keep the temperature for 0.5h, and collect the expanded graphite after cooling. Mix the expanded graphite with the esterified starch prepared in S1 and grind them thoroughly, with the mass ratio of esterified starch to expanded graphite being 1:1, and collect the granular mixture.
[0034] S3, carbonization: under the protection of argon atmosphere, the precursor particles obtained in S1 were heated to 1100°C at 1-2°C / min, kept warm for 2h, and cooled to room temperature with the furnace to obtain starch-based hard carbon composite graphite negative electrode material.
[0035] S4. Preparation of negative electrode: Use the above-mentioned starch-based hard carbon composite graphite negative electrode material as the negative electrode active material to prepare the negative electrode sheet, grind the negative electrode material with the conductive agent and the binder in a mass ratio of 8:1:1, then mix with N-methylpyrrolidone to prepare the negative electrode slurry, and coat it on the current collector, place it in a vacuum oven at 100°C for 10 hours, dry and cut it into disc-shaped negative electrode sheets.
[0036] S5. Half-cell assembly: A lithium sheet was used as the counter electrode. The electrolyte was prepared by 1.0 mol LiPF6 in a solution of ethylene carbonate, diethyl carbonate and dimethyl carbonate (EC / DEC / DMC, v / v / v=1:1:1). The above-mentioned starch-based negative electrode sheets were assembled into button cells in a glove box under an argon atmosphere.
[0037] <Example 2>
[0038] S1. Pretreatment of starch-based raw materials: taking a certain amount of corn starch and putting it into a container, putting the container containing soluble starch into a vacuum drying oven at 50-100° C. for drying for 24 hours, then taking out the container, adding it into a reactor according to a starch to melamine mass ratio of 4:1, and performing dry powder hydrothermal treatment at 50-150° C. to obtain a precursor material, and then crushing it to obtain precursor particles, the precursor particle size is 40-500 mesh.
[0039] S2, composite graphite: heat the expandable graphite to 600°C in a muffle furnace at a rate of 0-10°C / min, keep the temperature for 0.5h, cool it down and collect the expanded graphite. Mix the expanded graphite with the esterified starch prepared in S1 and grind them thoroughly, the mass ratio of esterified starch to expanded graphite is 5:1, and collect the granular mixture.
[0040] S3, carbonization: under the protection of argon atmosphere, the precursor particles obtained in S1 were heated to 1100°C at a rate of 1-2°C / min, kept at this temperature for 2 hours, and cooled to room temperature with the furnace to obtain a starch-based hard carbon composite graphite negative electrode material.
[0041] S4. Preparation of negative electrode: Use the above-mentioned starch-based hard carbon composite graphite negative electrode material as the negative electrode active material to prepare the negative electrode sheet, grind the negative electrode material with the conductive agent and the binder in a mass ratio of 8:1:1, then mix with N-methylpyrrolidone to prepare the negative electrode slurry, and coat it on the current collector, place it in a vacuum oven at 100°C for 10 hours, dry and cut it into disc-shaped negative electrode sheets.
[0042] S5. Half-cell assembly: A lithium sheet was used as the counter electrode. The electrolyte was prepared by 1.0 mol LiPF6 in a solution of ethylene carbonate, diethyl carbonate and dimethyl carbonate (EC / DEC / DMC, v / v / v=1:1:1). The above-mentioned starch-based negative electrode sheets were assembled into button cells in a glove box under an argon atmosphere.
[0043] <Example 3>
[0044] S1. Pretreatment of starch-based raw materials: taking a certain amount of corn starch and putting it into a container, putting the container containing soluble starch into a vacuum drying oven at 50-100° C. for drying for 24 hours, then taking out the container, adding it into a reactor according to a starch to melamine mass ratio of 4:1, and performing dry powder hydrothermal treatment at 50-150° C. to obtain a precursor material, and then crushing it to obtain precursor particles, the precursor particle size is 40-500 mesh.
[0045] S2, composite graphite: the expandable graphite is heated to 600°C in a muffle furnace at a rate of 20-30°C / min, kept at this temperature for 0.5h, cooled and collected to obtain the expanded graphite. The expanded graphite is mixed with the esterified starch prepared in S1 and fully ground, the mass ratio of the esterified starch to the expanded graphite is 10:1, and a granular mixture is collected.
[0046] S3, carbonization: under the protection of argon atmosphere, the precursor particles obtained in S1 were heated to 1100°C at a rate of 1-2°C / min, kept at this temperature for 2 hours, and cooled to room temperature with the furnace to obtain a starch-based hard carbon composite graphite negative electrode material.
[0047] S4. Preparation of negative electrode: Use the above-mentioned starch-based hard carbon composite graphite negative electrode material as the negative electrode active material to prepare the negative electrode sheet, grind the negative electrode material with the conductive agent and the binder in a mass ratio of 8:1:1, then mix with N-methylpyrrolidone to prepare the negative electrode slurry, and coat it on the current collector, place it in a vacuum oven at 100°C for 10 hours, dry and cut it into disc-shaped negative electrode sheets.
[0048] S5. Half-cell assembly: A lithium sheet was used as the counter electrode. The electrolyte was prepared by 1.0 mol LiPF6 in a solution of ethylene carbonate, diethyl carbonate and dimethyl carbonate (EC / DEC / DMC, v / v / v=1:1:1). The above-mentioned starch-based negative electrode sheets were assembled into button cells in a glove box under an argon atmosphere.
[0049] The double transition metals selected in Examples 1, 2 and 3 are iron / cobalt, nickel / cobalt and iron / manganese respectively, and the organic ligand reagents selected are fumaric acid, benzoic acid and oxalic acid respectively.
[0050] <Example 4>
[0051] S1. Pretreatment of starch-based raw materials: taking a certain amount of corn starch and putting it into a container, putting the container containing soluble starch into a vacuum drying oven at 50-100° C. for drying for 24 hours, then taking out the container, adding it into a reactor according to a starch to melamine mass ratio of 4:1, and performing dry powder hydrothermal treatment at 50-150° C. to obtain a precursor material, and then crushing it to obtain precursor particles, the precursor particle size is 40-500 mesh.
[0052] S2, composite graphite: heat the expandable graphite to 600°C in a muffle furnace at a rate of 20-30°C / min, keep the temperature for 0.5h, cool it down and collect the expanded graphite. Mix the expanded graphite with the esterified starch prepared in S1 and grind them thoroughly, the mass ratio of esterified starch to expanded graphite is 15:1, and collect the granular mixture.
[0053] S3, carbonization: under the protection of argon atmosphere, the precursor particles obtained in S1 were heated to 1100°C at a rate of 1-2°C / min, kept warm for 2 hours, and cooled to room temperature with the furnace to obtain a starch-based hard carbon composite graphite negative electrode material.
[0054] S4. Preparation of negative electrode: Use the above-mentioned starch-based hard carbon composite graphite negative electrode material as the negative electrode active material to prepare the negative electrode sheet, grind the negative electrode material with the conductive agent and the binder in a mass ratio of 8:1:1, then mix with N-methylpyrrolidone to prepare the negative electrode slurry, and coat it on the current collector, place it in a vacuum oven at 100°C for 10 hours, dry and cut it into disc-shaped negative electrode sheets.
[0055] S5. Half-cell assembly: A lithium sheet was used as the counter electrode. The electrolyte was prepared by 1.0 mol LiPF6 in a solution of ethylene carbonate, diethyl carbonate and dimethyl carbonate (EC / DEC / DMC, v / v / v=1:1:1). The above-mentioned starch-based negative electrode sheets were assembled into button cells in a glove box under an argon atmosphere.
[0056] <Example 5>
[0057] S1. Pretreatment of starch-based raw materials: taking a certain amount of corn starch and putting it into a container, putting the container containing soluble starch into a vacuum drying oven at 50-100° C. for drying for 24 hours, then taking out the container, adding it into a reactor according to a starch to melamine mass ratio of 4:1, and performing dry powder hydrothermal treatment at 50-150° C. to obtain a precursor material, and then crushing it to obtain precursor particles, the precursor particle size is 40-500 mesh.
[0058] S2, composite graphite: the expandable graphite is heated to 600°C in a muffle furnace at a rate of 20-30°C / min, kept at this temperature for 0.5h, and then cooled to obtain the expanded graphite. The expanded graphite is mixed with the esterified starch prepared in S1 and fully ground, the mass ratio of the esterified starch to the expanded graphite is 20:1, and a granular mixture is obtained.
[0059] S3, carbonization: under the protection of argon atmosphere, the precursor particles obtained in S1 were heated to 1100°C at a rate of 1-2°C / min, kept warm for 2 hours, and cooled to room temperature with the furnace to obtain a starch-based hard carbon composite graphite negative electrode material.
[0060] S4. Preparation of negative electrode: Use the above-mentioned starch-based hard carbon composite graphite negative electrode material as the negative electrode active material to prepare the negative electrode sheet, grind the negative electrode material with the conductive agent and the binder in a mass ratio of 8:1:1, then mix with N-methylpyrrolidone to prepare the negative electrode slurry, and coat it on the current collector, place it in a vacuum oven at 100°C for 10 hours, dry and cut it into disc-shaped negative electrode sheets.
[0061] S5. Half-cell assembly: A lithium sheet was used as the counter electrode. The electrolyte was prepared by 1.0 mol LiPF6 in a solution of ethylene carbonate, diethyl carbonate and dimethyl carbonate (EC / DEC / DMC, v / v / v=1:1:1). The above-mentioned starch-based negative electrode sheets were assembled into button cells in a glove box under an argon atmosphere.
[0062] <Example 6>
[0063] S1. Pretreatment of starch-based raw materials: taking a certain amount of corn starch and putting it into a container, putting the container containing soluble starch into a vacuum drying oven at 50-100° C. for drying for 24 hours, then taking out the container, adding it into a reactor according to a starch to melamine mass ratio of 4:1, and performing dry powder hydrothermal treatment at 50-150° C. to obtain a precursor material, and then crushing it to obtain precursor particles, the precursor particle size is 40-500 mesh.
[0064] S2, composite graphite: the expandable graphite is heated to 600°C in a muffle furnace at a rate of 20-30°C / min, kept at this temperature for 0.5h, and then cooled to obtain the expanded graphite. The expanded graphite is mixed with the esterified starch prepared in S1 and fully ground, the mass ratio of the esterified starch to the expanded graphite is 30:1, and a granular mixture is obtained.
[0065] S3, carbonization: under the protection of argon atmosphere, the precursor particles obtained in S1 were heated to 1100°C at a rate of 1-2°C / min, kept warm for 2 hours, and cooled to room temperature with the furnace to obtain a starch-based hard carbon composite graphite negative electrode material.
[0066] S4. Preparation of negative electrode: Use the above-mentioned starch-based hard carbon composite graphite negative electrode material as the negative electrode active material to prepare the negative electrode sheet, grind the negative electrode material with the conductive agent and the binder in a mass ratio of 8:1:1, then mix with N-methylpyrrolidone to prepare the negative electrode slurry, and coat it on the current collector, place it in a vacuum oven at 100°C for 10 hours, dry and cut it into disc-shaped negative electrode sheets.
[0067] S5. Half-cell assembly: A lithium sheet was used as the counter electrode. The electrolyte was prepared by 1.0 mol LiPF6 in a solution of ethylene carbonate, diethyl carbonate and dimethyl carbonate (EC / DEC / DMC, v / v / v=1:1:1). The above-mentioned starch-based negative electrode sheets were assembled into button cells in a glove box under an argon atmosphere.
[0068] <Comparative Example 1>
[0069] S1. Pretreatment of starch-based raw materials: taking a certain amount of corn starch and putting it into a container, putting the container containing soluble starch into a vacuum drying oven at 50-100° C. for drying for 24 hours, then taking out the container, adding it into a reactor according to a starch to melamine mass ratio of 4:1, and performing dry powder hydrothermal treatment at 50-150° C. to obtain a precursor material, and then crushing it to obtain precursor particles, the precursor particle size is 40-500 mesh.
[0070] S2. Carbonization: Under the protection of argon atmosphere, the precursor particles obtained in S1 were heated to 900°C at a rate of 1-2°C / min, kept at this temperature for 2 hours, and cooled to room temperature with the furnace to obtain a starch-based hard carbon negative electrode material.
[0071] S3. Preparation of negative electrode: The starch-based hard carbon negative electrode material is used as the negative electrode active material to prepare the negative electrode sheet. The negative electrode material is evenly ground with the conductive agent and the binder in a mass ratio of 8:1:1, and then mixed with N-methylpyrrolidone to prepare the negative electrode slurry, which is coated on the current collector, placed in a vacuum oven at 100°C for 10 hours, and dried and cut into disc-shaped negative electrode sheets.
[0072] S4. Half-cell assembly: A lithium sheet was used as the counter electrode. The electrolyte was prepared by 1.0 mol LiPF6 in a solution of ethylene carbonate, diethyl carbonate and dimethyl carbonate (EC / DEC / DMC, v / v / v=1:1:1). The above-mentioned starch-based negative electrode sheet was assembled into a button cell in a glove box under an argon atmosphere.
[0073] <Comparative Example 2>
[0074] S1. Pretreatment of starch-based raw materials: taking a certain amount of corn starch and putting it into a container, putting the container containing soluble starch into a vacuum drying oven at 50-100° C. for drying for 24 hours, then taking out the container, adding it into a reactor according to a starch to melamine mass ratio of 4:1, and performing dry powder hydrothermal treatment at 50-150° C. to obtain a precursor material, and then crushing it to obtain precursor particles, the precursor particle size is 40-500 mesh.
[0075] S2. Carbonization: Under the protection of argon atmosphere, the precursor particles obtained in S1 were heated to 1100°C at a rate of 1-2°C / min, kept warm for 2 hours, and cooled to room temperature with the furnace to obtain a starch-based hard carbon negative electrode material.
[0076] S3. Preparation of negative electrode: The starch-based hard carbon negative electrode material is used as the negative electrode active material to prepare the negative electrode sheet. The negative electrode material is evenly ground with the conductive agent and the binder in a mass ratio of 8:1:1, and then mixed with N-methylpyrrolidone to prepare the negative electrode slurry, which is coated on the current collector, placed in a vacuum oven at 100°C for 10 hours, and dried and cut into disc-shaped negative electrode sheets.
[0077] S4. Half-cell assembly: A lithium sheet was used as the counter electrode. The electrolyte was prepared by 1.0 mol LiPF6 in a solution of ethylene carbonate, diethyl carbonate and dimethyl carbonate (EC / DEC / DMC, v / v / v=1:1:1). The above-mentioned starch-based negative electrode sheet was assembled into a button cell in a glove box under an argon atmosphere.
[0078] <Comparative Example 3>
[0079] S1. Pretreatment of starch-based raw materials: taking a certain amount of corn starch and putting it into a container, putting the container containing soluble starch into a vacuum drying oven at 50-100° C. for drying for 24 hours, then taking out the container, adding it into a reactor according to a starch to melamine mass ratio of 4:1, and performing dry powder hydrothermal treatment at 50-150° C. to obtain a precursor material, and then crushing it to obtain precursor particles, the precursor particle size is 40-500 mesh.
[0080] S2. Carbonization: Under the protection of argon atmosphere, the precursor particles obtained in S1 were heated to 1300°C at a rate of 1-2°C / min, kept at this temperature for 2 hours, and cooled to room temperature with the furnace to obtain a starch-based hard carbon negative electrode material.
[0081] S3. Preparation of negative electrode: The starch-based hard carbon negative electrode material is used as the negative electrode active material to prepare the negative electrode sheet. The negative electrode material is evenly ground with the conductive agent and the binder in a mass ratio of 8:1:1, and then mixed with N-methylpyrrolidone to prepare the negative electrode slurry, which is coated on the current collector, placed in a vacuum oven at 100°C for 10 hours, and dried and cut into disc-shaped negative electrode sheets.
[0082] S4. Half-cell assembly: A lithium sheet was used as the counter electrode. The electrolyte was prepared by 1.0 mol LiPF6 in a solution of ethylene carbonate, diethyl carbonate and dimethyl carbonate (EC / DEC / DMC, v / v / v=1:1:1). The above-mentioned starch-based negative electrode sheet was assembled into a button cell in a glove box under an argon atmosphere.
[0083] <Comparative Example 4>
[0084] S1. Pretreatment of starch-based raw materials: a certain amount of corn starch is put into a container, and the container containing soluble starch is placed in a vacuum drying oven at 50-100°C for 24 hours. Then, the container is taken out, and the starch and maleic anhydride mass ratio is 5:1. The mixture is added into a reactor and subjected to dry powder hydrothermal treatment at 50-150°C to obtain a precursor material, and the precursor material is crushed to obtain precursor particles, and the precursor particle size is 40-500 mesh.
[0085] S2. Carbonization: Under the protection of argon atmosphere, the precursor particles obtained in S1 were heated to 1100°C at a rate of 1-2°C / min, kept warm for 2 hours, and cooled to room temperature with the furnace to obtain a starch-based hard carbon negative electrode material.
[0086] S3. Preparation of negative electrode: The starch-based hard carbon negative electrode material is used as the negative electrode active material to prepare the negative electrode sheet. The negative electrode material is evenly ground with the conductive agent and the binder in a mass ratio of 8:1:1, and then mixed with N-methylpyrrolidone to prepare the negative electrode slurry, which is coated on the current collector, placed in a vacuum oven at 100°C for 10 hours, and dried and cut into disc-shaped negative electrode sheets.
[0087] S4. Half-cell assembly: A lithium sheet was used as the counter electrode. The electrolyte was prepared by 1.0 mol LiPF6 in a solution of ethylene carbonate, diethyl carbonate and dimethyl carbonate (EC / DEC / DMC, v / v / v=1:1:1). The above-mentioned starch-based negative electrode sheet was assembled into a button cell in a glove box under an argon atmosphere.
[0088] <Comparative Example 5>
[0089] S1. Preparation of negative electrode: commercial graphite material is used as the negative electrode active material to prepare the negative electrode sheet, the negative electrode material is evenly ground with the conductive agent and the binder in a mass ratio of 8:1:1, then mixed with N-methylpyrrolidone to prepare the negative electrode slurry, and coated on the current collector, placed in a vacuum oven at 100°C for 10 hours, dried and cut into disc-shaped negative electrode sheets.
[0090] S2. Half-cell assembly: A lithium sheet was used as the counter electrode. The electrolyte was prepared by 1.0 mol LiPF6 in a solution of ethylene carbonate, diethyl carbonate and dimethyl carbonate (EC / DEC / DMC, v / v / v=1:1:1). The above-mentioned starch-based negative electrode sheet was assembled into a button cell in a glove box under an argon atmosphere.
[0091] Figure 1 This is a SEM image of the starch-based hard carbon composite graphite negative electrode material prepared in Example 4. Figure 1 It can be seen that graphite is evenly coated on the surface of spherical hard carbon. Due to the introduction of melamine cross-linking agent, the spherical structure of starch is maintained during high-temperature carbonization.
[0092] Figure 2 The XRD diagrams of starch-based hard carbon composite graphite negative electrode materials prepared in Example 1, Example 4, and Example 6 are shown in FIG. Figure 2 It can be seen that with the increase of the proportion of composite graphite, the intensity of the (002) peak increases, and the degree of graphitization of the material continues to increase.
[0093] Figure 3The battery assembled with the starch-based hard carbon composite graphite negative electrode material prepared in Example 4 of the present invention was subjected to a low current density of 25 mA g -1 The specific capacity of the starch-based hard carbon composite graphite negative electrode material prepared in Example 4 is as high as 425.6 mAh g -1 .
[0094] Figure 4 This is a GCD performance diagram of a battery assembled with starch-based hard carbon composite graphite negative electrode material prepared in Example 4 of the present invention. Figure 4 It can be seen that the starch-based hard carbon composite graphite anode material has excellent rate performance at 1A g -1 Still has 142.8mAh g -1 This is attributed to the good kinetics and abundant lithium storage sites of the graphite-coated spherical structure.
[0095] Figure 5 The battery assembled with the starch-based hard carbon composite graphite negative electrode material prepared in Examples 1-6 of the present invention was subjected to a current density of 0.1A g -1 The cycle performance comparison chart below. Figure 5 It can be seen that among the samples with different ratios of graphite and starch precursor, the electrochemical performance is best when the mass ratio of esterified starch to expanded graphite is 15:1.
[0096] Figure 6 The batteries assembled from the materials prepared in Comparative Examples 1-4 of the present invention were respectively subjected to a current density of 0.1Ag. -1 The cycle performance diagram below. Figure 6 It can be seen that the introduction of melamine cross-linking agent effectively improves the lithium storage capacity of esterified starch, and compared with other carbonization temperatures, the carbonization effect at 1100°C is the best.
[0097] Figure 7 The batteries assembled from the materials prepared in Comparative Examples 1-4 of the present invention were respectively subjected to a current density of 25m Ag -1 Comparison of the galvanostatic intermittent titration (GITT) curves and the calculated diffusion coefficients D during the lithiation and delithiation processes. Figure 7 It can be seen that the diffusion coefficient of Comparative Example 2 is the highest, indicating that the introduction of melamine makes the esterified starch have more active sites, which is more conducive to the storage of lithium ions.
[0098] Figure 8 The batteries assembled from the materials prepared in Example 3 of the present invention and Comparative Examples 2 and 4 were respectively subjected to a current density of 25m Ag. -1 Comparison of the galvanostatic intermittent titration (GITT) curves and the calculated diffusion coefficients D during the lithiation and delithiation processes. Figure 8It can be seen that the diffusion coefficient of Example 3 is the highest, and the starch-based hard carbon composite graphite has more active sites, which is more conducive to the storage of lithium ions.
[0099] Fig. 9 The battery assembled with the negative electrode materials prepared in Comparative Examples 2 and 5 of the present invention was subjected to a low current density of 25 mA g -1 The charge and discharge curves are shown below. Fig. 9 It can be seen that graphite negative electrode materials have a significant platform capacity, while hard carbon negative electrode materials are mainly based on slope capacity, which corresponds to their different lithium storage mechanisms. Figure 3 and Fig. 9 It can be seen that the specific capacity of the negative electrode material prepared in Example 4 is higher than that of the negative electrode materials prepared in Comparative Examples 2 and 5, and the starch-based hard carbon composite graphite obtains a negative electrode material with high lithium storage capacity.
[0100] For matters not mentioned above, the prior art applies.
[0101] Although some specific embodiments of the present invention have been described in detail through examples, those skilled in the art should understand that the above examples are for illustration only and are not intended to limit the scope of the present invention. Those skilled in the art to which the present invention belongs may make various modifications or supplements to the specific embodiments described or replace them in a similar manner, but they will not deviate from the direction of the present invention or exceed the scope defined by the attached claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc. made to the above embodiments based on the technical essence of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a starch-based hard carbon composite graphite negative electrode material, characterized in that: The expanded graphite and esterified starch are mixed, fully ground, and then carbonized to obtain the starch-based hard carbon composite graphite negative electrode material.
2. The preparation method according to claim 1, characterized in that: The mass ratio of the expanded graphite to the esterified starch is 1:1-30.
3. The preparation method according to claim 1, characterized in that: The carbonization temperature is 900-1300°C, and the carbonization time is 1-8h.
4. The preparation method according to claim 1, characterized in that: The heating rate of carbonization is 1-10°C / min.
5. The preparation method according to claim 1, characterized in that: The preparation method of esterified starch is as follows: corn starch is vacuum dried, and then hydrothermally reacted with melamine to obtain esterified starch.
6. The preparation method according to claim 5, characterized in that: The mass ratio of corn starch to melamine is 4:
1.
7. The preparation method according to claim 5, characterized in that: The hydrothermal reaction temperature is 50-150°C.
8. The preparation method according to claim 1, characterized in that: The expandable graphite is heated to 600° C. at a rate of 20-30° C. / min in a muffle furnace, kept at this temperature for 0.5-3 hours, and then cooled and collected to obtain the expandable graphite.
9. A starch-based hard carbon composite graphite negative electrode material prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the starch-based hard carbon composite graphite negative electrode material as claimed in claim 9 in a lithium battery.
Citation Information
Patent Citations
Hard carbon micro-spherical composite anode material of lithium battery and preparation method for hard carbon micro-spherical composite anode material
CN102364727A
Hard carbon / graphite composite negative electrode material and lithium ion battery as well as preparation method and application thereof
CN111244407A
Hard carbon negative electrode material, preparation method thereof and secondary battery
CN115838165A
Preparation method of starch-based hard carbon negative electrode material, negative electrode material and sodium ion battery
CN116768190A
Carbon based anode materials for lithium ion capacitor and preparation method thereof
KR101173673B1