Negative electrode material, negative electrode plate and battery
By forming a high-density cladding layer on the silicon-based negative electrode material and optimizing the carbon matrix structure, the problem of changes in production gas and volume in contact with the silicon material and the electrolyte is solved, and the circulation performance and conductivity of lithium-ion batteries are improved.
Patent Information
- Application Number
- CN202411359588.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-09-28
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-29
AI Technical Summary
The existing silicon-based anode material has poor coating effect in lithium-ion batteries, causing silicon material to come into contact with the electrolyte to produce gas, and volume changes lead to damage to the surface SEI film, affecting battery capacity and cycling performance.
Using a high-density cladding layer, the composite structure of carbon matrix and silicon material is formed on the surface of the silicon material, and the density of the cladding layer is ≥80% and the total pore volume is ≤0.02cm3/g, reducing the silicon material and electrolyte. The reaction is carried out and the carbon matrix structure is optimized by pressurization treatment and impregnation solution filling to reduce the number of macropores.
It effectively reduces the gas production value of the negative electrode material, improves circulation and expansion performance, improves conductivity and processing performance, and extends the service life of the battery.
Smart Images

Figure CN119050328A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of negative electrode materials, and in particular to a negative electrode material, a negative electrode plate and a battery. Background Art
[0002] Lithium-ion batteries have the advantages of high energy density, long service life and no environmental pollution, and have been widely used in the 3C field. With the development of the market, lithium-ion batteries are not only widely used in mobile devices such as smart phones and portable computers, but also in large equipment such as electric vehicles and power tools. In order to improve the energy density of batteries, the research and development of silicon-based negative electrode materials are becoming more mature.
[0003] On the one hand, the silicon-based negative electrode material includes a core and a coating layer on its surface, but the coating effect of the coating layer of the existing silicon-based negative electrode material is poor. During the preparation of the silicon-based negative electrode material into a lithium-ion battery, the dissolved silicon material will come into contact with the electrolyte, resulting in gas production.
[0004] On the other hand, silicon-based negative electrode materials have the advantages of high specific capacity, low voltage platform, environmental friendliness and abundant resources, and are expected to replace graphite negative electrodes for the next generation of high specific energy lithium-ion batteries. However, silicon has a huge volume change during the extraction / insertion process, which easily leads to particle pulverization and then falling off the current collector. In addition, the repeated changes in the volume of silicon-based negative electrode materials during the electrochemical cycle also lead to the continuous destruction and regeneration of the SEI film formed on the surface of the silicon-based negative electrode material, resulting in the continuous consumption of lithium ions, which will eventually lead to the rapid decay of capacity. Usually, the silicon material in the negative electrode material is improved by nano-sizing, carbon coating, polymer coating and other processes, which can inhibit the volume expansion of silicon materials to a certain extent. For the carbon coating process, the silicon active material is usually deposited in porous carbon to achieve carbon coating. At present, the preparation of porous carbon by biomass method is an important direction, but the porous carbon prepared by biomass usually has large pores with relatively large diameters. The large number of macropores affects the compaction performance of porous carbon, making the prepared negative electrode material unable to meet the requirements of high compaction. Moreover, since the macropores in porous carbon are generated during the natural growth process, it is difficult to completely remove them, resulting in the deterioration of the initial efficiency, expansion performance and processing performance of the negative electrode material.
[0005] Therefore, how to reduce the reaction between silicon materials and electrolytes, lower the gas production value, and develop a negative electrode material with high initial efficiency, high cycle and low expansion performance remains a technical challenge in the field. Summary of the invention
[0006] The present application provides a negative electrode material, a negative electrode plate and a battery. The negative electrode material can reduce the reaction between silicon material and electrolyte, reduce gas production value and improve the cycle performance of the material through a high-density coating layer. It can further improve the capacity, expansion performance and cycle performance of the negative electrode material.
[0007] In a first aspect, the present application provides a negative electrode material, the negative electrode material comprising a core and a coating layer located on the surface of the core, the core comprising a silicon material; the total pore volume of the negative electrode material is ≤0.02cm 3 / g, and the density of the coating layer β≥80%;
[0008] The density β of the coating layer is measured by the following test method: m1 g of negative electrode material is immersed in a 20% HF solution for 1 hour, then washed and dried, and the mass of the negative electrode material after washing and drying is weighed as m2. The density of the coating layer is calculated as β=m2 / m1×100%.
[0009] In some embodiments, the inner core includes a carbon matrix having pores and a silicon material located within the pores of the carbon matrix.
[0010] In some embodiments, the inner core includes a carbon matrix with pores and a silicon material located in the pores of the carbon matrix. The area ratio of pores with a pore size greater than 50 nm in any cross-section of the negative electrode material is α, satisfying: α≤10%; wherein, α is obtained by the following test method: in the figure shown by SEM section processing of a single negative electrode material particle, select any A×B area, wherein A=1μm~10μm, B=1μm~10μm, the sum of the cross-sectional areas of pores with a pore size greater than 50 nm in the cross-section of a single negative electrode material particle in the region is recorded as S0, the cross-sectional area of a single negative electrode material particle in the region is recorded as S, and the area ratio of pores with a pore size greater than 50 nm in the cross-section of a single negative electrode material particle is defined as α', α'=S0 / S, and α is the arithmetic mean of the α' values of at least 10 negative electrode material particles.
[0011] In some embodiments, the carbon matrix includes at least one of artificial graphite, natural graphite, amorphous carbon, activated carbon, activated carbon fiber, carbon black, capacitive carbon, carbon molecular sieve, mesophase carbon microbeads, carbon nanotubes, carbon nanofibers, porous carbon and graphene.
[0012] In some embodiments, the silicon material includes at least one of crystalline silicon, silicon oxide, amorphous silicon, silicon alloys, silicates, and composite particles of crystalline and amorphous silicon.
[0013] In some embodiments, the average particle size of the silicon material is 0.1 nm to 500 nm.
[0014] In some embodiments, the morphology of the silicon material includes at least one of a dot shape, a sphere shape, an ellipsoid shape, and a flake shape.
[0015] In some embodiments, the purity of the silicon material is greater than 99%.
[0016] In some embodiments, the pore volume of the negative electrode material is less than or equal to 0.1 cm3 / g.
[0017] In some embodiments, in a cross section of the negative electrode material, the area of pores with a pore diameter greater than or equal to 500 nm accounts for less than or equal to 5%.
[0018] In some embodiments, the carbon matrix has a median particle size of 15 μm or less.
[0019] In some embodiments, the mass percentage of silicon in the negative electrode material is 40% to 80%.
[0020] In some embodiments, the mass percentage of carbon in the negative electrode material is 20% to 60%.
[0021] In some embodiments, the material of the coating layer includes at least one of a carbon material, a metal oxide, amorphous silicon, a conductive polymer, a fluoride, a phosphate, and a nitride.
[0022] In some embodiments, the material of the coating layer includes a carbon material, and the carbon material includes at least one of graphene, soft carbon, hard carbon, a conductive polymer, and amorphous carbon.
[0023] In some embodiments, the material of the coating layer includes metal oxide, and the material of the metal oxide layer includes at least one of the oxides of Sn, Ge, Fe, Si, Cu, Ti, Na, Mg, Al, Li, Co, V, Ca and Zn.
[0024] In some embodiments, the material of the coating layer includes a conductive polymer, and the conductive polymer includes at least one of polyaniline, polyacetylene, polypyrrole, polythiophene, poly-3-hexylthiophene, poly(p-phenylene vinylene), polypyridine, and polystyrene vinylene.
[0025] In some embodiments, the material of the coating layer includes a fluoride, and the fluoride includes at least one of polyvinyl fluoride, fluoropolymer, sodium fluoride, potassium fluoride, fluorocarbon polymer, fluorosilicone polymer, hexafluorobutyl acrylate, polytetrafluoroethylene (PTFE), fluorinated ethylene-propylene copolymer (FEP), perfluoroalkoxy resin (PFA), polychlorotrifluoroethylene (PCTFE), ethylene-chlorotrifluoroethylene copolymer (ECTFE), polyvinylidene fluoride (PVDF) and polyvinyl fluoride.
[0026] In some embodiments, the material of the coating layer includes phosphate, and the phosphate includes at least one of magnesium phosphate, calcium phosphate, aluminum phosphate, titanium phosphate, chromium phosphate, cobalt phosphate, nickel phosphate, germanium phosphate, zirconium phosphate, niobium phosphate, molybdenum phosphate, tantalum phosphate, tungsten phosphate, and lanthanum phosphate.
[0027] In some embodiments, the material of the coating layer includes nitride, and the nitride includes at least one of titanium nitride, silicon nitride, vanadium nitride, cobalt nitride, nickel nitride, and carbon nitride.
[0028] In some embodiments, the coating layer has a thickness of 0.1 nm to 3000 nm, preferably 1 nm to 300 nm.
[0029] In some embodiments, the coating layer accounts for ≤10% by mass of the negative electrode material.
[0030] In some embodiments, the median particle size of the negative electrode material is ≤15 μm, preferably ≤10 μm.
[0031] In some embodiments, the specific surface area of the negative electrode material is ≤5 m 2 / g.
[0032] In a second aspect, the present application provides a negative electrode plate, which includes a negative electrode current collector and a negative electrode active material distributed on one side of the negative electrode current collector, and the negative electrode active material includes the negative electrode material according to any one of the first aspect.
[0033] In some embodiments, the critical withstand pressure P of the negative electrode plate is greater than or equal to 100 MPa; the critical withstand pressure P of the negative electrode plate is obtained by the following test method: the thickness of the negative electrode plate is 60 μm to 70 μm, and an electron scanning microscope SEM is used to observe the cross-section of a single negative electrode plate, and the minimum pressure corresponding to the crushing of the negative electrode material particles is P.
[0034] In some embodiments, the compaction density of the negative electrode sheet is 1.3 g / cm 3 ~1.9g / cm 3 .
[0035] In a third aspect, the present application provides a battery, comprising the negative electrode material according to any one of the first aspects.
[0036] The technical solution of this application has at least the following beneficial effects:
[0037] The negative electrode material provided in the present application includes a core and a coating layer, and the density β of the coating layer is ≥80%. Within this range, the coating layer can reduce the dissolution amount of the negative electrode material during the cycle, thereby reducing the reaction between the dissolved silicon material and the electrolyte, effectively reducing the gas production value of the negative electrode material; and the total pore volume of the negative electrode material is ≤0.02cm 3 / g. Within this range, the amount of electrolyte that directly penetrates into the particles of the negative electrode material through the pore structure can be effectively reduced, thereby reducing the side reactions occurring when the electrolyte contacts the silicon material and improving the cycle performance of the lithium-ion battery.
[0038] Further, the area ratio of pores with a pore size greater than 50 nm in any cross section of the negative electrode material of the present application is α, and α≤10%. It can be understood that pores with a pore size greater than 50 nm are macropores, that is, α represents the area ratio of macropores in the cross section of the core. The area ratio of macropores in the cross section of the negative electrode material of the present application is relatively small. On the one hand, macropores with a relatively small area ratio can effectively reduce the specific surface area of the negative electrode material. During the first charge and discharge process, the occurrence of side reactions between the negative electrode material and the electrolyte can be reduced, gas production can be reduced, and the first efficiency, expansion performance and cycle performance of the negative electrode material can be improved. On the other hand, macropores with a relatively small area ratio can improve the tap density and compaction density of the negative electrode material, reduce the problems of breakage and cracks in the process of rolling the negative electrode material into a pole piece, improve the processing performance of the negative electrode material, and further improve the processing performance of the negative electrode material. Moreover, the relatively small area ratio of macropores in the cross section of the negative electrode material indicates that the porosity of the negative electrode material is low, and the carbon content in the negative electrode material with a low porosity is high, so that the negative electrode material has good electronic conductivity, provides a developed conductive network for the negative electrode material, and improves the conductivity of the negative electrode material. In the cross section of the negative electrode material of the present application, by controlling the area ratio of the macropores in the cross section of the negative electrode material, the conductivity, capacity, initial efficiency, cycle performance and processing performance of the negative electrode material can be effectively improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0040] Figure 1 This is a scanning electron microscope (SEM) image of the negative electrode material prepared in Example 1 of the present application;
[0041] Figure 2 XRD diagram of the negative electrode material prepared in Example 1 of the present application;
[0042] Figure 3 The first charge and discharge curve of the negative electrode material prepared in Example 1 of the present application;
[0043] Figure 4 The cycle performance curve of the negative electrode material prepared in Example 1 of the present application;
[0044] Figure 5 This is a SEM image of the negative electrode material prepared in Example 10 of the present application;
[0045] Figure 6 This is the XRD pattern of the negative electrode material prepared in Example 10 of the present application;
[0046] Figure 7 This is the first charge and discharge curve of the negative electrode material prepared in Example 10 of the present application;
[0047] Figure 8 This is the cycle performance curve of the negative electrode material prepared in Example 10 of the present application. DETAILED DESCRIPTION
[0048] The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and should not be construed as limiting the present application.
[0049] It should be clear that the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.
[0050] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0051] It should be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0052] Lithium-ion batteries have the advantages of high energy density, long service life and no environmental pollution, and have been widely used in the 3C field. With the development of the market, lithium-ion batteries are not only widely used in mobile devices such as smart phones and portable computers, but also in large equipment such as electric vehicles and power tools. In order to improve the energy density of batteries, the research and development of silicon-based negative electrode materials are becoming more mature. Silicon-based negative electrode materials include a core and a coating layer on its surface, but the coating effect of the coating layer of existing silicon-based negative electrode materials is poor. In the process of preparing silicon-based negative electrode materials into lithium-ion batteries, the dissolved silicon material will come into contact with the electrolyte, resulting in the problem of gas production.
[0053] In a first aspect, the present application provides a negative electrode material, the negative electrode material comprising a core and a coating layer located on the surface of the core, the core comprising a silicon material; the total pore volume of the negative electrode material is ≤0.02cm 3 / g, and the density of the coating layer β≥80%;
[0054] The density β of the coating layer is measured by the following test method: m1 g of negative electrode material is immersed in a 20% HF solution for 1 hour, then washed and dried, and the mass of the negative electrode material after washing and drying is weighed as m2. The density of the coating layer is calculated as β=m2 / m1×100%.
[0055] In the above scheme, the surface of the negative electrode material has a high-density coating layer, which can reduce the dissolution of the negative electrode material during the cycle, thereby reducing the reaction of the dissolved silicon material with the electrolyte, effectively reducing the gas production value of the negative electrode material; and controlling the total pore volume of the negative electrode material within the above range can effectively reduce the direct penetration of the electrolyte into the particles of the negative electrode material through the pore structure, reduce the side reactions occurring when the electrolyte contacts the silicon material, and improve the cycle performance of the lithium-ion battery.
[0056] In some embodiments, the negative electrode material has at least one of the following characteristics: (1) The core includes a carbon matrix with pores and a silicon material deposited in the pore structure of the carbon matrix. It can be understood that the components of the core include a carbon matrix, which can play a role in supporting the skeleton and has good electrical conductivity, which can improve the electrical conductivity of the negative electrode material; at the same time, nano-scale silicon material can be deposited inside the carbon matrix to reduce the contact between the silicon material and the electrolyte, ensure the stability of the SEI film, and improve the first coulomb efficiency; and the carbon matrix with pores can effectively alleviate the volume expansion of the silicon material during the cycle and improve the cycle performance.
[0057] (2) The inner core includes a carbon matrix with pores and a silicon material located in the pores of the carbon matrix. The area ratio of pores with a pore size greater than 50 nm in any cross section of the negative electrode material is α, satisfying: α≤10%; wherein α is obtained by the following test method: in a diagram of a single negative electrode material particle shown by SEM section processing, select any A×B area, wherein A=1μm~10μm, B=1μm~10μm, the sum of the cross-sectional areas of pores with a pore size greater than 50 nm in the cross section of a single negative electrode material particle in the region is denoted as S0, the cross-sectional area of a single negative electrode material particle in the region is denoted as S, the area ratio of pores with a pore size greater than 50 nm in the cross section of a single negative electrode material particle is defined as α', α'=S0 / S, α is the arithmetic mean of the α' values of at least 10 negative electrode material particles.
[0058] In the above scheme, the area ratio of pores with a pore size greater than 50 nm in any cross section of the negative electrode material of the present application is α, and α≤10%. It can be understood that pores with a pore size greater than 50 nm are macropores, that is, α represents the area ratio of macropores in the cross section of the negative electrode material. The area ratio of macropores in the cross section of the negative electrode material of the present application is relatively small. On the one hand, macropores with a relatively small area ratio can effectively reduce the specific surface area of the core, and during the first charge and discharge process, can reduce the occurrence of side reactions between the negative electrode material and the electrolyte, reduce gas production, and improve the first efficiency, expansion performance and cycle performance of the negative electrode material. On the other hand, macropores with a relatively small area ratio can improve the tap density and compaction density of the negative electrode material, reduce the problems of breakage and cracks in the process of rolling the negative electrode material into a pole piece, and improve the processing performance of the negative electrode material. Moreover, the relatively small area ratio of macropores in the cross section of the negative electrode material indicates that the porosity of the negative electrode material is low, and the carbon content in the negative electrode material with a low porosity is high, so that the negative electrode material has good electronic conductivity, provides a developed conductive network for the negative electrode material, and improves the conductivity of the negative electrode material. The negative electrode material of the present application can effectively improve the conductivity, capacity, initial efficiency, cycle performance and processing performance of the negative electrode material by controlling the area ratio of the macropores in the cross section of the negative electrode material.
[0059] In the present application, α can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%, etc., and of course it can also be other values within the above range, which is not limited in the present application. Within the above-mentioned limited range, it indicates that the number of macropores in the cross section of the negative electrode material of the present application is small or the pore size of the macropores is small, which is beneficial to improve the compaction density of the negative electrode material, reduce the specific surface area, and improve the structural stability of the negative electrode material, so that the negative electrode material is not easy to break during processing, thereby improving the processing performance and cycle performance of the negative electrode material. If α is greater than 10%, the pore size of the macropores in the cross section of the negative electrode material is too large or the number of macropores is too large. During the first charge and discharge process, the electrolyte is easy to penetrate into the negative electrode material particles, resulting in an increase in side reactions between the negative electrode material and the electrolyte. Moreover, the macropores are the locations where stress is concentrated inside the negative electrode material. The pore size of the macropores is too large or the number of macropores is too large, which makes the negative electrode material particles prone to rupture, pulverization and other problems during the lithium extraction / insertion process, resulting in rapid decay of the cycle performance of the negative electrode material.
[0060] The core particles were subjected to SEM section processing, and the area of a single negative electrode material particle and the area of all pores were counted and calculated using the AztecFeature software of the SEM electron microscope OXFORD Instruments. Specifically:
[0061] (1) Electron microscope and energy spectrum conditions
[0062] Electron microscope: Select a target particle area that is as monodisperse as possible and adjust appropriate parameters (acceleration voltage 20 kV or 15 kV, electron beam rotation 0 degrees) to obtain a clear backscattered field of view.
[0063] Energy spectrum: When testing, open the AZtec Feature software and execute probe cooling. When the blue indicator light of the energy spectrum probe is on, start the test.
[0064] (2) Testing process
[0065] Provide a reference standard matrix of the negative electrode material of the present application, first move the field of view to the reference standard matrix, adjust the brightness contrast, obtain the image grayscale of the reference standard matrix, and ensure that the grayscale of the negative electrode material particles of the present application and the reference standard matrix are separated. Note: After the reference image grayscale is adjusted, the brightness contrast of the electron microscope cannot be adjusted.
[0066] Move the field of view to the monodisperse negative electrode material particles, collect BSE electron images, adjust and set the appropriate threshold range, so that the field of view has typical characteristic particles, moderate size and grayscale, and the particle marking is optimized under the field of view. (Particles can be selected at the time through threshold filtering, multiple-image resolution filtering, pixel filtering and secondary image filtering)
[0067] Set the negative electrode material particle detection method, filtering conditions and acquisition time, etc. Select the pores with a pore size greater than 50nm as the filtering conditions. After the settings are completed, click Detect Negative Electrode Material Particles to obtain the negative electrode material particle list information that meets the conditions on the right side of the software (for example: number of pores, element list and content, etc.).
[0068] After the AZtec Feature is finished running, the user can check all detected features in this interface, and can reposition the specified features and re-collect images and spectra. After highlighting the feature of interest (i.e., the pores with a pore size greater than 50nm in this application), select any A×B area, where A=1μm~10μm, B=1μm~10μm, and illustratively, calculate the cross-sectional area of pores with a pore size greater than 50nm in any 10μm×10μm area. During the calculation process, the pores with a pore size greater than 50nm are regarded as the closest regular morphology based on their morphology. For example, the morphology of pores with a pore size greater than 50nm can be regarded as spheres, rectangles, ellipses, etc. that are close to their shapes. The cross-sectional area of pores with a pore size greater than 50nm is calculated according to the area calculation formula of the above regular morphology, and the cross-sectional areas of all pores with a pore size greater than 50nm in the 10μm×10μm area are added to obtain S0, and S is 10×10=100μm 2, S0 is divided by S to obtain the area ratio α' of pores with a pore diameter greater than 50 nm in the cross section of a single negative electrode material particle, and then the arithmetic mean of the α' values of at least 10 negative electrode material particles is calculated, which is α.
[0069] In some embodiments, the carbon matrix includes at least one of artificial graphite, natural graphite, amorphous carbon, activated carbon, activated carbon fiber, carbon black, capacitor carbon, carbon molecular sieve, mesophase carbon microbeads, carbon nanotubes, carbon nanofibers, porous carbon and graphene, and the silicon material includes at least one of crystalline silicon, silicon oxide, amorphous silicon, silicon alloy, silicate, crystalline and amorphous silicon composite particles. The types of carbon matrix and silicon material can be selected according to actual needs, and are not limited here. It can be understood that the carbon matrix selects the above materials, which can all play the role of supporting the skeleton, and also has good electrical conductivity to ensure the electrical conductivity of the negative electrode material, and the silicon material is deposited inside the carbon matrix, which has an excellent lithium storage effect.
[0070] Among them, silicon oxide SiO x , wherein 0<x≤2, silicon oxide is a silicon-oxygen composite, comprising oxygen atoms and silicon atoms, and the molar ratio of oxygen atoms to silicon atoms is 0 to 2 and does not include 0. It can be Si, SiO 0.2 、SiO 0.5 、SiO 0.8 、SiO、SiO 1.2 、SiO 1.5 、SiO 1.8 Or SiO2, etc., a compound of two or more, or a substance with the chemical formula SiO x The silicon alloy may be a silicon-lithium alloy, a silicon-magnesium alloy, etc. Of course, it should be noted that in some cases, the silicon alloy includes single silicon particles and alloys.
[0071] In some embodiments, the average particle size of the silicon material is 0.1nm to 500nm. Optionally, the average particle size of the silicon material can be specifically 0.1nm, 1nm, 100nm, 200nm, 300nm, 400nm and 500nm, etc., or other values within the range, which can be selected according to actual needs and are not limited here. The mechanical stress during silicon material expansion decreases as the particle size decreases, and the electron and ion transmission paths can be shortened after the size is reduced. At the same time, the size of the silicon material decreases, and the gap between adjacent silicon materials increases, which can reserve space for expansion. It can be understood that the average particle size of the silicon material is within the above range, which can ensure the battery capacity of the lithium-ion battery and reduce the irreversible capacity loss. Preferably, the average particle size of the silicon material is 0.1nm to 50nm, and more preferably, the average particle size of the silicon material is 0.1nm to 5nm or 1nm to 500nm.
[0072] In some embodiments, the morphology of the silicon material includes at least one of a dot shape, a sphere, an ellipsoid shape, and a flake shape. The morphology of the silicon material can be selected according to actual needs and is not limited here.
[0073] In some embodiments, the purity of the silicon material is greater than 99%. It can be understood that high-purity silicon material is conducive to Li-Si alloying with lithium, thereby improving the cycle performance of lithium-ion batteries.
[0074] In some embodiments, the pore volume of the negative electrode material is less than or equal to 0.1 cm 3 / g. Specifically, it can be 0.01cm 3 / g, 0.03cm 3 / g, 0.05cm 3 / g, 0.07cm 3 / g, 0.09cm 3 / g or 0.1cm 3 / g, etc., and of course, it can also be other values within the above range, and this application is not limited here. Within the above-defined range, it indicates that the number of macropores in the negative electrode material is small or the pore size is small, which is conducive to improving the compaction density of the negative electrode material and then improving the structural stability of the negative electrode material, making it less likely for the negative electrode material to break during processing, thereby improving the processing performance and cycle performance of the negative electrode material.
[0075] In some embodiments, the area ratio of pores with a pore size greater than or equal to 500 nm in the cross section of the negative electrode material is less than or equal to 5%. Specifically, it can be 0.1%, 0.5%, 1%, 2%, 3%, 4% or 5%, etc., and of course it can also be other values within the above range, which is not limited in this application. Within the above-mentioned limited range, it shows that the number of macropores with larger pore sizes in the negative electrode material of the present application is small, which is beneficial to improve the compaction density of the negative electrode material, improve the structural stability of the negative electrode material, and thus improve the processing performance and cycle performance of the negative electrode material. It can be understood that the area ratio of pores with a pore size greater than or equal to 500 nm in the cross section of the negative electrode material is calculated in a similar manner to the area ratio of pores with a pore size greater than 50 nm in the negative electrode material.
[0076] In some embodiments, the average particle size of the carbon matrix is less than or equal to 15 μm, and can be 1 μm, 3 μm, 5 μm, 7 μm, 10 μm, 12 μm or 15 μm, etc., and can also be other values within the above range, which is not limited in the present application.
[0077] In some embodiments, the mass percentage of silicon in the negative electrode material is 40% to 80%, which can be 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%, etc., and can also be other values within the above range, which are not limited in this application.
[0078] In some embodiments, the mass percentage of carbon in the negative electrode material is 20% to 60%, which can be 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55% or 60%, etc., and can also be other values within the above range, which are not limited in this application.
[0079] The coating layer can, on the one hand, reduce the side reactions caused by the electrolyte entering the negative electrode material, thereby improving the initial efficiency and capacity of the negative electrode material. On the other hand, the coating layer can cooperate with the carbon matrix to alleviate the volume expansion of the active material, reduce the volume expansion of the entire negative electrode material, and reduce the swelling of the negative electrode material when prepared as a pole piece.
[0080] In some embodiments, the material of the coating layer includes at least one of a carbon material, a metal oxide, amorphous silicon, a conductive polymer, a fluoride, a phosphate and a nitride. Among them, the carbon material includes at least one of graphene, soft carbon, hard carbon, a conductive polymer and amorphous carbon, the material of the metal oxide layer includes at least one of Sn, Ge, Fe, Si, Cu, Ti, Na, Mg, Al, Li, Co, V, Ca and Zn oxides, the conductive polymer includes at least one of polyaniline, polyacetylene, polypyrrole, polythiophene, poly3-hexylthiophene, polyphenylene, polypyridine and polyvinylene, the fluoride includes vinyl fluoride, fluoropolymer, sodium fluoride, potassium fluoride, fluorocarbon polymer, fluorosilicone polymer, hexafluorobutyl acrylate, polytetrafluoroethylene (PTFE), fluoro The invention relates to a poly(ethylene-propylene) copolymer (FEP), a perfluoroalkoxy resin (PFA), a polychlorotrifluoroethylene (PCTFE), an ethylene-chlorotrifluoroethylene copolymer (ECTFE), a polyvinylidene fluoride (PVDF) and a polyvinyl fluoride. The phosphate comprises at least one of magnesium phosphate, calcium phosphate, aluminum phosphate, titanium phosphate, chromium phosphate, cobalt phosphate, nickel phosphate, germanium phosphate, zirconium phosphate, niobium phosphate, molybdenum phosphate, tantalum phosphate, tungsten phosphate and lanthanum phosphate. The nitride comprises at least one of titanium nitride, silicon nitride, vanadium nitride, cobalt nitride, nickel nitride and carbon nitride. The material of the coating layer can be selected according to actual needs and is not limited here.
[0081] Furthermore, the coating layer can be a single-layer coating layer formed by the above-mentioned single material, or a coating layer formed by a combination of the above-mentioned multiple materials, or a single material forming a multi-layer coating layer, or a multi-layer coating layer formed by multiple materials, etc. For example, it can be carbon coating followed by polymer coating, or carbon coating followed by polymer coating, or polymer coating followed by oxide coating, etc. The layer structure of the coating layer can be selected according to actual needs, and is not limited here. It can be understood that when the coating layer is a multi-layer coating structure, the density is higher.
[0082] In some embodiments, the thickness of the coating layer is 0.1nm to 3000nm, preferably 1nm to 300nm. Optionally, the thickness of the coating layer can be 0.1nm, 1nm, 50nm, 100nm, 150nm, 200nm, 250nm, 300nm, 500nm, 1000nm, 2000nm or 3000nm, etc., or other values within the range, which can be selected according to actual needs and are not limited here. It can be understood that the coating layer can reduce the solubility of the negative electrode material, thereby reducing the gas production of the dissolved silicon material reacting with the electrolyte. Controlling the thickness of the coating layer within the above range is beneficial to the negative electrode material to maintain the stability of the particle structure during the cycle, reduce the dissolution of the silicon material, and is beneficial to improve the transmission efficiency of lithium ions and enhance the charge and discharge performance of the negative electrode material. Preferably, the thickness of the coating layer is 1nm to 50nm, and more preferably, the thickness of the coating layer is 1nm to 30nm.
[0083] In some embodiments, the mass proportion of the coating layer in the negative electrode material is ≤10%. It can be understood that the coating layer can reduce the solubility of the negative electrode material, thereby reducing the gas production of the dissolved silicon material reacting with the electrolyte. The mass proportion of the coating layer in the negative electrode material is within the above range, which can ensure the amount of lithium that can be embedded in the negative electrode material, thereby ensuring the charge and discharge capacity of the lithium-ion battery prepared from the negative electrode material.
[0084] In some embodiments, the median particle size of the negative electrode material composed of the core and coating layer of the above composition and parameters is ≤15μm, preferably ≤10μm. It can be understood that the median particle size refers to the particle size of the negative electrode material in the middle position after the particles of the negative electrode material are sorted by size. The median particle size of the negative electrode material is within the above range, which can ensure the time for lithium ion insertion and detachment, so that the negative electrode material can achieve a state of rapid and sufficient lithium insertion, thereby ensuring the charge and discharge performance of the lithium ion battery. For example, it can be 1μm, 5μm, 8μm, 10μm, 12μm or 15μm, etc., of course, it can also be other values within the above range, and this application is not limited here. Controlling the average particle size of the negative electrode material within the above range is beneficial to improving the cycle performance of the negative electrode material.
[0085] The specific surface area of the negative electrode material is ≤5m 2 / g, specifically 0.1m 2 / g, 0.5m 2 / g, 1m 2 / g, 2m 2 / g, 3m 2 / g, 4m 2 / g or 5m 2 / g, etc., of course, it can also be other values within the above range, and this application is not limited here. Controlling the specific surface area of the negative electrode material within the above range can suppress the volume expansion of the negative electrode material, which is beneficial to improving the cycle performance of the negative electrode material. It can be understood that the specific surface area of the negative electrode material will affect the contact area between the negative electrode material and the electrolyte. The specific surface area of the negative electrode material within the above range can reduce the amount of lithium ions consumed by the SEI film formed during the initial charge and discharge process of the lithium-ion battery, and reduce the irreversible capacity loss of the lithium-ion battery.
[0086] In some embodiments, the density test of the negative electrode material of the present application can be performed, and the test principle is: after the negative electrode material is placed in the dissolving solution, under ideal conditions, if the density of the coating layer is 100%, the negative electrode material will not dissolve due to the isolation effect of the coating layer, and then no dissolved silicon material will come into contact with the dissolving solution and react. However, the conventionally prepared coating layer is in a non-ideal state, so that the negative electrode material will have a certain amount of dissolution in the dissolving solution, so that the dissolving solution contains dissolved silicon material. At this time, the density β of the coating layer can be measured by the following test method: a negative electrode material with a mass of m1 g is immersed in a HF dissolving solution with a mass fraction of 20%, and the immersion time is 1h, then washed and dried, and the mass of the negative electrode material after washing and drying is weighed as m2, and the density of the coating layer is calculated to be β = m2 / m1×100%.
[0087] It should be noted that the dissolving liquid used in the present application is a hydrofluoric acid solution, and the type of dissolving liquid can be selected according to actual needs and is not limited here.
[0088] Through the above tests, it can be obtained that the density β of the coating layer of the negative electrode material of the present application is ≥80%. Within this range, the coating layer can reduce the dissolution amount of the negative electrode material during the cycle, thereby reducing the reaction of the dissolved silicon material with the electrolyte, and effectively reducing the gas production value of the negative electrode material.
[0089] In addition, during the coating process, the materials used to prepare the coating layer will further fill the voids in the core, reducing the total pore volume of the negative electrode material to ≤ 0.02 cm 3 / g. Within this range, the amount of electrolyte that directly penetrates into the particles of the negative electrode material through the pore structure can be effectively reduced, thereby reducing the side reactions occurring when the electrolyte contacts the silicon material and improving the cycle performance of the lithium-ion battery.
[0090] In a second aspect, the present application further provides a negative electrode plate, which includes a negative electrode current collector and a negative electrode active material distributed on one side of the negative electrode current collector, and the negative electrode active material includes the above-mentioned negative electrode material.
[0091] In some embodiments, the critical withstand pressure P of the negative electrode sheet is greater than or equal to 100MPa, and can be specifically 100MPa, 120MPa, 150MPa, 200MPa, 250MPa, 300MPa, 350MPa, 400MPa, 500MPa, 600MPa, etc., and of course it can also be other values within the above range, and the present application is not limited here. Within the above range, the critical withstand pressure P of the negative electrode material of the present application is relatively large, indicating that the negative electrode sheet of the present application has excellent withstand pressure capability, which is beneficial to improving the processing performance of the negative electrode sheet. It can be understood that the critical withstand pressure refers to the pressure when the negative electrode sheet is in a critical state, that is, the maximum pressure at which the negative electrode material particles in the negative electrode sheet do not break. The critical withstand pressure of the negative electrode sheet is obtained by the following test method: the thickness of the negative electrode sheet is 60μm to 70μm, and the cross section of a single negative electrode sheet is observed using an electron scanning microscope SEM, and the minimum pressure corresponding to the breakage of the negative electrode material particles is P.
[0092] In some embodiments, the compaction density of the negative electrode sheet is 1.3 g / cm 3 ~1.9g / cm 3 , specifically 1.3 g / cm 3 , 1.4g / cm 3 , 1.5g / cm 3 , 1.6g / cm 3 , 1.7g / cm 3 , 1.8g / cm 3 or 1.9 g / cm 3 Of course, it can also be other values within the above range, and this application does not limit it. Within the above limited range, the compaction density of the negative electrode plate of this application is relatively large, and the pore size inside the negative electrode plate is relatively small, which is conducive to improving the capacity, initial efficiency and cycle performance of the negative electrode plate.
[0093] In a third aspect, the present application provides a battery, which comprises the above-mentioned negative electrode material.
[0094] In a fourth aspect, the present application provides a method for preparing a negative electrode material, comprising the following steps:
[0095] Step S10, preparing a composite, the composite comprising a core;
[0096] Step S20, forming a coating layer on the surface of the composite to obtain a negative electrode material; wherein the total pore volume of the negative electrode material is ≤0.02cm 3 / g, and the density of the coating layer β≥80%.
[0097] In the above scheme, a catalyst is added when the inner core is prepared. In the process of forming the coating layer, the catalyst prompts the coating material to form a high-density coating layer on the surface of the inner core, thereby solving the problem that when the coating layer is prepared by vapor deposition in the prior art, a high cracking temperature is used to ensure complete cracking of the gas source, resulting in the consumption of highly active silicon materials by the reaction with the carbon matrix, thereby ensuring the charge and discharge capacity of the lithium-ion battery.
[0098] In the prior art, the gas sources commonly used in gas phase coating, such as methane and acetylene, require relatively high temperatures (methane>1000°C, acetylene>800°C) to be completely cracked to form a relatively dense coating layer. However, at high temperatures, due to the high activity of the deposited silicon material, SiC is usually generated. Therefore, gas phase coating is currently usually carried out at a relatively low temperature (500°C~800°C). However, at a temperature of 500°C~800°C, the gas source precursor is not fully cracked, the carbon coating layer formed on the surface of the particles is not dense, and there are a large number of incomplete cracking products, resulting in the gas production problem cannot be completely solved.
[0099] The preparation method of the present application is described in detail below with reference to the examples:
[0100] Method 1: In step S10, the specific steps of preparing the composite include: soaking the carbon matrix in a solution containing a catalyst, and depositing silicon material on the product after solid-liquid separation to obtain a core.
[0101] Method 2: In step S10, the specific steps of preparing the composite include:
[0102] Step S100, pre-treating the porous carbonaceous raw material to obtain a carbon matrix, the pre-treating of the porous carbonaceous raw material includes the following steps: pressurizing the porous carbonaceous raw material, the pressure of the pressurization treatment is greater than or equal to 100MPa; or immersing the porous carbonaceous raw material in a treatment solution under a vacuum pressure of 0.1Pa to 500Pa, the treatment solution includes an organic compound with a molecular weight greater than 10000. Step S200, immersing the carbon matrix in a solution containing a catalyst, depositing silicon material on the product after solid-liquid separation, to obtain a core; or
[0103] Step S100, pre-treating the porous carbonaceous raw material to obtain a carbon matrix, the pre-treating of the porous carbonaceous raw material includes the following steps: pressurizing the porous carbonaceous raw material, the pressure of the pressurization treatment is greater than or equal to 100MPa; or immersing the porous carbonaceous raw material in a treatment solution under a vacuum pressure of 0.1Pa to 500Pa, the treatment solution includes an organic compound with a molecular weight greater than 10000. Step S200, immersing the carbon matrix in a solution containing a catalyst, and vapor-depositing the product after solid-liquid separation using a vapor-phase active substance precursor to obtain a core.
[0104] In the above-mentioned method 2, the present application obtains the carbon matrix by pretreating the porous carbonaceous raw material. The pretreatment can be a pressurized treatment or an impregnation treatment of the porous carbonaceous raw material with a treatment solution. The pressurized treatment causes the pores with larger pore sizes in the porous carbonaceous raw material to preferentially crack or be directly crushed, and the micropores and mesopores with smaller pore sizes can be retained during the pressurized treatment, thereby reducing the number of macropores in the carbon matrix. The porous carbon raw material is impregnated with a treatment solution, which includes an organic compound with a molecular weight greater than 10,000. During the impregnation process, due to the effect of capillaries, it is difficult for the molecules of the treatment solution to enter the micropores, and they are mainly filled into the mesopores and macropores of the porous carbon raw material. The organic compound with a molecular weight greater than 10,000 can be preferentially filled into the macropores of the porous carbon raw material, so that the macropores are transformed into macropores, mesopores or micropores with smaller pore sizes, which is beneficial to increase the number of micropores and mesopores in the carbon matrix, while reducing the number and volume proportion of macropores in the carbon material, and reducing the porosity of the carbon matrix. The carbon matrix is then immersed in a solution containing a catalyst, and silicon material is deposited on the product after solid-liquid separation, or vapor deposition is performed on the product after solid-liquid separation using a vapor-phase active substance precursor.
[0105] On the one hand, the number and volume proportion of large pores are small, which makes the deposition uniformity of the gas-phase active substance precursor in the porous carbon matrix good, and the active substance generated by the gas-phase active substance precursor is not easy to agglomerate when deposited in the porous carbon matrix, which can reduce the volume expansion of the negative electrode material; on the other hand, the active substance generated by the gas-phase active substance precursor is filled in the carbon matrix, which further reduces the number and volume proportion of large pores in the inner core, so that the area proportion of pores with a pore diameter greater than 50nm in the cross section of the negative electrode material is α≤10%, which is beneficial to improve the tap density of the negative electrode material, and then improve the compaction performance of the negative electrode material, reduce the problems of breakage and cracking of the negative electrode material during the rolling process, and improve the capacity, first efficiency, cycle performance and processing performance of the negative electrode material.
[0106] In some embodiments, the carbon matrix used in the above preparation method includes at least one of artificial graphite, natural graphite, amorphous carbon, activated carbon, mesophase carbon microbeads, carbon nanotubes, carbon nanofibers, porous carbon and graphene. It can be understood that the carbon matrix selected from the above materials can all play the role of supporting the skeleton and have good electrical conductivity to ensure the electrical conductivity of the negative electrode material.
[0107] In some embodiments, the prepared carbon matrix is soaked in a catalyst solution so that the catalyst adheres to the surface or interior of the carbon matrix. The catalyst solution is a salt solution containing at least one of Cu, Ni, Co, Fe and B. It can be understood that the catalyst contains the above elements, which can reduce the temperature during the coating process and achieve a dense coating layer at a lower temperature.
[0108] In some embodiments, the concentration of the solution containing the catalyst is 0.1mol / L to 12mol / L. Optionally, the concentration can be 0.1mol / L, 0.5mol / L, 1.2mol / L, 2.5mol / L, 3.4mol / L, 5.0mol / L, 8.8mol / L and 10.9mol / L, etc., or other values within the range. It can be selected according to actual needs and is not limited here. It can be understood that the concentration of the catalyst within the above range is conducive to the formation of a high-density coating layer.
[0109] In some embodiments, the soaking time is 10 min to 600 min. Optionally, the soaking time can be 10 min, 50 min, 180 min, 240 min, 400 min, 520 min, 600 min, etc., or other values within the range. It can be selected according to actual needs and is not limited here. It can be understood that the soaking time within the above range can increase the amount of catalyst adhesion, thereby facilitating the formation of a high-density coating layer.
[0110] In some embodiments, the silicon material includes at least one of crystalline silicon, silicon oxide, amorphous silicon, silicon alloy, and composite particles of crystalline and amorphous silicon. The type of silicon material can be selected according to actual needs and is not limited here.
[0111] In some embodiments, the average particle size of the silicon material is 0.1nm to 500nm. Optionally, the average particle size of the silicon material can be specifically 0.1nm, 100nm, 200nm, 300nm, 400nm and 500nm, etc., or other values within the range, which can be selected according to actual needs and are not limited here. The mechanical stress of the silicon material during expansion decreases as the particle size decreases, and the electron and ion transmission paths can be shortened after the size is reduced. At the same time, the size of the silicon material decreases, and the gap between adjacent silicon materials increases, which can reserve space for expansion. It can be understood that the average particle size of the silicon material is within the above range, which can ensure the battery capacity of the lithium-ion battery and reduce the irreversible capacity loss. Preferably, the average particle size of the silicon material is 0.1nm to 50nm, and more preferably, the average particle size of the silicon material is 0.1nm to 5nm.
[0112] In some embodiments, the morphology of the silicon material includes at least one of a dot shape, a sphere, an ellipsoid shape, and a flake shape. The morphology of the silicon material can be selected according to actual needs and is not limited here.
[0113] In some embodiments, the purity of the silicon material is greater than 99%. It can be understood that high-purity silicon material is conducive to Li-Si alloying with lithium, thereby improving the cycle performance of lithium-ion batteries.
[0114] In some embodiments, the deposition method of the silicon material may be vapor deposition or liquid deposition. The deposition method of the silicon material may be selected according to actual needs and is not limited herein.
[0115] Preferably, the silicon material is deposited by vapor phase chemical deposition, and the steps include: introducing a silicon-containing gas source and a carbon matrix to carry out a vapor phase chemical deposition reaction.
[0116] In some embodiments, the silicon-containing gas source includes at least one of monosilane, disilane, trisilane and tetrasilane, which can be selected according to actual needs and is not limited here.
[0117] In some embodiments, the concentration of the silicon-containing gas source is 1% to 80%. Optionally, the concentration of the silicon-containing gas source can be 1%, 13%, 26%, 43%, 55%, 68%, 80%, etc., or other values within the range. It can be selected according to actual needs and is not limited here.
[0118] In some embodiments, the temperature of the vapor phase chemical deposition reaction is 300°C to 800°C, and the holding time is 1h to 15h. Optionally, the temperature can be 300°C, 420°C, 500°C, 600°C, 700°C, 750°C, and 800°C, and the time can be 1h, 3h, 4h, 6h, 7h, 8h, 10h, 12h, and 15h, or other values within the range, which can be selected according to actual needs and are not limited here.
[0119] When the specific steps of preparing the composite in method 2 include the following steps: step S100, pre-treating the porous carbonaceous raw material to obtain a carbon matrix, the pre-treating of the porous carbonaceous raw material includes the following steps: pressurizing the porous carbonaceous raw material, the pressure of the pressurization treatment is greater than or equal to 100MPa; or under the condition of a vacuum pressure of 0.1Pa to 500Pa, immersing the porous carbonaceous raw material in a treatment solution, the treatment solution includes an organic compound with a molecular weight greater than 10,000. Step S200, immersing the carbon matrix in a solution containing a catalyst, and using a gas phase active substance precursor to vapor-deposit the product after solid-liquid separation to obtain a core. Wherein:
[0120] Step S100: pretreating the porous carbonaceous raw material to obtain a carbon matrix.
[0121] In some embodiments, step S100 includes: subjecting the porous carbonaceous raw material to a pressure treatment to obtain a carbon matrix, wherein the pressure of the pressure treatment is greater than or equal to 100 MPa.
[0122] In some embodiments, the pressure of the pressure treatment is greater than or equal to 100MPa, and can be specifically 100MPa, 150MPa, 200MPa, 250MPa, 300MPa, 350MPa, 400MPa, 500MPa or 650MPa, etc., and of course, it can also be other values within the above range, and the present application is not limited here. The pressure of the pressure treatment of the present application is relatively large. By pressurizing the porous carbonaceous raw material, the porous carbonaceous raw material will preferentially crack at the macropores, and then rupture, thereby reducing the number of macropores in the porous carbonaceous raw material. Preferably, the pressure of the pressure treatment is greater than or equal to 150MPa. If the pressure of the pressure treatment is less than 100MPa, it cannot be guaranteed that cracks will occur at the macropores in the porous carbonaceous raw material, resulting in a large number of macropores in the porous carbonaceous raw material, which is not conducive to improving the compaction density of the negative electrode material.
[0123] In some embodiments, the time of pressurization treatment is 0.5h to 10h, specifically 0.5h, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h or 10h, etc., and of course, it can also be other values within the above range, which is not limited in this application.
[0124] In some embodiments, the pressurizing equipment includes at least one of a cold rolling mill and a die press.
[0125] In some embodiments, after the pressure treatment, the step of crushing and screening the material obtained by the pressure treatment is further included. During the crushing process, part of the porous carbonaceous raw material is easily broken from the macropores where cracks are generated, further reducing the number of macropores in the carbon matrix.
[0126] In some embodiments, the mesh size of the screening is 10 to 500 mesh, specifically 10 mesh, 50 mesh, 100 mesh, 200 mesh, 300 mesh, 400 mesh or 500 mesh, etc. Of course, it can also be other values within the above range, and this application is not limited here.
[0127] In some embodiments, step S100 includes: under a vacuum pressure of 0.1 Pa to 500 Pa, immersing the porous carbonaceous raw material in a treatment solution to obtain a carbon matrix, wherein the treatment solution includes an organic compound with a molecular weight greater than 10,000.
[0128] In some embodiments, the vacuum pressure is 0.1Pa to 500Pa, and can be specifically 0.1Pa, 1Pa, 10Pa, 50Pa, 100Pa, 200Pa, 300Pa, 400Pa or 500Pa, etc., and of course, it can also be other values within the above range, and the present application is not limited here. Within the above range, the pressure on the surface of the porous carbonaceous raw material is less than the pressure of the treatment solution, and the treatment solution can be infiltrated into the porous carbonaceous raw material, so that the treatment solution enters the interior of the porous carbonaceous raw material through the pores or defects of the porous carbonaceous raw material, thereby serving the purpose of filling the macropores in the porous carbonaceous raw material, reducing the number or pore size of the macropores, and improving the compaction density of the negative electrode material. If the vacuum pressure is greater than 500Pa, it is easy to cause cracks in some mesopores and micropores, so that the porosity of the negative electrode material is too low, which is not conducive to the deposition of active substances. If the vacuum pressure is less than 0.1Pa, it is not guaranteed that cracks will occur at the macropores in the porous carbonaceous raw material, resulting in a large number of macropores in the porous carbonaceous raw material, which is not conducive to improving the compaction density of the negative electrode material.
[0129] In some embodiments, the treatment solution includes a solute and a solvent, and the solute includes an organic compound with a molecular weight greater than 10,000. Exemplarily, the solute includes at least one of a protein, a nucleic acid, a vinyl polymer, and a monomer cross-linked polymer. The monomer cross-linked polymer may be, for example, polyurethane, polyimide, polyacrylic acid, poly-N-methylpyrrolidone, polyamine, and polyvinyl alcohol. The protein is a macromolecular protein, such as soy protein and collagen. The main components of soy protein include 11S globulin and 7S globulin, the molecular weight of 11S globulin is 340kDa, and the molecular weight of 7S globulin is 440kDa. Polysaccharides may be, for example, starch and cellulose. The particle size of the solute molecules in the above-mentioned treatment solution is relatively large, which is conducive to preferentially filling the macropores during the impregnation treatment process, so that the pore size of the macropores is reduced, and the pore size of the micropores is too small, so that the treatment solution is difficult to enter the micropores due to capillary action, so that the number of macropores in the porous carbonaceous raw material is greatly reduced, and the number of micropores and mesopores is increased.
[0130] In some embodiments, the solvent includes water and an organic solvent, and the organic solvent includes at least one of an alcohol solvent, an ether solvent, an aliphatic hydrocarbon solvent, a ketone solvent, and dimethyl sulfoxide. Of course, it can also be other types of solvents, which are not limited in this application.
[0131] In some embodiments, the treatment solution includes a vinyl polymer grafted with a polyether polyol. The vinyl polymer may be, for example, polyethylene, polyvinyl chloride, and the like.
[0132] In some embodiments, the particle size of the solute is greater than or equal to 0.5 nm, specifically 0.5 nm, 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 8 nm, 10 nm or 15 nm, etc., and of course, other values within the above range can also be used, and the present application does not limit this. It can be understood that the particle size of the solute particles in the treatment solution refers to the equivalent volume diameter, that is, the diameter of a sphere with the same volume as the actual particle of the solute particles in the treatment solution, for example, the particle size of the solute can be measured by a BI-90Plus laser particle size analyzer / Zeta potential analyzer using the DLS (dynamic light scattering) principle.
[0133] In some embodiments, the concentration of the treatment solution is 1 mol / L to 15 mol / L, specifically 1 mol / L, 3 mol / L, 5 mol / L, 7 mol / L, 10 mol / L, 12 mol / L or 15 mol / L, etc., and of course other values within the above range are also possible, and the present application is not limited thereto. Within the above range, it is beneficial for the solute in the treatment solution to enter the pores of the porous carbonaceous raw material, thereby improving the utilization efficiency of the solute.
[0134] In some embodiments, the immersion time is 1 h to 15 h, specifically 1 h, 3 h, 5 h, 7 h, 10 h, 12 h or 15 h, etc., and of course, it can also be other values within the above range, which is not limited in the present application.
[0135] In some embodiments, the impregnation apparatus comprises a vacuum impregnator.
[0136] In some embodiments, after the porous carbonaceous raw material is impregnated in the treatment solution, the method further comprises: drying the impregnated material.
[0137] In some embodiments, the drying temperature is -40°C to 600°C, specifically -40°C, -20°C, -10°C, 0°C, 30°C, 50°C, 100°C, 200°C, 300°C, 400°C, 500°C or 600°C, etc., and of course it can also be other values within the above range, which is not limited in this application.
[0138] In some embodiments, the drying time is 0.5 h to 24 h, specifically 0.5 h, 1 h, 3 h, 5 h, 8 h, 12 h, 16 h, 20 h or 24 h, etc., and of course other values within the above range may also be possible, and this application is not limited thereto.
[0139] In some embodiments, the porous carbonaceous raw material is prepared by the following method: carbonizing a carbon source, and mixing the carbonized material with an activating agent for activation.
[0140] In some embodiments, the carbon source includes at least one of lignin, coconut shell, fruit shell, peanut shell, rice husk, coal-based biomass and resin. Among them, coal-based biomass is a biomass briquette, such as a low-pressure compression product of sawdust, agricultural waste and paper. The resin can be, for example, polyethylene (PE), polypropylene (PP), polyvinyl chloride (PVC) and polystyrene (PS).
[0141] In some embodiments, the carbonization temperature is 600°C to 900°C, specifically 600°C, 650°C, 700°C, 750°C, 800°C, 850°C or 900°C, etc. Of course, it can also be other values within the above range, which is not limited in this application.
[0142] In some embodiments, the carbonization time is 1 h to 20 h, specifically 1 h, 3 h, 5 h, 10 h, 12 h, 15 h, 18 h, 20 h, etc., and of course, it can also be other values within the above range, which is not limited in the present application.
[0143] In some embodiments, the carbonization is performed under a protective gas atmosphere, and the protective gas includes at least one of nitrogen, helium, neon, argon, krypton, and xenon.
[0144] In some embodiments, after obtaining the carbonized material, the method further includes: pickling the carbonized material, wherein the pickling acid is at least one of hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, phosphoric acid, perchloric acid, acetic acid and benzoic acid.
[0145] In some embodiments, the concentration of the pickling solution is 1 mol / L to 10 mol / L, for example, 1 mol / L, 3 mol / L, 5 mol / L, 8 mol / L or 10 mol / L, etc., and of course, it can be other values within the above range, which are not limited here. It can be understood that the purpose of pickling is to remove impurities in the material, and the material obtained by carbonization treatment is pickled and then washed with deionized water to wash the product to near neutrality.
[0146] In some embodiments, the pickling time is 3 h to 8 h, for example, 3 h, 4 h, 5 h, 6 h, 7 h or 8 h, etc., and of course, it can also be other values within the above range, which is not limited here.
[0147] In some embodiments, the activator used in the activation treatment can be a gaseous activator or a solid activator. Exemplarily, the gaseous activator includes at least one of water vapor, oxygen and air, and the solid activator includes an alkaline substance, and the alkaline substance includes at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide and rubidium hydroxide.
[0148] In some embodiments, when the activator is a gaseous activator, it reacts with carbon at high temperature through gaseous water vapor, oxygen and air to generate hydrogen and carbon monoxide, and the carbonized material is etched by this reaction to obtain activated pores.
[0149] In some embodiments, the concentration of the gaseous activator is 3% to 20%, specifically 3%, 5%, 7%, 9%, 10%, 12%, 15%, 18% and 20%, etc., and of course other values within the above range, which are not limited in this application. Within the above-defined range, the amount of the activator added is large, the activation ability is strong, and more and evenly distributed activation pores can be formed in the material obtained by carbonization treatment, which is conducive to the subsequent filling of the active substance in the activation pores.
[0150] It can be understood that when the activating agent is water vapor, the concentration of the water vapor can be regarded as the humidity of the water vapor.
[0151] In some embodiments, when the activator is a solid activator, the mass ratio of the carbonized material to the activator is 1:(0.5-30), specifically 1:0.5, 1:1, 1:5, 1:10, 1:20 and 1:30, etc., and of course other values within the above range, which are not limited here. Within the above-defined range, the amount of activator added is large, the activation ability is strong, and more and evenly distributed activation pores can be formed in the carbonized material, which is conducive to the subsequent filling of active substances in the activation pores.
[0152] In some embodiments, the activation treatment time is 1 h to 20 h, for example, it can be 1 h, 5 h, 8 h, 10 h, 12 h, 15 h, 18 h or 20 h, etc., and of course it can also be other values within the above range, which is not limited in this application.
[0153] In some embodiments, the temperature of the activation treatment is 500°C to 1200°C, specifically 500°C, 600°C, 700°C, 800°C, 900°C, 950°C, 1000°C, 1100°C and 1200°C, etc. Of course, it can also be other values within the above range, and this application is not limited here.
[0154] It is understandable that the porous carbon raw material can also be directly purchased through commercial channels to use as a finished porous carbon product.
[0155] Step S200, immersing the carbon substrate in a solution containing a catalyst, and performing vapor deposition on the product after solid-liquid separation using a vapor-phase active material precursor to obtain a core.
[0156] The present application preferably uses a gas-phase active substance precursor to perform vapor deposition on a carbon matrix. The active substance generated by the gas-phase active substance precursor can fill the macropores of the carbon matrix, further reducing the proportion of macropores in the negative electrode material, increasing the compaction density of the negative electrode material, reducing the specific surface area, and reducing problems such as breakage and cracking of the negative electrode material during the rolling process, thereby improving the processing performance and cycle performance of the negative electrode material. Moreover, the active substance is not easy to agglomerate when deposited in the carbon matrix, which is beneficial to improving the tap density of the negative electrode material, thereby improving the capacity, initial efficiency and cycle performance of the negative electrode material.
[0157] In some embodiments, the gas-phase reactive species precursor includes a gaseous silicon source.
[0158] In some embodiments, the gaseous silicon source includes at least one of monosilane, hexylsilane, and trisilane.
[0159] In some embodiments, the introduction concentration of the gas-phase active substance precursor is 5% to 30%, specifically 5%, 8%, 10%, 12%, 15%, 18%, 20%, 23%, 26%, 28% or 30%, etc., and of course it can also be other values within the above range, which is not limited in this application.
[0160] In some embodiments, the temperature of vapor deposition is 300°C to 800°C, specifically 300°C, 400°C, 500°C, 600°C, 700°C and 800°C, etc. Of course, it can also be other values within the above range, which is not limited in this application.
[0161] In some embodiments, the insulation time of vapor deposition is 2 h to 25 h, specifically 2 h, 5 h, 10 h, 15 h, 20 h, 25 h, etc., and of course other values within the above range may also be possible, and the present application does not limit this.
[0162] In some embodiments, the thickness of the coating layer prepared in step S20 is 1nm to 300nm. Optionally, the thickness of the coating layer can be 1nm, 50nm, 150nm, 200nm, 250nm and 300nm, etc., or other values within the range. It can be selected according to actual needs and is not limited here. It can be understood that the coating layer can reduce the solubility of the negative electrode material, thereby reducing the gas production of the dissolved silicon material reacting with the electrolyte. Controlling the thickness of the coating layer within the above range is beneficial to maintaining the stability of the particle structure of the negative electrode material during the cycle, reducing the dissolution of the silicon material, and is beneficial to improving the transmission efficiency of lithium ions and improving the charge and discharge performance of the negative electrode material. Preferably, the thickness of the coating layer is 1nm to 50nm, and more preferably, the thickness of the coating layer is 1nm to 30nm.
[0163] In some embodiments, the mass proportion of the coating layer in the negative electrode material is ≤10%. It can be understood that the coating layer can reduce the solubility of the negative electrode material, thereby reducing the gas production of the dissolved silicon material reacting with the electrolyte. The mass proportion of the coating layer in the negative electrode material is within the above range, which can ensure the amount of lithium that can be embedded in the negative electrode material, thereby ensuring the charge and discharge capacity of the lithium-ion battery prepared from the negative electrode material.
[0164] In some embodiments, the inner core is coated, comprising: mixing the inner core with a coating material and performing heat treatment, wherein the material of the coating layer comprises at least one of carbon material, metal oxide, amorphous silicon, conductive polymer, fluoride, phosphate and nitride.
[0165] In some embodiments, the material of the coating layer includes a carbon material, and the carbon material includes at least one of crystalline carbon and amorphous carbon.
[0166] In some embodiments, the material of the coating layer includes metal oxide, and the material of the metal oxide layer includes at least one of oxides of Sn, Ge, Fe, Si, Cu, Ti, Na, Mg, Al, Ca and Zn.
[0167] In some embodiments, the material of the coating layer includes a conductive polymer, and the conductive polymer includes at least one of polyaniline, polyacetylene, polypyrrole, polythiophene, poly-3-hexylthiophene, poly(p-phenylene vinylene), polypyridine, and polystyrene vinylene.
[0168] In some embodiments, the material of the coating layer includes a fluoride, and the fluoride includes at least one of vinyl fluoride, fluoropolymer, sodium fluoride, potassium fluoride, fluorocarbon polymer, fluorosilicone polymer, hexafluorobutyl acrylate, polytetrafluoroethylene (PTFE), fluorinated ethylene-propylene copolymer (FEP), perfluoroalkoxy resin (PFA), polychlorotrifluoroethylene (PCTFE), ethylene-chlorotrifluoroethylene copolymer (ECTFE), polyvinylidene fluoride (PVDF) and polyvinyl fluoride.
[0169] In some embodiments, the material of the coating layer includes phosphate, and the phosphate includes at least one of magnesium phosphate, calcium phosphate, aluminum phosphate, titanium phosphate, chromium phosphate, cobalt phosphate, nickel phosphate, germanium phosphate, zirconium phosphate, niobium phosphate, molybdenum phosphate, tantalum phosphate, tungsten phosphate, and lanthanum phosphate.
[0170] In some embodiments, the material of the coating layer includes nitride, and the nitride includes at least one of titanium nitride, vanadium nitride, cobalt nitride, nickel nitride, and carbon nitride.
[0171] In some embodiments, the mass ratio of the core to the coating material is 100:(1-100). Optionally, the mass ratio can be 100:1, 100:10, 100:20, 100:40, 100:60, 100:70 and 100:100, etc., or other values within the range. It can be selected according to actual needs and is not limited here.
[0172] In some embodiments, the temperature of the heat treatment is 300°C to 1100°C, preferably 400°C to 800°C, and the heat preservation time of the heat treatment is 1h to 15h, preferably 2h to 10h. Optionally, the temperature can be 400°C, 500°C, 600°C, and 800°C, etc., and the time can be 1h, 3h, 5h, 6h, 8h, 10h, 11h, 12h, and 15h, etc., or other values within the range. It can be selected according to actual needs and is not limited here. If the temperature of the heat treatment is lower than 300°C, the carbonization of the coating material is incomplete, and a dense coating layer cannot be obtained; if the temperature of the heat treatment is higher than 1100°C, the silicon material in the negative electrode material is crystallized, resulting in poor cycle performance and expansion performance of the negative electrode material.
[0173] In some embodiments, the heat treatment is performed under a protective gas, and the protective gas includes at least one of nitrogen, helium, neon, argon and krypton, which can be selected according to actual needs and are not limited here.
[0174] In the above technical solution, the surface of the negative electrode active material is coated to form a coating layer on the surface of the negative electrode active material, which can prevent the electrolyte from entering the negative electrode material to cause side reactions and reduce the initial coulomb efficiency and specific capacity, and can further solve the large volume expansion of silicon negative electrode materials, improve the conductivity of negative electrode materials, and thus reduce the volume expansion of the entire composite material and reduce the swelling of the electrode sheet. During the coating process, a small amount of coating material will enter the pores of crystalline silicon.
[0175] It should be noted that the coating process of the present application is carried out on the premise of reducing the crystal changes of the silicon-carbon negative electrode material.
[0176] Preferably, in step S20, the inner core is subjected to a carbon coating treatment, and the carbon coating treatment includes at least one of solid phase carbon coating, liquid phase carbon coating and gas phase carbon coating.
[0177] In some embodiments, the carbon coating process is gas-phase carbon coating, and the steps include: heating the inner core, introducing a protective gas and a carbon source gas, and thermally cracking the carbon source gas to obtain a negative electrode material.
[0178] In some embodiments, the carbon source gas is a hydrocarbon.
[0179] In some embodiments, the carbon source gas includes at least one of methane, ethane, propane, butane, ethylene, propylene, acetylene, gaseous benzene, gaseous toluene, gaseous xylene, gaseous methanol, gaseous ethanol, and gaseous acetone.
[0180] In some embodiments, the temperature of thermal cracking is 400°C to 800°C, and the insulation time is 0.5h to 18h. Optionally, the temperature can be 400°C, 500°C, 600°C, 700°C and 800°C, etc., and the insulation time can be 0.5h, 1.5h, 3h, 5h, 6h, 7h, 8h, 10h and 18h, etc., or other values within the range. It can be selected according to actual needs and is not limited here.
[0181] In some embodiments, the volume ratio of the carbon source gas and the protective gas is 1:(0.1-20). Optionally, the volume ratio can be 1:0.1, 1:1, 1:2, 1:5, 1:10, 1:15 and 1:20, etc., or other values within the range. It can be selected according to actual needs and is not limited here.
[0182] In some embodiments, the carbon coating process is solid-phase carbon coating, and the steps include: carbonizing a mixture obtained by mixing the core with a solid-phase carbon source to obtain a negative electrode material.
[0183] In some embodiments, the temperature of the carbonization treatment is 400° C. to 800° C., and the time of the carbonization treatment is 1 h to 15 h. Optionally, the temperature may be 400° C., 500° C., 600° C., 700° C., and 800° C., and the time may be 1 h, 2 h, 4 h, 6 h, 8 h, 9 h, 11 h, 12 h, and 15 h, or other values within the range, which may be selected according to actual needs and are not limited here.
[0184] In some embodiments, the solid carbon source includes at least one of sugars, esters, hydrocarbons, organic acids and high molecular weight polymers.
[0185] In some embodiments, the solid carbon source includes at least one of polyvinyl chloride, polyvinyl butyral, polyacrylonitrile, polyacrylic acid, polyethylene glycol, polypyrrole, polyaniline, sucrose, glucose, maltose, fructose, polyimide, amino resin, polystyrene, carboxymethyl cellulose, cellulose acetate butyrate, citric acid, asphalt, furfural resin, epoxy resin and phenolic resin.
[0186] In some embodiments, the mass ratio of the solid carbon source to the inner core is 100:(10-200). Optionally, the mass ratio can be 100:10, 100:40, 100:60, 100:100, 100:130, 100:160 and 100:200, etc., or other values within the range. It can be selected according to actual needs and is not limited here.
[0187] In some embodiments, the carbon coating process is liquid phase carbon coating, and the steps include: carbonizing a mixture obtained by mixing the inner core with a liquid phase carbon source to obtain a negative electrode material.
[0188] In some embodiments, the mass ratio of the liquid carbon source to the inner core is 100:(5-300). Optionally, the mass ratio can be 100:5, 100:10, 100:60, 100:150, 100:200, 100:240 and 100:300, etc., or other values within the range. It can be selected according to actual needs and is not limited here.
[0189] In some embodiments, the liquid carbon source includes at least one of n-hexane, toluene, benzene, xylene, methanol, ethanol, propanol, butanol, pentanol, acetone, butanone, 2-pentanone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate and pentyl acetate.
[0190] In some embodiments, the temperature of the carbonization treatment is 400°C to 800°C, and the time of the carbonization treatment is 1h to 15h. Optionally, the temperature can be 400°C, 500°C, 600°C, 700°C and 800°C, etc., and the time can be 1h, 3h, 5h, 7h, 9h, 10h, 12h, 13h and 15h, etc., or other values within the range. It can be selected according to actual needs and is not limited here.
[0191] In some embodiments, the core is subjected to carbon coating treatment, the carbon coating treatment is gas phase carbon coating, and the steps include: heating the core, introducing protective gas and carbon source gas, and thermally cracking the carbon source gas to obtain the negative electrode material; wherein the carbon source gas introduction flow rate is 0.1L / min to 100L / min. Specifically, it can be 0.1L / min, 1L / min, 10L / min, 30L / min, 600L / min and 100L / min, etc. Of course, it can also be other values within the above range, and this application is not limited here.
[0192] In some embodiments, the core is subjected to carbon coating treatment, and the carbon coating treatment is solid-phase carbon coating, and the steps include: carbonizing the mixture obtained by mixing the core with a solid-phase carbon source to obtain a negative electrode material; wherein the mass ratio of the solid-phase carbon source to the core is (1-100):100. Specifically, it can be 1:100, 10:100, 30:100, 50:100, 80:100 and 100:100, etc., and of course, it can also be other values within the above range, and this application is not limited here.
[0193] Those skilled in the art will understand that the above-described method for preparing a lithium-ion battery is only an example, and other commonly used methods in the art may be used without departing from the contents disclosed in the present application.
[0194] The following is a further description of the embodiments of the present application in multiple embodiments. The embodiments of the present application are not limited to the following specific embodiments. Within the scope of the unchanged main rights, appropriate changes can be made to the implementation.
[0195] It should be noted that in the following embodiments, the average particle size of the silicon material deposited in the carbon matrix by the silicon source is 0.1nm to 500nm, the purity of the silicon material is greater than 99%, the thickness of the coating layer is 1nm to 300nm, and the mass proportion of the coating layer in the negative electrode material is ≤10%. Embodiment 1:
[0196] (1) using bamboo charcoal as a raw material, performing carbonization treatment, and then acid washing to obtain a porous carbon matrix; adding the porous carbon matrix into a 1.2 mol / L copper nitrate solution, soaking for 30 min, and then vacuum drying to obtain a porous carbon matrix containing a catalyst;
[0197] (2) placing the porous carbon substrate containing the catalyst in a CVD device, then introducing silane into the CVD device at a silane concentration of 26%, raising the temperature to 600° C., and reacting for 5 hours to obtain a core;
[0198] (3) The core and the phenolic resin were mixed in a mass ratio of 50:15, and then the mixed materials were placed in a high-temperature box furnace, nitrogen was introduced, and heat-treated at 800°C for 2 hours.
[0199] (4) The sample after heat preservation is crushed, sieved, and then classified to obtain a negative electrode material.
[0200] The negative electrode material comprises a core and a coating layer located on the surface of the core, and the coating layer comprises a carbon material.
[0201] Embodiment 2:
[0202] (1) Starch is used as a raw material, subjected to carbonization treatment, and then acid-washed to obtain a porous carbon matrix; the porous carbon matrix is added to a 1.2 mol / L ferric nitrate solution, soaked for 30 min, and then vacuum dried to obtain a porous carbon matrix containing a catalyst;
[0203] (2) placing the porous carbon substrate containing the catalyst in a CVD device, then introducing silane into the CVD device at a silane concentration of 15%, raising the temperature to 450° C., and reacting for 3 hours to obtain a core;
[0204] (3) The core and the epoxy resin were mixed in a mass ratio of 50:55, and then the mixed materials were placed in a high-temperature box furnace, nitrogen was introduced, and heat-treated at 620°C for 2 hours.
[0205] (4) The sample after heat preservation is crushed, sieved, and then classified to obtain a negative electrode material.
[0206] The negative electrode material comprises a core and a coating layer located on the surface of the core, and the coating layer comprises a carbon material.
[0207] Embodiment 3:
[0208] (1) mixing activated carbon and boric acid in a mass ratio of 100:2, drying, and treating at 900° C. to obtain a porous carbon matrix containing a catalyst;
[0209] (2) placing the porous carbon substrate containing the catalyst in a CVD device, then introducing silane into the CVD device at a silane concentration of 60%, raising the temperature to 880° C., and reacting for 5 hours to obtain a core;
[0210] (3) The kernels were mixed with sucrose in a mass ratio of 50:45, and then the mixed material was placed in a high-temperature box furnace, nitrogen was introduced, and heat-treated at 720°C for 2 h.
[0211] (4) The sample after heat preservation is crushed, sieved, and then classified to obtain a negative electrode material.
[0212] The negative electrode material comprises a core and a coating layer located on the surface of the core, and the coating layer comprises a carbon material.
[0213] Embodiment 4:
[0214] (1) mixing activated carbon and nickel carbonate in a mass ratio of 100:2, drying, and treating at 960° C. to obtain a porous carbon matrix containing a catalyst;
[0215] (2) placing the porous carbon substrate containing the catalyst in a CVD device, then introducing silane into the CVD device at a silane concentration of 60%, raising the temperature to 600° C., and reacting for 3 hours to obtain a core;
[0216] (3) Methane gas was introduced into the CVD equipment, the temperature was raised to 650°C, and the temperature was maintained for 6 hours to obtain a carbon-coated core.
[0217] (4) The sample after heat preservation is crushed, sieved, and then classified to obtain a negative electrode material.
[0218] The negative electrode material comprises a core and a coating layer located on the surface of the core, and the coating layer comprises a carbon material.
[0219] Embodiment 5:
[0220] (1) using chitosan as a raw material, performing carbonization treatment and activation treatment, and then acid washing to obtain a porous carbon matrix; adding the porous carbon matrix into a 1.2 mol / L copper nitrate solution, soaking for 30 minutes, and then vacuum drying to obtain a porous carbon matrix containing a catalyst;
[0221] (2) placing the porous carbon substrate containing the catalyst in a CVD device, then introducing silane into the CVD device at a silane concentration of 31%, raising the temperature to 700° C., and reacting for 5 hours to obtain a core;
[0222] (3) The core was placed in a high-temperature box furnace, and a 3% oxygen and argon mixed gas was introduced, and heat-treated at 320°C for 2 hours.
[0223] (4) The sample after heat preservation is crushed, sieved, and then classified to obtain a negative electrode material.
[0224] The negative electrode material includes a core and a coating layer located on the surface of the core, and the coating layer includes SiO2.
[0225] Embodiment 6:
[0226] (1) Using coconut shell as raw material, carbonizing it, and then acid washing it to obtain a porous carbon matrix; adding the porous carbon matrix into a 1.2 mol / L copper nitrate solution, soaking it for 30 min, and then vacuum drying it to obtain a porous carbon matrix containing a catalyst;
[0227] (2) placing the porous carbon substrate containing the catalyst in a CVD device, then introducing silane into the CVD device at a silane concentration of 15%, raising the temperature to 700° C., reacting for 5 hours, and obtaining a core;
[0228] (3) The core and the epoxy resin were mixed in a mass ratio of 50:10, and then the mixed materials were placed in a high-temperature box furnace, nitrogen was introduced, and heat-treated at 620°C for 2 hours.
[0229] (4) The sample after heat preservation is crushed, sieved, and then classified to obtain a negative electrode material.
[0230] The negative electrode material comprises a core and a coating layer located on the surface of the core, and the coating layer comprises a carbon material.
[0231] Embodiment 7:
[0232] (1) using bamboo charcoal as a raw material, performing carbonization treatment, and then acid washing to obtain a porous carbon matrix; adding the porous carbon matrix into a 1.2 mol / L copper nitrate solution, soaking for 30 min, and then vacuum drying to obtain a porous carbon matrix containing a catalyst;
[0233] (2) placing the porous carbon substrate containing the catalyst in a CVD device, then introducing silane into the CVD device at a silane concentration of 26%, raising the temperature to 700° C., reacting for 5 hours, and obtaining a core;
[0234] (3) The core and phenolic resin were mixed in a mass ratio of 50:15, and then the mixed materials were placed in a high-temperature box furnace, nitrogen was introduced, and heat-treated at 720°C for 2 hours.
[0235] (4) The coated core was mixed with phenolic resin in a mass ratio of 50:15, and then the mixed material was placed in a high-temperature box furnace, nitrogen was introduced, and heat-treated at 720° C. for 2 h.
[0236] (5) The sample after heat preservation is crushed, sieved, and then classified to obtain a negative electrode material.
[0237] The negative electrode material comprises a core and a coating layer located on the surface of the core, and the coating layer comprises a carbon material.
[0238] Embodiment 8:
[0239] (1) using bamboo charcoal as a raw material, performing carbonization treatment, and then acid washing to obtain a porous carbon matrix; adding the porous carbon matrix into a 1.2 mol / L copper nitrate solution, soaking for 30 min, and then vacuum drying to obtain a porous carbon matrix containing a catalyst;
[0240] (2) placing the porous carbon substrate containing the catalyst in a CVD device, then introducing silane into the CVD device at a silane concentration of 60%, raising the temperature to 880° C., and reacting for 5 hours to obtain a core;
[0241] (3) The core and the phenolic resin were mixed in a mass ratio of 50:15, and then the mixed materials were placed in a high-temperature box furnace, nitrogen was introduced, and heat-treated at 800°C for 2 hours.
[0242] (4) The sample after heat preservation is crushed, sieved, and then classified to obtain a negative electrode material.
[0243] The negative electrode material comprises a core and a coating layer located on the surface of the core, and the coating layer comprises a carbon material.
[0244] Embodiment 9:
[0245] (1) using bamboo charcoal as a raw material, performing carbonization treatment, and then acid washing to obtain a porous carbon matrix; adding the porous carbon matrix into a 1.2 mol / L copper nitrate solution, soaking for 30 min, and then vacuum drying to obtain a porous carbon matrix containing a catalyst;
[0246] (2) placing the porous carbon substrate containing the catalyst in a CVD device, then introducing silane into the CVD device at a silane concentration of 35%, raising the temperature to 550° C., and reacting for 15 hours to obtain a core;
[0247] (3) The core and the phenolic resin were mixed in a mass ratio of 50:15, and then the mixed materials were placed in a high-temperature box furnace, nitrogen was introduced, and heat-treated at 800°C for 2 hours.
[0248] (4) The sample after heat preservation is crushed, sieved, and then classified to obtain a negative electrode material.
[0249] The negative electrode material comprises a core and a coating layer located on the surface of the core, and the coating layer comprises a carbon material.
[0250] Comparative Example 1:
[0251] (1) using bamboo charcoal as a raw material, performing carbonization treatment, and then acid washing to obtain a porous carbon matrix; adding the porous carbon matrix into a 1.2 mol / L copper nitrate solution, soaking for 30 min, and then vacuum drying to obtain a porous carbon matrix containing a catalyst;
[0252] (2) placing the porous carbon substrate containing the catalyst in a CVD device, then introducing silane into the CVD device at a silane concentration of 26%, raising the temperature to 700° C., reacting for 5 hours, and obtaining a core;
[0253] (3) The inner core is crushed, sieved, and then classified to obtain a negative electrode material.
[0254] Comparative Example 2:
[0255] (1) Using bamboo charcoal as raw material, carbonizing it, and then acid washing it to obtain a porous carbon matrix;
[0256] (2) placing the porous carbon substrate in a CVD device, then introducing silane into the CVD device at a silane concentration of 26%, raising the temperature to 700° C., reacting for 5 hours, and obtaining a core;
[0257] (3) The core and phenolic resin were mixed in a mass ratio of 50:15, and then the mixed materials were placed in a high-temperature box furnace, nitrogen was introduced, and heat-treated at 720°C for 2 hours.
[0258] (4) The sample after heat preservation is crushed, sieved, and then classified to obtain a negative electrode material.
[0259] The test results are shown in Table 1:
[0260] Table 1
[0261]
[0262] As shown by the test results, in Examples 1 to 7, after the catalyst is added to the inner core, during the process of forming the coating layer, the catalyst prompts the coating material to form a high-density coating layer on the inner core surface, thereby solving the problem in the prior art of using vapor deposition to prepare the coating layer, in order to ensure complete cracking of the gas source, a high cracking temperature is used, resulting in the consumption of the highly active silicon material by the reaction with the carbon matrix, thereby ensuring that the lithium-ion battery has high reversible capacity, high coulomb efficiency and high cycle capacity retention rate.
[0263] Figure 1 This is a scanning electron microscope (SEM) image of the negative electrode material prepared in Example 1 of the present application. From the SEM image, it can be seen that the negative electrode material is a micron-sized powder.
[0264] Figure 2 This is the XRD diagram of the negative electrode material prepared in Example 1 of the present application. It can be observed from the diagram that the negative electrode material is amorphous.
[0265] Figure 3 This is the first charge and discharge curve of the negative electrode material prepared in Example 1 of the present application. As can be seen from the figure, the first charge and discharge capacity of the negative electrode material is relatively high, and the first efficiency is also relatively high.
[0266] Figure 4 This is the cycle performance curve of the negative electrode material prepared in Example 1 of the present application. As can be seen from the figure, the negative electrode material has excellent cycle performance, and the capacity retention rate after 50 cycles is 92.2%.
[0267] The negative electrode material prepared in Example 7 was coated twice compared with Example 1, and the coating layer of the negative electrode material had a higher density and a lower gas production value.
[0268] According to the test data of Example 1 and Example 8, due to the higher silane concentration and higher heating temperature in Example 8, the high temperature easily induces the secondary growth of the silicon material, and the size of the silicon material is also easy to increase. In addition, the higher concentration of silane gas will make part of the silane gas not have time to enter the pores of the carbon matrix, and the amount of silane gas deposited on the surface of the carbon matrix increases, resulting in an increase in the gas production compared to Example 1 after the negative electrode material contacts the electrolyte, and the cycle performance of the negative electrode material will also decrease slightly.
[0269] According to the test data of Example 1 and Example 9, since the reaction time of silane in Example 9 is too long, the long-term vapor deposition will easily induce the secondary growth of silicon material, and the size of the silicon material will also easily increase. The large-sized silicon material is not easy to fill into the carbon matrix, which will increase the silicon on the surface of the carbon matrix, resulting in an increase in the gas production after the negative electrode material contacts the electrolyte compared to Example 1, and the cycle performance of the negative electrode material will also decrease slightly.
[0270] The negative electrode material prepared in Comparative Example 1 does not have a coating layer on the inner core. When a solid electrolyte film is formed on the surface of the negative electrode material, a large amount of active lithium ions are consumed, the initial coulomb efficiency of the battery is greatly reduced, and the volume expansion rate of the battery after cycling is also greatly increased.
[0271] In the negative electrode material prepared in Comparative Example 2, no catalyst was added, and the density of the prepared negative electrode material decreased and the gas production value increased.
[0272] Embodiment 10:
[0273] (1) The coconut shell is carbonized at a carbonization temperature of 850°C, and then pickled with 8 mol / L hydrochloric acid for 5 h. The resulting material is dried and then activated by a mixture of water vapor and nitrogen, wherein the water vapor concentration is 12%, the activation time is 7 h, and the activation temperature is 750°C.
[0274] (2) The material obtained in step (1) is placed in a molding machine, the pressure is set to 250 MPa, and the pressing is performed for 50 minutes. The pressed material is then crushed, pulverized, and sieved to obtain a carbon matrix.
[0275] (3) The carbon substrate is added to a 1.2 mol / L copper nitrate solution and soaked for 30 min, followed by vacuum drying to obtain a carbon substrate containing a catalyst, which is placed in a CVD device. Silane is then introduced into the CVD device with the silane concentration controlled at 15%. The temperature is raised to 490°C and the reaction is performed for 7 h to obtain a core.
[0276] (4) The core and the phenolic resin were mixed in a mass ratio of 50:15, and then the mixed materials were placed in a high-temperature box furnace, nitrogen was introduced, and heat-treated at 800°C for 2 hours.
[0277] (5) The sample after heat preservation is crushed, sieved, and then classified to obtain a negative electrode material.
[0278] The negative electrode material comprises a core and a coating layer located on the surface of the core, and the coating layer comprises a carbon material.
[0279] like Figure 5 , which is a SEM image of the negative electrode material prepared in Example 10, it can be seen that a small amount of macropores exist in the negative electrode material prepared in Example 10.
[0280] like Figure 6 , which is the XRD diagram of the negative electrode material prepared in Example 10; it can be seen that the silicon material in the negative electrode material is amorphous.
[0281] like Figure 7 As shown, it is the first charge and discharge curve of the negative electrode material prepared in Example 10; it can be seen that the first charge and discharge capacity of the negative electrode material is relatively high, and the first efficiency is also relatively high.
[0282] like Figure 8 As shown, it is the cycle performance curve of the negative electrode material prepared in Example 10, which shows that the negative electrode material has excellent cycle performance.
[0283] Embodiment 11:
[0284] (1) The fruit shell is carbonized at a carbonization temperature of 850°C, and then pickled with hydrochloric acid at a concentration of 4 mol / L for 5 h. The resulting material is dried and then activated by a mixture of water vapor and nitrogen, wherein the water vapor concentration is 12%, the activation time is 8 h, and the activation temperature is 850°C.
[0285] (2) The material obtained in step (1) is placed in a molding machine, the pressure is set to 150 MPa, and the pressing is performed for 50 minutes. The pressed material is then crushed, pulverized, and sieved to obtain a carbon matrix.
[0286] (3) The carbon substrate is added into a 1.2 mol / L ferric nitrate solution and soaked for 30 min, followed by vacuum drying to obtain a carbon substrate containing a catalyst, which is placed in a CVD device, and then silane is introduced into the CVD device with the silane concentration controlled at 15%. The temperature is raised to 490°C and the reaction is carried out for 7 h to obtain a core.
[0287] (4) The core and the phenolic resin were mixed in a mass ratio of 50:15, and then the mixed materials were placed in a high-temperature box furnace, nitrogen was introduced, and heat-treated at 800°C for 2 hours.
[0288] (5) The sample after heat preservation is crushed, sieved, and then classified to obtain a negative electrode material.
[0289] The negative electrode material comprises a core and a coating layer located on the surface of the core, and the coating layer comprises a carbon material.
[0290] Embodiment 12:
[0291] (1) The fruit shell is carbonized at a carbonization temperature of 850°C, and then pickled with hydrochloric acid at a concentration of 4 mol / L for 5 h. The resulting material is dried and then activated by a mixture of water vapor and nitrogen, wherein the water vapor concentration is 12%, the activation time is 8 h, and the activation temperature is 850°C.
[0292] (2) The material obtained in step (1) is placed in a molding machine, the pressure is set to 100 MPa, and the pressing is performed for 50 minutes. Then, the pressed material is crushed, pulverized, and sieved to obtain a carbon matrix.
[0293] (3) The carbon matrix and boric acid are mixed in a mass ratio of 100:2, and then dried and treated at 900°C to obtain a carbon matrix containing a catalyst, which is placed in a CVD device, and then silane is introduced into the CVD device, with the silane concentration controlled at 15%, and the temperature is raised to 490°C, and the reaction is carried out for 7 hours to obtain a core.
[0294] (4) The core and the phenolic resin were mixed in a mass ratio of 50:15, and then the mixed materials were placed in a high-temperature box furnace, nitrogen was introduced, and heat-treated at 800°C for 2 hours.
[0295] (5) The sample after heat preservation is crushed, sieved, and then classified to obtain a negative electrode material.
[0296] The negative electrode material comprises a core and a coating layer located on the surface of the core, and the coating layer comprises a carbon material.
[0297] Embodiment 13:
[0298] (1) The fruit shell is carbonized at a carbonization temperature of 850°C, then pickled with hydrochloric acid at a concentration of 4 mol / L for 5 h, and the resulting material is dried and then activated by a mixture of water vapor and nitrogen, wherein the water vapor concentration is 6%, the activation time is 8 h, and the activation temperature is 550°C;
[0299] (2) The material obtained in step (1) is placed in a molding machine, the pressure is set to 300 MPa, and the pressing is performed for 30 minutes. Then, the pressed material is crushed, pulverized, and sieved to obtain a carbon matrix.
[0300] (3) The carbon matrix and nickel carbonate are mixed in a mass ratio of 100:2, and then dried and treated at 960°C to obtain a carbon matrix containing a catalyst, which is placed in a CVD device, and then silane is introduced into the CVD device, with the silane concentration controlled at 22%, and the temperature is raised to 490°C, and the reaction is carried out for 7 hours to obtain a core.
[0301] (4) The core and the phenolic resin were mixed in a mass ratio of 50:15, and then the mixed materials were placed in a high-temperature box furnace, nitrogen was introduced, and heat-treated at 800°C for 2 hours.
[0302] (5) The sample after heat preservation is crushed, sieved, and then classified to obtain a negative electrode material.
[0303] The negative electrode material comprises a core and a coating layer located on the surface of the core, and the coating layer comprises a carbon material.
[0304] Embodiment 14:
[0305] (1) The fruit shell is carbonized at a carbonization temperature of 850°C, and then pickled with hydrochloric acid at a concentration of 4 mol / L for 5 h. The resulting material is dried and then activated by a mixture of water vapor and nitrogen, wherein the water vapor concentration is 12%, the activation time is 8 h, and the activation temperature is 850°C.
[0306] (2) Dissolve 10 g of soy protein in 90 mL of water to obtain a treatment solution, the concentration of the treatment solution is 10 mol / L, place the material obtained in step (1) in a vacuum impregnation machine, add the treatment solution, set the vacuum pressure to 500 Pa, press for 50 min, and then heat treat at 500 ° C for 4 h to obtain a carbon matrix.
[0307] (3) The carbon substrate is added to a 1.2 mol / L copper nitrate solution and soaked for 30 min, followed by vacuum drying to obtain a carbon substrate containing a catalyst, which is placed in a CVD device. Silane is then introduced into the CVD device with the silane concentration controlled at 15%. The temperature is raised to 540°C and the reaction is performed for 5 h to obtain a core.
[0308] (4) The core and the phenolic resin were mixed in a mass ratio of 50:15, and then the mixed materials were placed in a high-temperature box furnace, nitrogen was introduced, and heat-treated at 800°C for 2 hours.
[0309] (5) The sample after heat preservation is crushed, sieved, and then classified to obtain a negative electrode material.
[0310] The negative electrode material comprises a core and a coating layer located on the surface of the core, and the coating layer comprises a carbon material.
[0311] Embodiment 15:
[0312] (1) The fruit shell is carbonized at a carbonization temperature of 850°C, and then pickled with hydrochloric acid at a concentration of 4 mol / L for 5 h. The resulting material is dried and then activated by a mixture of water vapor and nitrogen, wherein the water vapor concentration is 12%, the activation time is 8 h, and the activation temperature is 850°C.
[0313] (2) Dissolve 10 g of soy protein in 90 mL of water to obtain a treatment solution, the concentration of the treatment solution is 10 mol / L, place the material obtained in step (1) in a vacuum impregnation machine, add the treatment solution, set the vacuum pressure to 201 Pa, press for 50 min, and then heat treat at 500° C. for 4 h to obtain a carbon matrix.
[0314] (3) The carbon substrate is added to a 1.2 mol / L copper nitrate solution and soaked for 30 min, followed by vacuum drying to obtain a carbon substrate containing a catalyst, which is placed in a CVD device. Silane is then introduced into the CVD device with the silane concentration controlled at 15%. The temperature is raised to 540°C and the reaction is performed for 5 h to obtain a core.
[0315] (4) The core and the phenolic resin were mixed in a mass ratio of 50:15, and then the mixed materials were placed in a high-temperature box furnace, nitrogen was introduced, and heat-treated at 800°C for 2 hours.
[0316] (5) The sample after heat preservation is crushed, sieved, and then classified to obtain a negative electrode material.
[0317] The negative electrode material comprises a core and a coating layer located on the surface of the core, and the coating layer comprises a carbon material.
[0318] Embodiment 16:
[0319] (1) The fruit shell is carbonized at a carbonization temperature of 850°C, and then pickled with hydrochloric acid at a concentration of 4 mol / L for 5 h. The resulting material is dried and then activated by a mixture of water vapor and nitrogen, wherein the water vapor concentration is 12%, the activation time is 8 h, and the activation temperature is 850°C.
[0320] (2) Dissolve 10 g of soy protein in 90 mL of water to obtain a treatment solution, the concentration of the treatment solution is 10 mol / L, place the material obtained in step (1) in a vacuum impregnation machine, add the treatment solution, set the vacuum pressure to 47 Pa, press for 50 min, and then heat treat at 500 ° C for 4 h to obtain a carbon matrix.
[0321] (3) The carbon substrate is added to a 1.2 mol / L copper nitrate solution and soaked for 30 min, followed by vacuum drying to obtain a carbon substrate containing a catalyst, which is placed in a CVD device. Silane is then introduced into the CVD device with the silane concentration controlled at 15%. The temperature is raised to 540°C and the reaction is performed for 5 h to obtain a core.
[0322] (4) The core and the phenolic resin were mixed in a mass ratio of 50:15, and then the mixed materials were placed in a high-temperature box furnace, nitrogen was introduced, and heat-treated at 800°C for 2 hours.
[0323] (5) The sample after heat preservation is crushed, sieved, and then classified to obtain a negative electrode material.
[0324] The negative electrode material comprises a core and a coating layer located on the surface of the core, and the coating layer comprises a carbon material.
[0325] Embodiment 17:
[0326] (1) The fruit shell is carbonized at a carbonization temperature of 850°C, and then pickled with hydrochloric acid at a concentration of 4 mol / L for 5 h. The resulting material is dried and then activated by a mixture of water vapor and nitrogen, wherein the water vapor concentration is 12%, the activation time is 8 h, and the activation temperature is 850°C.
[0327] (2) Dissolve 10 g of soy protein in 90 mL of water to obtain a treatment solution, the concentration of the treatment solution is 10 mol / L, place the material obtained in step (1) in a vacuum impregnation machine, add the treatment solution, set the vacuum pressure to 0.1 Pa, press for 50 minutes, and then heat treat at 500°C for 4 hours to obtain a carbon matrix.
[0328] (3) The carbon substrate is added to a 1.2 mol / L copper nitrate solution and soaked for 30 min, followed by vacuum drying to obtain a carbon substrate containing a catalyst, which is placed in a CVD device. Silane is then introduced into the CVD device with the silane concentration controlled at 15%. The temperature is raised to 540°C and the reaction is performed for 5 h to obtain a core.
[0329] (4) The core and the phenolic resin were mixed in a mass ratio of 50:15, and then the mixed materials were placed in a high-temperature box furnace, nitrogen was introduced, and heat-treated at 800°C for 2 hours.
[0330] (5) The sample after heat preservation is crushed, sieved, and then classified to obtain a negative electrode material.
[0331] The negative electrode material comprises a core and a coating layer located on the surface of the core, and the coating layer comprises a carbon material.
[0332] Embodiment 18:
[0333] (1) The coconut shell is carbonized at a carbonization temperature of 850°C, and then pickled with 8 mol / L hydrochloric acid for 5 h. The resulting material is dried and then activated by a mixture of water vapor and nitrogen, wherein the water vapor concentration is 12%, the activation time is 7 h, and the activation temperature is 750°C.
[0334] (2) 10 g starch (C6H 10 O5) 74 The treated solution was dissolved in 82 mL of DMSO, the concentration of which was 10 mol / L. The material obtained in step (1) was placed in a vacuum impregnation machine, the treated solution was added, the vacuum pressure was set to 500 Pa, the mixture was pressed for 50 min, and then heat treated at 500 ° C for 4 h to obtain a carbon matrix.
[0335] (3) The carbon substrate is added to a 1.2 mol / L copper nitrate solution and soaked for 30 min, followed by vacuum drying to obtain a carbon substrate containing a catalyst, which is placed in a CVD device. Silane is then introduced into the CVD device with the silane concentration controlled at 15%. The temperature is raised to 490°C and the reaction is performed for 7 h to obtain a core.
[0336] (4) The core and the phenolic resin were mixed in a mass ratio of 50:15, and then the mixed materials were placed in a high-temperature box furnace, nitrogen was introduced, and heat-treated at 800°C for 2 hours.
[0337] (5) The sample after heat preservation is crushed, sieved, and then classified to obtain a negative electrode material.
[0338] The negative electrode material comprises a core and a coating layer located on the surface of the core, and the coating layer comprises a carbon material.
[0339] Embodiment 19:
[0340] (1) The coconut shell is carbonized at a carbonization temperature of 850°C, and then pickled with 8 mol / L hydrochloric acid for 5 h. The resulting material is dried and then activated by a mixture of water vapor and nitrogen, wherein the water vapor concentration is 12%, the activation time is 7 h, and the activation temperature is 750°C.
[0341] (2) 10g polyvinyl chloride (C2H3Cl) 160The treated solution was dissolved in 68 mL of dichloroethane, the concentration of which was 10 mol / L. The material obtained in step (1) was placed in a vacuum impregnation machine, the treated solution was added, the vacuum pressure was set to 500 Pa, the mixture was pressed for 50 min, and then heat treated at 500 ° C for 4 h to obtain a carbon matrix.
[0342] (3) The carbon substrate is added to a 1.2 mol / L copper nitrate solution, soaked for 30 min, and then vacuum dried to obtain a carbon substrate containing a catalyst. The carbon substrate is placed in a CVD device, and then silane is introduced into the CVD device with the silane concentration controlled at 15%. The temperature is raised to 490°C and the reaction is carried out for 7 h to obtain a core.
[0343] (4) The core and the phenolic resin were mixed in a mass ratio of 50:15, and then the mixed materials were placed in a high-temperature box furnace, nitrogen was introduced, and heat-treated at 800°C for 2 hours.
[0344] (5) The sample after heat preservation is crushed, sieved, and then classified to obtain a negative electrode material.
[0345] The negative electrode material comprises a core and a coating layer located on the surface of the core, and the coating layer comprises a carbon material.
[0346] Comparative Example 3
[0347] The difference from Example 10 is that step (2) is not performed.
[0348] Comparative Example 4
[0349] The difference from Example 10 is that the pressure in step (2) is 90 MPa.
[0350] Comparative Example 5
[0351] The difference from Example 14 is that step (2) is not performed.
[0352] Comparative Example 6
[0353] The difference from Example 14 is that the pressure in step (2) is normal pressure, specifically 101 KPa.
[0354] In the above embodiments, the inner core includes a carbon matrix and silicon particles, the carbon matrix has pores, and the silicon particles are filled in the pores of the carbon matrix. The pore ratio, carbon content, silicon content, pore volume, compacted density and specific surface area tests are shown in Tables 2 to 4.
[0355] Performance Testing
[0356] 1. Density β test: Soak m1 g of negative electrode material in 20% HF solution for 1 hour, then wash and dry. Weigh the mass of the negative electrode material after washing and drying as m2, and calculate the density of the coating layer β = m2 / m1×100%.
[0357] 2. Coating thickness: The material is sectioned using a FIB-SEM device. Ten particles are randomly selected from the SEM and the coating thickness of each particle is measured three times to obtain the average coating thickness.
[0358] 3. Test method for pore diameter and pore volume ratio:
[0359] The test was carried out using the ASAP2460 equipment from Micromeritics, USA. The pore volume V was calculated using the BJH Desorption cumulative volume of pores model. Calculated within the aperture range.
[0360] Micromeretics ASAP 2460 was used for micropore and mesopore analysis. At liquid nitrogen temperature, the equilibrium adsorption of nitrogen on the surface of an object is related to its pore size and other characteristics. Combined with the law of the change of adsorption amount with relative pressure during adsorption, multiple models can be fitted to calculate the pore size. The report generated by the software uses density functional theory (abbreviated as DFT) method to calculate the pore size distribution, total pore volume and pore volume within a certain range.
[0361] The true density P of the negative electrode material is tested, and the porosity of the negative electrode material is calculated to be V / (V+1 / P).
[0362] 4. Specific surface area test method of negative electrode material:
[0363] The specific surface area was measured using the American Micromeritics TriStar 3000 specific surface area and pore size analyzer.
[0364] 5. Test method for particle size of negative electrode material:
[0365] D50 was measured using a laser particle size analyzer, and it had a symmetrical distribution similar to a normal distribution. In its volume reference distribution, the cumulative 50% diameter is D50, and by analogy, the cumulative 90% diameter is D90, and the cumulative 10% diameter is D10.
[0366] 6. Test method for average particle size of carbon matrix and silicon material:
[0367] The particles of the material to be tested are observed by a field emission scanning electron microscope or a transmission electron microscope. The particle sizes of 5-10 particles are randomly measured using a scale, and the average value of the particle sizes is taken as the final material particle size.
[0368] 7. Type of silicon material: The type of silicon material was confirmed by measuring the diffraction peak using an X-ray diffractometer (XRD).
[0369] 8. Test of silicon mass content in negative electrode material:
[0370] Use a box-type atmosphere furnace (model: SA2-9-17TP) to burn in an oxygen atmosphere, so that the silicon and silicon oxide in the sample react to form silicon dioxide, and the carbon is burned and converted into carbon dioxide and discharged. The mass content of silicon in the negative electrode material is weighed and calculated.
[0371] 9. Test of carbon mass content in negative electrode material:
[0372] Using the German Bruker / German Airt infrared carbon and sulfur analyzer G4 ICARUS HF / CS-i, the sample is burned in a high-temperature, oxygen-rich state. The carbon element it contains is oxidized into carbon dioxide and enters the infrared detector with the carrier gas. The carbon content is calculated by quantitatively analyzing the changes in the intensity of the infrared absorption wavelength of the carbon dioxide signal.
[0373] 10. Powder conductivity test:
[0374] The MCP-PD51 powder resistance test system of Mitsubishi Chemical of Japan was used to test the conductivity under the pressure point of 20KN, and the four-probe method was used to determine the volume resistivity of the sample. The instrument can measure the resistance of the powder, and then the computer automatically calculates the conductivity and resistivity of the powder.
[0375] 11. Gas production test: add 20g active substance to 50g SBR glue, mix well, then seal with aluminum plastic film, place in a 2000ml sealed container, store at a certain temperature such as 25, 45℃ or 60℃, then test the volume change ΔV of the sealed aluminum plastic film bag by drainage method every 24h, test the gas production D = ΔV / m, m is the mass of active substance, record for 6 consecutive days, and obtain the gas production value for 6 days, D6 value;
[0376] 12. The electrochemical performance of the negative electrode material was tested using the following method:
[0377] The negative electrode material, conductive agent and binder with a mass ratio of 94:1:5 are dissolved in a solvent, and the solid content is controlled at 50%. The above mixture is coated on the copper foil current collector, vacuum dried, and the negative electrode plate is obtained; then the ternary positive electrode plate prepared by the traditional mature process, 1mol / L LiPF6 / EC+DMC+EMC (v / v / v=1:1:1) electrolyte, Celgard2400 diaphragm, and shell are assembled into 18650 cylindrical single cells using conventional production processes. The charge and discharge test of the cylindrical battery was carried out on the LAND battery test system of Wuhan Jinnuo Electronics Co., Ltd. at room temperature, 0.2C constant current charge and discharge, and the charge and discharge voltage was limited to 2.75~4.2V.
[0378] 13. Use the following method to perform a withstand voltage test on the negative electrode:
[0379] The negative electrode material, conductive agent and binder with a mass ratio of 94:2:4 are dissolved in a solvent, and the solid content is controlled to be 30%. The mixture is coated on a copper foil current collector and vacuum dried to obtain a negative electrode sheet. The negative electrode sheet is then rolled by a roller machine according to a set pressure. The thickness of the negative electrode sheet is controlled to be 60μm to 70μm. The negative electrode sheet is then cross-sectionally tested to observe whether there is any crushing of the negative electrode material particles in the negative electrode sheet. The minimum pressure value corresponding to the crushing of the negative electrode material particles is the critical withstand pressure P of the negative electrode sheet.
[0380] 14. The compaction density of the negative electrode sheet was tested according to Appendix L of GBT 24533-2019. The American McNorway CARVER 4350.22 powder compaction density meter was used. A sample of specified mass m was placed in a mold and a pressure of 1.0T was applied. After maintaining the pressure for 30S, the pressure was removed to test its thickness and the compaction density was calculated.
[0381] Table 2. Alpha test of negative electrode materials of various embodiments and comparative examples
[0382] sample α’1 α’2 α’3 α’4 α’5 α’6 α’7 α’8 α’9 α’10 α% Example 10 2.5 2.6 2.3 2.5 2.4 2.5 2.7 2.5 2.7 2.6 2.53 Embodiment 11 3.4 3.5 4.3 4.0 4.1 4.2 4.3 4.2 3.7 4.5 3.71 Example 12 9.3 9.2 9.4 9.2 9.6 9.4 9.3 9.6 9.4 10.0 9.44 Embodiment 13 1.4 1.3 1.7 2.0 2.0 2.1 1.9 1.5 1.6 1.7 1.72 Embodiment 14 9.3 9.2 9.6 9.2 9.4 9.6 10.0 10.1 9.5 9.8 9.57 Embodiment 15 7.1 7.1 7.3 8.0 7.6 7.4 7.3 7.4 7.2 8.0 7.44 Example 16 4.2 4.1 4.3 3.4 3.2 4.0 4.0 3.6 3.8 3.7 3.83 Embodiment 17 2.2 2.1 2.3 2.5 2.6 2.5 2.2 2.0 2.1 2.3 2.28 Embodiment 18 8.1 8.2 8.0 8.2 8.4 8.4 8.3 8.0 8.1 8.3 8.2 Embodiment 19 7.1 7.3 7.2 8.6 7.2 7.4 7.4 7.0 8.0 7.7 7.49 Comparative Example 3 15.1 14.3 15.0 15.2 15.6 15.0 15.2 15.6 14.3 14.4 14.97 Comparative Example 4 10.1 10.3 10.2 10.1 10.6 10.4 11.2 11.0 10.3 11.0 10.52 Comparative Example 5 20.1 22.4 20.8 20.9 22.3 21.7 22.1 22.5 23.0 22.6 21.84 Comparative Example 6 10.3 9.2 9.6 10.0 10.5 10.2 9.6 10.1 10.3 10.0 9.98
[0383] Table 3. Performance test of negative electrode materials and negative electrode sheets prepared in various embodiments and comparative examples 1
[0384]
[0385] Table 4. Performance test of negative electrode materials and negative electrode sheets prepared in various embodiments and comparative examples 2
[0386]
[0387]
[0388] As shown in Tables 2 to 4, the number and volume of macropores in the negative electrode material prepared in the present application are small, satisfying α≤10%, which can effectively reduce the specific surface area of the negative electrode material, and during the first charge and discharge process, can reduce the occurrence of side reactions between the negative electrode material and the electrolyte, reduce gas production, and improve the first efficiency, expansion performance and cycle performance of the negative electrode material. Moreover, the number and volume of macropores are small, which can improve the tap density and compaction density of the negative electrode material, reduce the problems of breakage and cracking of the negative electrode material during the roller pressing process, and improve the processing performance of the negative electrode material.
[0389] In Comparative Examples 3 and 4, the porous carbonaceous raw material was not pressurized in Comparative Example 3, and the pressure at which the porous carbonaceous raw material was pressurized in Comparative Example 4 was too small, resulting in a large number of macropores in the negative electrode material and a large pore size, which leads to the negative electrode material having low capacity, low initial efficiency and poor cycle performance. Moreover, the negative electrode material is prepared into a negative electrode sheet, and the critical withstand pressure P and compaction density of the negative electrode sheet are small, resulting in the deterioration of the processing performance of the negative electrode sheet.
[0390] In Comparative Example 5, the porous carbonaceous raw material was not impregnated with the treatment solution, resulting in a large number of macropores in the negative electrode material, causing the negative electrode material to have low capacity, low initial efficiency and poor cycle performance. Moreover, the negative electrode material was prepared into a negative electrode plate, and the critical withstand pressure P and compaction density of the negative electrode plate were relatively small, resulting in deterioration in the processing performance of the negative electrode plate.
[0391] The pressure of the impregnation treatment in Comparative Example 6 is normal pressure, which makes it difficult for the treatment solution to enter the macropores of the carbon matrix, resulting in a large number of macropores in the negative electrode material, causing the negative electrode material to have low capacity, low initial efficiency and poor cycle performance. Moreover, the negative electrode material is prepared into a negative electrode plate, and the critical withstand pressure P and compaction density of the negative electrode plate are relatively small, resulting in the degradation of the processing performance of the negative electrode plate.
[0392] The above describes in detail the structure, features and effects of the present application based on the embodiments shown in the drawings. The above are only preferred embodiments of the present application, but the present application does not limit the scope of implementation to what is shown in the drawings. Any changes made in accordance with the concept of the present application, or modifications to equivalent embodiments with equivalent changes, which still do not exceed the spirit covered by the description and drawings, should be within the protection scope of the present application.
Claims
1. A negative electrode material, characterized in that: The negative electrode material comprises a core and a coating layer located on the surface of the core, wherein the core comprises silicon material; the total pore volume of the negative electrode material is ≤0.02 cm 3 / g, and the density β of the coating layer is ≥80%; Wherein, the density β of the coating layer is measured by the following test method: The negative electrode material with a mass of m1 g is immersed in a HF solution with a mass fraction of 20% for 1 hour, then washed and dried. The mass of the negative electrode material after washing and drying is weighed and recorded as m2, and the density of the coating layer is calculated to be β=m2 / m1×100%.
2. The negative electrode material according to claim 1, characterized in that The negative electrode material has at least one of the following characteristics: (1) The core includes a carbon matrix having pores and the silicon material located in the pores of the carbon matrix; (2) The inner core includes a carbon matrix with pores and the silicon material located in the pores of the carbon matrix. The area ratio of pores with a pore size greater than 50 nm in any cross section of the negative electrode material is α, satisfying: α≤10%; wherein α is obtained by the following test method: in a diagram of a single negative electrode material particle shown after SEM section processing, select any A×B area, wherein A=1μm~10μm, B=1μm~10μm, the sum of the cross-sectional areas of pores with a pore size greater than 50 nm in the cross section of a single negative electrode material particle in the region is denoted as S0, the cross-sectional area of a single negative electrode material particle in the region is denoted as S, the area ratio of pores with a pore size greater than 50 nm in the cross section of a single negative electrode material particle is defined as α', α'=S0 / S, α is the arithmetic mean of the α' values of at least 10 negative electrode material particles.
3. The negative electrode material according to claim 2, characterized in that The negative electrode material has at least one of the following characteristics: (1) The carbon matrix includes at least one of artificial graphite, natural graphite, amorphous carbon, activated carbon, activated carbon fiber, carbon black, capacitor carbon, carbon molecular sieve, mesophase carbon microbeads, carbon nanotubes, carbon nanofibers, porous carbon and graphene; (2) The silicon material includes at least one of crystalline silicon, silicon oxide, amorphous silicon, silicon alloy, silicate, and crystalline and amorphous silicon composite particles; (3) The average particle size of the silicon material is 0.1 nm to 500 nm; (4) The morphology of the silicon material includes at least one of a dot-shaped, spherical, ellipsoidal and flake-shaped shape; (5) The purity of the silicon material is greater than 99%.
4. The negative electrode material according to claim 2, characterized in that The negative electrode material has at least one of the following characteristics: (1) The area of pores with a pore diameter of 500 nm or more in the cross section of the negative electrode material accounts for less than or equal to 5%; (2) The average particle size of the carbon matrix is less than or equal to 15 μm; (3) The mass proportion of silicon in the negative electrode material is 40% to 80%; (4) The mass proportion of carbon element in the negative electrode material is 20% to 60%.
5. The negative electrode material according to claim 1, characterized in that The negative electrode material has at least one of the following characteristics: (1) The material of the coating layer includes at least one of carbon material, metal oxide, amorphous silicon, conductive polymer, fluoride, phosphate and nitride; (2) The material of the coating layer includes a carbon material, and the carbon material includes at least one of graphene, soft carbon, hard carbon, conductive polymer and amorphous carbon; (3) The material of the coating layer includes metal oxide, and the material of the metal oxide layer includes at least one of the oxides of Sn, Ge, Fe, Si, Cu, Ti, Na, Mg, Al, Li, Co, V, Ca and Zn; (4) The material of the coating layer includes a conductive polymer, and the conductive polymer includes at least one of polyaniline, polyacetylene, polypyrrole, polythiophene, poly-3-hexylthiophene, poly(p-phenylene vinylene), polypyridine and poly(styrene vinylene); (5) The material of the coating layer includes a fluoride, and the fluoride includes at least one of polyvinyl fluoride, fluoropolymer, sodium fluoride, potassium fluoride, fluorocarbon polymer, fluorosilicone polymer, hexafluorobutyl acrylate, polytetrafluoroethylene (PTFE), fluorinated ethylene-propylene copolymer (FEP), perfluoroalkoxy resin (PFA), polychlorotrifluoroethylene (PCTFE), ethylene-chlorotrifluoroethylene copolymer (ECTFE), polyvinylidene fluoride (PVDF) and polyvinyl fluoride; (6) The material of the coating layer includes phosphate, and the phosphate includes at least one of magnesium phosphate, calcium phosphate, aluminum phosphate, titanium phosphate, chromium phosphate, cobalt phosphate, nickel phosphate, germanium phosphate, zirconium phosphate, niobium phosphate, molybdenum phosphate, tantalum phosphate, tungsten phosphate, and lanthanum phosphate; (7) The material of the coating layer includes nitride, and the nitride includes at least one of titanium nitride, silicon nitride, vanadium nitride, cobalt nitride, nickel nitride and carbon nitride.
6. The negative electrode material according to claim 1, characterized in that The negative electrode material has at least one of the following characteristics: (1) The thickness of the coating layer is 0.1 nm to 3000 nm, preferably 1 nm to 300 nm; (2) The mass proportion of the coating layer in the negative electrode material is ≤10%.
7. The negative electrode material according to claim 1, characterized in that The negative electrode material has at least one of the following characteristics: (1) The median particle size of the negative electrode material is ≤15 μm, preferably ≤10 μm; (2) The specific surface area of the negative electrode material is ≤5m 2 / g.
8. A negative electrode plate, characterized in that: The negative electrode sheet comprises a negative electrode current collector and a negative electrode active material distributed on one side of the negative electrode current collector, and the negative electrode active material comprises the negative electrode material according to any one of claims 1 to 7.
9. The negative electrode sheet according to claim 8, characterized in that: The negative electrode plate includes at least one of the following features: (1) The critical withstand pressure P of the negative electrode plate is greater than or equal to 100 MPa; (2) The compaction density of the negative electrode sheet is 1.3 g / cm 3 ~1.9g / cm 3 ; The critical withstand pressure P of the negative electrode plate is obtained by the following test method: the thickness of the negative electrode plate is 60 μm to 70 μm, and a cross section of a single negative electrode plate is observed using an electron scanning microscope SEM. The minimum pressure corresponding to the crushing of particles of the negative electrode material is P.
10. A battery, characterized in that: The battery comprises the negative electrode material according to any one of claims 1 to 7.
Citation Information
Cited By
Closed valve control type power battery with high energy and high charging efficiency
CN120073090A
Negative electrode material and battery
WO2026098355A1