Method for enhancing high-temperature strong plasticity of titanium-based composite material by using nano TiB whiskers

Through low-energy ball milling and hot pressing sintering technology, the problems of complex process and high manufacturing cost of nanoscale TiB whisker-enhanced titanium-based composite materials are solved, and the high temperature and strong plasticity of titanium-based composite materials are improved and large-scale industrial production is achieved, and the compactness is obtained. NanoTiB whisker-reinforced titanium-based composite material.

CN119040694APending Publication Date: 2024-11-29HARBIN INST OF TECH
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411158483.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing nanoscale TiB whisker-reinforced titanium-based composite materials have complex processes and high manufacturing costs. They are not suitable for large-scale industrial production, and it is difficult to obtain large-size titanium-based composite components.

Method used

Nano-scale TiB2 powder is uniformly embedded on the surface of titanium alloy powder through low-energy ball milling. Combined with hot pressing and sintering technology, nanoscale TiB whiskers are generated, avoiding the breaking of TiB2 nanoparticles during thermomechanical deformation and forming dense nanoTiB whiskers Reinforced titanium-based composite material.

Benefits of technology

The high-temperature strong plasticity of titanium-based composite materials has been improved, which reduces manufacturing costs, and is suitable for large-scale industrial production, and has obtained nanoscale TiB whisker-reinforced titanium-based composite materials with excellent high-temperature performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040694A_ABST
    Figure CN119040694A_ABST
Patent Text Reader

Abstract

The invention discloses a method for enhancing high-temperature and high-plasticity of a titanium-based composite material by using nano TiB whiskers, and relates to a method for enhancing high-temperature and high-plasticity of a titanium-based composite material by using TiB whiskers. The preparation method aims at solving the technical problems that an existing preparation method of the nanoscale TiB whisker reinforced titanium-based composite material is complex in technological process, high in manufacturing cost and not suitable for large-scale industrial production. According to the preparation method, the near-alpha type high-temperature titanium alloy is selected as a matrix of the metal-based composite material, the TiB2 nanoparticles are selected as a reinforcing phase, and the TiB2 nanoparticles and the Ti element in the titanium alloy are subjected to an in-situ synthesis reaction in the sintering process to generate the nano-scale TiB whiskers; the nanoscale TiB whiskers can effectively improve the load transfer strengthening effect of the titanium-based composite material and improve the high-temperature performance of the titanium-based composite material. Compared with a traditional method for refining the size of the reinforced phase through complex hot working deformation, the method has the advantages of being simple in process, short in technological process and low in manufacturing cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for reinforcing high-temperature strength and plasticity of titanium-based composite materials by using TiB whiskers. Background Art

[0002] Titanium alloys have the characteristics of high specific strength and excellent high temperature resistance, and are widely used in aviation, aerospace, military weapons and other fields. With the rapid development of industry, higher requirements have been put forward for the performance of titanium alloys. Single-component titanium alloys have been difficult to meet application requirements. At present, many researchers have introduced reinforcing phases to realize the composite of titanium alloys to improve their high temperature performance, and the application of titanium-based composite materials has also received more and more attention. TiB2, as a reinforcing phase with excellent strength, stiffness and hardness, and has a similar thermal expansion coefficient to the alloy matrix, can increase the use temperature of titanium alloys by 100-200°C by in-situ autogenous reaction with Ti elements during high-temperature sintering to generate TiB whiskers. The size, morphology, preparation process parameters and mixed powder state of TiB whiskers in titanium-based composite materials will have an important impact on their performance. Nanoscale reinforcement phase has a very good strengthening effect. However, the current method of obtaining titanium-based composite materials reinforced with nanoscale TiB whiskers mostly uses thermomechanical deformation after sintering, such as hot forging, hot extrusion or hot rolling, to break TiB whiskers into fine micron-level or even nanoscale reinforcement phases. However, this preparation method has the disadvantages of complex process flow and high manufacturing cost. In addition, the final billet is limited by the size of forging and extrusion, making it difficult to obtain large-sized titanium-based composite parts, which is not suitable for large-scale industrial production. Therefore, seeking a titanium-based composite material with nano-TiB whiskers and making it have excellent high-temperature strength and plasticity is a problem that needs to be solved urgently. Summary of the invention

[0003] The present invention aims to solve the technical problems that the current preparation method of nano-scale TiB whisker reinforced titanium-based composite materials has complex process flow, high manufacturing cost and is not suitable for large-scale industrial production, and provides a method for using nano-TiB whiskers to enhance the high-temperature strength and plasticity of titanium-based composite materials.

[0004] The method for enhancing high temperature strength and plasticity of titanium-based composite materials by using nano-TiB whiskers of the present invention is carried out according to the following steps:

[0005] 1. Low-energy ball milling is performed on titanium alloy powder and nano-scale TiB2 powder to mix the titanium alloy powder and evenly embed the TiB2 powder on the surface of the titanium alloy powder to obtain a uniformly mixed composite powder; the mass fraction of the nano-scale TiB2 powder in the uniformly mixed composite powder is 1% to 2.5%;

[0006] 2. Put the mixed composite powder into a graphite mold, and perform hot pressing sintering at 1200℃~1300℃ (higher than the β phase transition temperature of titanium alloy), keep the temperature for 0.75h~2h, apply a pressure of 20MPa~40MPa, and cool naturally to room temperature with the furnace after hot pressing sintering;

[0007] 3. Remove the graphite mold to obtain a dense titanium-based composite material reinforced by nano-TiB whiskers.

[0008] The present invention selects near-α-type titanium alloy and TiB2 nanoparticles as raw materials, and uniformly embeds nano-TiB2 on the surface of titanium alloy powder by adjusting the particle size of TiB2 reinforcing phase, reinforcing phase content and ball milling parameters, while preventing the spherical powder of titanium alloy from extrusion deformation, effectively avoiding all TiB2 nanoparticles directly contacting with Ti matrix to generate coarse micron-level whiskers during hot pressing sintering; and then selecting appropriate hot pressing sintering parameters, such as sintering temperature, time and sintering pressure, during the hot pressing sintering process, as the sintering temperature increases, the diffusion distance and speed of B element along the

[010] direction increase in a leap-like manner, so that the growth speed of TiB whiskers along the

[010] direction increases. When the TiB whiskers grow to a certain extent along the

[010] direction, the migration speed along the

[010] direction slows down due to the limitation of the diffusion distance. At this time, the migration path of the B element changes, and it grows along the

[010] direction of the whiskers that have not yet grown. While these whiskers grow, the growth of the surrounding TiB whiskers that have grown in the

[001] direction is inhibited by the B element content, reducing the width of the whiskers and forming nano-scale fine needle-shaped and granular whiskers. TiB2 nanoparticles promote the crystallization of α grains in the TiB whisker-rich area, produce a large number of equiaxed α grains, and intensify the equiaxed β / α lamellar structure in the TiB whisker-depleted area, forming a titanium-based composite material with nano-TiB whiskers and a bimodal structure. High-temperature tensile tests were carried out at 600℃, 650℃ and 700℃, and the tensile strength reached 589MPa, 487MPa and 392MPa respectively, and the elongation was 16.2%, 16.4% and 25% respectively. Compared with the titanium-based composite material reinforced with large-sized TiB2 (3-5μm) in-situ self-generated micron-sized TiB whiskers, the high-temperature strength and plasticity have been greatly improved.

[0009] The present invention has the following advantages:

[0010] (1) The present invention uses the method of low-energy ball milling + hot pressing sintering to utilize the in-situ autogenous reaction of TiB to generate nano-scale TiB whiskers at the original β grain boundary. The aspect ratio of the nano-scale TiB whiskers is increased, so that the degree of equiaxed α grains inside the titanium-based composite material is increased, which can effectively improve the high-temperature performance of the titanium-based composite material. The load transfer strengthening effect of the TiB whiskers is enhanced at high temperatures;

[0011] (2) The nanoscale TiB-reinforced titanium-based composite material obtained by the present invention: In the nano-TiB whisker-depleted area, α / β layers are regularly distributed. Compared with the titanium-based composite material reinforced with large-sized TiB2 (3-5μm) in-situ self-generated micron-sized TiB whiskers, the equiaxed degree of the structure in the matrix alloy is increased, and in the nano-TiB whisker-enriched area, there are a large number of equiaxed α grain structures and continuously networked nano-TiB whiskers, obtaining a bimodal grain structure characteristic with equiaxed grains wrapped in lamellae; the increase of equiaxed α grains can generate more dislocations during deformation, further improving the high-temperature strength and plasticity of the titanium-based composite material;

[0012] (3) The present invention can be prepared by only mixing the raw material powders in appropriate proportions by low-energy ball milling and hot pressing, thus avoiding subsequent thermal deformation treatment, reducing costs, and ensuring excellent high-temperature performance;

[0013] (4) The present invention breaks through the limitation of the traditional complex thermal deformation process to obtain nano whisker reinforced titanium-based composite materials, and can effectively reduce the manufacturing cost of nano whisker reinforced titanium-based composite materials. This method can not only prepare large-sized titanium-based composite material blanks, but also has a simple process flow and can realize large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 The microstructure of the matrix alloy of the TiB2 reinforced titanium matrix composite material prepared for comparison test under optical microscope;

[0015] Figure 2 The microstructure of the titanium matrix composite material reinforced by nano-TiB whiskers prepared in Experiment 1;

[0016] Figure 3 SEM image of TiB2 reinforced titanium matrix composite prepared for comparative test;

[0017] Figure 4 This is the SEM image of the titanium-based composite material reinforced with nano-TiB whiskers prepared in Experiment 1;

[0018] Figure 5 is the tensile stress-strain curve of the material at 600°C;

[0019] Figure 6 is the tensile stress-strain curve of the material at 650°C;

[0020] Figure 7 It is the tensile stress-strain curve of the material at 700℃. DETAILED DESCRIPTION

[0021] Specific implementation method 1: This implementation method is a method for enhancing the high temperature strength and plasticity of titanium-based composite materials using nano-TiB whiskers, which is specifically carried out in the following steps:

[0022] 1. Low-energy ball milling is performed on titanium alloy powder and nano-scale TiB2 powder to mix the titanium alloy powder and evenly embed the TiB2 powder on the surface of the titanium alloy powder to obtain a uniformly mixed composite powder; the mass fraction of the nano-scale TiB2 powder in the uniformly mixed composite powder is 1% to 2.5%;

[0023] 2. Put the evenly mixed composite powder into a graphite mold, perform hot pressing sintering at 1200℃~1300℃, keep the temperature for 0.75h~2h, apply a pressure of 20MPa~40MPa, and naturally cool to room temperature with the furnace after hot pressing sintering;

[0024] 3. Remove the graphite mold to obtain a dense titanium-based composite material reinforced by nano-TiB whiskers.

[0025] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that the titanium alloy powder described in step 1 is spherical powder with a particle size of 75 μm to 150 μm and a purity of 99.9%. Other aspects are the same as specific implementation method 1.

[0026] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the particle size of the nano-scale TiB2 powder described in step 1 is 100nm-200nm, and the purity is greater than 99%. Other aspects are the same as specific implementation method 1 or 2.

[0027] Specific embodiment 4: This embodiment is different from specific embodiments 1 to 3 in that the chemical composition of the titanium alloy powder described in step 1 is: Ti-(3.3-8)Al-(0-2.5)Mo-(0-3.5)V-(1-4.4)Zr, wherein Al is an α-stabilizing element, and V and Mo are both β-phase stabilizing elements. The rest is the same as specific embodiments 1 to 3.

[0028] Specific embodiment 5: This embodiment differs from specific embodiment 4 in that the rotation speed of the low-energy ball mill described in step 1 is 180 rpm to 230 rpm, the mass ratio of the ball to the material is (3 to 5): 1, and the ball milling time is 4 h to 6 h. Other aspects are the same as specific embodiment 4.

[0029] Specific implementation example 6: This implementation example is different from specific implementation example 5 in that the inner diameter of the graphite mold described in step 2 is 40 mm to 120 mm. The rest is the same as specific implementation example 5.

[0030] Specific embodiment 7: This embodiment is different from specific embodiment 6 in that: before putting the mixed composite powder into the graphite mold in step 2, a layer of boron nitride slurry needs to be evenly applied on the inner wall and bottom surface of the graphite mold, and then air-dried to reduce the friction between the blank and the mold during hot pressing and sintering. The rest is the same as specific embodiment 6.

[0031] Specific embodiment eight: This embodiment differs from specific embodiment seven in that the boron nitride slurry described in step two is prepared by mixing boron nitride powder and alcohol in a volume ratio of 1:(2-3). The rest is the same as specific embodiment seven.

[0032] Specific embodiment 9: This embodiment is different from specific embodiment 8 in that: step 2 is hot-pressed and sintered at 1200° C. The rest is the same as specific embodiment 8.

[0033] Specific embodiment 10: This embodiment differs from specific embodiment 9 in that: in step 2, the temperature is kept at 1200° C. for 1 hour, and the pressure during the keeping is 35 MPa. The rest is the same as specific embodiment 9.

[0034] The present invention is verified by the following tests:

[0035] Experiment 1: This experiment is a method for enhancing the high temperature strength and plasticity of titanium-based composite materials using nano-TiB whiskers, which is specifically carried out in the following steps:

[0036] 1. The titanium alloy powder and the nano-scale TiB2 powder are mixed by low-energy ball milling to evenly embed the TiB2 powder on the surface of the titanium alloy powder to obtain a uniformly mixed composite powder; the mass fraction of the nano-scale TiB2 powder in the uniformly mixed composite powder is 2%;

[0037] The titanium alloy powder described in step 1 is TA15 (Ti-6.5Al-2Zr-Mo-V) which is a spherical powder with a particle size of 75 μm to 150 μm and a purity of 99.9%;

[0038] The nano-scale TiB2 powder described in step 1 has a particle size of 100 nm and a purity greater than 99%;

[0039] The rotation speed of the low-energy ball mill described in step 1 is 220 rpm, the mass ratio of balls to materials is 4:1, the ball milling time is 5 h, and the ball mill is paused for 15 minutes after each ball milling for 1 h to allow the ball mill to fully cool down to prevent the temperature from being too high, and the forward and reverse rotations are alternately operated to make the ball milling more uniform; the balls used for ball milling are made of stainless steel;

[0040] 2. First, a gasket is arranged on the bottom surface of the inner cavity of a graphite mold (with an inner diameter of 100 mm), and a layer of boron nitride slurry is evenly brushed on the inner wall and the gasket of the graphite mold, and then air-dried to reduce the friction between the blank and the mold during hot pressing and sintering. The boron nitride slurry is mixed with boron nitride powder and alcohol in a volume ratio of 1: (2-3); then the composite powder mixed evenly in step 1 is placed in the graphite mold, and the heating time from room temperature to 800°C is 80 minutes, the heating time from 800°C to 1000°C is 45 minutes, and the heating time from 1000°C to 1200°C is 45 minutes. The temperature is kept at 1200°C for 1 hour, and the pressure during the temperature is 35MPa. After sintering, the mixture is cooled to room temperature with the furnace;

[0041] 3. Remove the graphite mold to obtain a dense titanium-based composite material reinforced by nano-TiB whiskers.

[0042] It has been verified that the nano-TiB whisker reinforced titanium-based composite material obtained in Experiment 1 has tensile strengths of 589MPa, 487MPa and 392MPa at 600℃, 650℃ and 700℃, respectively, and elongations of 16.2%, 16.4% and 25%, respectively.

[0043] Comparative test: This test is different from the first test in that the particle size of the TiB2 powder in step 1 is 5 μm. The rest is the same as the first test.

[0044] Figure 1 The microstructure of the matrix alloy of the TiB2 reinforced titanium matrix composite material prepared by the comparison test under an optical microscope is shown in Figure 2. Figure 2 In order to test the microstructure of the prepared nano-TiB whisker reinforced titanium matrix composite material, Figure 2 There are a large number of equiaxed α grains in the TiB whisker-rich region, with a number greater than Figure 1 There are a large number of equiaxed α grains in the TiB whisker-rich area. Figure 2 The degree of equiaxed β / α lamellae is also greater than Figure 1 .

[0045] Figure 3 SEM image of TiB2 reinforced titanium matrix composite prepared for comparison test. Figure 4 This is the SEM image of the titanium matrix composite material reinforced with nano-TiB whiskers prepared in Experiment 1. Figure 4 In the TiB whisker-rich area, the shapes of TiB are mostly fine needles and particles, and the scale is nanometer-scale; Figure 3 In the TiB whisker-rich area, the shape of TiB is mostly long rods with a size of micrometers.

[0046] Figure 5The blue curve is the titanium-based composite material reinforced with nano-TiB whiskers prepared in the first experiment, and the black curve is the titanium-based composite material reinforced with TiB2 prepared in the comparative experiment. At 600°C, when the particle size of the added TiB2 is 100nm, the tensile strength of the titanium-based composite material is 589MPa and the elongation is 16.2%; when the particle size of the added TiB2 is 5μm, the tensile strength of the titanium-based composite material is 524MPa and the elongation is 10.2%. As the particle size of TiB2 decreases, the mechanical properties of the titanium-based composite material at 600°C improve.

[0047] Figure 6 The tensile stress-strain curve of the material at 650℃, the blue curve is the nano-TiB whisker reinforced titanium-based composite material prepared in test 1, and the black curve is the TiB2 reinforced titanium-based composite material prepared in the comparative test. At 650℃, when the added TiB2 particle size is 100nm, the tensile strength of the titanium-based composite material is 487MPa and the elongation is 16.4%; when the added TiB2 particle size is 5μm, the tensile strength of the titanium-based composite material is 429MPa and the elongation is 12.2%. As the TiB2 particle size decreases, the mechanical properties of the titanium-based composite material at 650℃ improve.

[0048] Figure 7 The blue curve is the titanium-based composite material reinforced by nano-TiB whiskers prepared in the first experiment, and the black curve is the titanium-based composite material reinforced by TiB2 prepared in the comparative experiment. At 700°C, when the particle size of the added TiB2 is 100nm, the tensile strength of the titanium-based composite material is 392MPa and the elongation is 25%; when the particle size of the added TiB2 is 5μm, the tensile strength of the titanium-based composite material is 336MPa and the elongation is 16.6%. As the particle size of TiB2 decreases, the mechanical properties of the titanium-based composite material at 700°C improve.

Claims

1. A method for enhancing the high temperature strength and plasticity of titanium-based composite materials using nano-TiB whiskers, characterized in that The method of using nano-TiB whiskers to enhance the high temperature strength and plasticity of titanium-based composite materials is carried out in the following steps:

1. Low-energy ball milling is performed on titanium alloy powder and nano-scale TiB2 powder to mix the titanium alloy powder and evenly embed the TiB2 powder on the surface of the titanium alloy powder to obtain a uniformly mixed composite powder; the mass fraction of the nano-scale TiB2 powder in the uniformly mixed composite powder is 1% to 2.5%; 2. Put the evenly mixed composite powder into a graphite mold, perform hot pressing sintering at 1200℃~1300℃, keep the temperature for 0.75h~2h, apply a pressure of 20MPa~40MPa, and naturally cool to room temperature with the furnace after hot pressing sintering; 3. Remove the graphite mold to obtain a dense titanium-based composite material reinforced by nano-TiB whiskers.

2. The method of claim 1, wherein the method comprises: The titanium alloy powder described in step 1 is a spherical powder with a particle size of 75 μm to 150 μm and a purity of 99.9%.

3. The method of claim 1 for enhancing high temperature strength and plasticity of titanium-based composite materials by using nano-TiB whiskers, characterized in that The particle size of the nano-scale TiB2 powder described in step 1 is 100nm-200nm, and the purity is greater than 99%.

4. The method of claim 2 for enhancing high temperature strength and plasticity of titanium-based composite materials by using nano-TiB whiskers, characterized in that The chemical composition of the titanium alloy powder described in step 1 is: Ti-(3.3-8)Al-(0-2.5)Mo-(0-3.5)V-(1-4.4)Zr, wherein Al is an α-stabilizing element, and V and Mo are both β-phase stabilizing elements.

5. The method of claim 1 for enhancing high temperature strength and plasticity of titanium-based composite materials by using nano-TiB whiskers, characterized in that The rotation speed of the low-energy ball mill described in step 1 is 180 rpm to 230 rpm, the mass ratio of balls to materials is (3 to 5):1, and the ball milling time is 4 h to 6 h.

6. The method of claim 1 for enhancing high temperature strength and plasticity of titanium-based composite materials using nano-TiB whiskers, characterized in that The inner diameter of the graphite mold described in step 2 is 40 mm to 120 mm.

7. The method of claim 1 for enhancing high temperature strength and plasticity of titanium-based composite materials by using nano-TiB whiskers, characterized in that Before placing the evenly mixed composite powder into the graphite mold in step 2, a layer of boron nitride slurry needs to be evenly applied on the inner wall and bottom surface of the graphite mold, and then air-dried to reduce the friction between the blank and the mold during hot pressing and sintering.

8. The method of claim 7, wherein the method comprises: The boron nitride slurry described in step 2 is prepared by mixing boron nitride powder and alcohol in a volume ratio of 1:(2-3).

9. The method of claim 1 for enhancing high temperature strength and plasticity of titanium-based composite materials using nano-TiB whiskers, characterized in that Step 2: hot pressing and sintering at 1200°C.

10. The method of using nano-TiB whiskers to enhance the high temperature strength and plasticity of titanium-based composite materials according to claim 9, characterized in that In step 2, the temperature is kept at 1200° C. for 1 hour, and the pressure during the heat preservation is 35 MPa.

Citation Information

Patent Citations

  • Process for preparing TiBw / Ti alloy-based composite material

    CN101333607A

  • Nano TiB2 particle reinforced metal-base composite material and preparation method thereof

    CN102925737A

  • Preparation method of TiBw / Ti-6Al-4V composite bar adopting quasi-continuous reticular structure

    CN104263984A

  • Titanium boride nanowhisker reinforced titanium-based composite material and preparation method thereof

    CN108342667A

  • Preparation method for high-plasticity titanium-based composite material

    CN109338159A