Method for reducing carbon dioxide
By using polishing and electroplating in electrochemical reduction method, the problem of poor corrosion of the electrode is solved, efficient reduction and stability of carbon dioxide are achieved, and important application value is achieved.
Patent Information
- Application Number
- CN202410950359.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the existing electrochemical reduction methods, the electrodes are prone to corrosion and difficult to use for a long time, resulting in insufficient carbon dioxide reduction efficiency and stability.
A three-electrode system is adopted, in which the working electrode is a ferrotin alloy prepared by polishing and electroplating. The electroplating solution prepared by stannous sulfate, ferrous sulfate, sodium citrate, sodium hydroxide and other materials is electroplating to form a ferrotin alloy electrode to improve the electrode corrosion resistance and carbon dioxide reduction activity.
It improves the corrosion resistance of the electrode and the reduction activity of carbon dioxide, ensures the stability and efficiency of long-term use, and reduces production costs.
Smart Images

Figure BDA0004947047350000051
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of carbon dioxide reduction, and in particular, relates to a method for reducing carbon dioxide. Background Art
[0002] Energy is an important material basis for economic development and people's lives. At present, the social economy is in a stage of rapid development, and the demand for energy continues to increase. 2 The emission of gases is also increasing. According to the latest report of the International Energy Agency (IEA), in 2012, the global CO 2 By 2030, annual carbon dioxide emissions are expected to increase to 43 billion tons, an increase of 60%. This will lead to CO 2 The increase in CO concentrations has caused global warming. 2 emissions, effectively utilize CO 2 It has become a research hotspot in recent years.
[0003] CO 2 There are three main ways to reduce and utilize CO2: (i) capture and storage. 2 Capture by chemical or physical adsorption and then store underground; (ii) Chemical conversion, including catalytic hydrogenation and reforming, that is, under the action of a catalyst, CO 2 Chemical reactions with other chemical raw materials to synthesize valuable chemicals, such as synthetic urea, cyclic carbonates, etc. (iii) Preparation of corresponding chemicals by electrochemical reduction, photoelectrochemical or bioelectrochemical reduction. Among them, electrochemical reduction of carbon dioxide is a technology that uses electrochemical methods to convert carbon dioxide into useful chemicals or fuels. This technology not only helps to reduce greenhouse gas emissions in the atmosphere, but also can convert renewable energy into chemical energy, providing a new way for energy storage. However, the electrodes used in the current electrochemical reduction method are prone to corrosion and difficult to use for a long time. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a method for reducing carbon dioxide.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for reducing carbon dioxide comprises the following steps: placing a three-electrode system in an electrolyte containing carbon dioxide for electrolysis.
[0007] Furthermore, the three-electrode system includes a working electrode, a counter electrode and a reference electrode.
[0008] Furthermore, the counter electrode and the reference electrode are the same platinum sheet.
[0009] Furthermore, the working electrode is a tin-iron alloy.
[0010] Furthermore, the tin-iron alloy is prepared by the following steps:
[0011] A1. Place the copper sheet on a polishing machine and polish it until the surface of the plated piece is flat and has a metallic luster to obtain a polished copper sheet;
[0012] A2. The polished copper sheet is added to a dilute hydrochloric acid solution and soaked for 10 minutes, then taken out, ultrasonically cleaned, blown dry with a cold air blower, and dried to obtain a pretreated copper sheet;
[0013] A3. Place the pretreated copper sheet in the electroplating solution and use the constant current method to electroplate for 20-30 minutes. After the electroplating is completed, rinse with acetone for three times, then treat at a high temperature of 250-300°C for 2-3 hours, and then use chromate passivation for 1-3 minutes to obtain a tin-iron alloy.
[0014] Furthermore, in step A1, the polishing machine speed is controlled to be 30-35 r / s.
[0015] Furthermore, the mass fraction of the dilute hydrochloric acid in step A2 is 6%-12%.
[0016] Furthermore, the drying condition in step A2 is drying in an argon drying vessel for 2-6 hours.
[0017] By pre-treating the copper sheet, the bonding ability between the copper sheet and the plating layer can be improved.
[0018] Furthermore, the electroplating solution is prepared by the following steps:
[0019] Sodium citrate and deionized water were added to a three-necked flask, and magnetic stirring was started until the sodium citrate was completely dissolved. Stannous sulfate and ferrous sulfate were then added, and stirring was started until the solid was completely dissolved. Then, sodium hydroxide solution was added to adjust the pH to 7 to obtain an electroplating solution.
[0020] Furthermore, the usage ratios of sodium citrate, deionized water, stannous sulfate and ferrous sulfate are 1.4705 g, 50 mL, 0.0215 g and 0.0278 g.
[0021] Beneficial effects of the present invention:
[0022] 1. By pre-treating the copper sheet, the bonding ability between the copper sheet and the coating can be improved, and the coating can effectively protect the copper sheet from corrosion;
[0023] 2. Using stannous sulfate, ferrous sulfate, sodium citrate, sodium hydroxide and copper sheet to make tin-iron alloy is not only cheaper, but also contains more surface oxygen vacancies and has strong reduction activity for carbon dioxide;
[0024] 3. After being treated with acetone, the tin-iron alloy becomes more stable and its reduction activity remains excellent even after being placed for a long time.
[0025] Therefore, based on the above points, the method for reducing carbon dioxide provided by the present invention has important application value in the field of carbon dioxide reduction technology. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Example 1
[0028] Prepare the plating solution:
[0029] Add 1.4705 g of sodium citrate and 50 mL of deionized water into a three-necked flask, start magnetic stirring until the sodium citrate is completely dissolved, then add 0.0215 g of stannous sulfate and 0.0278 g of ferrous sulfate, start stirring until the solid is completely dissolved, add sodium hydroxide solution to adjust the pH to 7, and obtain an electroplating solution.
[0030] Example 2
[0031] Prepare the plating solution:
[0032] Add 2.941 g of sodium citrate and 100 mL of deionized water into a three-necked flask, start magnetic stirring until the sodium citrate is completely dissolved, then add 0.043 g of stannous sulfate and 0.0556 g of ferrous sulfate, start stirring until the solid is completely dissolved, add sodium hydroxide solution to adjust the pH to 7, and obtain an electroplating solution.
[0033] Example 3
[0034] Preparation of tin-iron alloy:
[0035] A1. Place the copper sheet on a polishing machine (the speed is controlled at 30r / s) and polish until the surface of the plated piece is smooth and has a metallic luster to obtain a polished copper sheet;
[0036] A2. The polished copper sheet was added to a dilute hydrochloric acid solution (mass fraction 6%) and soaked for 10 min, then taken out, ultrasonically cleaned, blown dry with a cold air blower, and dried in an argon drying vessel for 2 h to obtain a pretreated copper sheet;
[0037] A3. The pretreated copper sheet was placed in the electroplating solution prepared in Example 1, and electroplated for 20 minutes using a constant current method. After the electroplating was completed, it was rinsed with acetone for a total of three times, and then subjected to high-temperature treatment at 250° C. for 2 hours, and then subjected to chromate passivation treatment for 1 minute to obtain a tin-iron alloy.
[0038] Example 4
[0039] Preparation of tin-iron alloy:
[0040] A1. Place the copper sheet on a polishing machine (the speed is controlled at 35r / s) and polish until the surface of the plated piece is smooth and has a metallic luster to obtain a polished copper sheet;
[0041] A2. The polished copper sheet was added to a dilute hydrochloric acid solution (mass fraction 12%) and soaked for 10 min, then taken out, ultrasonically cleaned, blown dry with a cold air blower, and dried in an argon drying vessel for 6 h to obtain a pretreated copper sheet;
[0042] A3. The pretreated copper sheet was placed in the electroplating solution prepared in Example 2, and electroplated for 20-30 min using a constant current method. After the electroplating was completed, it was rinsed with acetone for a total of three times, and then subjected to a high-temperature treatment at 300° C. for 3 h, and then subjected to a chromate passivation treatment for 3 min to obtain a tin-iron alloy.
[0043] Example 5
[0044] A platinum counter electrode, a reference electrode and the tin-iron alloy working electrode prepared in Example 3 were used as a three-electrode system and placed in a saturated CO 2 In a NaCl (potassium bicarbonate) solution, the voltage was controlled at -1.5V, and the electrolysis experiment was carried out. The electrolysis time was controlled at 3600s and the electrolysis interval was 100mV.
[0045] Example 6
[0046] A platinum counter electrode, a reference electrode and the tin-iron alloy working electrode prepared in Example 4 were used as a three-electrode system and placed in a saturated CO 2 In a NaCl (potassium bicarbonate) solution, the voltage was controlled at -1.5V, and the electrolysis experiment was carried out. The electrolysis time was controlled at 3600s and the electrolysis interval was 100mV.
[0047] Comparative Example
[0048] A copper sheet was used as the working electrode, and the remaining steps were the same as those in Example 6.
[0049] The electrocatalytic reduction of carbon dioxide was carried out on Examples 5-6 and the comparative example, and the product CO was detected by gas chromatography. 2 and H 2 The measured results are shown in the following table:
[0050]
[0051] It can be seen from the above table that the method for reducing carbon dioxide in the embodiment of the present invention has good reducing performance, high efficiency, and good stability, and has important application value in the field of carbon dioxide reduction technology.
[0052] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0053] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for reducing carbon dioxide, comprising the following steps: The three-electrode system is placed in an electrolyte containing carbon dioxide for electrolysis, wherein the three-electrode system comprises a working electrode, a counter electrode and a reference electrode.
2. A method for reducing carbon dioxide according to claim 1, characterized in that: The working electrode is tin-iron alloy.
3. A method for reducing carbon dioxide according to claim 2, characterized in that: The tin-iron alloy is prepared by the following steps: A1. Place the copper sheet on a polishing machine and polish it until the surface of the plated piece is flat and has a metallic luster to obtain a polished copper sheet; A2. The polished copper sheet is added to a dilute hydrochloric acid solution and soaked for 10 minutes, then taken out, ultrasonically cleaned, blown dry with a cold air blower, and dried to obtain a pretreated copper sheet; A3. Place the pretreated copper sheet in the electroplating solution and use the constant current method to electroplate for 20-30 minutes. After the electroplating is completed, rinse with acetone for three times, then treat at a high temperature of 250-300°C for 2-3 hours, and then use chromate passivation for 1-3 minutes to obtain a tin-iron alloy.
4. A method for reducing carbon dioxide according to claim 2, characterized in that: In step A1, the polishing machine speed is controlled to be 30-35 r / s.
5. A method for reducing carbon dioxide according to claim 2, characterized in that: The mass fraction of the dilute hydrochloric acid in step A2 is 6%-12%.
6. A method for reducing carbon dioxide according to claim 2, characterized in that: The drying condition in step A2 is drying in an argon drying vessel for 2-6 hours.
7. A method for reducing carbon dioxide according to claim 2, characterized in that: The electroplating solution is prepared by the following steps: Sodium citrate and deionized water were added to a three-necked flask, and magnetic stirring was started until the sodium citrate was completely dissolved. Stannous sulfate and ferrous sulfate were then added, and stirring was started until the solid was completely dissolved. Then, sodium hydroxide solution was added to adjust the pH to 7 to obtain an electroplating solution.
8. A method for reducing carbon dioxide according to claim 2, characterized in that: The usage ratios of the sodium citrate, deionized water, stannous sulfate and ferrous sulfate are 1.4705 g, 50 mL, 0.0215 g and 0.0278 g.