Cr < 3 + >-doped non-spherical silicon oxide composite abrasive particle as well as preparation method and application thereof

By converting spherical silicon oxide into an non-spherical structure and blending Cr3+ to form composite abrasive particles, the problem of low polishing rate of SiC surface of traditional abrasive particles is solved, and efficient removal of SiC materials is achieved, and the polishing rate and efficiency are improved.

CN119039935APending Publication Date: 2024-11-29TAICANG SILICON SOURCE NANOMATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411285352.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Traditional silicon dioxide abrasive particles have a low polishing rate on the surface of silicon carbide, resulting in low processing efficiency and high cost of SiC materials, hindering the wider application of SiC materials.

Method used

Spherical silicon oxide is converted into an anion-induced method and Cr3+ is added thereto to form Cr3+ doped non-spherical silicon oxide composite abrasive particles, increasing the contact site between the abrasive particles and the SiC wafer, and passing through permanganic acid The oxidation effect of potassium accelerates the formation of the surface oxide layer of silicon carbide, and synergistically improves polishing efficiency.

Benefits of technology

The material removal rate of SiC wafers is significantly improved and the polishing rate is increased by 222%, solving the problem of low efficiency of traditional abrasive particles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039935A_ABST
    Figure CN119039935A_ABST
Patent Text Reader

Abstract

The invention discloses Cr < 3 + >-doped non-spherical silicon oxide composite abrasive particles as well as a preparation method and application thereof, and belongs to the field of silicon carbide surface polishing. According to the non-spherical silicon oxide, spherical silicon oxide is induced to be formed through sodium metaaluminate, then Cr < 3 + > is further doped into the non-spherical silicon oxide, and the material removal rate after silicon carbide wafer polishing is improved in the two aspects of chemical reaction and mechanical action. Compared with conventional spherical silicon oxide abrasive particles, the Cr < 3 + >-doped non-spherical silicon oxide composite abrasive particles have the advantage that the material removal rate of silicon carbide can be maximally increased by 222%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a non-spherical nano-level abrasive grain and a preparation method thereof, in particular to a preparation method of a non-spherical silicon oxide composite abrasive grain, which is used in the polishing process of silicon carbide round crystals and belongs to the field of surface polishing technology. Background Art

[0002] Single crystal silicon carbide (SiC) has excellent electronic and thermal properties. It is a typical third-generation semiconductor power device material and occupies an important position in the modern electronic information industry. Due to the excellent comprehensive performance of SiC materials, with the gradual development of SiC materials in my country, the requirements for its processing accuracy are becoming increasingly in-depth. The quality of SiC surface flattening directly affects the performance of the product and determines the yield of the product. However, due to its high hardness and chemical inertness, it faces problems such as low processing efficiency and high cost in flattening processing, which hinders the wider application of SiC.

[0003] Chemical mechanical polishing (CMP) is the only method that can achieve global polishing of SiC surface. The SiC wafer fixed on the carrier and the polishing pad move relative to each other in the polishing liquid under a certain pressure. The oxidant in the polishing liquid reacts chemically with the sample surface under friction to form a soft layer. After the soft layer is removed by the mechanical action of the abrasive, a flat SiC surface can be obtained. Among the many abrasives, silicon dioxide (SiO 2 ) has been widely studied by scholars at home and abroad because of its moderate hardness, good dispersibility and stability, but the traditional SiO 2 The polishing rate of abrasive particles on SiC is very low. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the existing processing technology and provide a Cr 3+ Doped non-spherical silicon oxide abrasive particles, preparation method thereof, and application thereof. Compared with conventional silicon oxide abrasive particles, the present invention converts spherical silicon oxide into a non-spherical structure by anion induction method, and then adds metal Cr 3+ Added into non-spherical silicon oxide to form composite abrasives. The non-spherical silicon oxide structure can increase the contact points between the abrasive and the SiC wafer, thus improving the mechanical effect during the CMP process. 3+ The addition of improves the oxidation effect of potassium permanganate, accelerates the formation of oxide layer on the surface of silicon carbide, and accelerates the chemical reaction in the CMP process. The chemical action and mechanical action work together to improve the material removal rate of SiC wafers.

[0005] In order to achieve the above object, the present invention adopts the following technical solution:

[0006] A Cr 3+ The method for preparing doped non-spherical silicon oxide abrasive particles comprises the following steps:

[0007] S1 preparation of non-spherical silicon oxide abrasive particles;

[0008] S2 Preparation of Cr 3+ Doped non-spherical silicon oxide composite abrasive.

[0009] Furthermore, the method for preparing the non-spherical silicon oxide abrasive grains in step S1 is:

[0010] S11: dispersing silica sol in deionized water, mixing well, placing under reflux and magnetic stirring at 100° C., adding sodium aluminate solution into the silica sol at one time, and obtaining a solution after the reaction is completed;

[0011] S12: The solution after the reaction is left to age to obtain a solution containing non-spherical silicon oxide abrasive grains.

[0012] Furthermore, in step S11, the concentration of the sodium aluminate solution is 0.3 wt. %; the particle size of the silica sol is 100 nm; the solid content of the silica sol is 40 wt. %, and the mass ratio of the sodium aluminate solution, the silica sol and the deionized water is 8:15:33.

[0013] Furthermore, in step S11, the heating method is oil bath heating; and the heating time is 3 hours.

[0014] Furthermore, during the aging process in step S12, the aging temperature is 100° C. and the aging time is 2 h.

[0015] Further, in step S2, Cr is prepared 3+ The process of doping non-spherical silicon oxide composite abrasive is:

[0016] S21: adding chromium nitrate to deionized water, stirring at room temperature to obtain a chromium nitrate solution, adding solid sodium hydroxide to deionized water, stirring at room temperature to obtain a sodium hydroxide solution;

[0017] S22: adding chromium nitrate solution and sodium hydroxide solution dropwise to the solution containing non-spherical silicon oxide abrasive particles, and stirring under reflux at 100° C. after the addition is complete. After the reaction is complete, a chromium nitrate solution and a sodium hydroxide solution are obtained. 3+ A solution doped with non-spherical silicon oxide composite abrasive particles.

[0018] Further, the Cr 3+ In the process of doping non-spherical silicon oxide composite abrasives, the chromium nitrate is chromium nitrate nine hydrate, the concentration of sodium hydroxide is 1.0wt.%, the mass ratio of the chromium nitrate solution to the solution containing non-spherical silicon oxide abrasives is 1:7, the sodium hydroxide solution adjusts the solution pH to 9, and the reaction time is 5h.

[0019] The present application also provides a Cr 3+The doped non-spherical silicon oxide composite abrasive is obtained by the preparation method as described above, wherein the Cr 3+ The doped non-spherical silicon oxide composite abrasive grains have a non-spherical structure.

[0020] The present application also provides a Cr 3+ The application of doped non-spherical silicon oxide composite abrasive particles is characterized in that it is used to prepare a polishing liquid for a single crystal silicon carbide sheet, specifically comprising: adding potassium permanganate and deionized water to a Cr-containing 3+ The solution doped with non-spherical silicon oxide composite abrasive particles is ultrasonically prepared into a polishing liquid, wherein the Cr 3+ The mass fraction of the doped non-spherical silicon oxide composite abrasive grains is 7.5wt.%, the mass fraction of the potassium permanganate is 1wt.%, and the pH value of the polishing liquid is 9.

[0021] The present invention has the following beneficial effects:

[0022] The present invention prepares Cr by oil bath method under mild conditions. 3+ The non-spherical silicon oxide composite abrasive is doped, and the hydroxyl groups generated by the hydrolysis of negatively charged aluminate anions in the aqueous solution undergo dehydration condensation with the hydroxyl groups on the surface of silicon oxide to form -Si-O-Al-O-Si-, so that the spherical silicon oxide particles are combined to form a non-spherical structure.

[0023] The Cr prepared by the present invention 3+ Compared with conventional commercially available silicon oxide abrasives, the doped non-spherical silicon oxide composite abrasives greatly improve the material removal rate of single crystal silicon carbide wafers after CMP.

[0024] The silicon oxide composite abrasive polishing liquid prepared by the present invention is applied to the CMP process of single crystal silicon carbide wafers. Compared with conventional commercially available silicon oxide abrasives, Cr 3+ The polishing rate of doped non-spherical silicon oxide composite abrasive can be increased by 222%. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a graph showing the effects of different abrasive polishing solutions on SiC wafer material removal rate. DETAILED DESCRIPTION

[0026] In order to make the objectives, technical solutions and advantages of the present invention more clear, the specific implementation modes of the present invention are further described in detail below with reference to the accompanying drawings.

[0027] This application provides Cr 3+ The method for preparing doped non-spherical silicon oxide composite abrasive particles comprises the following steps:

[0028] S1 prepares non-spherical silicon oxide abrasive particles; specifically comprising:

[0029] S11: Disperse silica sol in deionized water, mix well and place under reflux magnetic stirring and heating at 100°C, add sodium aluminate solution into the silica sol at one time, and obtain a solution after the reaction is completed; wherein, the concentration of the sodium aluminate solution is 0.3wt.%; the particle size of the silica sol is 100nm; the solid content of the silica sol is 40wt.%, and the mass ratio of the sodium aluminate solution, the silica sol and the deionized water is 8:15:33.

[0030] In this step, oil bath heating can be used; the heating time is 3 hours.

[0031] S12: placing the solution after the reaction for aging to obtain a solution containing non-spherical silicon oxide abrasive particles, wherein the aging temperature is 100° C. and the aging time is 2 hours.

[0032] S2 Preparation of Cr 3+ Doped non-spherical silicon oxide composite abrasive; specifically comprising:

[0033] S21: adding chromium nitrate to deionized water, stirring at room temperature to obtain a chromium nitrate solution, adding solid sodium hydroxide to deionized water, stirring at room temperature to obtain a sodium hydroxide solution; wherein the chromium nitrate is chromium nitrate nonahydrate, the concentration of sodium hydroxide is 1.0 wt.%, the mass ratio of the chromium nitrate solution to the solution containing non-spherical silicon oxide abrasives is 1:7, the sodium hydroxide solution is used to adjust the solution pH to 9, and the reaction time is 5 hours.

[0034] S22: adding chromium nitrate solution and sodium hydroxide solution dropwise to the solution containing non-spherical silicon oxide abrasive particles, and stirring under reflux at 100° C. after the addition is complete. After the reaction is complete, a chromium nitrate solution and a sodium hydroxide solution are obtained. 3+ A solution doped with non-spherical silicon oxide composite abrasive particles.

[0035] The present application also provides a Cr 3+ Doped non-spherical silicon oxide composite abrasive, and Cr 3+ The doped non-spherical silicon oxide composite abrasive has a non-spherical structure. Cr is prepared by oil bath method under mild conditions. 3+ Doped non-spherical silicon oxide composite abrasives, the negatively charged aluminate anions in the aqueous solution are hydrolyzed to produce hydroxyl groups that undergo dehydration condensation with the hydroxyl groups on the surface of silicon oxide to form -Si-O-Al-O-Si-, which combines the spherical silicon oxide particles to form a non-spherical structure. The non-spherical silicon oxide structure can increase the contact points between the abrasive and the SiC wafer, and improve the mechanical action during the CMP process. 3+ The addition of improves the oxidation effect of potassium permanganate, accelerates the formation of oxide layer on the surface of silicon carbide, and accelerates the chemical reaction in the CMP process. The chemical action and mechanical action work together to improve the material removal rate of SiC wafers.

[0036] The present application also provides a Cr 3+ The application of doped non-spherical silicon oxide composite abrasive particles is used to prepare a polishing liquid for single crystal silicon carbide wafers. The specific preparation method includes: adding potassium permanganate and deionized water to a Cr-containing 3+ The solution doped with non-spherical silicon oxide composite abrasive particles is ultrasonically prepared into a polishing liquid, wherein the Cr 3+ The mass fraction of the doped non-spherical silicon oxide composite abrasive grains is 7.5wt.%, the mass fraction of the potassium permanganate is 1wt.%, and the pH value of the polishing liquid is 9. The ultrasonic time is greater than or equal to 10 minutes.

[0037] Example 1

[0038] This embodiment provides a Cr 3+ The preparation method of doped non-spherical silicon oxide composite abrasive particles comprises the following steps:

[0039] S1 prepares non-spherical silicon oxide abrasive particles; specifically comprising:

[0040] S11: 93.75g of silica sol is diluted to 300g, and loaded into a three-necked flask. Under magnetic stirring and 100°C oil bath reflux heating, sodium aluminate solution is added into the three-necked flask at once, and reacted for 3h. The steps of preparing the sodium aluminate solution are as follows: 0.15g of sodium aluminate is dissolved in 50g of deionized water, and ultrasonically dispersed for later use.

[0041] S12: After the reaction is completed, the stirring device is turned off and the mixture is aged at 100° C. for 2 h.

[0042] S2 Preparation of Cr 3+ Doped non-spherical silicon oxide composite abrasive; specifically comprising:

[0043] 0.63 g Cr(NO 3 ) 3 9H 2 O was dissolved in 50 mL of pure water and added dropwise to a Cr 3+ After the addition of the non-spherical silicon oxide composite abrasive particles into a three-necked flask, the reaction was continued for 5 hours.

[0044] Comparative Example 1

[0045] Commercially available silica sol with an average particle size of 100 nm was directly used as a spherical silicon oxide comparison sample.

[0046] Comparative Example 2

[0047] A method for preparing a non-spherical silicon oxide composite abrasive grain is provided, and the method steps are as follows:

[0048] S1 prepares non-spherical silicon oxide abrasive particles; specifically comprising:

[0049] S11: 93.75g of silica sol is diluted to 300g, and loaded into a three-necked flask. Under magnetic stirring and 100°C oil bath reflux heating, sodium aluminate solution is added into the three-necked flask at once, and reacted for 3h. The steps of preparing the sodium aluminate solution are as follows: 0.15g of sodium aluminate is dissolved in 50g of deionized water, and ultrasonically dispersed for later use.

[0050] S12: After the reaction is completed, the stirring device is turned off and the mixture is aged at 100° C. for 2 h.

[0051] The Cr prepared in Example 1 is described below. 3+ The process of forming a single crystal silicon carbide wafer polishing liquid by doping non-spherical silicon oxide composite abrasive grains, spherical silicon oxide abrasive grains in Comparative Example 1 and non-spherical silicon oxide abrasive grains prepared in Comparative Example 2 comprises the following specific steps:

[0052] 5 g of potassium permanganate and an appropriate amount of deionized water were respectively added to the solutions containing different types of abrasives prepared in Example 1, Comparative Example 1 and Comparative Example 2, and ultrasonically prepared into 500 g of polishing liquid, in which the mass fraction of the silicon oxide composite abrasive was 7.5 wt.%, the mass fraction of the potassium permanganate was 1 wt.%, the pH of the polishing liquid was adjusted to 9 with sodium hydroxide, and the ultrasonic time was 10 min.

[0053] The following polishing tests were conducted on the above-mentioned different silicon oxide abrasives and the corresponding polishing liquids:

[0054] 2. Comparative experiment on polishing effect of polishing liquid on silicon carbide

[0055] The experimental steps are:

[0056] The above three polishing solutions were used to carry out polishing tests on single crystal silicon carbide under certain polishing conditions.

[0057] The polishing liquid configuration for the polishing test is as follows:

[0058] Total mass of polishing liquid: 500g;

[0059] Abrasive: 7.5wt.%;

[0060] Potassium permanganate: 1wt.%;

[0061] pH: 9;

[0062] The polishing conditions of the polishing test are as follows:

[0063] Polishing machine: UNIPOL-1502 automatic pressure grinding and polishing machine;

[0064] Workpiece: Si surface of single crystal silicon carbide wafer with a diameter of 50 mm;

[0065] Polishing pad: polyurethane polishing pad;

[0066] Polishing pressure: 6kg;

[0067] Polishing disc speed: 70rpm;

[0068] Polishing time: 1h;

[0069] After polishing, the single crystal silicon carbide wafer was washed and dried in the order of acetone, cleaning solution, deionized water, and anhydrous ethanol, and the mass of the single crystal silicon carbide wafer before and after polishing was weighed with a precision analytical balance to calculate the material removal rate (MRR).

[0070] The polishing effects of the polishing liquids of Example 1, Comparative Examples 1 and 2 on silicon carbide are shown in Table 1.

[0071] As shown in Table 1 and Figure 1 As shown, under the same polishing conditions, it can be seen from the comparison between Comparative Example 1 and Comparative Example 2 that compared with the spherical silicon oxide polishing liquid, the material removal rate of the non-spherical silicon oxide polishing liquid formed after induction by sodium metaaluminate is improved. 3+ Compared with non-spherical silicon oxide abrasive grains, the material removal rate of the doped non-spherical silicon oxide composite abrasive grains after polishing is increased by 81%, and compared with spherical silicon oxide abrasive grains, the material removal rate of the doped non-spherical silicon oxide composite abrasive grains after polishing is increased by 222%.

[0072] Table 1 Polishing effect of three polishing fluids on silicon carbide

[0073]

[0074] In summary, compared with conventional commercially available silica sol (silicon oxide) abrasive grains, the Cr 3+ The doped non-spherical silicon oxide composite abrasive increases the contact points with the SiC wafer and improves the mechanical action during the CMP process. 3+ The addition of potassium permanganate improves the oxidation effect of potassium permanganate, accelerates the formation of the oxide layer on the surface of silicon carbide, and accelerates the chemical reaction during the CMP process. The chemical action and mechanical action work together to improve the material removal rate of SiC wafers to a certain extent. 3+ The material removal rate of doped non-spherical silicon oxide composite abrasive is increased by 222% compared with spherical silicon oxide abrasive.

[0075] The above description is only a preferred embodiment of the present invention, and the embodiment is not intended to limit the patent protection scope of the present invention. Therefore, all equivalent structural changes made using the description and drawings of the present invention should be included in the protection scope of the claims attached to the present invention.

Claims

1. A Cr 3+ The method for preparing doped non-spherical silicon oxide composite abrasive particles is characterized in that: The following steps are involved: S1 preparation of non-spherical silicon oxide abrasive particles; S2 Preparation of Cr 3+ Doped non-spherical silicon oxide composite abrasive.

2. A Cr as claimed in claim 1 3+ The method for preparing doped non-spherical silicon oxide composite abrasive particles is characterized in that: The method for preparing the non-spherical silicon oxide abrasive grains in step S1 is: S11: dispersing silica sol in deionized water, mixing well, placing under reflux and magnetic stirring at 100° C., adding sodium aluminate solution into the silica sol at one time, and obtaining a solution after the reaction is completed; S12: The solution after the reaction is left to age to obtain a solution containing non-spherical silicon oxide abrasive grains.

3. A Cr as claimed in claim 2 3+ The method for preparing doped non-spherical silicon oxide composite abrasive particles is characterized in that: In step S11, the concentration of the sodium aluminate solution is 0.3 wt. %; the particle size of the silica sol is 100 nm; the solid content of the silica sol is 40 wt. %, and the mass ratio of the sodium aluminate solution, the silica sol and the deionized water is 8:15:

33.

4. A Cr as claimed in claim 2 3+ The method for preparing doped non-spherical silicon oxide composite abrasive particles is characterized in that: In step S11, the heating method is oil bath heating; the heating time is 3 hours.

5. A Cr as claimed in claim 2 3+ The method for preparing doped non-spherical silicon oxide composite abrasive particles is characterized in that: During the aging process in step S12, the aging temperature is 100° C. and the aging time is 2 hours.

6. A Cr as claimed in claim 1 3+ The method for preparing doped non-spherical silicon oxide composite abrasive particles is characterized in that: Preparation of Cr in step S2 3+ The process of doping non-spherical silicon oxide composite abrasive is: S21: adding chromium nitrate to deionized water, stirring at room temperature to obtain a chromium nitrate solution, adding solid sodium hydroxide to deionized water, stirring at room temperature to obtain a sodium hydroxide solution; S22: adding chromium nitrate solution and sodium hydroxide solution dropwise to the solution containing non-spherical silicon oxide abrasive particles, and stirring under reflux at 100° C. after the addition is complete. After the reaction is complete, a chromium nitrate solution and a sodium hydroxide solution are obtained. 3+ A solution doped with non-spherical silicon oxide composite abrasive particles.

7. A Cr as claimed in claim 6 3+ The method for preparing doped non-spherical silicon oxide composite abrasive particles is characterized in that: Preparation of the Cr 3+ In the process of doping non-spherical silicon oxide composite abrasives, the chromium nitrate is chromium nitrate nine hydrate, the concentration of sodium hydroxide is 1.0wt.%, the mass ratio of the chromium nitrate solution to the solution containing non-spherical silicon oxide abrasives is 1:7, the sodium hydroxide solution adjusts the solution pH to 9, and the reaction time is 5h.

8. A Cr 3+ Doped non-spherical silicon oxide composite abrasive grains, characterized in that: The Cr 3+ The doped non-spherical silicon oxide composite abrasive grains have a non-spherical structure.

9. A Cr as claimed in claim 8 3+ The application of doped non-spherical silicon oxide composite abrasive particles is characterized in that: The polishing liquid for preparing a single crystal silicon carbide wafer specifically comprises: adding potassium permanganate and deionized water into a Cr 3+ The solution doped with non-spherical silicon oxide composite abrasive particles is ultrasonically prepared into a polishing liquid, wherein the Cr 3+ The mass fraction of the doped non-spherical silicon oxide composite abrasive grains is 7.5wt.%, the mass fraction of the potassium permanganate is 1wt.%, and the pH value of the polishing liquid is 9.