Water-based double-component high-adhesion white primer and preparation method thereof

Through the formula of water-based two-component high adhesion white primer, the problems of long drying time, poor adhesion and insufficient filling are solved, and rapid drying, preventing prickly heat and dark bubbles are achieved, and adhesion and filling are improved. It is suitable for furniture manufacturing of medium fiber boards.

CN119039841APending Publication Date: 2024-11-29ZHUHAI ZHANCHEN NEW MATERIALS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411291053.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The water-based white primer has a long drying time on the medium fiber board, which is prone to prickly heat and dark bubbles, has poor adhesion and poor filling properties, making it difficult to meet the production needs of the furniture manufacturing industry.

Method used

Use aqueous two-component high adhesion white primer formula, including aqueous hydroxyacrylic emulsion, wetting agent, defoaming agent, film forming additive, low shear thickening agent, lithium acid rheology agent, gas-silicon dispersion liquid, Dispersants, titanium dioxide, silicon powder, preservatives and polishing additives are designed to improve the adhesion and filling of the paint film through resin screening, rheology additive selection and rapid defoaming agent combination.

Benefits of technology

It realizes rapid drying of water-based paint, prevents prickly heat and dark bubbles, improves adhesion and fillability, and achieves a surface effect similar to oil-based paint. It is suitable for forced drying at high temperatures and thick coatings, which are not prone to problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a water-based double-component high-adhesion white primer and a preparation method thereof, and the water-based double-component high-adhesion white primer comprises the following components by weight: 35-45% of a water-based hydroxyl acrylic emulsion; 0.2%-0.5% of a wetting agent; 1.3 to 3.6 percent of a defoaming agent; 2-5% of a coalescing agent; 0.1 to 0.5 percent of a low-shear thickening agent; 0.2%-0.8% of a lithium acid salt rheological agent; 1-3% of a gas silicon dispersion liquid; 1-3% of a dispersant; 28-35% of titanium dioxide; 5-15% of silica powder; 0.1 to 0.3 percent of preservative; 1-3% of a polishing auxiliary agent; and 3-15% of water. According to the water-based double-component high-adhesion white primer disclosed by the invention, through new formula design concepts such as resin screening, rheological additive selection and rapid defoaming agent matching, the defects of water-based paint are overcome, and the surface effect of oil paint is achieved. The coating is widely applicable to substrates such as wood boards and fiber boards, is forcibly dried at high temperature, is not easy to sag, does not generate miliaria when being thickly coated, and is high in covering power and filling property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to a water-based two-component high-adhesion white primer and a preparation method thereof. Background Art

[0002] With the increasing demand for water-based mechanical coating and the standards for customized furniture, the oil-to-water solution has been introduced in the furniture manufacturing industry. Under the supervision of the national environmental protection, water-based wood paint has made great progress, but it also faces a series of challenges. In the traditional oil-based construction process, spraying two coats of oil-based white primer can basically seal the MDF, but after switching to water-based coating, many problems have appeared. The impact is as follows:

[0003] 1. Water-based single-component and double-component white primers dry relatively slowly. Conventional water-based double-component white primers also need to be dried on the surface first (temperature and humidity 25°C / 40-80% RH, surface drying 30-60 minutes), and then forced drying (temperature 35-40°C, humidity less than 30% RH, drying 10 hours). Due to the large number of product shipments and limited space, the drying time that is more easily accepted by general furniture companies is about 4 hours.

[0004] 2. During the forced drying process, water-based white primer is prone to heat rash, dark bubbles, etc. due to the thick coating of powder and coating. The process and equipment on site are still oil-based. In order to ensure normal delivery to customers, this process does not have a long surface drying time for water-based paint, which means that it is a great challenge for the drying of water-based paint. Water-based paint that is forced to dry without surface drying is very likely to have heat rash, dark bubbles, etc. After polishing, pinholes will appear on the surface and the flatness is not ideal.

[0005] 3. The adhesion of water-based white primer on MDF is not as good as that of oil-based paint. After thick coating, the interlayer adhesion becomes poor. Since the formula design of water-based paint is limited by the solid content of the emulsion, and the water-based paint contains water, it is absorbed by the lignin and fiber of the MDF, so the filling property is poor, it is easy to sink, and the spray topcoat film is not full enough. Summary of the invention

[0006] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a water-based two-component high-adhesion white primer and a preparation method thereof.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A water-based two-component high-adhesion white primer, the components and weight ratio of which include:

[0009] Water-based hydroxy acrylic emulsion 35-45%;

[0010] Wetting agent 0.2-0.5%;

[0011] Defoamer 1.3-3.6%;

[0012] Film-forming aid 2-5%;

[0013] Low shear thickener 0.1-0.5%;

[0014] Lithium salt rheological agent 0.2-0.8%;

[0015] Gas silicon dispersion 1-3%;

[0016] Dispersant 1-3%;

[0017] Titanium dioxide 28-35%;

[0018] Silica powder 5-15%;

[0019] Preservatives 0.1-0.3%;

[0020] Grinding aid 1-3%;

[0021] Water 3-15%.

[0022] Preferably, the water-based hydroxy acrylic emulsion is selected from Oubaodi AC31 or Wanhua 4708 or Dow PROSPERSE 200 or Wanhua 2035 or Dow PROSPERSE 800 or Zhanchen hydroxyacrylic emulsion S7810.

[0023] Preferably, the wetting agent is BYK-346 wetting agent.

[0024] Preferably, the defoamer includes BYK-1789 defoamer, TEGO-923 defoamer, TEGO-904W defoamer, and TEGO-Foamex11 defoamer, wherein the weight proportion of the BYK-1789 defoamer is 0.2-0.5%, the weight proportion of the TEGO-923 defoamer is 0.3-0.8%, the weight proportion of the TEGO-904W defoamer is 0.3-0.8%, and the weight proportion of the TEGO-Foamex11 defoamer is 0.5-1.5%.

[0025] Preferably, the film-forming aid is DOW-dipropylene glycol butyl ether, the low-shear thickener is Wanhua U605 water-based polyurethane thickener; and the lithium salt rheological agent is BYK-S482 rheological aid.

[0026] Preferably, the fumed silica dispersion uses WF7620 fumed silica rheology control agent; and the dispersant uses BYK190 dispersant.

[0027] Preferably, the titanium dioxide is Longbai 996 titanium dioxide; the silicon micropowder is Haiyang silicon micropowder.

[0028] Preferably, the preservative is DOW342 preservative; the polishing aid is HS2000 polishing aid.

[0029] The present invention also protects a method for preparing a water-based two-component high-adhesion white primer, comprising the following steps:

[0030] The following steps are involved:

[0031] S1, adding the water-based hydroxy acrylic emulsion into a stirring tank according to the proportion and stirring evenly;

[0032] S2, adding wetting agent and defoaming agent into the stirring tank according to the proportion and stirring;

[0033] S3, film-forming aid and water in a ratio of 1:1, add into the stirring kettle and stir;

[0034] S4, adding low shear thickener, lithium salt rheological agent, gas silicon dispersion, dispersant, titanium dioxide and silicon micropowder into a stirring kettle according to the proportion and stirring;

[0035] S5, adding preservative, grinding aid and water 3-15% into the stirring kettle according to the proportion and stirring;

[0036] S6. After preparation, send it for inspection and preservation.

[0037] Preferably, the stirring speed in step S1 is 500 rpm / min; the stirring speed in step S2 is 900 rpm / min, and the stirring time is 5 min; when adding the raw materials in step S3, the speed is first adjusted to 400 rpm / min, and after the addition is completed, the speed is adjusted to 1500 rpm / min, and high-speed dispersion is performed for 30 min, the fineness is less than 40 μm, and there is no shrinkage cavity; in step S4, the speed is adjusted to 500 rpm / min and dispersed for 15 min.

[0038] The water-based two-component high-adhesion white primer of the present invention removes the shortcomings of water-based paint and achieves the surface effect of oil-based paint through new formula design concepts such as resin screening, rheological additive selection, and rapid defoaming agent matching. It is suitable for substrates such as wood boards and fiber boards, and is forced to dry at high temperatures, is not easy to sag, does not cause prickly heat when thickly applied, and has strong hiding power and filling properties. DETAILED DESCRIPTION

[0039] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0040] Examples 1-6

[0041] When choosing resin, the first thing to consider is that the water-based emulsion itself has good powder encapsulation, so that the overall solid content can be increased and high filling capacity can be provided; at the same time, it does not have stable foaming properties. If the foaming properties are strong, it will have a serious impact on the defoaming of the system and is not conducive to formula adjustment; finally, the resin drying time must be considered to see if it can meet the production and delivery needs of customers. Therefore, the commercially available water-based resins were screened and evaluated as follows, and the specific ratios of Examples 1-6 shown in Table 1 were obtained:

[0042] Table 1 Component ratio table of Examples 1-6

[0043]

[0044] The paints of Examples 1-6 were prepared according to the ratio of main paint: water-based curing agent: water of 100:10:10, with a coating amount of 220 μm and baked at 30° C. The results are shown in Table 2.

[0045] Table 2 Comparison of experimental data of Examples 1-6

[0046]

[0047] The data in Table 2 show that different water-based resins have great differences in drying time, and can better meet the production needs of customers. For example, the grinding time of Example 3 is longer than that of other solutions. The same resin has different performances. For example, Example 1 has good grinding and filling properties, but its defoaming performance is average. Example 2 has good grinding and defoaming properties, but the fullness of the paint film is poor, showing that the filling property is not as good as other solutions. Examples 4-6 are better overall, among which Example 6 performs better in all aspects, especially in viscosity stability.

[0048] Examples 7-10

[0049] The resin of Example 6 was used as the main film-forming substance, and its dosage was compared to confirm the appropriate dosage range, and Examples 7-10 were obtained. The specific scheme is shown in Table 3.

[0050] Table 3 Component ratio table of Examples 6-10

[0051]

[0052] Examples 6-10 were prepared according to the ratio of main paint: water-based curing agent: water of 100:10:10, and the performance of the paint was compared. The coating amount was 220 microns and the paint was baked at 30°C. The results are shown in Table 4.

[0053] Table 4 Comparison of experimental data of Examples 6-10

[0054] Detection indicators Standard requirements Example 6 Example 7 Example 8 Example 9 Example 10 Foam stability in tank Overnight without bubbles none none none none none Construction defoaming Defoams within 3 minutes excellent excellent excellent excellent excellent Grinding time 2-4h 3 2.5 3 3 3.5 Polishability Sand sticking good good good good middle Dry film defoaming No pinholes or prickly heat Small amount Small amount Small amount Small amount Small amount Filling Smooth and non-transparent bottom good middle middle middle good Thermal storage stability 50℃ hot storage state Stablize Gelation Thickening is obvious Stablize Stablize

[0055] The above data show that the resin dosage is in the range of 30-50%, wherein the drying time will become faster when the resin content is 30%, but the powder wrapping is poor when the resin content is small, resulting in extremely unstable viscosity; and the polishing property will become worse when the resin content is 50%; the overall better range is 35-45%, wherein 40% resin content performs best, as shown in Example 6.

[0056] Examples 11-16

[0057] The construction method involved has a vertical sag requirement due to the workpiece, so the anti-sag performance must be much stronger than the conventional formula. The anti-sag additives on the market were tested as follows to obtain Examples 11-16, as shown in Table 5.

[0058] Table 5 Component ratios of Examples 11-16

[0059]

[0060] The paint performance of Examples 6, 11-16 was compared, with the main paint: water-based curing agent: water being 100:10:10, the coating amount being 220 microns, and the baking being 30°C. The results are shown in Table 6:

[0061] Table 6 Comparison of experimental data of Examples 11-16

[0062]

[0063] Note: Performance is scored on a scale of 0-5, with higher numbers indicating better performance.

[0064] According to the above data, it is far from enough to use polyurethane thickeners to improve anti-sagging, and different types of thickeners need to be used to assist. For example, in Examples 6, 11, and 12, the non-sagging film thickness is only about 75 μm, while it can reach 125 μm when combined with lithium salts. The best solution is Example 16, which is a polyurethane thickener combined with lithium salts and gas silicon dispersions to achieve the best effect of three thickening rheological modes, 150-175 μm. The bentonite used in Example 14 has an effect on defoaming, and no compounding test was performed.

[0065] Examples 17-18

[0066] For the forced drying process, it is particularly important for high solid content and high viscosity coatings to have good defoaming properties. Excellent defoaming can make the bubbles in the paint film come out before the surface is dry, avoiding the defects of pinholes, dark bubbles, etc. caused by the bubbles remaining in the paint film. In order to improve the anti-prickly heat ability, Examples 17-18 were obtained, as shown in Table 7.

[0067] Table 7 Component ratios of Examples 17-18

[0068]

[0069] Examples 16-18 were prepared according to the ratio of main paint: water-based curing agent: water of 100:10:10, and the performance was compared. The coating amount was 220 microns and the baking was performed at 30°C. The results are shown in Table 8:

[0070] Table 8 Comparison of experimental data of Examples 17-18

[0071] Detection indicators Standard requirements Example 16 Embodiment 17 Embodiment 18 Foam stability in tank Overnight without bubbles 4.6 4.6 4.6 Construction defoaming Defoams within 3 minutes 4.4 4.6 4.8 Dry film surface effect No pinholes or prickly heat 3.8 3.8 4.5

[0072] Note: Performance is scored on a scale of 0-5, with higher numbers indicating better performance.

[0073] The above data show that the use of silicone defoamer BYK-1789 on the basis of Example 16 can significantly improve the defoaming properties of the dry film, and when combined with TEGOFoamex11, there can be almost no obvious pinholes or dark bubbles, which fully meets the use requirements.

[0074] The main resin used in this patent is a water-based self-produced hydroxypropyl emulsion with patent protection. The test method and evaluation method using the proportion of this emulsion are within the scope of protection.

[0075] In the embodiments provided in this application, the rheological additives used are BYK S-482 rheological additives and Evonik Chemical gas silicon dispersion WF7620, which are not limited to these brands, and other similar models can achieve similar effects of this patent. The defoamer used is a combination of BYK-1789, TEGO923, TEGO904W, and TEGOFoamex11, which are not limited to these brands of defoamers, and other similar models can achieve the same effect.

[0076] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A water-based two-component high-adhesion white primer, characterized in that : Components and weight proportions include: Water-based hydroxy acrylic emulsion 35-45%; Wetting agent 0.2-0.5%; Defoaming agent 1.3-3.6%; Film-forming aid 2-5%; Low shear thickener 0.1-0.5%; Lithium salt rheological agent 0.2-0.8%; Gas silicon dispersion 1-3%; Dispersant 1-3%; Titanium dioxide 28-35%; Silica powder 5-15%; Preservatives 0.1-0.3%; Grinding aid 1-3%; Water 3-15%.

2. A water-based two-component high-adhesion white primer according to claim 1, characterized in that: The water-based hydroxy acrylic emulsion is selected from Oubaodi AC31 or Wanhua 4708 or Dow PROSPERSE 200 or Wanhua 2035 or Dow PROSPERSE 800 or Zhanchen hydroxyacrylic emulsion S7810.

3. A water-based two-component high-adhesion white primer according to claim 1, characterized in that: The wetting agent is BYK-346 wetting agent.

4. The water-based two-component high-adhesion white primer according to claim 1, characterized in that: The defoamer includes BYK-1789 defoamer, TEGO-923 defoamer, TEGO-904W defoamer, and TEGO-Foamex11 defoamer, wherein the weight proportion of the BYK-1789 defoamer is 0.2-0.5%, the weight proportion of the TEGO-923 defoamer is 0.3-0.8%, the weight proportion of the TEGO-904W defoamer is 0.3-0.8%, and the weight proportion of the TEGO-Foamex11 defoamer is 0.5-1.5%.

5. The water-based two-component high-adhesion white primer according to claim 1, characterized in that: The film-forming aid is DOW-dipropylene glycol butyl ether, the low-shear thickener is Wanhua U605 water-based polyurethane thickener; and the lithium salt rheological agent is BYK-S482 rheological aid.

6. The water-based two-component high-adhesion white primer according to claim 1, characterized in that: The fumed silica dispersion uses WF7620 fumed silica rheology control agent; the dispersant uses BYK190 dispersant.

7. The water-based two-component high-adhesion white primer according to claim 1, characterized in that: The titanium dioxide is Longbai 996 titanium dioxide; the silicon micropowder is Haiyang silicon micropowder.

8. The water-based two-component high-adhesion white primer according to claim 1, characterized in that: The preservative is DOW342 preservative; the polishing aid is HS2000 polishing aid.

9. A method for preparing a water-based two-component high-adhesion white primer according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1, adding the water-based hydroxy acrylic emulsion into a stirring tank according to the proportion and stirring evenly; S2, adding wetting agent and defoaming agent into the stirring tank according to the proportion and stirring; S3, film-forming aid and water in a ratio of 1:1, add into a stirring kettle and stir; S4, adding low shear thickener, lithium salt rheological agent, gas silicon dispersion, dispersant, titanium dioxide and silicon micropowder into a stirring kettle according to the proportion and stirring; S5, adding preservative, grinding aid and water 3-15% into the stirring kettle according to the proportion and stirring; S6. After preparation, send it for inspection and preservation.

10. The method for preparing a water-based two-component high-adhesion white primer according to claim 9, characterized in that: The stirring speed in step S1 is 500 rpm / min; the stirring speed in step S2 is 900 rpm / min, and the stirring time is 5 min; when adding the raw materials in step S3, the speed is first adjusted to 400 rpm / min, and after the addition is completed, the speed is adjusted to 1500 rpm / min, and high-speed dispersion is performed for 30 min, the fineness is less than 40 μm, and there is no shrinkage cavity; in step S4, the speed is adjusted to 500 rpm / min, and dispersion is performed for 15 min.

Citation Information

Patent Citations

  • Easy-to-polish water-based woodware double-component white primer and preparation method thereof

    CN105419603A

  • Water-based bi-component white primer and preparation method thereof

    CN105482586A

  • Water-based two-component seal white primer and preparation method thereof

    CN109370398A

  • Water-based two-component white primer and preparation method thereof

    CN112029392A

  • Water-borne wood paint and preparation method thereof

    CN116875167A