Preparation method of aluminum nitride powder and aluminum nitride powder

Through the mixing and heating treatment of lactose and alumina in deionized water, combined with carbon-heat reduction and decarbonization treatment, the problems of complex preparation process and poor product quality of aluminum nitride powder are solved, and high fine particle size and low cost are achieved Preparation of aluminum nitride powder, suitable for industrial production.

CN119039006APending Publication Date: 2024-11-29XIAN RARE METAL MATERIALS RES INST CO LTD

Patent Information

Application Number
CN202410935658.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The preparation process of aluminum nitride powder is complex and the product quality is poor. The prior art has problems such as uneven mixing of raw materials, high nitriding temperature and introduction of impurities.

Method used

The mixture of lactose and alumina in deionized water was prepared by mixing it with stirring and heating, and then carbon-heat reduction and decarbonization in an air atmosphere were carried out in a nitrogen atmosphere to prepare a porous alumina substance with uniform carbon coating. , improve the contact area between carbon source and aluminum source, and achieve uniform mixing and low-temperature processes.

Benefits of technology

The process flow is simplified, the raw materials and process costs are reduced, and the aluminum nitride powder with high fine particle size is prepared, which is suitable for industrial production, and avoids the introduction of impurities and high temperature problems in traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039006A_ABST
    Figure CN119039006A_ABST
Patent Text Reader

Abstract

The invention provides an aluminum nitride powder preparation method and aluminum nitride powder, and relates to the technical field of ceramic materials. The preparation method of the aluminum nitride powder comprises the following steps: dispersing lactose and aluminum oxide in deionized water to obtain a mixed solution; stirring and heating the mixed solution to obtain jelly; heating the jelly, and carrying out foaming and curing processes on the jelly to obtain a reaction precursor; and sequentially carrying out carbon thermal reduction nitridation treatment in a nitrogen atmosphere and decarburization treatment in an air atmosphere on the reaction precursor to obtain the aluminum nitride powder. The preparation method of the aluminum nitride powder is simple in process, and the prepared aluminum nitride powder is high in quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of ceramic materials, and in particular to a method for preparing aluminum nitride powder and aluminum nitride powder. Background Art

[0002] Aluminum nitride is a new type of ceramic with excellent comprehensive properties and has attracted widespread attention in recent years. The theoretical thermal conductivity of aluminum nitride ceramics is as high as 320W / mK, which is 10 to 15 times that of the traditional substrate material aluminum oxide and close to the thermal conductivity of beryllium oxide, which is highly toxic. In addition, aluminum nitride also has excellent electrical insulation properties and a thermal expansion coefficient close to that of silicon. It can be used as a heat dissipation and packaging material for large-scale integrated circuits, semiconductor module circuits, and high-power devices.

[0003] High-quality powder raw materials are a prerequisite for obtaining high-performance products. The preparation of ceramic materials with excellent performance usually requires the use of powder raw materials with high purity, fine particle size and good sintering performance.

[0004] Currently, the preparation scheme of aluminum nitride powder has the problems of complicated process or poor quality of aluminum nitride powder product.

[0005] It should be noted that the information disclosed in the above background technology section is only used to enhance the understanding of the background of the present disclosure, and therefore may include information that does not constitute the prior art known to ordinary technicians in the field. Summary of the invention

[0006] The purpose of the present disclosure is to provide a method for preparing aluminum nitride powder and aluminum nitride powder, thereby overcoming the problem of complex aluminum nitride powder preparation process or poor product quality at least to a certain extent.

[0007] According to the first aspect of the present disclosure, a method for preparing aluminum nitride powder is provided, comprising: dispersing lactose and aluminum oxide in deionized water to obtain a mixed solution; stirring and heating the mixed solution to obtain a colloid; heating the colloid to subject the colloid to a foaming and solidification process to obtain a reaction precursor; and sequentially subjecting the reaction precursor to a carbon thermal reduction nitridation treatment in a nitrogen atmosphere and a decarburization treatment in an air atmosphere to obtain aluminum nitride powder.

[0008] Optionally, dispersing lactose and alumina in deionized water to obtain a mixed solution includes: adding lactose to deionized water and stirring until the lactose is dissolved in the deionized water; adding alumina to the deionized water in which the lactose is dissolved to obtain a mixed solution.

[0009] Optionally, dispersing lactose and aluminum oxide in deionized water to obtain a mixed solution includes: adding lactose and aluminum oxide into deionized water and stirring the deionized water by magnetic stirring to obtain a mixed solution.

[0010] Optionally, the molar ratio of alumina to lactose is 1:1 to 1:4.

[0011] Optionally, the particle size of the aluminum oxide is 0.01 μm to 4.8 μm.

[0012] Optionally, stirring and heating the mixed solution to obtain a jelly comprises: stirring the mixed solution at a heating temperature of 50° C. to 90° C. to obtain a jelly.

[0013] Optionally, the colloid is heated to undergo a foaming and curing process to obtain a reaction precursor, including: placing the colloid in an oven, heating the colloid at an oven temperature of 100° C. to 300° C., and subjecting the colloid to a foaming and curing process to obtain a reaction precursor.

[0014] Optionally, the temperature of the carbon thermal reduction nitriding treatment is 1500° C. to 1600° C., and the holding time is 1 h to 5 h.

[0015] Optionally, the decarburization treatment temperature is 600° C. to 800° C., and the holding time is 1 h to 5 h.

[0016] According to a second aspect of the present disclosure, an aluminum nitride powder is provided, wherein the aluminum nitride powder is prepared by any of the above-mentioned aluminum nitride powder preparation methods.

[0017] According to a third aspect of the present disclosure, there is provided an aluminum nitride product, which is prepared from the above-mentioned aluminum nitride powder.

[0018] According to the aluminum nitride powder preparation scheme of the embodiment of the present disclosure, on the one hand, the present disclosure scheme uses alumina and lactose as raw materials, and after mixing, a porous alumina substance uniformly coated with carbon can be obtained, which can achieve uniform mixing of the carbon source and the aluminum source, and the contact area is significantly increased, which is conducive to the full and rapid progress of the carbon thermal reduction reaction, and at least solves the problems of uneven raw material mixing, high nitriding temperature and easy introduction of impurities during the ball milling process in the traditional solid phase mixing scheme; on the other hand, the present disclosure uses alumina as the aluminum source, breaking the limitation of only using soluble aluminum salts as the aluminum source in the wet chemical scheme, and the present disclosure scheme does not need to add dispersants, chelating agents, pH adjusters and other additives, and has low preparation requirements; on the other hand, the process of the present disclosure is simple, the raw material and process costs are low, and fine-grained aluminum nitride powder can be prepared and is conducive to industrial production.

[0019] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The accompanying drawings herein are incorporated into the specification and constitute a part of the specification, illustrate embodiments consistent with the present disclosure, and together with the specification are used to explain the principles of the present disclosure. Obviously, the accompanying drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without creative work.

[0021] Figure 1 A flow chart of a method for preparing aluminum nitride powder according to an exemplary embodiment of the present disclosure is schematically shown.

[0022] Figure 2 The SEM (Scanning Electron Microscope) image of the aluminum nitride powder prepared in Example 1 of the present disclosure is schematically shown.

[0023] Figure 3 The SEM image of the aluminum nitride powder prepared in Example 2 of the present disclosure is schematically shown.

[0024] Figure 4 The SEM image of the aluminum nitride powder prepared in Example 3 of the present disclosure is schematically shown.

[0025] Figure 5 The SEM image of the aluminum nitride powder prepared in Example 4 of the present disclosure is schematically shown.

[0026] Figure 6 The SEM image of the aluminum nitride powder prepared in Example 5 of the present disclosure is schematically shown.

[0027] Figure 7 The XRD (X-Ray Diffraction) comparison diagram of the powders prepared in Example 1, Example 2, Example 3 and Comparative Example 1 of the present disclosure is schematically shown. DETAILED DESCRIPTION

[0028] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as being limited to the examples set forth herein; on the contrary, these embodiments are provided so that the present disclosure will be more comprehensive and complete, and the concepts of the example embodiments are fully conveyed to those skilled in the art. The described features, structures, or characteristics may be combined in any suitable manner in one or more embodiments. In the following description, many specific details are provided to provide a full understanding of the embodiments of the present disclosure. However, those skilled in the art will appreciate that the technical solutions of the present disclosure may be practiced while omitting one or more of the specific details, or other methods, processes, steps, etc. may be adopted. In other cases, known technical solutions are not shown or described in detail to avoid obscuring various aspects of the present disclosure.

[0029] In addition, the accompanying drawings are only schematic illustrations of the present disclosure and are not necessarily drawn to scale. The same reference numerals in the figures represent the same or similar parts, and thus their repeated descriptions will be omitted. The flowcharts shown in the accompanying drawings are only exemplary illustrations and do not necessarily include all the steps. For example, some steps can also be decomposed, while some steps can be combined or partially combined, so the actual execution order may change according to the actual situation.

[0030] The carbon thermal reduction method is one of the main methods for industrial production of aluminum nitride powder. The method includes subjecting a mixed raw material containing aluminum and carbon or a reaction precursor to a carbon thermal reduction reaction at high temperature in a nitrogen atmosphere to generate aluminum nitride. This method has the advantages of low raw material prices, simple process, stable performance of the prepared aluminum nitride powder, controllable powder morphology and particle size, and good forming and sintering performance. It is generally believed that the smaller the particle size of the raw material, the more uniform the mixing, the higher the reaction activity, the faster the carbon thermal reduction reaction rate, and the finer the prepared aluminum nitride powder.

[0031] The schemes for mixing raw materials or reaction precursors include solid-phase mixing method and wet chemical method. The solid-phase mixing method is to mechanically mix the solid aluminum source and carbon source. Although this method has a simple process, it has problems such as uneven mixing of raw materials, high nitridation temperature, easy introduction of impurities during ball milling, and easy agglomeration of products. The wet chemical method is to synthesize the reaction precursor in the liquid phase. This method has the characteristics of precise control of the content of product components and molecular / atomic scale mixing. It can prepare powders with narrow particle size distribution and regular morphology. However, the aluminum source and carbon source of this method need to be soluble aluminum salts and soluble carbon, which has high raw material requirements, and needs to add dispersants, chelating agents and other additives as well as pH adjustment processes, and the preparation process is complicated.

[0032] In order to solve or at least alleviate the above problems, the embodiments of the present disclosure provide a new method for preparing aluminum nitride powder.

[0033] Figure 1 The flowchart of the method for preparing aluminum nitride powder according to an exemplary embodiment of the present disclosure is schematically shown. Figure 1 The method for preparing aluminum nitride powder according to the embodiment of the present disclosure comprises the following steps: S12. Disperse lactose and aluminum oxide in deionized water to obtain a mixed solution.

[0034] According to some embodiments of the present disclosure, first, lactose is added to deionized water and stirred until the lactose is dissolved in the deionized water. Next, aluminum oxide is added to the deionized water in which the lactose is dissolved to obtain a mixed solution.

[0035] According to some other embodiments of the present disclosure, lactose and aluminum oxide may be added to deionized water at the same time and stirred sufficiently to obtain a mixed solution.

[0036] In the process of obtaining the mixed solution, the solution may be stirred continuously to make it uniform. Specifically, regardless of all the above embodiments, lactose and aluminum oxide may be added to deionized water and stirred by, for example, magnetic stirring to obtain a mixed solution.

[0037] The molar ratio of alumina to lactose can be configured to be 1:1 to 1:4. Thus, sufficient carbon can be guaranteed to participate in the subsequent nitridation reaction, ensuring complete nitridation of the alumina.

[0038] The particle size of the aluminum oxide used in the embodiment of the present disclosure is 0.01 μm to 4.8 μm, thereby ensuring that the particle size of the aluminum nitride generated subsequently is fine.

[0039] The disclosed embodiment uses lactose and micron-sized or even nano-sized alumina as the carbon source and aluminum source. The mixed solution thereof can form a porous alumina substance uniformly coated with carbon after subsequent treatment, thereby increasing the contact area between the carbon source and the aluminum source and significantly improving the mixing uniformity of the carbon source and the aluminum source.

[0040] S14. The mixed solution is stirred and heated to obtain a jelly.

[0041] After the mixed solution is obtained in step S12, the mixture is continuously stirred and heated to obtain a jelly, wherein the jelly can also be referred to as a jelly-like substance. Compared with the mixed solution, the jelly is viscous, and the present disclosure does not limit the degree of the viscosity.

[0042] Specifically, the mixed solution can be stirred at a heating temperature of 50° C. to 90° C. to obtain a jelly. It is understood that the heating time at this stage is related to the specific temperature and the amount of the mixed solution, and the present disclosure does not limit the time.

[0043] S16. The colloid is heated to make the colloid undergo a foaming and curing process to obtain a reaction precursor.

[0044] According to some embodiments of the present disclosure, the jelly obtained in step S14 can be placed in an oven and heated at an oven temperature of 100° C. to 300° C. to make the jelly undergo a foaming and curing process to obtain a reaction precursor. Similarly, the present disclosure does not limit the time of this heating process.

[0045] It should be understood that the above-mentioned method of heating in an oven is only an exemplary description. In other embodiments of the present disclosure, heating can also be performed by, for example, using an open flame, and the present disclosure does not limit this.

[0046] Through the heating process of step S14 and step S16, the purpose of removing water in the solution and carbonizing lactose can be effectively achieved.

[0047] S18. The reaction precursor is sequentially subjected to a carbon thermal reduction nitridation treatment in a nitrogen atmosphere and a decarburization treatment in an air atmosphere to obtain an aluminum nitride powder.

[0048] In an exemplary embodiment of the present disclosure, the temperature of the carbothermal reduction nitriding treatment is 1500° C. to 1600° C., and the holding time is 1 to 5 hours. The temperature of the decarburization treatment is 600° C. to 800° C., and the holding time is 1 to 5 hours.

[0049] By configuring the above process parameters, the carbon thermal reduction nitridation reaction and decarburization can be smoothly carried out to obtain aluminum nitride powder.

[0050] According to the test, the particle size of the aluminum nitride powder prepared by the above preparation method of the present disclosure ranges from 0.05 μm to 6 μm.

[0051] In order to illustrate the aluminum nitride powder preparation scheme disclosed in the present invention in more detail, it is described in detail below through examples and comparative examples.

[0052] Example 1 First, 10 nm alumina and lactose were added to deionized water at a molar ratio of 1:1, and magnetic stirring was performed to obtain a mixed solution.

[0053] Next, the mixed solution is continuously stirred magnetically and heated to a colloid, and the colloid is placed in an oven to heat and foam it and finally solidify it to obtain a reaction precursor in which aluminum oxide and carbon are uniformly mixed. The heating temperature of the magnetic stirring is set to 90°C, and the oven temperature is set to 200°C.

[0054] Then, the reaction precursor is subjected to a carbon thermal reduction nitridation reaction in a nitrogen atmosphere at 1600° C. for 2 hours and a decarburization treatment in an air atmosphere at 700° C. for 3 hours to obtain aluminum nitride powder. Figure 2 The SEM image of the aluminum nitride powder prepared in Example 1 of the present disclosure is schematically shown. According to the test, Example 1 prepared aluminum nitride powder with an average particle size of about 60 nm.

[0055] Example 2 First, 10 nm alumina and lactose were added to deionized water at a molar ratio of 1:2, and magnetic stirring was performed to obtain a mixed solution.

[0056] Next, the mixed solution is continuously stirred magnetically and heated to a colloid, and the colloid is placed in an oven to heat and foam it and finally solidify it to obtain a reaction precursor in which aluminum oxide and carbon are uniformly mixed. The heating temperature of the magnetic stirring is set to 50°C, and the oven temperature is set to 300°C.

[0057] Then, the reaction precursor is subjected to a carbon thermal reduction nitridation reaction in a nitrogen atmosphere at 1600° C. for 2 hours and a decarburization treatment in an air atmosphere at 600° C. for 5 hours to obtain aluminum nitride powder. Figure 3 The SEM image of the aluminum nitride powder prepared in Example 2 of the present disclosure is schematically shown. According to the test, Example 2 prepared aluminum nitride powder with an average particle size of about 80 nm.

[0058] Example 3 First, 10 nm alumina and lactose were added to deionized water at a molar ratio of 1:1, and magnetic stirring was performed to obtain a mixed solution.

[0059] Next, the mixed solution is continuously stirred magnetically and heated to a colloid, and the colloid is placed in an oven, heated to foam and finally solidified to obtain a reaction precursor in which aluminum oxide and carbon are uniformly mixed. The heating temperature of the magnetic stirring is set to 50°C, and the oven temperature is set to 100°C.

[0060] Then, the reaction precursor is subjected to a carbon thermal reduction nitridation reaction in a nitrogen atmosphere at 1500° C. for 2 hours and a decarburization treatment in an air atmosphere at 800° C. for 1 hour to obtain aluminum nitride powder. Figure 4 The SEM image of the aluminum nitride powder prepared in Example 3 of the present disclosure is schematically shown. According to the test, Example 3 prepared aluminum nitride powder with an average particle size of about 50 nm.

[0061] Example 4 First, 1.1 μm alumina and lactose were added to deionized water at a molar ratio of 1:1, and magnetic stirring was performed to obtain a mixed solution.

[0062] Next, the mixed solution is continuously stirred magnetically and heated to a colloid, and the colloid is placed in an oven to heat and foam it and finally solidify it to obtain a reaction precursor in which aluminum oxide and carbon are uniformly mixed. The heating temperature of the magnetic stirring is set to 80°C, and the oven temperature is set to 200°C.

[0063] Then, the reaction precursor is subjected to a carbon thermal reduction nitridation reaction in a nitrogen atmosphere at 1600° C. for 2 hours and a decarburization treatment in an air atmosphere at 700° C. for 3 hours to obtain aluminum nitride powder. Figure 5 The SEM image of the aluminum nitride powder prepared in Example 4 of the present disclosure is schematically shown. According to the test, Example 4 prepared aluminum nitride powder with an average particle size of about 1.5 μm.

[0064] Example 5 First, 4.8 μm alumina and lactose were added to deionized water at a molar ratio of 1:1, and magnetic stirring was performed to obtain a mixed solution.

[0065] Next, the mixed solution is continuously stirred magnetically and heated to a colloid, and the colloid is placed in an oven to heat and foam it and finally solidify it to obtain a reaction precursor in which aluminum oxide and carbon are uniformly mixed. The heating temperature of the magnetic stirring is set to 90°C, and the oven temperature is set to 300°C.

[0066] Then, the reaction precursor is subjected to a carbon thermal reduction nitridation reaction in a nitrogen atmosphere at 1600° C. for 5 hours and a decarburization treatment in an air atmosphere at 600° C. for 5 hours in order to obtain aluminum nitride powder. Figure 6 The SEM image of the aluminum nitride powder prepared in Example 5 of the present disclosure is schematically shown. According to the test, Example 5 prepared aluminum nitride powder with an average particle size of about 6 μm.

[0067] Comparative Example 1 Carbon black and aluminum oxide are mixed and nitrogen is introduced into a high-temperature furnace for reaction to generate aluminum nitride. The temperature of the high-temperature furnace is set to 1600°C. After the reaction is completed, the product is cooled to room temperature to obtain a powder.

[0068] Figure 7 The XRD comparison diagrams of the powders prepared in Example 1, Example 2, Example 3 and Comparative Example 1 of the present disclosure are schematically shown. The abscissa of the XRD diagram represents the 2θ angle, in degrees, which represents the angle between the extended line of the incident X-ray and the reflected X-ray. The ordinate of the XRD diagram represents the relative intensity (intensity au), which reflects the number of photons collected.

[0069] refer to Figure 7It can be seen that the aluminum nitride powder preparation method of the present disclosure in Example 1, Example 2 and Example 3 can prepare aluminum nitride powder with a single component, while for Comparative Example 1, in addition to aluminum nitride, there is also incompletely converted aluminum oxide. Therefore, based on the description of the above process, compared with Comparative Example 1, the aluminum nitride powder preparation scheme of the present disclosure embodiment can at least achieve the advantages of lower process temperature and higher powder quality.

[0070] Furthermore, the embodiment of the present disclosure also provides an aluminum nitride powder, which is prepared by the above-mentioned aluminum nitride powder preparation method.

[0071] Furthermore, the embodiments of the present disclosure also provide an aluminum nitride product, which is prepared from the above-mentioned aluminum nitride powder.

[0072] It should be noted that although the steps of the method in the present disclosure are described in a specific order in the drawings, this does not require or imply that the steps must be performed in this specific order, or that all the steps shown must be performed to achieve the desired results. Additionally or alternatively, some steps may be omitted, multiple steps may be combined into one step, and / or one step may be decomposed into multiple steps, etc.

[0073] In addition, the above-mentioned figures are only schematic illustrations of the processes included in the method according to the exemplary embodiments of the present disclosure, and are not intended to be limiting. It is easy to understand that the processes shown in the above-mentioned figures do not indicate or limit the time sequence of these processes. In addition, it is also easy to understand that these processes can be performed synchronously or asynchronously, for example, in multiple modules.

[0074] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing what is disclosed herein. This application is intended to cover any variations, uses, or adaptations of the present disclosure that follow the general principles of the present disclosure and include common knowledge or customary technical means in the art that are not disclosed in the present disclosure. The specification and embodiments are to be considered merely as exemplary, and the true scope and spirit of the present disclosure are indicated by the claims.

[0075] It should be understood that the present disclosure is not limited to the exact structures that have been described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof. The scope of the present disclosure is limited only by the appended claims.

Claims

1. A method for preparing aluminum nitride powder, characterized in that: include: dispersing lactose and aluminum oxide in deionized water to obtain a mixed solution; Stirring and heating the mixed solution to obtain a jelly; Heating the colloid so as to make the colloid undergo a foaming and curing process to obtain a reaction precursor; The reaction precursor is subjected to a carbon thermal reduction nitridation treatment in a nitrogen atmosphere and a decarburization treatment in an air atmosphere in sequence to obtain aluminum nitride powder.

2. The method for preparing aluminum nitride powder according to claim 1, characterized in that: Lactose and alumina are dispersed in deionized water to obtain a mixed solution comprising: Adding lactose into deionized water and stirring until the lactose is dissolved in the deionized water; Alumina is added into the deionized water in which the lactose is dissolved to obtain a mixed solution.

3. The method for preparing aluminum nitride powder according to claim 1, characterized in that: Lactose and alumina are dispersed in deionized water to obtain a mixed solution comprising: Lactose and alumina are added into deionized water and stirred by magnetic stirring to obtain a mixed solution.

4. The method for preparing aluminum nitride powder according to any one of claims 1 to 3, characterized in that: The molar ratio of the aluminum oxide to the lactose is 1:1 to 1:

4.

5. The method for preparing aluminum nitride powder according to any one of claims 1 to 3, characterized in that: The particle size of the aluminum oxide is 0.01 μm to 4.8 μm.

6. The method for preparing aluminum nitride powder according to claim 1, characterized in that: The mixed solution is stirred and heated to obtain a jelly, comprising: The mixed solution is stirred at a heating temperature of 50° C. to 90° C. to obtain a jelly.

7. The method for preparing aluminum nitride powder according to claim 1, characterized in that: The colloid is heated to make the colloid undergo a foaming and curing process to obtain a reaction precursor, comprising: The colloid is placed in an oven and heated at an oven temperature of 100° C. to 300° C., so that the colloid undergoes a foaming and curing process to obtain a reaction precursor.

8. The method for preparing aluminum nitride powder according to claim 1, characterized in that: The temperature of the carbon thermal reduction nitriding treatment is 1500° C. to 1600° C., and the insulation time is 1 hour to 5 hours.

9. The method for preparing aluminum nitride powder according to claim 1, characterized in that: The decarburization treatment temperature is 600° C. to 800° C., and the insulation time is 1 hour to 5 hours.

10. An aluminum nitride powder, characterized in that: The aluminum nitride powder is prepared by the aluminum nitride powder preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for synthesizing aluminum nitride power

    CN105837223A

  • Preparation method of silicon carbon negative pole composite material

    CN106784768A

  • Preparation method of aluminum nitride powder

    CN109293368A

  • Multilayer porous hollow bowl-shaped carbon material and preparation method thereof

    CN110171812A

  • High-activity aluminum nitride powder precursor, preparation method and application thereof

    CN110668823A

Cited By

  • Low-oxygen-content aluminum nitride powder and preparation method thereof

    CN121134700A