Environment-friendly water-based resin slurry, preparation method thereof and modified polyolefin diaphragm

By coating the polyolefin separator with environmentally friendly water-based resin slurry on the polyolefin separator, the problems of poor thermal stability and flammability of the polyolefin separator are solved, and the high electrochemical performance and safety performance of the modified separator are achieved.

CN119391260APending Publication Date: 2025-02-07JIANGHAN UNIVERSITY

Patent Information

Application Number
CN202411293333.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2025-02-07

AI Technical Summary

Technical Problem

Polyolefin lithium-ion battery separators have problems of poor thermal stability and flammability, resulting in thermal shrinkage and safety accidents that may occur under high temperature conditions.

Method used

Using an environmentally friendly water-based resin slurry, a modified polyolefin separator is formed by mixing benzoxazine resin particles and zirconia nanoparticles with water to form a modified polyolefin separator, which improves the high-temperature and electrochemical performance of the separator.

Benefits of technology

The modified polyolefin separator has high electrolyte wetting, thermal stability, high ion conductivity and good lithium ion migration number, which improves the safety and electrochemical performance of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119391260A_ABST
    Figure CN119391260A_ABST
Patent Text Reader

Abstract

The invention discloses environment-friendly water-based resin slurry, a preparation method thereof and a modified polyolefin diaphragm. The environment-friendly water-based resin slurry is prepared from the following raw materials in percentage by weight: 5 to 98.88 percent of water, 0.01 to 30 percent of dispersing wetting agent, 0.1 to 5 percent of binder, 1 to 50 percent of benzoxazine resin particles and 0 to 15 percent of zirconium oxide nanoparticles. The environment-friendly water-based resin slurry disclosed by the invention takes water as a solvent, is green and environment-friendly and is low in cost; by adopting the benzoxazine resin and the zirconium oxide nanoparticles, the high-temperature performance of the diaphragm can be improved; the modified polyolefin diaphragm electrolyte obtained by coating the environment-friendly water-based resin slurry is high in wettability, good in thermal stability, high in ionic conductivity and good in lithium ion transference number, and the safety performance and the electrochemical performance of a battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of battery separators, and in particular to an environmentally friendly water-based resin slurry, a preparation method thereof and a modified polyolefin separator. Background Art

[0002] With the rapid development of electric vehicles, lithium-ion batteries have received more and more attention from scientists. Lithium-ion batteries are composed of a separator soaked in electrolyte between the positive and negative electrodes. The separator is also called the "third electrode" of lithium-ion batteries and is an important component of lithium-ion batteries. Its most important function is to isolate the positive and negative electrodes, prevent internal short circuits, and provide ion channels for the battery during charging and discharging. Since the characteristics and quality of the separator material play a decisive role in the battery rate performance, cycle life and basic electrical properties, the performance of the separator restricts the overall performance of the lithium-ion battery. On the other hand, organic separators often experience thermal shrinkage. Unstoppable thermal shrinkage will cause the two poles of the lithium-ion battery to short-circuit, causing safety accidents. Therefore, the quality of the separator also plays a vital role in the safety performance of lithium-ion batteries. Among them, polyolefin-based separators have a low melting temperature and poor thermal dimensional stability at high temperatures. Under high-current and high-rate charging and discharging conditions, the internal temperature rises sharply, which will cause the separator to undergo severe thermal shrinkage deformation, resulting in internal short circuits in the battery and serious safety accidents.

[0003] Therefore, it is urgent to modify the polyolefin lithium-ion battery separator to solve the above technical problems. Summary of the invention

[0004] The purpose of the present invention is to overcome the above technical deficiencies, to provide an environmentally friendly water-based resin slurry, a preparation method thereof and a modified polyolefin diaphragm, and to solve the technical problems of poor thermal stability and flammability of polyolefin diaphragms in the prior art.

[0005] In a first aspect, the present invention provides an environmentally friendly water-based resin slurry, wherein the raw materials thereof include, by weight percentage: 5-98.88% water, 0.01-30% dispersing wetting agent, 0.1-5% binder, 1-50% benzoxazine resin particles, and 0-15% zirconium oxide nanoparticles.

[0006] In a second aspect, the present invention provides a method for preparing an environmentally friendly water-based resin slurry, comprising the following steps: The benzoxazine resin particles, zirconium oxide nanoparticles, a dispersing wetting agent, a binder and water are uniformly mixed to obtain an environmentally friendly water-based resin slurry.

[0007] In a third aspect, the present invention provides a modified polyolefin membrane, which is obtained by coating the environmentally friendly water-based resin slurry provided by the first aspect of the present invention on the surface of a polyolefin membrane and drying it.

[0008] Compared with the prior art, the beneficial effects of the present invention include: The environmentally friendly water-based resin slurry of the present invention uses water as a solvent, is green, environmentally friendly and low in cost; by adopting benzoxazine resin and zirconium oxide nanoparticles, the high-temperature performance of the diaphragm can be improved; the modified polyolefin diaphragm electrolyte obtained by coating the environmentally friendly water-based resin slurry has high wettability, good thermal stability, high ion conductivity and good lithium ion migration number, which is beneficial to improving the safety performance and electrochemical performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] Figure 1 This is a SEM image of the PE diaphragm in Comparative Example 3 of the present invention; Figure 2 This is a SEM image of the front side of the modified polyolefin separator in Example 3 of the present invention; Figure 3 This is a SEM image of the reverse side of the modified polyolefin separator in Example 3 of the present invention; Figure 4 The thermal stability diagrams are of the PE diaphragm in Comparative Example 3 of the present invention before and after heating at 180°C for 30 minutes, the PE diaphragm in Example 2 before and after heating at 180°C for 30 minutes, and the modified polyolefin diaphragm obtained in Example 4 after heating at 180°C for 30 minutes; Figure 5 The voltage-specific capacity curve of the button cell made of the modified polyolefin separator in Example 3 of the present invention. DETAILED DESCRIPTION

[0010] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0011] In a first aspect, the present invention provides an environmentally friendly water-based resin slurry, wherein the raw materials thereof include, by weight percentage: 5-98.88% water, 0.01-30% dispersing wetting agent, 0.1-5% binder, 1-50% benzoxazine resin particles, and 0-15% zirconium oxide nanoparticles.

[0012] The present invention uses water as a dispersion system, which can not only significantly reduce costs, but also eliminate the environmental pollution caused by the use of organic solvents. The dispersed wetting agent not only ensures the dispersion stability of the benzoxazine resin particles in the slurry, but also enables the slurry to form a uniform coating on the polyolefin diaphragm; the flame retardant properties of the benzoxazine resin particles themselves can provide flame retardancy for the polyolefin diaphragm, and zirconium oxide can improve the thermal stability of the diaphragm; with an appropriate amount of zirconium oxide added, the benzoxazine resin stacking structure can be regularized, the lithium ion migration number can be increased, the impedance can be reduced, and the ion conductivity can be improved.

[0013] In this embodiment, the benzoxazine resin particles are at least one of bisphenol A type benzoxazine resin particles, bisphenol F type benzoxazine resin particles, phenol type benzoxazine resin particles, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide type benzoxazine resin particles, phenolphthalein type benzoxazine resin particles, bisphenol AF type benzoxazine resin particles, magnolol-furfurylamine type benzoxazine resin particles, cardanol-aniline type benzoxazine resin particles, dicyclopentadiene type benzoxazine resin particles, and diaminodiphenylmethane type benzoxazine resin particles.

[0014] In this embodiment, the average particle size of the benzoxazine resin fine particles is 100 nm to 10 μm, preferably 500 nm to 1 μm.

[0015] In this embodiment, the average particle size of the zirconium oxide nanoparticles is 500 nm to 1 μm.

[0016] In this embodiment, the dispersing wetting agent is at least one of fluoroalkyl methoxy alcohol ether, polyoxyethylene alkylamine, sodium methylene bisnaphthalene sulfonate, polyether modified silicone, sodium aryl naphthalene sulfonate, sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, sodium perfluorooctanoate, nonylphenol polyoxyethylene ether, sodium butyl naphthalene sulfonate, polyacrylate, polyethylene glycol, carboxymethyl cellulose, and sodium carboxymethyl cellulose.

[0017] In this embodiment, the binder is at least one of styrene-butadiene rubber, sodium carboxymethyl cellulose, lithium polyacrylate, and polyacrylonitrile multipolymer.

[0018] In this embodiment, the environmentally friendly water-based resin slurry includes, by weight percentage, 30-86% water, 0.2-16% dispersing wetting agent, 2-6% binder, 7-40% benzoxazine resin particles, and 1-10% zirconium oxide nanoparticles.

[0019] Preferably, the environmentally friendly water-based resin slurry comprises, by weight percentage, 60-85% water, 1-10% dispersing wetting agent, 2-6% binder, 10-20% benzoxazine resin particles and 1-5% zirconium oxide nanoparticles.

[0020] In a second aspect, the present invention provides a method for preparing an environmentally friendly water-based resin slurry, comprising the following steps: The benzoxazine resin particles, zirconium oxide nanoparticles, a dispersing wetting agent, a binder and water are uniformly mixed to obtain an environmentally friendly water-based resin slurry.

[0021] The preparation method of the invention is simple and easy to operate and to industrialize.

[0022] In this embodiment, the step of uniformly mixing the benzoxazine resin particles, zirconium oxide nanoparticles, a dispersing wetting agent, a binder and water comprises: S1, mixing benzoxazine resin particles, zirconium oxide nanoparticles and water and ultrasonically dispersing them to obtain a first intermediate solution; S2, uniformly mixing the dispersing wetting agent and the first intermediate solution to obtain a second intermediate solution; S3. Evenly mix the second intermediate solution and the binder to obtain an environmentally friendly water-based resin slurry.

[0023] Preferably, in step S1, the ultrasonic dispersion time is ≥ 20 minutes.

[0024] Preferably, in step S2, the mixture is mixed evenly by stirring, and the stirring time is ≥ 6 h.

[0025] Preferably, in step S2, the mixture is mixed evenly by stirring, and the stirring time is ≥ 2 h.

[0026] In a third aspect, the present invention provides a modified polyolefin membrane, which is obtained by coating the environmentally friendly water-based resin slurry provided by the first aspect of the present invention on the surface of a polyolefin membrane and drying it.

[0027] The present invention modifies the polyolefin diaphragm by coating the above-mentioned environmentally friendly water-based resin slurry on the surface of the polyolefin diaphragm. The obtained modified polyolefin diaphragm has good electrolyte wettability, thermal stability, ion conductivity and lithium ion migration number, which is beneficial to improving the overall performance of the lithium ion battery.

[0028] In this embodiment, the thickness of the polyolefin diaphragm is 5~20μm, including but not limited to 5μm, 10μm, 15μm, 20μm, etc.; the air permeability is 50~120s / 100mL, including but not limited to 50s / 100mL, 60s / 100mL, 70s / 100mL, 80s / 100mL, 90s / 100mL, 100s / 100mL, 110s / 100mL, 120s / 100mL, etc.

[0029] In this embodiment, the polyolefin separator is a polyethylene (PE) film, a polypropylene (PP) membrane, or the like.

[0030] In this embodiment, the drying method is: placing the polyolefin separator coated with the environmentally friendly water-based resin slurry in an oven to evaporate the solvent, and then transferring it to a vacuum oven for drying to obtain a modified polyolefin separator.

[0031] Preferably, the oven temperature is 70-90° C., further 80° C.; the drying time is 2-10 minutes, further 5 minutes.

[0032] Preferably, the vacuum drying temperature is 70-90° C., further 80° C.; and the drying time is 16 h to 24 h.

[0033] In this embodiment, the thickness of the modified polyolefin separator is 10~35μm, including but not limited to 10μm, 12μm, 15μm, 18μm, 20μm, 22μm, 25μm, 28μm, 30μm, 32μm, 35μm, etc.

[0034] In this embodiment, the ionic conductivity of the modified polyolefin separator is 0.3mS / cm~0.8mS / cm, including but not limited to 0.3mS / cm, 0.4mS / cm, 0.5mS / cm, 0.6mS / cm, 0.7mS / cm, 0.8mS / cm, etc.; the lithium ion migration number is 0.2~0.7, including but not limited to 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, etc.; the electrolyte absorption rate is 80~430%, including but not limited to 80%, 140%, 200%, 260%, 320%, 380%, 430%, etc.; 180 o C. The heat shrinkage rate is ≤5%; the air permeability is 90~460s / 100mL, including but not limited to 90s / 100mL, 150s / 100mL, 200s / 100mL, 250s / 100mL, 300s / 100mL, 350s / 100mL, 400s / 100mL, 460s / 100mL, etc.

[0035] To avoid redundancy, some of the raw materials in the following embodiments and comparative examples of the present invention are summarized as follows: Benzoxazine resin: model CB3100, average particle size 600nm; The first dispersing wetting agent: model is CMC (1000-1400m.ps); Second dispersing wetting agent: model WA-6212; Adhesive: Model LA132; Zirconia nanoparticles: The average particle size is 500nm.

[0036] Example 1 Prepare 10g of slurry, mix 0.7g of benzoxazine resin particles and 0.3g of zirconium oxide nanoparticles with 8.56g of water, 0.02g of a first dispersing wetting agent, and 0.02g of a second dispersing wetting agent until completely dissolved, then add 0.4g of a binder and stir for more than 2 hours to complete the preparation. Apply the slurry on the surface of the polyolefin diaphragm, put it in an oven at 80°C and dry it for 5 minutes, and then put it in a vacuum oven at 80°C and dry it for 24 hours to obtain a modified polyolefin diaphragm.

[0037] Example 2 Prepare 10g of slurry, mix 1g of benzoxazine resin particles and 0.1g of zirconium oxide nanoparticles with 8.3g of water, 0.1g of the first dispersing wetting agent, and 0.1g of the second dispersing wetting agent until they are completely dissolved, then add 0.4g of the binder and stir and mix for more than 2 hours to complete the preparation. After scraping the slurry on the surface of the polyolefin diaphragm, put it in an oven at 80°C and dry it for 5 minutes, and then put it in a vacuum oven at 80°C and dry it for 24 hours to obtain a modified polyolefin diaphragm.

[0038] Example 3 Prepare 10g of slurry, mix 1g of benzoxazine resin particles and 0.3g of zirconium oxide nanoparticles with 7.9g of water, 0.2g of the first dispersing wetting agent, and 0.2g of the second dispersing wetting agent until they are completely dissolved, then add 0.4g of the binder and stir for more than 2 hours to complete the preparation. After applying the slurry on the surface of the polyolefin diaphragm, put it in an oven at 80°C and dry it for 5 minutes, and then put it in a vacuum oven at 80°C and dry it for 24 hours to obtain a modified polyolefin diaphragm.

[0039] Example 4 Prepare 10g of slurry, mix 2g of benzoxazine resin particles and 0.5g of zirconium oxide nanoparticles with 6.1g of water, 0.5g of the first dispersing wetting agent, and 0.5g of the second dispersing wetting agent until they are completely dissolved, then add 0.4g of the binder and stir for more than 2 hours to complete the preparation. After applying the slurry on the surface of the polyolefin diaphragm, put it in an oven at 80°C and dry it for 5 minutes, and then put it in a vacuum oven at 80°C and dry it for 24 hours to obtain a modified polyolefin diaphragm.

[0040] Example 5 Prepare 10g of slurry, mix 3g of benzoxazine resin particles and 0.7g of zirconium oxide nanoparticles with 4.3g of water, 0.8g of the first dispersing wetting agent, and 0.8g of the second dispersing wetting agent until they are completely dissolved, then add 0.4g of the binder and stir for more than 2 hours to complete the preparation. After applying the slurry on the surface of the polyolefin diaphragm, put it in an oven at 80°C and dry it for 5 minutes, and then put it in a vacuum oven at 80°C and dry it for 24 hours to obtain a modified polyolefin diaphragm.

[0041] Example 6 Prepare 10g of slurry, mix 4g of benzoxazine resin particles and 1g of zirconium oxide nanoparticles with 3g of water, 0.8g of the first dispersing wetting agent, and 0.8g of the second dispersing wetting agent until they are completely dissolved, then add 0.4g of the binder and stir for more than 2 hours to complete the preparation. After applying the slurry on the surface of the polyolefin diaphragm, put it in an oven at 80°C and dry it for 5 minutes, and then put it in a vacuum oven at 80°C and dry it for 24 hours to obtain a modified polyolefin diaphragm.

[0042] Comparative Example 1 Comparative Example 1 is a Celgard PE separator with a thickness of 6 μm.

[0043] Comparative Example 2 Prepare 10g of slurry, mix 1g of benzoxazine resin particles with 8.56g of water, 0.02g of the first dispersing wetting agent, and 0.02g of the second dispersing wetting agent until they are completely dissolved, then add 0.4g of the binder and stir for more than 2 hours to complete the preparation. Apply the slurry on the surface of the polyolefin diaphragm (PE diaphragm with a thickness of 6μm), put it in an oven at 80°C to dry for 5 minutes, and then put it in a vacuum oven at 80°C to dry for 24h to obtain a modified polyolefin diaphragm.

[0044] Comparative Example 3 Comparative Example 1 is a Celgard PE separator with a thickness of 10 μm.

[0045] Comparative Example 4 Prepare 10g of slurry, mix 1g of benzoxazine resin particles with 8.56g of water, 0.02g of the first dispersing wetting agent, and 0.02g of the second dispersing wetting agent until they are completely dissolved, then add 0.4g of the binder and stir for more than 2 hours to complete the preparation. Apply the slurry on the surface of the polyolefin diaphragm (PE diaphragm with a thickness of 10μm), put it in an oven at 80°C to dry for 5 minutes, and then put it in a vacuum oven at 80°C to dry for 24h to obtain a modified polyolefin diaphragm.

[0046] Comparative Example 5 Prepare 10g of slurry, mix 1g of zirconium oxide nanoparticles with 8.56g of water, 0.02g of the first dispersing wetting agent, and 0.02g of the second dispersing wetting agent until they are completely dissolved, then add 0.4g of the binder and stir for more than 2 hours to complete the preparation. Apply the slurry on the surface of the polyolefin diaphragm (PE diaphragm with a thickness of 10μm), put it in an oven at 80°C and dry it for 5 minutes, and then put it in a vacuum oven at 80°C and dry it for 24h to obtain a modified polyolefin diaphragm.

[0047] Performance Testing The polyolefin separators of Examples 1 to 6 of the present invention and Comparative Examples 1 to 5 were tested for performance such as thickness, liquid absorption, morphology, ionic conductivity, and thermal stability. The test results are shown in Table 1.

[0048] Among them, SEM images of the front and back surfaces of the PE diaphragm in Comparative Example 3 and the modified diaphragm obtained in Example 3 of the present invention were observed under a cold field scanning electron microscope.

[0049] Among them, the liquid absorption rate is tested by weighing method, that is, the liquid absorption rate of the membrane is calculated by the change in weight before and after the membrane absorbs liquid. Specifically, the dry film is weighed, and then immersed in a liquid electrolyte of 1.0 M LiPF6EC:DMC (1:1, v / v) at 25°C for 2 hours, taken out and the surface liquid is absorbed with filter paper and weighed. The liquid absorption rate EU is calculated using the following formula: EU(%)=(W ’ 2-W ’ 1) / W ’ 1×100% Where W'1 and W'2 are the masses (g) of the separator before and after it is immersed in the electrolyte.

[0050] Among them, the heat shrinkage test: observe the dimensional changes of the composite diaphragm before and after heating at 180 °C for 30 min.

[0051] Among them, ion conductivity test: punch the diaphragm into a disc with a diameter of 16 mm, measure its thickness and record it as d, and assemble it in a glove box. Let it stand for 12 hours, and use an electrochemical workstation to perform AC impedance test after the battery is stable. The test frequency is 0.1~10Hz, calculated according to the following formula: σ = d / (R b A) In the formula, σ represents the ionic conductivity, d represents the thickness of the separator in cm, and R b It represents the bulk resistance of the diaphragm, which is the intercept of the curve on the X-axis on the impedance spectrum. A represents the surface area of ​​the diaphragm in cm -2 .

[0052] Among them, lithium ion transfer number measurement: button cells were assembled and doped with liquid electrolyte 1.0 M LiPF6EC:DMC (1:1, v / v) to assemble Li metal / separator / Li metal cells and equilibrated at 25 °C for 12 hours. + The migration number is expressed by Li + The percentage of current provided by migration is obtained using the following equation: t + =I s (ΔV-I i R i ) / Ii(ΔV-I s R s ) Where ΔV is the transition voltage (10 mV); R i and R s are the interface resistances before and after polarization, respectively; I i and I s are the initial current and steady-state current during polarization, respectively.

[0053] Among them, the air permeability test: the American Gurley 4110N air permeability tester is used to test the air permeability of the diaphragm. The air permeability of the diaphragm reflects the tortuosity of the internal pores of the diaphragm and the true path of ion diffusion. It is proportional to the ion conductivity and can be evaluated by the Gurley value. The Gurley value refers to the time required for a certain amount of air to pass through a unit area of ​​the diaphragm at a certain specified pressure, and the unit is s / 100mL.

[0054] Among them, the battery performance test: lithium metal is used as the negative electrode, LiFePO4 is used as the positive electrode, 1.0 M LiPF6EC:DMC (1:1, v / v) is used as the liquid electrolyte, and the polyolefin separators of the embodiments of the present application and the comparative examples are used to prepare button batteries, and their battery performance is tested.

[0055] Table 1 Performance parameters of polyolefin membranes of Examples 1-6 of the present invention and Comparative Examples 1-5

[0056] It can be seen from Table 1 that the modified membranes obtained in Examples 1-6 of the present invention all have good heat resistance and liquid absorption rate, and the modified membrane in Example 3 of the present invention has the best performance in terms of ion conductivity and lithium ion migration number performance.

[0057] It can be seen from Comparative Examples 1-4 that, for a base membrane with a suitable porosity, the use of the slurry modification of the present invention can better improve the electrochemical properties of the composite membrane. If the base membrane has a high air permeability value (i.e., the corresponding porosity is low), the use of slurry coating will cause the resin material to block the pores, resulting in a sharp increase in permeability, thereby affecting the electrochemical properties of the composite membrane.

[0058] Under the condition of using a diaphragm with a suitable porosity, it can be seen from Comparative Examples 3-4 and Examples 2-3 that in the system of the present invention, with the increase in the amount of zirconium oxide nanoparticles, the liquid absorption rate, thermal shrinkage, ionic conductivity and lithium ion migration number all show an upward trend; it can be seen from Examples 3-6 that with the increase in the amount of benzoxazine resin particles and zirconium oxide nanoparticles, the liquid absorption rate, thermal shrinkage and air permeability increase, but the ionic conductivity and lithium ion migration number decrease. It can be seen that with the appropriate amount of zirconium oxide added, the resin arrangement structure can be regularized, the lithium ion migration number can be increased, the impedance can be reduced, and the ionic conductivity can be improved; at the same time, the benzoxazine resin and zirconium oxide nanoparticles improve the liquid absorption rate and high temperature performance of the diaphragm.

[0059] See also Figure 1 , Figure 1 This is a SEM image of the PE diaphragm in Comparative Example 3 of the present invention. Figure 1It can be seen that the SEM image of the commercial PE separator prepared by dry stretching shows a large number of uniformly distributed pores in the same direction.

[0060] See also Figure 2-3 , Figure 2 This is a SEM image of the front side of the modified polyolefin diaphragm in Example 3 of the present invention. Figure 3 This is a SEM image of the reverse side of the modified polyolefin diaphragm in Example 3 of the present invention. Figure 2-3 It can be seen that the resin is evenly deposited on both sides of the diaphragm, completely covering the surface of the diaphragm.

[0061] See also Figure 4 , Figure 4 The thermal stability diagrams are of the PE diaphragm in Comparative Example 3 of the present invention before and after heating at 180°C for 30 minutes, the PE diaphragm in Example 2 before and after heating at 180°C for 30 minutes, and the modified polyolefin diaphragm obtained in Example 4 after heating at 180°C for 30 minutes. Figure 4 It can be seen that compared with the PE diaphragm at 180 o In the case of melting at 400 °C, the modified polyolefin diaphragm obtained by the present invention has stronger thermal stability, which indicates that the resin slurry of the present application is helpful to improve the thermal stability.

[0062] See also Figure 5 , Figure 5 The voltage-specific capacity curve of the button cell made of the modified polyolefin separator in Example 3 of the present application. Figure 5 It can be seen that the button cell made of the modified polyolefin separator prepared in the present invention has excellent electrochemical properties.

[0063] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. An environmentally friendly water-based resin slurry, characterized in that: The raw materials include, by weight percentage, 5-98.88% of water, 0.01-30% of a dispersing wetting agent, 0.1-5% of a binder, 1-50% of benzoxazine resin particles, and 0-15% of zirconium oxide nanoparticles.

2. The environmentally friendly water-based resin slurry according to claim 1, characterized in that: The benzoxazine resin particles are at least one of bisphenol A type benzoxazine resin particles, bisphenol F type benzoxazine resin particles, phenol type benzoxazine resin particles, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide type benzoxazine resin particles, phenolphthalein type benzoxazine resin particles, bisphenol AF type benzoxazine resin particles, magnolol-furfurylamine type benzoxazine resin particles, cardanol-aniline type benzoxazine resin particles, dicyclopentadiene type benzoxazine resin particles, and diaminodiphenylmethane type benzoxazine resin particles.

3. The environmentally friendly water-based resin slurry according to claim 1, characterized in that: The dispersing wetting agent is at least one of fluoroalkyl methoxy alcohol ether, polyoxyethylene alkylamine, sodium methylene bisnaphthalene sulfonate, polyether modified silicone, sodium aryl naphthalene sulfonate, sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, sodium perfluorooctanoate, nonylphenol polyoxyethylene ether, sodium butylnaphthalene sulfonate, polyacrylate, polyethylene glycol, carboxymethyl cellulose, and sodium carboxymethyl cellulose; or, The binder is at least one of styrene-butadiene rubber, sodium carboxymethyl cellulose, lithium polyacrylate, and polyacrylonitrile multipolymer.

4. The environmentally friendly water-based resin slurry according to claim 1, characterized in that: The average particle size of the benzoxazine resin particles is 100 nm to 10 μm; or, The average particle size of the zirconium oxide nanoparticles is 500nm-1μm.

5. The environmentally friendly water-based resin slurry according to claim 1, characterized in that: The raw materials include, by weight percentage, 30-86% of water, 0.2-16% of a dispersing wetting agent, 2-6% of a binder, 7-40% of benzoxazine resin particles, and 1-10% of zirconium oxide nanoparticles.

6. The environmentally friendly water-based resin slurry according to claim 1, characterized in that: The raw materials include, by weight percentage, 60-85% of water, 1-10% of a dispersing wetting agent, 2-6% of a binder, 10-20% of benzoxazine resin particles and 1-5% of zirconium oxide nanoparticles.

7. A method for preparing the environmentally friendly water-based resin slurry according to any one of claims 1 to 6, characterized in that: The following steps are involved: The benzoxazine resin particles, zirconium oxide nanoparticles, a dispersing wetting agent, a binder and water are uniformly mixed to obtain an environmentally friendly water-based resin slurry.

8. A modified polyolefin diaphragm, characterized in that: The modified polyolefin separator is obtained by coating the environmentally friendly water-based resin slurry according to any one of claims 1 to 6 on the surface of a polyolefin separator and drying the slurry.

9. The modified polyolefin diaphragm according to claim 8, characterized in that: The thickness of the polyolefin separator is 5-20 μm, and the thickness of the modified polyolefin separator is 10-35 μm.

10. The modified polyolefin diaphragm according to claim 8, characterized in that: The modified polyolefin separator has an ionic conductivity of 0.3 mS / cm to 0.8 mS / cm, a lithium ion migration number of 0.2 to 0.7, an electrolyte absorption rate of 80 to 430%, and a o The heat shrinkage rate at C is ≤5%, and the air permeability is 90~460s / 100mL.

Citation Information

Patent Citations

  • Polypropylene battery diaphragm containing composite coating and preparation method of polypropylene battery diaphragm

    CN105098120A

  • Coating composition, composite isolating membrane, battery monomer, battery and electric equipment