Unsaturated amide copolymer, epoxy resin product, preparation method and application of unsaturated amide copolymer and epoxy resin product, curing agent composition and application of curing agent composition

By preparing unsaturated amide copolymers containing specific structural units as curing agents, the problem of insufficient curing of water-soluble epoxy resins at high temperatures was solved, resulting in epoxy resin products with high strength and high permeability, suitable for phase change fracturing fluids in oil and gas extraction.

CN119039512APending Publication Date: 2024-11-29CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311776257.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-12-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing water-soluble epoxy resins are not fully cured or are unstable at high temperatures, and are prone to curing at room temperature, which limits their application in conditions such as oil and gas well fracturing.

Method used

Unsaturated amide copolymers, containing specific structural units I, II, and III, are used as curing agents and prepared via solution polymerization to ensure curing at high temperatures and prevent precipitation or floating at room temperature. Emulsifiers and initiators are used to control the reaction.

Benefits of technology

It achieves stable curing of water-soluble epoxy resin at temperatures above 120℃, forming a high-strength cured product while maintaining suitable viscosity and permeability, making it suitable for phase change fracturing fluids in oil and gas extraction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039512A_ABST
    Figure CN119039512A_ABST
Patent Text Reader

Abstract

The invention relates to the field of high polymer materials and oil and gas exploitation, and discloses an unsaturated amide copolymer and a preparation method and application thereof, a curing agent composition and application thereof, an epoxy resin composition and application thereof, and epoxy resin and application thereof. The unsaturated amide copolymer comprises a structural unit I, a structural unit II and a structural unit III, the structural unit I has a structure as shown in a formula 1, the structural unit II has a structure as shown in a formula 2, and the structural unit III has a structure as shown in at least one of a formula 3, a formula 4 and a formula 5; the unsaturated amide copolymer provided by the invention is used as a curing agent for curing epoxy resin, the epoxy resin can be cured at high temperature, and particularly, when the unsaturated amide copolymer is used as the curing agent for curing the epoxy resin, a cured epoxy resin product can have high curing strength, and the curing strength is high. And the epoxy resin product contains a pore structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of polymer materials and oil and gas exploitation, and in particular to an unsaturated amide copolymer and a preparation method and application thereof, a curing agent composition and application thereof, and an epoxy resin preparation and a preparation method and application thereof. Background Art

[0002] Epoxy thermosetting resins are widely used in coatings, paints, adhesives and engineering fields due to their excellent mechanical properties and bonding properties. For example, epoxy thermosetting resins can be found in wind turbine blades, pressure-bearing parts of aerospace, and sucker rods. However, water-based epoxy resins are required under some special working conditions, such as bonding of underwater engineering parts, underwater plugging, plugging of oil and gas wells in oil and gas production, oil and gas well fracturing, and sand control of oil and gas wells. Commonly used water-based epoxy resins are obtained by emulsification. According to the different emulsification methods, they can be divided into external emulsification and internal emulsification. External emulsification is to disperse the epoxy resin in water by adding an emulsifier to form a stable emulsion; internal emulsification is to introduce certain hydrophilic groups into the epoxy resin molecular chain. The modified epoxy resin itself has a certain emulsification ability, so it can be stably dispersed in water. In addition, there is a relatively rare type of water-soluble epoxy resin - aqueous solution epoxy resin, which is to enhance the hydrophilicity of epoxy resin to be able to dissolve in water to form a solution. Because water is the lowest cost solvent, this type of epoxy resin can be applied to large-scale applications such as oil and gas extraction. Regardless of the type of epoxy resin, a curing agent must be added to achieve curing in order to reflect its mechanical properties, bonding properties, etc., to achieve practical purposes.

[0003] The curing process is achieved through the ring-opening reaction between the epoxy groups of the epoxy resin itself and the amino groups, carboxyl groups and other groups to form a network structure. For the curing of epoxy resin, curing agents can be divided into three categories: (1) alkaline curing agents, which are composed of aliphatic polyamines, water molecule polyamines, aromatic polyamines, etc.; (2) acidic curing agents, including organic acids, acid anhydrides, hydrogen trifluoride, etc.; (3) additive curing agents. This type of curing is actually part of the curing product composed of the addition reaction of epoxy groups. At the same time, the linear molecules are crossed into three-dimensional structure molecules through gradual polymerization reactions. They are also called over-type curing agents. These curing agents are mainly for epoxy resin bodies. For water-soluble epoxy resins, there will be a phenomenon of non-curing or insufficient curing strength. This is determined by the characteristics of water-soluble epoxy resins.

[0004] Because epoxy groups have the problem of hydrolysis in aqueous solution, if the curing agent is not active or water-soluble enough, the reaction rate between the reactive groups of the curing agent and the epoxy groups is not as high as the hydrolysis rate of the epoxy groups when the curing reaction occurs at high temperature, resulting in the phenomenon of insufficient strength or non-curing. For water-soluble epoxy thermosetting resins, polyethylene polyamine can meet these two conditions at the same time, but its activity is too high. After adding, the curing reaction will occur immediately, causing the viscosity of the system to increase instantly, which is not conducive to the application in many working conditions, such as oil and gas well fracturing, which needs to maintain fluidity for a certain period of time to facilitate pumping and movement in the cracks.

[0005] Therefore, there is an urgent need to provide a polymer curing agent that can cure epoxy resin in situ in an aqueous solution and does not undergo a curing reaction at room temperature. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide an unsaturated amide copolymer and a preparation method and application thereof, a curing agent composition and application thereof, an epoxy resin composition and application thereof, an epoxy resin and application thereof. The unsaturated amide copolymer can be used as a curing agent for curing epoxy resin, can achieve curing of water-soluble epoxy resin at above 120°C, and can not precipitate or float during curing, and is not easy to cure at room temperature.

[0007] In order to achieve the above object, the first aspect of the present invention provides an unsaturated amide copolymer, wherein the unsaturated amide copolymer comprises a structural unit I, a structural unit II and a structural unit III;

[0008] The structural unit I has a structure shown in Formula 1, the structural unit II has a structure shown in Formula 2, and the structural unit III has a structure shown in at least one of Formula 3, Formula 4 and Formula 5;

[0009]

[0010] Wherein, in Formula 1, R1 is -H or -CH3, R2 and R3 are each independently -H or a C1-C18 alkyl group; R4 is -H, A, a C1-C20 alkyl group or -(CH2) n -OR 21 ; R 21 is -H or a C1-C18 alkyl group, and n is an integer of 0-12;

[0011] A has the structure shown in Formula 6;

[0012]

[0013] In formula 6, R 22 and R 23Each is independently -H or a C1-C18 alkyl group, and m is an integer of 0-18;

[0014] In Formula 2, R5, R6 and R7 are each independently -H, C1-C12 alkyl or -(CH2) r -OH, r is an integer of 1-12; X is -(CH2) z -, z is an integer from 0 to 5;

[0015] In formula 3, R8 is -H or -CH3;

[0016] In formula 4, R9 is -H or -CH3;

[0017] In formula 5, R 10 , R 11 and R 12 Each is independently -H or -NH2, and at least one is -NH2; R 13 It is -H or -CH3.

[0018] A second aspect of the present invention provides a method for preparing an unsaturated amide copolymer, wherein the method comprises the following steps:

[0019] Under solution polymerization conditions, in the presence of an initiator and an emulsifier, a monomer mixture is polymerized in water to obtain the unsaturated amide copolymer; the monomer mixture comprises monomer A, monomer B and monomer C;

[0020] The monomer A has a structure as shown in Formula 7, the monomer B has a structure as shown in Formula 8, and the monomer C has a structure as shown in at least one of Formula 9, Formula 10 and Formula 11;

[0021]

[0022] Wherein, in Formula 7, R1' is H or CH3, R2' and R3' are each independently -H or a C1-C18 alkyl group; R4' is -H, A', a C1-C20 alkyl group or -(CH2) n1 -OR 21 ';R 21 ' is -H or a C1-C18 alkyl group, and n1 is an integer of 0-12;

[0023] A' has the structure shown in Formula 12;

[0024]

[0025] In formula 12, R 22 ' and R 23 'Each independently represents -H, C1-C18 alkyl, M represents -H, Na or K; m1 represents an integer of 0-18;

[0026] In Formula 8, R5', R6' and R7' are each independently -H, C1-C12 alkyl or -(CH2) r1 -OH, r1 is an integer from 1 to 12; X is -(CH2) z1 -, z1 is an integer from 0 to 5;

[0027] In formula 9, R8' is -H or -CH3;

[0028] In formula 10, R9' is -H or -CH3;

[0029] In formula 11, R 10 '、R 11 ' and R 12 ' are each independently -H or -NH2, and at least one is -NH2; R 13 ' is -H or -CH3.

[0030] The third aspect of the present invention provides an unsaturated amide copolymer prepared by the above method.

[0031] The fourth aspect of the present invention provides use of the unsaturated amide copolymer described in the first aspect or the third aspect as a curing agent.

[0032] A fifth aspect of the present invention provides a curing agent composition, wherein the curing agent composition comprises a curing agent, an emulsifier and water;

[0033] The curing agent is the unsaturated amide copolymer described in the first aspect or the third aspect.

[0034] A sixth aspect of the present invention provides a method for preparing an epoxy resin product, characterized in that the preparation method comprises:

[0035] The first component containing epoxy resin is mixed with the curing agent composition and cured to obtain an epoxy resin product.

[0036] A seventh aspect of the present invention provides an epoxy resin product produced by the above-mentioned preparation method.

[0037] An eighth aspect of the present invention provides a use of the above-mentioned curing agent composition or the above-mentioned epoxy resin product in a phase change fracturing fluid.

[0038] Through the above technical scheme, the unsaturated amide polymer and its preparation method and application, epoxy resin composition and application, epoxy resin and application provided by the present invention achieve the following beneficial effects:

[0039] The unsaturated amide copolymer provided by the present invention includes an unsaturated amide copolymer having a large number of amine groups on the side groups, which can realize the curing of epoxy resin at high temperature. In particular, when the unsaturated amide copolymer is used as a curing agent for curing epoxy resin, the cured epoxy resin can have high curing strength, and the cured product contains a pore structure.

[0040] Furthermore, the molecular chain of the unsaturated amide copolymer provided by the present invention has a certain steric hindrance effect, which can limit its curing ability at room temperature. When it is used as a curing agent for epoxy resin, the water-soluble epoxy resin can be cured at above 120°C.

[0041] The epoxy resin composition including the curing agent composition provided by the present invention has a suitable apparent viscosity (200 mPa·s-300 mPa·s), can limit the thermal movement of the molecular chain, so that the epoxy resin is cured in situ, and the porosity loss caused by precipitation or floating during curing is avoided, and a certain permeability and porosity are maintained, so that the cured epoxy resin can be used as a phase change fracturing fluid in oil and gas production. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 is a photograph of the epoxy resin product prepared in Application Example 1;

[0043] Figure 2 This is a photo of the epoxy resin product prepared in Comparative Application Example 1. DETAILED DESCRIPTION

[0044] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0045] The first aspect of the present invention provides an unsaturated amide copolymer, wherein the unsaturated amide copolymer comprises a structural unit I, a structural unit II and a structural unit III;

[0046] The structural unit I has a structure shown in Formula 1, the structural unit II has a structure shown in Formula 2, and the structural unit III has a structure shown in at least one of Formula 3, Formula 4 and Formula 5;

[0047]

[0048]

[0049] Wherein, in Formula 1, R1 is -H or -CH3, R2 and R3 are each independently -H or a C1-C18 alkyl group; R4 is -H, A, a C1-C20 alkyl group or -(CH2) n -OR 21 ; R 21 is -H or a C1-C18 alkyl group, and n is an integer of 0-12;

[0050] A has the structure shown in Formula 6;

[0051]

[0052] In formula 6, R 22 and R 23 Each is independently -H or a C1-C18 alkyl group, and m is an integer of 0-18;

[0053] In Formula 2, R5, R6 and R7 are each independently -H, C1-C12 alkyl or -(CH2) r -OH, r is an integer of 1-12; X is -(CH2) z -, z is an integer from 0 to 5;

[0054] In formula 3, R8 is -H or -CH3;

[0055] In formula 4, R9 is -H or -CH3;

[0056] In formula 5, R 10 , R 11 and R 12 Each is independently -H or -NH2, and at least one is -NH2; R 13 It is -H or -CH3.

[0057] In the present invention, the unsaturated amide copolymer comprises the structural unit I, structural unit II and structural unit III having the above-mentioned specific structure. In particular, due to the introduction of structural unit III, the side groups of the unsaturated amide copolymer have a large number of amine groups. When the curing agent composition comprising the copolymer is used to cure epoxy resin, the epoxy resin can be cured at 90°C-150°C.

[0058] Specifically, the unsaturated amide copolymer of the present invention contains the structural unit II shown in Formula 2, which can not only adjust the intrinsic viscosity of the unsaturated amide polymer to meet the demand of the curing agent for epoxy resin, but also because the structural unit III contains a rigid group, it can reduce the toughness of the cured product of the curing agent composed of the unsaturated amide polymer, and improve the strength of the cured product of the curing agent composed of the unsaturated amide polymer, especially the strength of the epoxy resin.

[0059] Further, in a specific embodiment of the present invention, in Formula 1, R1 is -H or -CH3, R2 and R3 are each independently -H or a C1-C12 alkyl group; R4 is -H, A, a C8-C12 alkyl group or -(CH2) n -OR 21 ; R 21 is a C1-C12 alkyl group, and n is an integer from 0 to 12. Preferably, R1 is -H or -CH3, R2 and R3 are each independently -H, and R4 is -H, a C2 alkyl group or a C12 alkyl group; more preferably, R1, R2, R3 and R4 are all -H.

[0060] In one specific embodiment of the present invention, A has a structure shown in Formula 6;

[0061]

[0062] In formula 6, R 22 and R 23 Each is independently -H or a C1-C12 alkyl group, m1 is an integer of 1-12, preferably, R 22 and R 23 Each is independently -H or a C1-C6 alkyl group, m is an integer of 1-6, more preferably, R 22 and R 23 Each is independently -H or a C1-C3 alkyl group, and m is an integer of 1-3.

[0063] In one embodiment of the present invention, in Formula 2, R5 is -(CH2) r -OH or -H, r is an integer of 1-3; R6 and R7 are each independently -H; X is -(CH2) z -, z is an integer from 0 to 2; more preferably, R5, R6 and R7 are each independently -H.

[0064] In a specific embodiment of the present invention, in Formula 3, R8 is -H.

[0065] In a specific embodiment of the present invention, in Formula 4, R9 is -H.

[0066] In one embodiment of the present invention, in Formula 5, R 10 , R 11 and R 12 Each is independently -H or -NH2, and at least one is -NH2; R 13 is -H.

[0067] According to the present invention, based on the total weight of the unsaturated amide copolymer, the content of the structural unit I is 65wt%-85wt%, the content of the structural unit II is 5wt%-7wt%, and the content of the structural unit III is 12wt%-27wt%.

[0068] In the present invention, when the content of each structural unit in the unsaturated amide copolymer is controlled to meet the above range, when the curing agent composition containing the copolymer is used to cure the epoxy resin, it has the characteristics of controllable curing time (complete curing within 6 hours), large porosity (about 30%), strong pressure bearing capacity (50MPa), and high permeability (100 millidarcy-5 darcy) of the cured epoxy resin.

[0069] Furthermore, based on the total weight of the unsaturated amide polymer, the content of the structural unit I is 70wt%-82wt%, the content of the structural unit II is 5wt%-6wt%, and the content of the structural unit III is 12.5wt%-20wt%.

[0070] In the present invention, the total content of the structural unit I, the structural unit II and the structural unit III is 100 wt %.

[0071] In the present invention, the content of each structural unit in the copolymer is calculated by the feed amount.

[0072] According to the present invention, at 25° C., the intrinsic viscosity of the copolymer is 200 mL / g-1200 mL / g, preferably 900 mL / g-1200 mL / g.

[0073] A second aspect of the present invention provides a method for preparing an unsaturated amide copolymer, wherein the method comprises the following steps:

[0074] Under solution polymerization conditions, in the presence of an initiator and an emulsifier, a monomer mixture is polymerized in water to obtain the unsaturated amide copolymer; the monomer mixture comprises monomer A, monomer B and monomer C;

[0075] The monomer A has a structure as shown in Formula 7, the monomer B has a structure as shown in Formula 8, and the monomer C has a structure as shown in at least one of Formula 9, Formula 10 and Formula 11;

[0076]

[0077]

[0078] Wherein, in Formula 7, R1' is H or CH3, R2' and R3' are each independently -H or a C1-C18 alkyl group; R4' is -H, A', a C1-C20 alkyl group or -(CH2)n1 -OR 21 ';R 21 ' is -H or a C1-C18 alkyl group, and n1 is an integer of 0-12;

[0079] A' has the structure shown in Formula 12;

[0080]

[0081] In formula 12, R 22 ' and R 23 'Each independently represents -H, C1-C18 alkyl, M represents -H, Na or K; m1 represents an integer of 0-18;

[0082] In Formula 8, R5', R6' and R7' are each independently -H, C1-C12 alkyl or -(CH2) r1 -OH, r1 is an integer from 1 to 12; X is -(CH2) z1 -, z1 is an integer from 0 to 5;

[0083] In formula 9, R8' is -H or -CH3;

[0084] In formula 10, R9' is -H or -CH3;

[0085] In formula 11, R 10 '、R 11 ' and R 12 ' are each independently -H or -NH2, and at least one is -NH2; R 13 ' is -H or -CH3.

[0086] In the present invention, monomer A, monomer B and monomer C having the above-mentioned specific structure are copolymerized in the presence of an emulsifier and an initiator to obtain an unsaturated amide copolymer, wherein the unsaturated amide copolymer contains a large number of amine groups as side groups. When the unsaturated amide copolymer is used to cure epoxy resin, the epoxy resin can be cured at 120°C-150°C, and the unsaturated amide copolymer is particularly suitable as a curing agent for epoxy resin used in phase change fracturing fluid.

[0087] In one embodiment of the present invention, in Formula 7, R1' is -H or -CH3, R2' and R3' are each independently -H or a C1-C12 alkyl group, and R4' is -H, A' or -(CH2) n -OR 21 ';R 21 ' is a C1-C12 alkyl group, and n1 is an integer of 0 to 12. Preferably, R1' is H or CH3, R2 and R3 are each independently -H, and R4 is -H, a C2 alkyl group or a C12 alkyl group; more preferably, R1', R2', R3' and R4' are all -H.

[0088] In the present invention, A' has the structure described in Formula 12:

[0089]

[0090] In formula 12, R 22 ' and R 23 ' are each independently -H or a C1-C12 alkyl group, m1 is an integer of 1-12, preferably, R 22 ' and R 23 'are each independently -H, C1-C6 alkyl, m1 is an integer of 1-6, more preferably, R 22 and R 23 Each is independently -H or a C1-C3 alkyl group, and m is an integer of 1-3.

[0091] In one embodiment of the present invention, in Formula 8, R5' is -(CH2) r -OH or -H, r is an integer of 1-3; R6' and R7' are each independently -H; X is -(CH2) z -, z is an integer of 0-2; more preferably, R5', R6' and R7' are each independently -H.

[0092] In one specific embodiment of the present invention, in Formula 9, R8' is -H.

[0093] In one specific embodiment of the present invention, in formula 10, R9' is -H.

[0094] In one embodiment of the present invention, in Formula 11, R 10 '、R 11 ' and R 12 ' are each independently -H or -NH2, and at least one is -NH2; R 13 ' is -H.

[0095] In the present invention, the monomer A having the structure described in Formula 7 is selected from acrylamide (R1', R2', R3' and R4' are -H), methacrylamide (R1' is -CH3, R2', R3' and R4' are -H), 2-methyl-2-acrylamidopropanesulfonic acid (in Formula 7, R1', R2' and R3' are -H, R4' is A', in Formula 12, R 22 ' and R 23 ' is -CH3, m1 is 1, M is H), sodium 2-methyl-2-acrylamidopropanesulfonate (in formula 7, R1', R2' and R3' are -H, R4' is A', in formula 12, R 22 ' and R 23' is -CH3, m1 is 1, M is Na), N-(methoxymethyl)acrylamide (in formula 7, R1', R2' and R3' are -H, R4' is -(CH2) n1 -OR 21 ', R 21 ' is -CH3, n1 is 1) and N-ethoxyacrylamide (in formula 7, R1', R2' and R3' are -H, R4' is -(CH2) n1 -OR 21 ', R 21 ' is -H, n1 is at least one of 2), preferably acrylamide and / or methacrylamide, more preferably acrylamide.

[0096] In the present invention, the monomer B having the structure described in Formula 8 is selected from styrene (in Formula 8, R5', R6' and R7' are -H; X is -(CH2) z1 -, z1 is 0), 2-methylstyrene (in formula 8, R5' and R6' are -H, R7' is -CH3; X is -(CH2) z1 -, z1 is 0), 3-methylstyrene (in formula 8, R5 and R7' are -H, R6' is -CH3; X is -(CH2) z1 -, z1 is 0), 4-methylstyrene (in formula 8, R6' and R7' are -H, R5' is -CH3; X is -(CH2) z1 -, z1 is 0) and vinylbenzyl alcohol (in formula 8, R6' and R7' are -H; R5 is -(CH2) r1 -OH, r1 is 1; X is -(CH2) z1 -, z1 is 0), preferably styrene and / or vinylbenzyl alcohol, more preferably styrene.

[0097] In the present invention, the monomer C having the structure described in Formula 9 is vinyl imidazole (in Formula 9, R8' is -H); the monomer C having the structure shown in Formula 10 is vinyl guanamine (in Formula 10, R9' is -H), and the monomer C having the structure described in Formula 11 is vinyl aromatic amine, preferably 3-vinyl aniline (in Formula 11, R 10 ' and R 12 'For -H, R 11 ' is -NH2; R 13 ' is -H) and / or 4-vinylaniline (in Formula 11, R 10 ' is -NH2, R 11 ' and R 12 ' is -H; R 13 ' is -H).

[0098] Furthermore, in a preferred embodiment of the present invention, monomer C is selected from 4-vinylaniline and / or vinylimidazole, preferably 4-vinylaniline.

[0099] According to the present invention, based on the total weight of the monomer mixture, the amount of the monomer A is 65wt%-85wt%, the amount of the monomer B is 5wt%-7wt%, and the amount of the monomer C is 12wt%-27wt%.

[0100] In the present invention, by controlling the amount of each monomer to meet the above range, the obtained unsaturated amide copolymer can contain suitable rigid groups and active groups, ensuring that when the unsaturated amide copolymer is used as a curing agent for curing epoxy resin, it has active groups that meet actual needs, and can ensure that the epoxy resin product obtained by curing has high compressive strength.

[0101] Furthermore, based on the total weight of the monomer mixture, the amount of the monomer A is 70wt%-82wt%, the amount of the monomer B is 5wt%-6wt%, and the amount of the monomer C is 12.5wt%-20wt%.

[0102] According to the present invention, based on the total weight of the monomer mixture, the amount of the emulsifier is 1 wt%-6 wt%.

[0103] In the present invention, when the amount of the emulsifier added meets the above range, each monomer, especially monomer B and monomer C, can be evenly dispersed in water, thereby allowing monomer B and monomer C to react with monomer A at the molecular level.

[0104] Furthermore, based on the total weight of the monomer mixture, the amount of the emulsifier is 3wt%-5wt%, preferably 4wt%-5wt%.

[0105] According to the present invention, the amount of the initiator is 0.01-0.1 wt % based on the total weight of the monomer mixture.

[0106] Furthermore, based on the total weight of the monomer mixture, the amount of the initiator is 0.02-0.08 wt%, preferably 0.04-0.06 wt%.

[0107] According to the present invention, the water is deionized water.

[0108] According to the present invention, the emulsifier is selected from at least one of sodium maleic anhydride monohexadecyl carboxylate, sodium maleic anhydride monomethacrylate hydroxyethyl carboxylate, octadecyl trimethyl ammonium chloride, hexadecyl trimethyl ammonium chloride, dodecyl trimethyl ammonium chloride, dihexadecyl dimethyl ammonium chloride, dodecyl dimethyl benzyl ammonium chloride, sodium dodecyl sulfonate, sodium dodecyl carboxylate and alkylphenol polyoxyethylene ether, and is preferably a mixture of sodium maleic anhydride monohexadecyl carboxylate, sodium maleic anhydride monomethacrylate hydroxyethyl carboxylate and alkylphenol polyoxyethylene ether.

[0109] In the present invention, the alkylphenol polyoxyethylene ether may be nonylphenol polyoxyethylene ether (OP-10, OP-15, etc.).

[0110] According to the present invention, the initiator is selected from a mixture of an oil-soluble initiator and a water-soluble initiator, or an amphiphilic initiator.

[0111] In the present invention, the oil-soluble initiator is at least one selected from azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate and terephthalamide, preferably azobisisobutyronitrile.

[0112] In the present invention, the water-soluble initiator is at least one selected from hydrogen peroxide, tert-butyl hydroperoxide, persulfate, sodium sulfite, sodium bisulfite, azobisisobutylamidine hydrochloride and azobisisobutylimidazoline hydrochloride.

[0113] In the present invention, the amphiphilic initiator is azoisobutylcyanamide.

[0114] In the present invention, the initiator is a mixture of azobisisobutyronitrile and azobisisobutylimidazoline hydrochloride.

[0115] According to the present invention, the mass ratio of the azobisisobutyronitrile to the azobisisobutylimidazoline hydrochloride is 1:1-9.

[0116] In the present invention, when the above two initiators are used and their mass ratio satisfies the above range, free radicals can be generated simultaneously in the water phase and the oil-soluble monomer, the initiation efficiency is high, the polymerization temperature can be uniformly increased, and the viscosity of the obtained unsaturated amide copolymer is controllable.

[0117] Furthermore, the mass ratio of azobisisobutyronitrile to azobisisobutylimidazoline hydrochloride is 1:2-9, preferably 1:2.

[0118] According to the present invention, the solution polymerization reaction conditions include: polymerization temperature of 30-50° C., and polymerization time of 2h-8h.

[0119] In the present invention, the monomer mixture is copolymerized under the above-mentioned solution polymerization reaction conditions to obtain an unsaturated polyamide copolymer with a specific characteristic viscosity. When the unsaturated polyamide copolymer is used as a curing agent for curing epoxy resin, the epoxy resin can be cured in the range of 90-150°C, preferably 130-150°C, and the cured epoxy resin has interconnected pores and can maintain a permeability of 100 millidarcy to 5 darcy under a confining pressure of 50 MPa.

[0120] Furthermore, the solution polymerization reaction conditions include: polymerization temperature of 35-45° C., preferably 40-42° C.; polymerization time of 2 h-6 h, preferably 3 h-4 h.

[0121] According to the present invention, the conditions for the solution polymerization reaction further include: being carried out in the presence of a protective atmosphere.

[0122] In the present invention, the protective atmosphere may be a conventional protective atmosphere in the art, such as nitrogen.

[0123] In the present invention, preferably, the solution polymerization reaction is carried out under stirring conditions, specifically, the stirring speed is 150r / min-300r / min.

[0124] In the present invention, the method further comprises: a step of purifying the product of the polymerization reaction. The purification step is not particularly limited and can be performed according to conventional purification steps in the art.

[0125] In a specific embodiment of the present invention, the product obtained by the polymerization reaction is not purified, that is, the composition containing the emulsifier, water and the unsaturated amide copolymer is directly used as a curing agent composition for curing the epoxy resin.

[0126] The third aspect of the present invention provides an unsaturated amide copolymer prepared by the above method.

[0127] The fourth aspect of the present invention provides use of the unsaturated amide copolymer described in the first aspect or the third aspect as a curing agent.

[0128] In the present invention, the unsaturated amide copolymer is used as a curing agent in epoxy resin.

[0129] A fifth aspect of the present invention provides a curing agent composition, wherein the curing agent composition comprises a curing agent, an emulsifier and water;

[0130] The curing agent is the unsaturated amide copolymer described in the first aspect or the third aspect.

[0131] In the present invention, the curing agent composition comprises an unsaturated amide copolymer, an emulsifier and water, so that the curing agent composition has the characteristics of good fluidity and good dispersibility. When it is used for curing epoxy resin, the cured epoxy resin can have interconnected pores while maintaining a high compressive strength.

[0132] According to the present invention, based on the total weight of the curing agent composition, the content of the unsaturated amide copolymer is 32wt%-58wt%, the content of the emulsifier is 1wt%-6wt%, and the content of water is 36wt%-67wt%.

[0133] Furthermore, based on the total weight of the curing agent composition, the content of the unsaturated amide copolymer is 45wt%-55wt%, the content of the emulsifier is 3wt%-5wt%, and the content of water is 40wt%-52wt%.

[0134] Furthermore, based on the total weight of the curing agent composition, the content of the unsaturated amide copolymer is 50wt%-55wt%, the content of the emulsifier is 4wt%-5wt%, and the content of water is 40wt%-46wt%.

[0135] According to the present invention, the emulsifier is selected from at least one of sodium maleic anhydride monohexadecyl carboxylate, sodium maleic anhydride monomethacrylate hydroxyethyl carboxylate, octadecyl trimethyl ammonium chloride, hexadecyl trimethyl ammonium chloride, dodecyl trimethyl ammonium chloride, dihexadecyl dimethyl ammonium chloride, dodecyl dimethyl benzyl ammonium chloride, sodium dodecyl sulfonate, sodium dodecyl carboxylate and alkylphenol polyoxyethylene ether, and is preferably a mixture of sodium maleic anhydride monohexadecyl carboxylate, sodium maleic anhydride monomethacrylate hydroxyethyl carboxylate and alkylphenol polyoxyethylene ether.

[0136] In the present invention, there is no particular limitation on the preparation method of the curing agent composition. The unsaturated amide copolymer of the present invention may be directly mixed with an emulsifier and water, or may be prepared according to the following steps:

[0137] S1. In the presence of nitrogen, monomer A, an emulsifier and deionized water are stirred and mixed at 20° C. to 30° C. and 1000 r / min to 1500 r / min for 10 min to 15 min to obtain a first mixture;

[0138] S2, stirring and mixing the first mixture, monomer B and monomer C for 10 min-15 min to obtain a second mixture;

[0139] S3, mixing the second mixture with an initiator, performing a polymerization reaction, and then cooling to obtain the curing agent composition.

[0140] According to the present invention, at 25° C., the apparent viscosity of the curing agent composition is 120 mPa·s-360 mPa·s, preferably 150 mPa·s-220 mPa·s.

[0141] In the present invention, the apparent viscosity of the curing agent composition is measured at room temperature using a six-speed rotational viscometer.

[0142] In the present invention, the curing agent composition also includes conventional auxiliary agents in the art, such as a curing accelerator. There is no particular limitation on the type and amount of the curing accelerator. Conventional curing accelerators in the art can be used and added in conventional amounts in the art.

[0143] A sixth aspect of the present invention provides a method for preparing an epoxy resin product, wherein the preparation method comprises:

[0144] The first component containing epoxy resin is mixed with the curing agent composition and cured to obtain an epoxy resin product.

[0145] According to the present invention, the content of the curing agent composition is 30-50 parts by weight relative to 100 parts by weight of the first component.

[0146] Furthermore, relative to 100 parts by weight of the first component, the content of the curing agent composition is 30-40 parts by weight, preferably 30-35 parts by weight.

[0147] In the present invention, the curing agent composition provided by the present invention is used for curing epoxy resin, which can form interconnected pores in the cured epoxy resin while maintaining a relatively high compressive strength (up to about 50 MPa).

[0148] In the present invention, the epoxy resin is a water-soluble epoxy resin and / or a solvent-based epoxy resin, wherein the water-soluble epoxy resin is preferably a water-soluble bisphenol epoxy resin.

[0149] In the present invention, the first component also includes conventional auxiliary agents in the art such as emulsifiers. The type and amount of the emulsifier are not particularly limited and are added in the conventional amount in the art.

[0150] In the present invention, conventional equipment in the art may be used to mix the first component including the epoxy resin with the components in the curing agent composition, such as a twin-screw extruder or a mixer.

[0151] In the present invention, the curing conditions include: a curing temperature of 90° C.-150° C., a curing time of 6 h-24 h, and a curing pressure of 0 MPa-50 MPa.

[0152] A seventh aspect of the present invention provides an epoxy resin product produced by the above-mentioned preparation method.

[0153] An eighth aspect of the present invention provides a use of the above-mentioned curing agent composition or epoxy resin product in a phase change fracturing fluid.

[0154] The present invention will be described in detail below by way of examples. In the following examples,

[0155] The intrinsic viscosity of the copolymer was measured by the five-point method of the Ubbelohde viscometer. The sample preparation method was as follows: the copolymer was washed with excess acetone or ethanol for 4-5 times to obtain a white powder, which was placed in a vacuum oven at 90°C and dried to constant weight, diluted with a 1 mol / L NaCl standard solution to a 0.1% solution, and then the intrinsic viscosity was measured with an Ubbelohde viscometer;

[0156] The apparent viscosity of the curing agent composition was measured using a six-speed rotational viscometer;

[0157] The raw materials used in the examples and comparative examples are all commercially available.

[0158] Monomer A1: acrylamide, wherein R1', R2', R3' and R4' are -H in formula 7;

[0159] Monomer A2: methacrylamide, wherein R1' is -CH3, and R2', R3' and R4' are H;

[0160] Monomer A3: sodium 2-methyl-2-acrylamidopropanesulfonate, in formula 7, R1', R2' and R3' are -H, R4' is A', in formula 12, R 22 ' and R 23 ' is -CH3, m1 is 1, M is Na;

[0161] Monomer A4: N-(methoxymethyl)acrylamide, in formula 7, R1', R2' and R3' are -H, and R4' is -(CH2) n1 -OR 21 ', R 21 ' is -CH3, n1 is 1;

[0162] Monomer A5: N-ethyl acrylamide, wherein in formula 7, R1', R2' and R3' are -H, and R4' is a C2 alkyl group;

[0163] Monomer A6: N-dodecyl acrylamide, wherein in formula 7, R1', R2' and R3' are -H; R4' is a C12 alkyl group;

[0164] Monomer B1: styrene, in formula 8, R5', R6' and R7' are -H; X is -(CH2) z1 -, z1 is 0;

[0165] Monomer B2: 4-methylstyrene, in formula 8, R6' and R7' are -H, R5' is -CH3; X is -(CH2) z1 -, z1 is 0;

[0166] Monomer B3: 2-methylstyrene, in formula 8, R5' and R6' are -H, R7' is -CH3; X is -(CH2) z1 -, z1 is 0;

[0167] Monomer B4: vinyl benzyl alcohol, in formula 8, R6' and R7' are -H; R5 is -(CH2) r1 -OH, r1 is 1; X is -(CH2) z1 -, z1 is 0;

[0168] Monomer C1: 4-vinylaniline, in formula 11, R 10 ' is -NH2, R 11 ' and R 12 ' is -H; R 13 'for-H;

[0169] Monomer C2: vinyl imidazole, wherein R8' is -H in formula 9;

[0170] Monomer C3: vinylguanamine, wherein R9' is -H in formula 10.

[0171] Example A - Preparation of unsaturated acrylamide copolymer

[0172] Example A1

[0173] S1. In the presence of nitrogen, a four-necked round-bottom flask containing 55 parts by weight of deionized water, 30 parts by weight of acrylamide (monomer A1), 3 parts by weight of sodium maleic anhydride monohexadecyl carboxylate (HEC16) (emulsifier), and 2 parts by weight of nonylphenol polyoxyethylene ether (OP-10) (emulsifier) ​​was placed in a constant temperature water bath at 30°C, stirred at 1000 r / min, and mixed for 10 minutes to obtain a first mixture.

[0174] S2. Add 8 parts by weight of 4-vinylaniline (monomer C1) and 2 parts by weight of styrene (monomer B1) to the first mixture, stir at 1000 r / min, and mix for 15 minutes to obtain a second mixture.

[0175] S3, add 0.01 parts by weight of azobisisobutyronitrile and 0.02 parts by weight of azobisisobutylimidazoline hydrochloride (VA044) to the second mixture, stir and mix, reduce the speed to 300 r / min, polymerize at 30° C. for 4 hours, discharge, and purify to obtain unsaturated amide copolymer A1. Based on the total amount of the monomer mixture, the amount of initiator used is 0.075wt%.

[0176] Based on the total weight of the monomer mixture, the amount of the monomer A1 is 75 wt %, the amount of the monomer B1 is 5 wt %, and the amount of the monomer C1 is 20 wt %.

[0177] Based on the total weight of the unsaturated amide copolymer, the content of the structural unit I was 75 wt %, the content of the structural unit II was 5 wt %, and the content of the structural unit III was 20 wt %. The results are shown in Table 3.

[0178] Examples A2-A17

[0179] An unsaturated acrylamide copolymer was prepared according to the method of Example A1, except that the types and amounts of monomer A, monomer B and monomer C were different from those in Example A1, as shown in Table 1 for details.

[0180] Table 1 (parts by weight)

[0181]

[0182] Embodiment A18

[0183] Unsaturated amide copolymer was prepared according to the method of Example A17, except that the amount of azobisisobutyronitrile AIBN was 0.02 parts by weight, the amount of azobisisobutylimidazole salt VA044 was 0.04 parts by weight, and the amount of initiator was 0.15 wt% based on the total amount of the monomer mixture.

[0184] Embodiment A19

[0185] The unsaturated amide copolymer was prepared according to the method of Example A17, except that the amount of azobisisobutyronitrile AIBN was 0.03 parts by weight, the amount of azobisisobutylimidazole salt VA044 was 0.05 parts by weight, and the amount of initiator was 0.2 wt % based on the total amount of the monomer mixture.

[0186] Example A20

[0187] The unsaturated amide copolymer was prepared according to the method of Example A17, except that the initiator was 0.02 parts of dimethyl azobisisobutyrate and 0.04 parts of azobisisobutylimidazole salt VA044. The amount of initiator used was 0.15 wt % based on the total amount of the monomer mixture.

[0188] Example A21

[0189] The unsaturated amide copolymer was prepared according to the method of Example A17, except that the initiator was 0.04 weight part of azobisisobutylimidazole salt VA044 and 0.02 weight part of terephthalamide. The amount of initiator used was 0.15 weight % based on the total amount of the monomer mixture.

[0190] Example A22

[0191] The unsaturated amide copolymer was prepared according to the method of Example A17, except that the initiator was 0.04 parts by weight of azobisisobutylamidine hydrochloride and 0.02 parts by weight of terephthalamide. The amount of initiator used was 0.15 wt % based on the total amount of the monomer mixture.

[0192] Example A23

[0193] An unsaturated amide copolymer was prepared according to the method of Example A17, except that the initiator was 0.02 parts by weight of sodium bisulfite, 0.03 parts by weight of tert-butyl hydroperoxide and 0.02 parts by weight of terephthalamide. The amount of initiator used was 0.175 wt % based on the total amount of the monomer mixture.

[0194] Embodiment 24

[0195] An unsaturated amide copolymer was prepared according to the method of Example A17, except that the initiator was 0.01 parts by weight of sodium bisulfite, 0.03 parts by weight of ammonium persulfate and 0.02 parts by weight of terephthalamide, and the amount of the initiator was 0.15 wt % based on the total amount of the monomer mixture.

[0196] Example A25-Example A34, Comparative Example DA1, Comparative Example DA2

[0197] Unsaturated acrylamide copolymer was prepared according to the method of Example A1, except that the types and amounts of monomer A, monomer B and monomer C, and the amounts of deionized water and emulsifier were different from those in Example A1, as shown in Table 2 for details.

[0198] Table 2

[0199]

[0200] In the unsaturated amide copolymers prepared in Examples A1-A34, the contents of structural unit I, structural unit II and structural unit III are shown in Table 3. The intrinsic viscosity of the unsaturated amide copolymers was tested, and the results are shown in Table 3.

[0201] Table 3

[0202]

[0203]

[0204] It can be seen from Table 3 that compared with Comparative Examples DA1 and DA2, the unsaturated amide copolymers provided by Examples A1-A34 contain specific structural units I, II and III, so that the obtained unsaturated amide copolymers have a suitable intrinsic viscosity. When used as a curing agent for epoxy resin curing, the toughness of the cured resin product can be reduced and the strength of the resin product can be improved.

[0205] Example B - Curing Agent Composition

[0206] The unsaturated amide copolymer, emulsifier and water prepared in Example A were mixed to obtain curing agent compositions B1-B34 and curing agent compositions DB1-DB2, wherein the specific types and amounts of the unsaturated amide copolymer and the emulsifier are shown in Table 4. The apparent viscosity of the curing agent composition was tested, and the results are shown in Table 5.

[0207] Table 4

[0208]

[0209]

[0210] Table 5

[0211]

[0212]

[0213] It can be seen from Table 5 that compared with Comparative Examples DB1 and DB2, the curing agent composition comprising the unsaturated amide polymer comprising specific structural units of the present invention provided by Examples B1 to B34 of the present invention has a more suitable apparent viscosity, which can ensure that the product after being cured by the resin composition has a permeability and porosity that meet the requirements while the resin composition has good injectability.

[0214] Application Examples

[0215] S1, 8g of epoxy resin E51, 16g of water-based epoxy resin solution (water-based propylene-modified epoxy resin WX-609) (mass concentration 50wt%), and 2g of emulsifier OP-15 were mixed to obtain a first component;

[0216] S2. After 8 g of the curing agent composition prepared in Example B is mixed evenly with the first component, the mixture is placed in a high-temperature reaction kettle and kept at a constant temperature of 150° C. for 6 hours. After being taken out, the mixture is completely cured to obtain epoxy resins P1-P34 and epoxy resins DP1-DP2.

[0217] The content of the curing agent composition is 44.4 parts by weight relative to 100 parts by weight of the first component. The porosity of the epoxy resin was tested using a saturated kerosene method, and the permeability of the epoxy resin was tested using a high-pressure displacement device. The test was conducted in accordance with the enterprise standard Q / SH1020 "Method for Determining the Permeability of High Permeability Consolidated Cores" of Sinopec Shengli Oilfield Administration, and the results are shown in Table 6.

[0218] Table 6

[0219]

[0220]

[0221] * In the present invention, 5000 mD in the application example does not represent the upper limit of permeability, but is only the upper limit of the high pressure displacement device test instrument.

[0222] It can be seen from the results in Table 6 that, compared with Comparative Application Examples 1 and 2, in Application Examples 1-34, the curing agent composition of the present invention is used as a curing agent, and the epoxy resin products prepared therefrom have certain permeability and porosity, and can be used as a phase change fracturing fluid in oil and gas production.

[0223] Furthermore, the epoxy resin products prepared in Application Examples 1-2 and 15-18 still have high permeability and porosity at the high pressure of 50 MPa compared with the epoxy resin products prepared in other Application Examples.

[0224] Figure 1 This is a picture of the epoxy resin product obtained in Application Example 1. Figure 1 It can be seen that the epoxy resin product obtained by curing with the unsaturated amide copolymer of the present invention as a curing agent has a pore structure, and there are a large number of pores in the epoxy resin product, so that the cured epoxy resin can be used as a phase change fracturing fluid in oil and gas production.

[0225] Figure 2 For the picture of the epoxy resin product obtained by using Comparative Example 1, Figure 2 It can be seen that the epoxy resin product obtained after curing is dense and non-porous, and cannot be used as a phase change fracturing fluid in oil and gas production.

[0226] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. An unsaturated amide copolymer, characterized in that: The unsaturated amide copolymer comprises structural unit I, structural unit II and structural unit III; The structural unit I has a structure shown in Formula 1, the structural unit II has a structure shown in Formula 2, and the structural unit III has a structure shown in at least one of Formula 3, Formula 4 and Formula 5; Wherein, in Formula 1, R1 is -H or -CH3, R2 and R3 are each independently -H or a C1-C18 alkyl group; R4 is -H, A, a C1-C20 alkyl group or -(CH2) n -OR 21 ; R 21 is -H or a C1-C18 alkyl group, and n is an integer of 0-12; A has the structure shown in Formula 6; In formula 6, R 22 and R 23 Each is independently -H or a C1-C18 alkyl group, and m is an integer of 0-18; In Formula 2, R5, R6 and R7 are each independently -H, C1-C12 alkyl or -(CH2) r -OH, r is an integer of 1-12; X is -(CH2) z -, z is an integer from 0 to 5; In formula 3, R8 is -H or -CH3; In formula 4, R9 is -H or -CH3; In formula 5, R 10 , R 11 and R 12 Each is independently -H or -NH2, and at least one is -NH2; R 13 It is -H or -CH3.

2. The unsaturated amide copolymer according to claim 1, wherein In Formula 1, R1 is -H or -CH3, R2 and R3 are each independently -H, and R4 is -H, a C2 alkyl group or a C12 alkyl group; preferably, R1, R2, R3 and R4 are all -H; Preferably, in Formula 2, R5 is -(CH2) r -OH or -H, r is an integer of 1-3; R6 and R7 are each independently -H; X is -(CH2) z -, z is an integer from 0 to 2; preferably, R5, R6 and R7 are each independently -H; Preferably, in Formula 3, R8 is -H; Preferably, in Formula 4, R9 is -H; Preferably, in Formula 5, R 10 , R 11 and R 12 Each is independently -H or -NH2, and at least one is -NH2; R 13 is -H.

3. The unsaturated amide copolymer according to claim 1 or 2, wherein Based on the total weight of the unsaturated amide copolymer, the content of the structural unit I is 65wt%-85wt%, the content of the structural unit II is 5wt%-7wt%, and the content of the structural unit III is 12wt%-27wt%; Preferably, based on the total weight of the unsaturated amide polymer, the content of the structural unit I is 70wt%-82wt%, the content of the structural unit II is 5wt%-6wt%, and the content of the structural unit III is 12.5wt%-20wt%.

4. The unsaturated amide copolymer according to any one of claims 1 to 3, wherein At 25° C., the intrinsic viscosity of the copolymer is 200 mL / g-1200 mL / g, preferably 900 mL / g-1200 mL / g.

5. A method for preparing an unsaturated amide copolymer, characterized in that: The method comprises the following steps: Under solution polymerization conditions, in the presence of an initiator and an emulsifier, a monomer mixture is polymerized in water to obtain the unsaturated amide copolymer; the monomer mixture comprises monomer A, monomer B and monomer C; The monomer A has a structure as shown in Formula 7, the monomer B has a structure as shown in Formula 8, and the monomer C has a structure as shown in at least one of Formula 9, Formula 10 and Formula 11; Wherein, in Formula 7, R1' is H or CH3, R2' and R3' are each independently -H or a C1-C18 alkyl group; R4' is -H, A', a C1-C20 alkyl group or -(CH2) n1 -OR 21 ';R 21 ' is -H or a C1-C18 alkyl group, and n1 is an integer of 0-12; A' has the structure shown in Formula 12; In formula 12, R 22 ' and R 23 'Each independently represents -H, C1-C18 alkyl, M represents -H, Na or K; m1 represents an integer of 0-18; In Formula 8, R5', R6' and R7' are each independently -H, C1-C12 alkyl or -(CH2) r1 -OH, r1 is an integer from 1 to 12; X is -(CH2) z1 -, z1 is an integer from 0 to 5; In formula 9, R8' is -H or -CH3; In formula 10, R9' is -H or -CH3; In formula 11, R 10 '、R 11 ' and R 12 ' are each independently -H or -NH2, and at least one is -NH2; R 13 ' is -H or -CH3.

6. The method according to claim 5, wherein: In Formula 7, R1' is -H or -CH3, R2' and R3' are each independently -H, and R4' is -H, a C2 alkyl group or a C12 alkyl group; preferably, R1', R2', R3' and R4' are all -H; Preferably, in Formula 8, R5' is -(CH2) r -OH or -H, r is an integer of 1-12; R6' and R7' are each independently -H; X is -(CH2) z1 -, z1 is an integer from 0 to 2; preferably, R5, R6 and R7 are each independently -H; Preferably, in Formula 9, R8' is -H; Preferably, in formula 10, R9' is -H; Preferably, in Formula 11, R 10 '、R 11 ' and R 12 ' are each independently -H or -NH2, and at least one is -NH2; R 13 ' is -H.

7. The method according to claim 5 or 6, wherein: Based on the total weight of the monomer mixture, the amount of the monomer A is 65wt%-85wt%, the amount of the monomer B is 5wt%-7wt%, and the amount of the monomer C is 12wt%-27wt%; Preferably, based on the total weight of the monomer mixture, the amount of the monomer A is 70wt%-82wt%, the amount of the monomer B is 5wt%-6wt%, and the amount of the monomer C is 12.5wt%-20wt%.

8. The method according to any one of claims 5 to 7, wherein: Based on the total weight of the monomer mixture, the amount of the emulsifier is 1wt%-6wt%, preferably 3wt%-5wt%, more preferably 4wt%-5wt%; Preferably, based on the total weight of the monomer mixture, the amount of the initiator is 0.01-0.1 wt %, preferably 0.02-0.08 wt %, more preferably 0.04-0.06 wt %.

9. The method according to claim 8, wherein: The emulsifier is selected from at least one of sodium maleic anhydride monohexadecyl carboxylate, sodium maleic anhydride monomethacrylate hydroxyethyl carboxylate, octadecyl trimethyl ammonium chloride, hexadecyl trimethyl ammonium chloride, dodecyl trimethyl ammonium chloride, dihexadecyl dimethyl ammonium chloride, dodecyl dimethyl benzyl ammonium chloride, sodium dodecyl sulfonate, sodium dodecyl carboxylate and alkylphenol polyoxyethylene ether, preferably a mixture of sodium maleic anhydride monohexadecyl carboxylate, sodium maleic anhydride monomethacrylate hydroxyethyl carboxylate and alkylphenol polyoxyethylene ether; Preferably, the initiator is selected from a mixture of an oil-soluble initiator and a water-soluble initiator, or an amphiphilic initiator; Preferably, the oil-soluble initiator is selected from at least one of azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate and terephthalamide, preferably azobisisobutyronitrile; Preferably, the water-soluble initiator is selected from at least one of hydrogen peroxide, tert-butyl hydroperoxide, persulfate, sodium sulfite, sodium bisulfite, azobisisobutylamidine hydrochloride and azobisisobutylimidazoline hydrochloride; Preferably, the amphiphilic initiator is azoisobutylcyanamide; Preferably, the initiator is a mixture of azobisisobutyronitrile and azobisisobutylimidazoline hydrochloride; Preferably, the mass ratio of the azobisisobutyronitrile to the azobisisobutylimidazoline hydrochloride is 1:1-9, preferably 1:2-9.

10. The method according to any one of claims 5 to 9, wherein: The solution polymerization reaction conditions include: polymerization temperature of 30-50°C, preferably 35-45°C, more preferably 40-42°C; polymerization time of 2h-8h, preferably 2h-6h, more preferably 3h-4h; Preferably, the solution polymerization reaction conditions further include: being carried out in the presence of a protective atmosphere.

11. An unsaturated amide copolymer prepared by the method according to any one of claims 5 to 10.

12. Use of the unsaturated amide copolymer according to any one of claims 1 to 4 and 11 as a curing agent, preferably as a curing agent in epoxy resin.

13. A curing agent composition, characterized in that: The curing agent composition comprises a curing agent, an emulsifier and water; The curing agent is the unsaturated amide copolymer according to any one of claims 1 to 4 and 11.

14. The curing agent composition according to claim 13, wherein Based on the total weight of the curing agent composition, the content of the unsaturated amide copolymer is 32wt%-58wt%, the content of the emulsifier is 1wt%-6wt%, and the content of water is 36wt%-67wt%; Preferably, based on the total weight of the curing agent composition, the content of the unsaturated amide copolymer is 45wt%-55wt%, the content of the emulsifier is 3wt%-5wt%, and the content of water is 40wt%-52wt%; More preferably, based on the total weight of the curing agent composition, the content of the unsaturated amide copolymer is 50wt%-55wt%, the content of the emulsifier is 4wt%-5wt%, and the content of water is 40wt%-46wt%.

15. The curing agent composition according to claim 13 or 14, wherein The emulsifier is selected from at least one of sodium maleic anhydride monohexadecyl carboxylate, sodium maleic anhydride monomethacrylate hydroxyethyl carboxylate, octadecyl trimethyl ammonium chloride, hexadecyl trimethyl ammonium chloride, dodecyl trimethyl ammonium chloride, dihexadecyl dimethyl ammonium chloride, dodecyl dimethyl benzyl ammonium chloride, sodium dodecyl sulfonate, sodium dodecyl carboxylate and alkylphenol polyoxyethylene ether, and is preferably a mixture of sodium maleic anhydride monohexadecyl carboxylate, sodium maleic anhydride monomethacrylate hydroxyethyl carboxylate and alkylphenol polyoxyethylene ether.

16. The curing agent composition according to any one of claims 13 to 15, wherein At 25° C., the apparent viscosity of the curing agent composition is 120 mPa·s-360 mPa·s, preferably 150 mPa·s-220 mPa·s.

17. A method for preparing an epoxy resin product, characterized in that: The preparation method comprises: Mixing a first component comprising an epoxy resin with a curing agent composition comprising any one of claims 13 to 16, and curing the mixture to obtain an epoxy resin product; Preferably, the content of the curing agent composition is 30-50 parts by weight relative to 100 parts by weight of the first component.

18. An epoxy resin product obtained by the preparation method according to claim 17.

19. Use of the curing agent composition according to any one of claims 13 to 16 or the epoxy resin product according to claim 18 in phase change fracturing fluid.