Ketoimine zinc complex as well as preparation method and application thereof
By preparing ketoimine zinc complex in a protected gas environment, the problems of low yield and insufficient catalytic activity in catalytic lactide ring-opening polymerization are solved, and high-efficiency catalytic lactide ring-opening is achieved Polymerization obtains high molecular weight PLA and has a wider application in the field of biomedicine.
Patent Information
- Application Number
- CN202310619837.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-05-29
AI Technical Summary
In the preparation and catalytic ring-opening polymerization of lactide, existing non-tin metal complex catalysts have problems such as low yield, insufficient catalytic activity and small PLA molecular weight, and the factors affect each other complexly, making it difficult to improve performance.
Using ketoimine zinc complex as a catalyst, the ZnEt2 solution dropwise to the β-ketoimine ligand solution in a protective gas environment to prepare a high yield of ketoimine zinc complex and catalyzed in the catalytic C. High-efficiency catalysis is achieved in the ring-opening polymerization of lactides with high molar ratio and short time.
Achieve high yield (99%) and high catalytic activity of ketoimine zinc complex, catalyzed ring-opening polymerization of lactide to obtain PLA with a molecular weight of more than 150,000 without purification, reducing economic losses, and in the field of biomedical medicine Have a wider application.
Smart Images

Figure CN119039162A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of complex preparation and application, and particularly relates to a ketimine zinc complex, a preparation method of the ketimine zinc complex, and application of the ketimine zinc complex in catalyzing the ring-opening polymerization of lactide. Background Art
[0002] Polylactide (PLA) is a polymer with good biocompatibility, biodegradability and physical and mechanical properties. PLA has good tensile strength and ductility and can be decomposed into carbon dioxide and water in the body, which makes it an ideal biomedical material. PLA can be used in drug delivery, surgical suture materials and artificial tissue materials, and has great research value.
[0003] At present, the industrial production of PLA is mainly through the ring-opening polymerization of lactide catalyzed by stannous octoate. However, the polymer obtained by the ring-opening polymerization of cyclic lactone catalyzed by metal complex catalysts will inevitably contain some metal residues. The PLA obtained by the ring-opening polymerization of lactide catalyzed by stannous octoate will contain tin residues. The tin element itself is toxic and harmful to the human body, which will limit the application of PLA in the food and medical fields. Therefore, it is of great significance to develop environmentally friendly metal complex catalysts and realize the green and environmentally friendly process to produce polylactide.
[0004] Nowadays, there are some studies on non-tin metal complex catalysts, such as Zn, Mg, and Al metal complex catalysts. However, these non-tin metal complex catalysts have many problems in the preparation process and in the process of catalyzing the ring-opening polymerization of lactide to produce PLA. Among them, the most important problems include the low yield of non-tin metal complex catalysts during preparation, which need to be purified before use, the small molecular weight of PLA produced by catalyzing the ring-opening polymerization of lactide, and the low activity when catalyzing the ring-opening polymerization of lactide to produce PLA. Among the existing non-tin metal complex catalysts, even the better solutions usually only have a yield of about 60% during the preparation process. When used to catalyze the ring-opening polymerization of lactide to produce PLA, the molecular weight of the PLA prepared is difficult to exceed 100,000, and the dosage ratio (molar ratio) with lactide usually needs to reach 1:100-1000 (for example, the metal complex catalyst provided in "Syntheses, structures and catalysis of tetranuclear zinc N-alkoxide ketoiminate complexes for ring-opening polymerization of rac-lactide" published in Inorganic Chemistry Communications, Issue 119, 2020). Therefore, researchers in the industry are committed to studying solutions that can improve the performance of non-tin metal complex catalysts.
[0005] However, it is very difficult to improve the performance of metal complex catalysts. The catalytic activity of metal complex catalysts is closely related to the ligands and metal ions used. The type of ligand, the site of the ligand substituent, the type of ligand substituent, the type of metal ion, and the coordination number of the metal ion all affect the preparation method, purification, yield, structure, catalytic activity, etc. of the complex individually and mutually. Due to the diversity of influencing factors and the uncertainty of the influence relationship between each influencing factor (for example, the type of ligand, the site of ligand substituent, the type of metal ion, and the coordination number of metal ion are all determined, and the only difference is that for a certain type of metal complex with different ligand substituents, the improvement in catalytic activity may be related to the existence of relationship A between the substituents, but when the coordination number of this type of metal complex is changed, the improvement in catalytic activity may be related to the existence of relationship B between the substituents that is completely opposite to or completely unrelated to relationship A, and when the coordination number and the type of metal ion of this type of metal complex are changed, the improvement in catalytic activity may be related to the existence of relationship C between the substituents that is completely opposite to or completely unrelated to relationship A and relationship B), it is difficult for researchers to simply infer and determine the factors that effectively improve the performance of the complex.
[0006] In summary, it is still necessary to study metal complexes that are easy to synthesize (with high yield), can catalyze the ring-opening polymerization of lactide to obtain high molecular weight PLA, and have high activity in catalyzing the ring-opening polymerization of lactide. Summary of the invention
[0007] The object of the present invention is to provide a metal complex which is easy to synthesize (with high yield), can catalyze the ring-opening polymerization of lactide to obtain high molecular weight PLA and has high activity in catalyzing the ring-opening polymerization of lactide, as well as a method for preparing the metal complex and a specific application of the metal complex.
[0008] In order to achieve the above objectives, the present invention provides the following four technical solutions.
[0009] In a first aspect, the present invention provides a ketimine zinc complex having a structure shown in Formula I:
[0010]
[0011] In formula I, R is any one of a C2-C4 straight-chain alkyl group and its derivatives, a C2-C4 branched-chain alkyl group and its derivatives.
[0012] According to a preferred embodiment of the first aspect, in Formula I, R is any one of a C2-C4 straight-chain alkyl group and a C2-C4 branched-chain alkyl group;
[0013] Further, in Formula I, R is one of -CH2CH2-, -CH(CH3)CH2-, -CH2CH(CH3)-, -CH2CH2CH2CH2-, -CH(CH3)CH2CH2-;
[0014] Furthermore, in Formula I, R is any one of -CH2CH2-, -CH(CH3)CH2-, -(R)-CH2CH(CH3)-, -(S)-CH2CH(CH3)-, -CH2CH2CH2CH2-, -(R)-CH(CH3)CH2CH2- and -(S)-CH(CH3)CH2CH2-. In the present invention, R in -(R)-CH2CH(CH3)- and -(R)-CH(CH3)CH2CH2- refers to chiral R type.
[0015] In a second aspect, the present invention provides a method for preparing the ketimine zinc complex provided in the first aspect, wherein the method comprises:
[0016] In a protective gas environment, adding a ZnEt2 solution dropwise to a β-ketimine ligand solution at a temperature range of 60° C. to 100° C. to react to obtain the ketimine zinc complex;
[0017] Wherein, the β-ketoimine ligand has a structure shown in Formula II:
[0018]
[0019] R in Formula II is the same as R in Formula I;
[0020] That is, in formula II, R is any one of a C2-C4 straight-chain alkyl group and its derivatives, a C1-C4 branched-chain alkyl group and its derivatives; further, R is any one of a C2-C4 straight-chain alkyl group and a C1-C4 branched-chain alkyl group; further, R is one of -CH2CH2-, -CH(CH3)CH2-, -CH2CH(CH3)-, -CH2CH2CH2CH2-, and -CH(CH3)CH2CH2-; further, R is any one of -CH2CH2-, -CH(CH3)CH2-, -(R)-CH2CH(CH3)-, -(S)-CH2CH(CH3)-, -CH2CH2CH2CH2-, -(R)-CH(CH3)CH2CH2-, and -(S)-CH(CH3)CH2CH2-.
[0021] According to a preferred embodiment of the second aspect, the molar ratio of ZnEt2 to the β-ketoimine ligand in the β-ketoimine ligand solution is 0.8-1.2:1 (eg 1:1).
[0022] According to a preferred embodiment of the second aspect, the solvent in the β-ketoimine ligand solution includes at least one of toluene, hexane, dichloromethane and tetrahydrofuran.
[0023] According to a preferred embodiment of the second aspect, the solvent in the ZnEt2 solution includes at least one of toluene and hexane.
[0024] According to a preferred embodiment of the second aspect, the reaction time is 30-60 min.
[0025] In a third aspect, the present invention provides use of the ketimine zinc complex provided in the first aspect as a catalyst in catalyzing the ring-opening polymerization of lactide.
[0026] According to a preferred embodiment of the third aspect, the application is the use of the ketimine zinc complex as a catalyst in catalyzing the ring-opening polymerization of lactide to prepare PLA with a number average molecular weight of more than 150,000.
[0027] In a fourth aspect, the present invention provides a method for preparing PLA by ring-opening polymerization of lactide, wherein the method comprises:
[0028] The lactide monomer is mixed with the ketimine zinc complex provided in the first aspect and then reacted to prepare PLA.
[0029] According to a preferred embodiment of the fourth aspect, the lactide monomer is mixed with the ketimine zinc complex provided in the first aspect at a molar ratio of 5000-50000:1;
[0030] Further, the lactide monomer is mixed with the ketimine zinc complex provided in the first aspect at a molar ratio of 15000-50000:1;
[0031] Furthermore, the lactide monomer is mixed with the ketimine zinc complex provided in the first aspect at a molar ratio of 15000-40000:1.
[0032] According to a preferred embodiment of the fourth aspect, the reaction temperature is 80-180°C;
[0033] Further, the reaction temperature is 130-180°C;
[0034] Furthermore, the reaction temperature is 130-150°C.
[0035] According to a preferred embodiment of the fourth aspect, the reaction is performed until the powder is completely converted into a gel solid;
[0036] Further, the lactide monomer and the ketimine zinc complex are mixed at a molar ratio of 5000-50000:1, the reaction temperature is 80-180° C., and the reaction time is 5 s-5 min;
[0037] Further, when the lactide monomer and the ketimine zinc complex are mixed at a molar ratio of 15000-50000:1 and the reaction temperature is 130-180° C., the reaction time is 5 s-4 min;
[0038] Furthermore, when the lactide monomer and the ketimine zinc complex are mixed at a molar ratio of 15000-40000:1 and the reaction temperature is 130-150° C., the reaction time is 5 s-3 min.
[0039] According to a preferred embodiment of the fourth aspect, the lactide monomer includes at least one of L-lactide and racemic lactide.
[0040] According to a preferred embodiment of the fourth aspect, the lactide monomer and the ketimine zinc complex provided by the first aspect can be mixed and reacted in the presence of a solvent or in the absence of a solvent;
[0041] Furthermore, the lactide monomer is mixed with the ketimine zinc complex provided in the first aspect and reacted in the absence of a solvent.
[0042] According to a preferred embodiment of the fourth aspect, the method for preparing PLA by ring-opening polymerization of lactide comprises:
[0043] The racemic lactide and the ketimine zinc complex provided in the first aspect are mixed at a molar ratio of 15000-40000:1 and reacted at 130-150°C to prepare PLA; this preferred technical solution can obtain PLA with a molecular weight greater than 150000 and a racemic lactide conversion rate of more than 80%;
[0044] Furthermore, racemic lactide and the ketimine zinc complex provided in the first aspect are mixed at a molar ratio of 15000-20000:1 and reacted at 130-150° C. to prepare PLA; this preferred technical solution can obtain PLA with a molecular weight greater than 150,000 and a racemic lactide conversion rate of more than 90%.
[0045] The ketimine zinc complex provided by the present invention is a tetranuclear zinc complex with zinc as the coordination metal and β-ketimine as the ligand, wherein the substituent on the carbon atom of the ligand skeleton is an isopropyl group and the substituent on the N atom is a C2-C4 alkyl group or its derivative. Compared with the prior art, it has the following beneficial effects:
[0046] 1. The yield of metal complexes provided by the prior art is generally low, usually only about 60%; while the metal complex provided by the present invention can achieve a yield of 99% when prepared by the preparation method provided by the present invention, which is far higher than the prior art, and can be used directly without purification, thus avoiding the economic loss caused by purifying the catalyst.
[0047] 2. The metal complex provided in the prior art is used in large amounts and for a long time to catalyze the ring-opening polymerization of lactide to prepare PLA. Usually, the amount ratio (molar ratio) to lactide needs to reach 1:100-1000, and the catalytic time is at least 3 minutes. However, the metal complex provided in the present invention is used in significantly reduced amounts and in a very short time to catalyze the ring-opening polymerization of lactide to prepare PLA. The amount ratio (molar ratio) to lactide is 1:15000-50000, and the catalytic time is as fast as 5 seconds, and the catalytic activity far exceeds the prior art.
[0048] 3. When the metal complex provided by the prior art is used to catalyze the ring-opening polymerization of lactide to prepare PLA, the molecular weight of the PLA prepared is relatively small, usually not exceeding 100,000; while when the metal complex provided by the present invention is used to catalyze the ring-opening polymerization of lactide to prepare PLA, the molecular weight of the PLA prepared is significantly increased, generally above 150,000, and in preferred embodiments can exceed 200,000.
[0049] 4. The metal complex provided by the present invention uses zinc metal as the coordination metal. Zinc is cheap and easily available, and as one of the trace elements of the human body, it has good biocompatibility, making the polymerization process more green and environmentally friendly. The synthesized polyester material also has less biological toxicity, making it have a wider application in the fields of biomedicine and the like.
[0050] 5. The metal complex provided by the present invention can directly catalyze the ring-opening polymerization of racemic lactide and L-lactide in the form of bulk or solution under the protection of anhydrous, oxygen-free and inert gas to obtain high molecular weight PLA with a narrow molecular weight distribution without the participation of a co-catalyst. DETAILED DESCRIPTION
[0051] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0052] In Examples 1 to 6 of the present invention, β-ketoimine ligand 1a, β-ketoimine ligand 1b, β-ketoimine ligand 1c, β-ketoimine ligand 1d, β-ketoimine ligand 1e, and β-ketoimine ligand 1f are used to prepare ketimine zinc complex 2a, ketimine zinc complex 2b, ketimine zinc complex 2c, ketimine zinc complex 2d, ketimine zinc complex 2e, and ketimine zinc complex 2f. The reaction formula involved is shown in Formula III:
[0053]
[0054] Example 1
[0055] This embodiment provides a ketimine zinc complex 2a, whose structural formula is [(CH3)2CHC(O)CHCN(CH2CH2O)CH(CH3)2]4Zn4, and the structural formula is 2a in Formula III. The preparation method comprises:
[0056] In an argon environment, 0.40 g (about 2.0 mmol) of β-ketimine ligand 1a (structural formula see 1a in Formula III) was dissolved in toluene that had been subjected to anhydrous and oxygen-free treatment to obtain a β-ketimine ligand solution, the β-ketimine ligand solution was heated to 60° C., and then 1.0 mL of diethyl zinc solution (concentration of 2 M, solvent of toluene, total amount of diethyl zinc 2.0 mmol) was added dropwise thereto, and the reaction was stirred at 60° C. for 30 min to obtain a colorless clear solution; the solvent was vacuum-evacuated to obtain a white powder, and the preparation of the ketimine zinc complex 2a was completed.
[0057] The products were characterized by NMR, elemental analysis and high-resolution mass spectrometry.
[0058] Yield of ketimine zinc complex 2a: 0.52 g (99%).
[0059] 1 H-NMR (400MHz, CDCl3): δ=4.84(s,4H,C(O)CH=CN),3.97-3.91(m,4H,NCH2CH2O),3.74-3.69(m,4H,NCH2CH2O),3.6-3.55(m,4H,NCH2CH2 O), 3.18-3.11(m,4H,NCH2CH2O), 2.94(sept,J=6.8Hz,4H,Me2CHC(O)), 2.34(sept,J=6.8Hz,4H,Me2CHC(N)), 1.13-1.07(m,48H,Me2CH). 13 C NMR (100MHz, CDCl3): δ=192.2,181.3,86.9,63.7,50.4,39.7,31.2,21.7,21.4,21.1,20.9.
[0060] Elemental analysis: C 44 H 76 Theoretical content of N4O8Zn4 (%): C, 50.30; H, 7.29; N, 5.33; measured content (%): C, 50.58; H, 7.317; N, 5.13.
[0061] MALDI-TOF HRMS:C 44 H 76 N4O8Zn4+H + The theoretical value is 1045.2902, and the measured value is 1045.2883.
[0062] Example 2
[0063] This embodiment provides a ketimine zinc complex 2b, whose structural formula is [(CH3)2CHC(O)CHCN((S)-CH2CH(CH3)O)CH(CH3)2]4Zn4, and the structural formula is 2b in Formula III. The preparation method comprises:
[0064] In an argon environment, 0.43 g (about 2.0 mmol) of β-ketimine ligand 1b (structural formula see 1b in Formula III) was dissolved in toluene that had been subjected to anhydrous and oxygen-free treatment to obtain a β-ketimine ligand solution, the β-ketimine ligand solution was heated to 60° C., and then 1.0 mL of diethyl zinc solution (concentration of 2 M, solvent of toluene, total amount of diethyl zinc 2.0 mmol) was added dropwise thereto, and the reaction was stirred at 60° C. for 30 min to obtain a colorless clear solution; the solvent was vacuum-evacuated to obtain a white powder, and the preparation of the ketimine zinc complex 2b was completed.
[0065] The products were characterized by NMR and elemental analysis.
[0066] Yield of ketimine zinc complex 2b: 0.55 g (99%).
[0067] 1 H-NMR (400MHz, CDCl3): δ=4.84(s,2H,C(O)CH=CN), 4.82(s,2H,C(O)CH=CN), 3.99-3.91(m,2H,CH2CHMeO), 3.84-3.76(m,2H,NCH2CHMeO),3.75-3.69(m,2H,CH2CHMeO),3.41-3.27(m,4H,NCH2CHMeO),3.06(sept,J= 6.8Hz,2H,Me2CHC(O)),2.83(sept,J=6.8Hz,2H,Me2CHC(O)),2.56-2.45(m,2H,NCH2CHMeO),2.38-2.24(m ,4H,Me2CHC(N)),1.39(d,J=6Hz,6H,NCH2CHMeO),1.19-0.95(48H,Me2CH),0.84(d,J=6Hz,6H,NCH2CHMeO). 13 C NMR (100MHz, CDCl3): δ=191.2,190.4,181.1,180.7,87.5,87.0,70.4,68. 8,55.7,55.3,39.7,39.2,31.3,31.2,22.5,22.2,21.6,21.3,21.1,20.9.
[0068] Elemental analysis: C 48 H 84 N4O8Zn 44 Theoretical content (%): C, 52.09; H, 7.65; N, 5.06; Measured content (%): C, 52.57; H, 7.690; N, 4.76.
[0069] Example 3
[0070] This embodiment provides a ketimine zinc complex 2c, whose structural formula is [(CH3)2CHC(O)CHCN((R)-CH(CH3)CH2CH2O)CH(CH3)2]4Zn4, and the structural formula is 2c in Formula III. The preparation method comprises:
[0071] In an argon environment, 0.45 g (about 2.0 mmol) of β-ketimine ligand 1c (structural formula see 1c in Formula III) was dissolved in toluene that had been subjected to anhydrous and oxygen-free treatment to obtain a β-ketimine ligand solution, the β-ketimine ligand solution was heated to 70° C., and then 1.0 mL of diethyl zinc solution (concentration of 2 M, solvent of toluene, total amount of diethyl zinc 2.0 mmol) was added dropwise thereto, and the reaction was stirred at 70° C. for 30 min to obtain a colorless clear solution; the solvent was vacuum-evacuated to obtain a white powder, and the preparation of the ketimine zinc complex 2c was completed.
[0072] The products were characterized by NMR and elemental analysis.
[0073] Yield of ketimine zinc complex 2c: 0.54 g (99%).
[0074] 1 H-NMR (400MHz, CDCl3): δ=4.75(s,4H,C(O)CH=CN), 3.79-3.70(m,4H,NCH(Me)CH2CH2), 3.53-3.23(m,8H,CHMeCH2CH2O), 2.99(sept,J=6. 8Hz,4H,Me2CHC(O)), 2.33(sept,J=6.8Hz,4H,Me2CHC(N)), 2.15-1.80(m,8H,NCH(Me)CH2CH2, 1.20-0.84(m,60H,Me2CH,NCH(Me)CH2CH2). 13 C NMR (100MHz, CDCl3): δ = 181.6, 87.3, 64.7, 48.5, 39.5, 33.3, 32.8, 30.1, 29.8, 21.4, 21.2, 20.2.
[0075] Elemental analysis: C 52 H 92 Theoretical content of N4O8Zn4 (%): C, 53.71; H, 7.98; N, 4.82; measured content (%): C, 53.83; H, 8.069; N, 4.78.
[0076] Example 4
[0077] This embodiment provides a ketimine zinc complex 2d, whose molecular formula is [(CH3)2CHC(O)CHCN(CH2CH2CH2CH2O)CH(CH3)2]4Zn4, and the structural formula is 2d in Formula III. The preparation method comprises:
[0078] In an argon environment, 0.45 g (about 2.0 mmol) of β-ketimine ligand 1d (structural formula see 1d in Formula III) was dissolved in toluene that had been subjected to anhydrous and oxygen-free treatment to obtain a β-ketimine ligand solution, the β-ketimine ligand solution was heated to 70° C., and then 1.0 mL of diethyl zinc solution (concentration of 2 M, solvent of toluene, total amount of diethyl zinc of 2.0 mmol) was added dropwise thereto, and the reaction was stirred at 70° C. for 60 min to obtain a colorless clear solution; the solvent was vacuum-evacuated to obtain a white powder, and the preparation of the ketimine zinc complex 2d was completed.
[0079] The products were characterized by NMR and elemental analysis.
[0080] Yield of ketimine zinc complex 2d: 0.54 g (99%).
[0081] 1 H-NMR (400MHz, CD2Cl2): δ=4.79(s,4H,C(O)CH=CN),3.79-3.54(m,8H,NCH2CH2CH2CH2O),3.53-3.28(8H,NCH2CH2CH2CH2O),3.02(se pt,J=6.8Hz,4H,Me2CHC(O)), 2.33(sept,J=6.8Hz,4H,Me2CHC(N)), 2.10-1.38(m,16H,NCH2CH2CH2CH2O), 1.16-1.00(m,48H,Me2CH). 13 C NMR (100MHz, CD2Cl2): δ=190.9,182.3,87.8,65.0,48.8,39.8,32.9,30.5,28.7,26.3,25.4,21.4,21.3,20.2.
[0082] Elemental analysis: C 52 H 92 Theoretical content of N4O8Zn4 (%): C, 53.71; H, 7.98; N, 4.82; measured content (%): C, 53.34; H, 8.008; N, 4.75.
[0083] Example 5
[0084] This embodiment provides a ketimine zinc complex 2e, whose molecular formula is [(CH3)2CHC(O)CHCN(CH2CH(CH3)O)CH(CH3)2]4Zn4, and the structural formula is 2e in Formula III. The difference from Example 2 is that the β-ketimine ligand used is a racemic β-ketimine ligand 1e (the structural formula is 1e in Formula III), and the preparation method includes:
[0085] In an argon environment, 0.43 g (about 2.0 mmol) of β-ketimine ligand 1e (structural formula see 1e in Formula III) was dissolved in toluene that had been subjected to anhydrous and oxygen-free treatment to obtain a β-ketimine ligand solution, the β-ketimine ligand solution was heated to 60° C., and then 1.0 mL of diethyl zinc solution (concentration of 2 M, solvent of toluene Tol, total amount of diethyl zinc 2.0 mmol) was added dropwise thereto, and the reaction was stirred at 60° C. for 30 min to obtain a colorless clear solution; the solvent was vacuum-evacuated to obtain a white powder, and the preparation of the ketimine zinc complex 2e was completed.
[0086] The product was characterized by NMR.
[0087] Yield of ketimine zinc complex 2e: 0.55 g (99%).
[0088] 1 H-NMR (400MHz, CDCl3): δ=4.89-4.79(m,4H,C(O)CH=CN)), 4.34-2.44(m,16H,CH2CHMeO,NC H2CHMeO,Me2CHC(O)), 2.4-2.23(m,4H,Me2CHC(N)), 1.46-0.77(m,60H,Me2CH,NCH2CHMeO).
[0089] Example 6
[0090] This embodiment provides a ketimine zinc complex 2f, whose molecular formula is [(CH3)2CHC(O)CHCN(CH(CH3)CH2O)CH(CH3)2]4Zn4, and the structural formula is 2f in Formula III. The preparation method comprises:
[0091] In an argon environment, 0.43 g (about 2.0 mmol) of β-ketimine ligand 1f (structural formula see 1f in Formula III) was dissolved in toluene that had been subjected to anhydrous and oxygen-free treatment to obtain a β-ketimine ligand solution, the β-ketimine ligand solution was heated to 70° C., and then 1.0 mL of diethyl zinc solution (concentration of 2 M, solvent of toluene, total amount of diethyl zinc 2.0 mmol) was added dropwise thereto, and the reaction was stirred at 70° C. for 30 min to obtain a colorless clear solution; the solvent was vacuum-evacuated to obtain a white powder, and the preparation of the ketimine zinc complex 2f was completed.
[0092] The product was characterized by NMR.
[0093] Yield of ketimine zinc complex 2f: 0.55 g (99%).
[0094] 1H-NMR (400MHz, CDCl3): 4.88-4.63 (m, 4H, C(O)CH=CN), 4.42-3.21 (m, 12H, NCHMeCH2O), 3.14-2 .68(m,4H,Me2CHC(O)),2.35-2.15(m,4H,Me2CHC(N)),1.35-0.83(m,60H,NCHMeCH2O,Me2CH).
[0095] Example 7
[0096] This example provides a ketimine zinc complex, the structure of which is the same as that of the ketimine zinc complex 2a provided in Example 1. The only difference from Example 1 is that the solvent in the β-ketimine ligand solution is hexane instead of toluene, and the solvent of the diethyl zinc solution is hexane instead of toluene.
[0097] The products were characterized by NMR, elemental analysis and high-resolution mass spectrometry.
[0098] The yield of the ketimine zinc complex is the same as that in Example 1 and can reach 99%.
[0099] The elemental analysis results and high-resolution mass spectrometry characterization results of the obtained ketimine zinc complex are not substantially different from those of the ketimine zinc complex 2a provided in Example 1.
[0100] Example 8
[0101] This embodiment provides a method for preparing PLA by ring-opening polymerization of lactide, wherein the method comprises:
[0102] Under argon protection, the lactide monomer racemic lactide (3.0 mmol) and the ketimine zinc complex 2a (0.00015 mmol) provided in Example 1 were accurately weighed, and the two (the molar ratio of the monomer to the ketimine zinc complex was 20000:1) were fully stirred in a reactor without solvent. The temperature was raised to 130° C. The reaction system was carefully observed until the solid powder was completely converted into a gel solid, and the reaction was stopped. The reaction time t=15 s was recorded, and the lactide ring-opening polymerization to prepare PLA reaction was completed.
[0103] The reactor lid was opened, the temperature was lowered in an ice-water bath, and a small amount (2 ml) of CH2Cl2 was added to the reaction mixture to completely dissolve it, thereby obtaining a sample for performance testing.
[0104] Take a small amount of sample and remove volatiles in vacuo. 1 The monomer conversion calculated by H NMR was conv.=97%.
[0105] The remaining sample solution was taken and a large amount (20 mL) of cold ethanol solution was added under vigorous stirring to precipitate to obtain a crude polymer. The polymer was then separated and washed with a small amount of cold ethanol to remove the residual catalyst and oligomers. The washing operation was repeated three times. The polymer was vacuum-dried at 60°C to constant weight to obtain a thin film plastic polymer sample. The molecular weight Mn of the polymer was 191505 g / mol and the molecular weight distribution PDI was 1.7 by gel permeation chromatography (GPC). At the same time, the stereoselectivity of the polymer was calculated by homonuclear decoupling hydrogen spectrum characterization, and its isotactic degree Pm was 0.43. See Table 1 for details.
[0106] Example 9
[0107] This embodiment provides a method for preparing PLA by ring-opening polymerization of lactide, wherein the method is different from Example 7 in that: the ketimine zinc complex 2b (0.0002 mmol) provided in Example 2 is weighed instead of the ketimine zinc complex 2a (0.00015 mmol) provided in Example 1, and the molar ratio of the monomer to the ketimine zinc complex is 15000:1 instead of 20000:1.
[0108] Reaction time t=1.5 min, monomer conversion rate conv.=96%, polymer molecular weight Mn=220698 g / mol, polymer molecular weight distribution PDI=1.61, polymer isotacticity Pm=0.46, see Table 1 for details.
[0109] Example 10
[0110] The present embodiment provides a method for preparing PLA by ring-opening polymerization of lactide, wherein the method is different from Example 7 in that: the lactide monomer L-lactide (3.0 mmol) is weighed instead of racemic lactide (3.0 mmol), the ketimine zinc complex 2b (0.0002 mmol) provided in Example 2 is weighed instead of the ketimine zinc complex 2a (0.00015 mmol) provided in Example 1, and the molar ratio of the monomer to the ketimine zinc complex is 15000:1 instead of 20000:1.
[0111] Reaction time t=2.1 min, monomer conversion rate conv.=91%, polymer molecular weight Mn=169279 g / mol, polymer molecular weight distribution PDI=1.89, see Table 1 for details.
[0112] Embodiment 11
[0113] This embodiment provides a method for preparing PLA by ring-opening polymerization of lactide, wherein the difference between this method and Example 7 is that the ketimine zinc complex 2c (0.0002 mmol) provided in Example 3 is weighed instead of the ketimine zinc complex 2a (0.00015 mmol) provided in Example 1, and the molar ratio of the monomer to the ketimine zinc complex is 15000:1 instead of 20000:1.
[0114] Reaction time t=1.5 min, monomer conversion rate conv.=96%, polymer molecular weight Mn=154268 g / mol, polymer molecular weight distribution PDI=1.5, polymer isotacticity Pm=0.58, see Table 1 for details.
[0115] Example 12
[0116] This embodiment provides a method for preparing PLA by ring-opening polymerization of lactide, wherein the method is different from Example 7 in that: the lactide monomer L-lactide (3.0 mmol) is weighed instead of racemic lactide (3.0 mmol), the ketimine zinc complex 2c (0.0002 mmol) provided in Example 3 is weighed instead of the ketimine zinc complex 2a (0.00015 mmol) provided in Example 1, and the molar ratio of the monomer to the ketimine zinc complex is 15000:1 instead of 20000:1.
[0117] Reaction time t=1.8 min, monomer conversion rate conv.=90%, polymer molecular weight Mn=93608 g / mol, polymer molecular weight distribution PDI=1.55, see Table 1 for details.
[0118] Embodiment 13
[0119] This embodiment provides a method for preparing PLA by ring-opening polymerization of lactide, wherein the method is different from Example 7 in that the ketimine zinc complex 2d (0.00015 mmol) provided in Example 4 is weighed instead of the ketimine zinc complex 2a (0.00015 mmol) provided in Example 1.
[0120] Reaction time t=5s, monomer conversion rate conv.=94%, polymer molecular weight Mn=176190g / mol, polymer molecular weight distribution PDI=1.85, polymer isotacticity Pm=0.46, see Table 1 for details.
[0121] Embodiment 14
[0122] This embodiment provides a method for preparing PLA by ring-opening polymerization of lactide, wherein the method is different from Example 7 in that: the ketimine zinc complex 2a (0.000075 mmol) provided in Example 1 is weighed instead of the ketimine zinc complex 2a (0.00015 mmol) provided in Example 1, and the molar ratio of the monomer to the ketimine zinc complex is 40000:1 instead of 20000:1.
[0123] Reaction time t=3 min, monomer conversion rate conv.=83%, polymer molecular weight Mn=171704 g / mol, polymer molecular weight distribution PDI=2.11, see Table 1 for details.
[0124] Embodiment 15
[0125] This embodiment provides a method for preparing PLA by ring-opening polymerization of lactide, wherein the method is different from Example 7 in that: the ketimine zinc complex 2a (0.00006 mmol) provided in Example 1 is weighed instead of the ketimine zinc complex 2a (0.00015 mmol) provided in Example 1, and the molar ratio of the ketimine zinc complex to the monomer is 50000:1 instead of 20000:1.
[0126] Reaction time t=4 min, monomer conversion rate conv.=61%, polymer molecular weight Mn=137103 g / mol, polymer molecular weight distribution PDI=2.14, see Table 1 for details.
[0127] Example 16
[0128] This embodiment provides a method for preparing PLA by ring-opening polymerization of lactide, wherein the method comprises:
[0129] Under argon protection, the lactide monomer racemic lactide (3.0 mmol) and the ketimine zinc complex 2a (0.0006 mmol) provided in Example 1 were accurately weighed, and the racemic lactide was dissolved in toluene to obtain a solution with a concentration of 1 M and the ketimine zinc complex 2a (the molar ratio of the monomer to the ketimine zinc complex was 5000:1) were fully stirred in a reactor, and the temperature was raised to 80° C. When the reaction system was completely converted into a gel solid, the reaction was stopped, and the reaction time t=5 min was recorded, and the lactide ring-opening polymerization to prepare PLA reaction was completed.
[0130] The monomer conversion rate conv.=90%, the polymer molecular weight Mn=143523 g / mol, and the polymer molecular weight distribution PDI=1.77 were determined in the same manner as in Example 8. See Table 1 for details.
[0131] Table 1
[0132]
[0133]
[0134] Note:
[0135] 1 The monomer conversion rate was 1 H-NMR spectrum measurement.
[0136] 2 The molecular weight of the polymer was measured by gel permeation chromatography (GPC) using polystyrene as the standard substance and tetrahydrofuran as the eluent.
[0137] 3 No solvent, bulk catalysis is carried out at 130-180°C, and the monomer used is racemic lactide.
[0138] 4 Homonuclear Decoupling 1 The results were confirmed by analysis of the methine region in the H-NMR spectrum.
[0139] 5 The monomer used is L-lactide.
[0140] 6 The initial monomer concentration was 1 M, and the monomer used was racemic lactide.
[0141] It can be seen from Table 1 that the ketimine zinc complex provided by the present invention exhibits excellent catalytic activity in catalyzing the ring-opening polymerization of lactide. The conversion rate of lactide monomer is as high as 97%, the number average molecular weight is 90,000-220,000 g / mol, and the molecular weight distribution is narrow. Compared with the existing method for catalyzing the ring-opening polymerization of lactide, the method provided by the present invention uses less catalyst when preparing polylactide and has higher activity. In addition, the ketimine zinc complex provided by the present invention has low toxicity, does not require the participation of a co-catalyst in the process of catalyzing the polymerization of lactide, can be catalyzed, the synthesis process of the catalyst is simple, the yield is high, and a high-purity catalyst (yield of 99%) can be obtained after removing the solvent, and can be used directly without purification, thereby reducing the economic loss caused by purifying the catalyst.
[0142] Comparative Example
[0143] This comparative example provides a comparative experiment of using another ligand to prepare a complex.
[0144] Specifically, the tetranuclear zinc complex was prepared by reacting a β-ketoimine ligand with diethylzinc, which was different from the β-ketoimine ligand used in Examples 1 to 6 only in that the substituent on the C atom on the ligand skeleton was tert-butyl instead of isopropyl, to prepare the tetranuclear zinc complex (the preparation method was similar to that in Examples 1 to 6). Ultimately, no purifiable tetranuclear zinc complex could be obtained (i.e., the yield was too low to be purified).
[0145] Specifically, the tetranuclear zinc complex was prepared by reacting a β-ketoimine ligand with diethylzinc, which was different from the β-ketoimine ligand used in Examples 1 to 6 only in that the substituent on the C atom on the ligand skeleton was not an isopropyl group but an aromatic substituent phenyl. The preparation method was similar to that of Examples 1 to 6, but ultimately no purifiable tetranuclear zinc complex could be obtained (i.e., the yield was too low to be purified).
[0146] Specifically, referring to the method in "Syntheses, structures and catalysis of tetranuclear zinc N-alkoxideketoiminate complexes for ring-opening polymerization of rac-lactide" published in Inorganic Chemistry Communications, Issue 119, 2020, the tetranuclear zinc complex was prepared by reacting a β-ketoiminine ligand with diethylzinc, which differs from the β-ketoiminine ligand used in the ketoiminine zinc complex provided by the present invention only in that the substituent on the C atom on the ligand skeleton is methyl instead of isopropyl. Ultimately, the tetranuclear zinc complex could not be obtained in high yield, and the highest yield could only reach 61%. In addition, the catalytic activity of the ketimine zinc complex prepared by the invention in catalyzing the ring-opening polymerization of lactide to prepare PLA is also significantly poorer than that of the ketimine zinc complex provided by the present invention. Similarly, when used for catalyzing the ring-opening polymerization of racemic lactide to prepare PLA at 130°C, the amount ratio (molar ratio) of the ketimine zinc complex prepared by the invention to lactide reaches 1:1000, the catalytic time is at least 3 minutes, and the molecular weight of the obtained polymer PLA is 15,000-91,000. The amount ratio (molar ratio) of the ketimine zinc complex provided by the present invention to lactide is 1:15000-20000, the catalytic time is only 5s-1.5min, and the molecular weight of the polymer PLA reaches more than 150,000.
Claims
1. A ketimine zinc complex having a structure shown in Formula I: In formula I, R is any one of a C2-C4 straight-chain alkyl group and its derivatives, a C2-C4 branched-chain alkyl group and its derivatives.
2. The ketimine zinc complex according to claim 1, wherein In formula I, R is any one of a C2-C4 straight-chain alkyl group and a C2-C4 branched-chain alkyl group.
3. The ketimine zinc complex according to claim 2, wherein In formula I, R is one of -CH2CH2-, -CH(CH3)CH2-, -CH2CH(CH3)-, -CH2CH2CH2CH2-, and -CH(CH3)CH2CH2-.
4. The ketimine zinc complex according to claim 3, wherein In formula I, R is any one of -CH2CH2-, -CH(CH3)CH2-, -(R)-CH2CH(CH3)-, -(S)-CH2CH(CH3)-, -CH2CH2CH2CH2-, -(R)-CH(CH3)CH2CH2- and -(S)-CH(CH3)CH2CH2-.
5. The method for preparing the ketimine zinc complex according to any one of claims 1 to 4, wherein: The method includes: In a protective gas environment, adding a ZnEt2 solution dropwise to a β-ketimine ligand solution at a temperature range of 60° C. to 100° C. to react to obtain the ketimine zinc complex; Wherein, the β-ketoimine ligand has a structure shown in Formula II: R in formula Ⅱ is the same as R in formula I.
6. The method according to claim 5, wherein: The molar ratio of ZnEt2 to the β-ketoimine ligand in the β-ketoimine ligand solution is 0.8-1.2:
1.
7. The method according to claim 5, wherein: The solvent in the β-ketoimine ligand solution includes at least one of toluene, hexane, dichloromethane and tetrahydrofuran; The solvent in the ZnEt2 solution includes at least one of toluene and hexane.
8. The method according to claim 5, wherein: The reaction time is 30-60 min.
9. Use of the ketimine zinc complex according to any one of claims 1 to 4 as a catalyst in catalyzing the ring-opening polymerization of lactide.
10. The use according to claim 9, wherein: The application is the use of the ketimine zinc complex described in any one of claims 1 to 4 as a catalyst in catalyzing the ring-opening polymerization of lactide to prepare PLA with a number average molecular weight of more than 150,000.
11. A method for preparing PLA by ring-opening polymerization of lactide, wherein: The method includes: PLA is prepared by mixing lactide monomer with the ketimine zinc complex according to any one of claims 1 to 4 and reacting them.
12. The method according to claim 11, wherein: The lactide monomer and the ketimine zinc complex are mixed at a molar ratio of 5000-50000:
1.
13. The method according to claim 12, wherein: The lactide monomer and the ketimine zinc complex are mixed at a molar ratio of 15000-50000:
1.
14. The method according to claim 13, wherein: The lactide monomer and the ketimine zinc complex are mixed at a molar ratio of 15000-40000:
1.
15. The method according to claim 11, wherein: The reaction temperature is 80-180°C.
16. The method according to claim 15, wherein: The reaction temperature is 130-180°C.
17. The method according to claim 16, wherein: The reaction temperature is 130-150°C.
18. The method according to claim 11, wherein: The lactide monomer includes at least one of L-lactide and racemic lactide.
19. The method according to claim 11, wherein: The method for preparing PLA by ring-opening polymerization of lactide comprises: The racemic lactide and the ketimine zinc complex are mixed at a molar ratio of 15000-40000:1 and reacted at 130-150° C. to prepare PLA.
20. The method according to claim 19, wherein: The racemic lactide and the ketimine zinc complex are mixed at a molar ratio of 15000-20000:1 and reacted at 130-150° C. to prepare PLA.
Citation Information
Patent Citations
Zinc ketoiminate complexes as catalysts for production of polyurethanes
CN111247187A
Bimetallic zinc complex and process of producing polycarbonate using the same as polymerization catalyst
US20060135743A1