Double-doped mixed coated lithium manganese iron phosphate positive electrode material, preparation method thereof and lithium battery

By coating the surface of lithium manganese iron phosphate material with N and F dual-doped carbon materials and Li3BO3/carbon fibers, a dense conductive network is formed, which solves the problem of low electron/ion conduction performance of lithium manganese iron phosphate and achieves a significant improvement in battery performance.

CN119050330APending Publication Date: 2024-11-29HUNAN YUNENG NEW ENERGY BATTERY MATERIALS CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411367107.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The low conductivity of existing lithium manganese iron phosphate materials for electrons/ions hinders their application in high-performance lithium-ion batteries.

Method used

The carbon material was prepared by combining solvothermal and electrospinning methods using N and F doped carbon materials and Li3BO3/carbon fiber as coating layers. The carbon material was then mixed and coated with lithium manganese iron phosphate particles to form a dense conductive network, thereby improving the electron and ion transport pathways.

Benefits of technology

It significantly improves the conductivity and lithium-ion diffusion rate of lithium manganese iron phosphate materials, thereby enhancing the rate performance and cycle stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a double-doped mixed coated lithium manganese iron phosphate positive electrode material, a preparation method thereof and a lithium battery, and belongs to the technical field of lithium batteries, the lithium manganese iron phosphate positive electrode material comprises lithium manganese iron phosphate particles and a coating layer on the surfaces of the lithium manganese iron phosphate particles, the coating layer is a mixed material of an N and F double-doped carbon material and Li3BO3 / carbon fiber, the double-doped mixed and coated lithium manganese iron phosphate positive electrode material is prepared by adopting wet ball milling and high-temperature solid phase methods. N and F double doping enables the carbon material to have better conductivity, Li3BO3 serving as an ion conductor can accelerate the diffusion rate of lithium ions, and mixed coating of the N and F double-doped carbon material and Li3BO3 / carbon fiber can reduce charge transfer resistance and accelerate the flow speed of the lithium ions by utilizing a synergistic effect; and the lithium battery adopting the lithium manganese iron phosphate positive electrode material has excellent rate capability and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium batteries, and specifically relates to a dual-doped mixed-coated lithium manganese iron phosphate positive electrode material and a preparation method thereof, and a lithium battery. Background Art

[0002] Lithium iron manganese phosphate (LiMn x Fe 1-x PO4) is a new type of phosphate lithium battery positive electrode material formed by doping a certain proportion of manganese on lithium iron phosphate (LiFePO4). On the one hand, doping allows the advantages of iron and manganese to be effectively combined, and on the other hand, manganese and iron are adjacent in the periodic table and have similar ionic radii, so doping will not significantly affect the original structure.

[0003] The manganese doping ratio has an important influence on the properties of lithium manganese iron phosphate. On the one hand, the voltage platform of lithium iron phosphate is around 3.4V, and after doping with manganese, the voltage platform can be increased to 3.8-4.1V, which can significantly improve the voltage platform; on the other hand, if the manganese doping ratio is too high, the specific capacity of the material will be reduced and decay rapidly due to the John-Teller effect, making it unsuitable for use as a positive electrode material for lithium-ion batteries.

[0004] Compared with lithium iron phosphate, the high voltage characteristic of manganese makes lithium manganese iron phosphate have a higher voltage platform, which also leads to higher energy density when the specific capacity is the same. Under the same conditions, the energy density is 10%-20% higher than that of lithium iron phosphate. However, the disadvantage is that the introduction of manganese significantly reduces the conductivity of the material. This defect greatly affects its energy storage capacity and rate performance, and seriously hinders its large-scale application in high-performance lithium-ion batteries. Therefore, improving the conductivity of lithium manganese iron phosphate is a key issue that needs to be solved at present. Summary of the invention

[0005] The object of the present invention is to provide a dual-doped mixed-coated lithium manganese iron phosphate positive electrode material and a preparation method thereof, and a lithium battery, so as to improve the electron / ion conductivity of lithium manganese iron phosphate.

[0006] The purpose of the present invention can be achieved through the following technical solutions: The present invention provides a dual-doped mixed-coated lithium iron manganese phosphate positive electrode material, wherein the lithium iron manganese phosphate positive electrode material comprises lithium iron manganese phosphate particles and a coating layer on the surface of the lithium iron manganese phosphate particles; The coating layer is N, F dual-doped carbon material and Li3BO3 / carbon fiber; LiMnFePO4 has inherent defects of olivine-type cathode materials, and its intrinsic electronic conductivity and lithium ion diffusion rate are low. Coating a layer of chemically stable and conductive material on the surface is conducive to improving the transmission path of electrons and ions between LiMnFePO4 particles. An appropriate amount of carbon coating can improve the electrical contact between material particles. Heteroatoms doped in the carbon layer help increase the active sites of the material and effectively promote electron migration. N and F form a donor-acceptor structure, which provides a path and channel for effective charge carrier transmission and improves the conductivity. The three-dimensional network structure of Li3BO3 gives it stable electrical properties at high temperatures, high conductivity and lithium ion conduction rate.

[0007] Furthermore, the preparation steps of the N and F dual-doped carbon material are as follows: Completely dissolve citric acid and urea in DMF, add ammonium fluoride and mix evenly with ultrasonic method, put into a reactor and react at 180°C for 4 hours, add 1.2M sodium hydroxide aqueous solution and stir after cooling to room temperature, adjust the pH to neutral, and obtain N, F dual-doped carbon material after centrifugation, washing, filtration and freeze-drying.

[0008] Furthermore, the mass ratio of the citric acid to urea is 1.8-5.3:1, and the volume ratio of the total mass of the citric acid and urea to DMF is 3g:10mL.

[0009] Furthermore, the mass ratio of the ammonium fluoride to the citric acid is 1:48-87.

[0010] Furthermore, the preparation steps of the Li3BO3 / carbon fiber are as follows: Polyvinyl alcohol was dissolved in deionized water to obtain a solution, wherein the mass concentration of polyvinyl alcohol in the solution was 20%, and the solution was fully dissolved at 90°C to obtain a spinning solution, and the spinning solution was prepared by electrospinning to obtain polyvinyl alcohol nanofibers, and the polyvinyl alcohol nanofibers were placed in a muffle furnace, oxygen was introduced into the muffle furnace, and the heating rate was set to 5°C / min, and the temperature was raised to 350°C and kept constant for 2h for pre-oxidation, and then placed in a tubular furnace and heated to 800°C under an inert atmosphere for carbonization treatment for 4h, and carbon fibers were obtained after cooling, and the carbon fibers were placed in a container, and a lithium carbonate aqueous solution with a mass concentration of 10% was added, and the mass ratio of lithium carbonate to carbon fibers was 0.3:1, and boric acid was added after heating to 80°C and ultrasonically mixed for 0.5h, and the molar ratio of boric acid to lithium carbonate was 2:3, and after stirring and mixing, it was heated to 200°C for dehydration, and then crystallized at a high temperature of 650°C to obtain Li3BO3 / carbon fibers.

[0011] The present invention also provides a method for preparing a dual-doped mixed-coated lithium manganese iron phosphate positive electrode material, comprising the following steps: S1. Preparation of lithium manganese iron phosphate precursor: The lithium source, iron source, manganese source and phosphorus source were prepared according to LiMn 0.6 Fe 0.4 The stoichiometric ratio of each element in PO4 is weighed and mixed, and the mixture is put into a ball mill at 500 r / min for 4 hours. After ball milling, the mixture is pre-sintered at 350° C. for 3 hours in an inert atmosphere, and then cooled to obtain lithium manganese iron phosphate particles. S2, coated lithium manganese iron phosphate particles: Li3BO3 / carbon fiber is mixed with N, F dual-doped carbon material to obtain a mixed material, the mixed material is mixed with lithium iron manganese phosphate particles, and liquid-phase ball milled in anhydrous ethanol medium on a planetary ball mill for 4 hours. The obtained slurry is dried and kept at 600-700°C in an argon atmosphere furnace for 10-16 hours, and cooled to room temperature with the furnace to obtain a dual-doped mixed-coated lithium iron manganese phosphate positive electrode material.

[0012] Further, the lithium source includes one of lithium acetate, lithium carbonate and lithium hydroxide monohydrate; The iron source includes one of ferrous acetate, ferric acetate and ferric sulfate; The manganese source includes one of manganese acetate, manganese carbonate and manganese sulfate; The phosphorus source includes one or more of phosphoric acid, diammonium hydrogen phosphate and ammonium dihydrogen phosphate.

[0013] Furthermore, the mass ratio of the N, F dual-doped carbon material and Li3BO3 / carbon fiber in the mixed material is 1:0.5-1.

[0014] Furthermore, the mass ratio of the mixed material to the lithium iron manganese phosphate particles is 2-5:100.

[0015] The present invention also provides a lithium battery, which is prepared by using the above-mentioned dual-doped mixed-coated lithium manganese iron phosphate positive electrode material.

[0016] The present invention provides a lithium battery, and the beneficial effects of the present invention are: N- is an electron donor group, and F- has a strong electron-withdrawing effect. The N and F double-doped carbon materials with a special electron donor / acceptor structure have easier electron migration, which greatly improves the conductivity of the material.

[0017] N and F dual-doped carbon materials were prepared by a solvothermal method, Li3BO3 / carbon fibers were prepared by combining electrospinning and liquid phase methods, and after mixing the carbon materials and Li3BO3 / carbon fibers, dual-doped mixed-coated lithium iron manganese phosphate positive electrode materials were obtained by wet ball milling and high-temperature solid-state combining with lithium iron manganese phosphate particles. The co-coating of Li3BO3 / carbon fibers and dual-doped carbon materials can effectively accelerate electron transfer and ion diffusion, reduce electrode polarization, inhibit manganese dissolution, and has a better effect on improving the discharge specific capacity and rate performance of the material.

[0018] Lithium borate in Li3BO3 / carbon fiber crystallizes on the surface of carbon fiber, which is beneficial to the dispersion of lithium borate. The anions in lithium borate inhibit the uneven aggregation of free anions nearby, promote the migration of lithium ions in the nearby carbon material, and lead to faster flow of lithium ions and increased ion diffusion rate of positive electrode material. Borate and fluoride ions have strong affinity and can form boron-fluorine bonds, and the doping of F element can form Mn-F bonds and C-F bonds, which is beneficial to the combination of Li3BO3 / carbon fiber and dual-doped carbon material, as well as coating layer and positive electrode material. Li3BO3 / carbon fiber and carbon material are mixed and coated to form a tight point-line conductive network, which has better electrochemical performance, reduces charge transfer resistance, and improves the rate performance of lithium manganese iron phosphate positive electrode material. DETAILED DESCRIPTION

[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] Example 1 S1. Preparation of N and F dual-doped carbon materials: Weigh citric acid and urea in a mass ratio of 5.3:1 and completely dissolve them in DMF. The total mass of citric acid and urea and the volume ratio of DMF are 3g:10mL. Weigh ammonium fluoride (mass of citric acid: mass of ammonium fluoride = 87:1) and add it to the above solution for ultrasonic mixing. Put it into a reactor and react at 180°C for 4 hours. After cooling to room temperature, add 1.2M sodium hydroxide aqueous solution and stir. Adjust the pH to neutral. After centrifugation, take the precipitate, wash it with deionized water, filter it and freeze-dry it to obtain N, F dual-doped carbon material.

[0021] S2. Preparation of Li3BO3 / carbon fiber: The polyvinyl alcohol with a molecular weight of 200,000-250,000 is dissolved in deionized water to obtain a solution, in which the mass concentration of polyvinyl alcohol is 20%. The solution is stirred at 90°C, cooled to room temperature after being fully dissolved, and a spinning solution is obtained. The spinning solution is prepared by electrospinning to obtain polyvinyl alcohol nanofibers. The polyvinyl alcohol nanofibers are placed in a muffle furnace, oxygen is introduced into the muffle furnace, and the heating rate is set to 5°C / min. The temperature is raised to 350°C and kept constant for 2h for pre-oxidation, and then placed in a tubular furnace and heated to 800°C under an inert atmosphere for carbonization treatment for 4h. After cooling, carbon fibers are obtained. The carbon fibers are placed in a container, and a lithium carbonate aqueous solution with a mass concentration of 10% is added. The mass ratio of lithium carbonate to carbon fibers is 0.3:1. Boric acid is added after heating to 80°C and ultrasonically mixed for 0.5h. The molar ratio of boric acid to lithium carbonate is 2:3. After stirring and mixing, it is heated to 200°C for dehydration, and then crystallized at a high temperature of 650°C to obtain Li3BO3 / carbon fibers.

[0022] S3, preparing lithium manganese iron phosphate particles: Lithium acetate, ferrous acetate, manganese acetate and phosphoric acid were mixed according to LiMn 0.6 Fe 0.4 The stoichiometric ratio of each element in PO4 is weighed and mixed, and the mixture is put into a ball mill at 500 r / min for 4 hours. After ball milling, the mixture is pre-sintered at 350° C. for 3 hours in an inert atmosphere, and then cooled to obtain lithium manganese iron phosphate particles. S4, coated lithium manganese iron phosphate particles: Li3BO3 / carbon fiber and N, F dual-doped carbon material are mixed in a mass ratio of 1:1 to obtain a mixed material, and the mixed material and lithium iron manganese phosphate particles are mixed in a mass ratio of 2:100, and liquid-phase ball milled in anhydrous ethanol medium on a planetary ball mill for 4 hours. The obtained slurry is dried and kept at 600°C in an argon atmosphere furnace for 16 hours, and cooled to room temperature with the furnace to obtain a dual-doped mixed-coated lithium iron manganese phosphate positive electrode material, a coating layer and lithium iron manganese phosphate particles.

[0023] The lithium manganese iron phosphate positive electrode material prepared in this embodiment is mixed with conductive carbon powder and PVDF binder in a mass ratio of 90:5:5, and after homogenization, it is coated on an aluminum foil sheet, rolled with a double roller machine after drying, and then a positive electrode sheet is obtained by a punching machine. The negative electrode sheet is a lithium sheet, and a CR2032 button battery is obtained after assembly.

[0024] Example 2 The difference from Example 1 is that the mass ratio of citric acid to urea in the preparation of N and F dual-doped carbon material is adjusted to 2.7:1, and the other steps are the same as Example 1.

[0025] Example 3 The difference from Example 1 is that the mass ratio of citric acid to urea in the preparation of N and F dual-doped carbon material is adjusted to 1.8:1, and the other steps are the same as Example 1.

[0026] Example 4 The difference from Example 1 is that in the preparation of N, F dual-doped carbon material, the mass ratio of citric acid to urea is adjusted to 2.7:1, the mass ratio of citric acid to ammonium fluoride is adjusted to 58:1, and the other steps are the same as Example 1.

[0027] Example 5 The difference from Example 1 is that the mass ratio of citric acid to urea in the preparation of N and F dual-doped carbon material is adjusted to 2.7:1, the mass ratio of citric acid to ammonium fluoride is adjusted to 48:1, and the other steps are the same as Example 1.

[0028] Example 6 The difference from Example 1 is that the mass ratio of Li3BO3 / carbon fiber to N, F dual-doped carbon material in the coating layer material is 0.8:1, and the other steps are the same as Example 1.

[0029] Example 7 The difference from Example 1 is that the mass ratio of Li3BO3 / carbon fiber to N, F dual-doped carbon material in the coating layer material is 0.5:1, and the other steps are the same as Example 1.

[0030] Example 8 The difference from Example 1 is that the mass ratio of the mixed material to the lithium iron manganese phosphate particles is 4:100, and the other steps are the same as Example 1.

[0031] Example 9 The difference from Example 1 is that the mass ratio of the mixed material to the lithium iron manganese phosphate particles is 5:100, and the other steps are the same as Example 1.

[0032] Comparative Example 1 The difference from Example 1 is that the coating layer of the lithium manganese iron phosphate positive electrode material is a N and F dual-doped carbon material, and the steps are as follows: S1. Preparation of N and F dual-doped carbon materials: Weigh citric acid and urea in a mass ratio of 5.3:1 and completely dissolve them in DMF. The total mass of citric acid and urea and the volume ratio of DMF are 3g:10mL. Weigh ammonium fluoride (mass of citric acid: mass of ammonium fluoride = 87:1) and add it to the above solution for ultrasonic mixing. Put it into a reactor and react at 180°C for 4 hours. After cooling to room temperature, add 1.2M sodium hydroxide aqueous solution and stir. Adjust the pH to neutral. After centrifugation, take the precipitate, wash it with deionized water, filter it and freeze-dry it to obtain N, F dual-doped carbon material.

[0033] S2. Preparation of lithium manganese iron phosphate particles: Lithium acetate, ferrous acetate, manganese acetate and phosphoric acid were mixed according to LiMn 0.6 Fe 0.4The stoichiometric ratio of each element in PO4 is weighed and mixed, and the mixture is put into a ball mill at 500 r / min for 4 hours. After ball milling, the mixture is pre-sintered at 350° C. for 3 hours in an inert atmosphere, and then cooled to obtain lithium manganese iron phosphate particles.

[0034] S3, coated lithium manganese iron phosphate particles: N, F dual-doped carbon materials and lithium iron manganese phosphate particles were mixed in a mass ratio of 2:100, and liquid-phase ball milled in anhydrous ethanol medium on a planetary ball mill for 4 hours. The obtained slurry was dried and kept at 600°C in an argon atmosphere furnace for 16 hours, and cooled to room temperature with the furnace to obtain a dual-doped carbon-coated lithium iron manganese phosphate positive electrode material.

[0035] The lithium iron manganese phosphate positive electrode material prepared in this comparative example is mixed with conductive carbon powder and PVDF binder in a mass ratio of 90:5:5, and after homogenization, it is coated on an aluminum foil sheet, rolled with a double roller machine after drying, and then a positive electrode sheet is obtained by a punching machine. The negative electrode sheet is a lithium sheet, and a CR2032 button battery is obtained after assembly.

[0036] Comparative Example 2 The difference from Example 1 is that the coating layer of the lithium manganese iron phosphate positive electrode material is Li3BO3 / carbon fiber, and the preparation steps are as follows: S1. Preparation of Li3BO3 / carbon fiber: The polyvinyl alcohol with a molecular weight of 200,000-250,000 is dissolved in deionized water to obtain a solution, in which the mass concentration of polyvinyl alcohol is 20%. The solution is stirred at 90°C, cooled to room temperature after being fully dissolved, and a spinning solution is obtained. The spinning solution is prepared by electrospinning to obtain polyvinyl alcohol nanofibers. The polyvinyl alcohol nanofibers are placed in a muffle furnace, oxygen is introduced into the muffle furnace, and the heating rate is set to 5°C / min. The temperature is raised to 350°C and kept constant for 2h for pre-oxidation, and then placed in a tubular furnace and heated to 800°C under an inert atmosphere for carbonization treatment for 4h. After cooling, carbon fibers are obtained. The carbon fibers are placed in a container, and a lithium carbonate aqueous solution with a mass concentration of 10% is added. The mass ratio of lithium carbonate to carbon fibers is 0.3:1. Boric acid is added after heating to 80°C and ultrasonically mixed for 0.5h. The molar ratio of boric acid to lithium carbonate is 2:3. After stirring and mixing, it is heated to 200°C for dehydration, and then crystallized at a high temperature of 650°C to obtain Li3BO3 / carbon fibers.

[0037] S2. Preparation of lithium manganese iron phosphate particles: Lithium acetate, ferrous acetate, manganese acetate and phosphoric acid were mixed according to LiMn 0.6 Fe 0.4 The stoichiometric ratio of each element in PO4 is weighed and mixed, and the mixture is put into a ball mill at 500 r / min for 4 hours. After ball milling, the mixture is pre-sintered at 350° C. for 3 hours in an inert atmosphere, and then cooled to obtain lithium manganese iron phosphate particles.

[0038] S3, coated lithium manganese iron phosphate particles: Li3BO3 / carbon fiber and lithium iron manganese phosphate particles were mixed in a mass ratio of 2:100, and liquid-phase ball milled in anhydrous ethanol medium on a planetary ball mill for 4 hours. The obtained slurry was dried and kept at 600°C in an argon atmosphere furnace for 16 hours, and cooled to room temperature with the furnace to obtain Li3BO3 / carbon fiber-coated lithium iron manganese phosphate positive electrode material.

[0039] The lithium iron manganese phosphate positive electrode material prepared in this comparative example is mixed with conductive carbon powder and PVDF binder in a mass ratio of 90:5:5, and after homogenization, it is coated on an aluminum foil sheet, rolled with a double roller machine after drying, and then a positive electrode sheet is obtained by a punching machine. The negative electrode sheet is a lithium sheet, and a CR2032 button battery is obtained after assembly.

[0040] Comparative Example 3 The difference from Example 1 is that the coating layer of the lithium manganese iron phosphate positive electrode material is a carbon material, and the steps are as follows: S1. Preparation of lithium manganese iron phosphate particles: Lithium acetate, ferrous acetate, manganese acetate and phosphoric acid were mixed according to LiMn 0.6 Fe 0.4 The stoichiometric ratio of each element in PO4 is weighed and mixed, and the mixture is put into a ball mill at 500 r / min for 4 hours. After ball milling, the mixture is pre-sintered at 350° C. for 3 hours in an inert atmosphere, and then cooled to obtain lithium manganese iron phosphate particles.

[0041] S2, coated lithium manganese iron phosphate particles: Weigh citric acid and lithium iron manganese phosphate particles in a mass ratio of 2:100, mix them, and perform liquid-phase ball milling in anhydrous ethanol medium on a planetary ball mill for 4 hours. After the obtained slurry is dried, it is kept at 600°C in an argon atmosphere furnace for 16 hours, and cooled to room temperature with the furnace to obtain a carbon material-coated lithium iron manganese phosphate positive electrode material.

[0042] The lithium manganese iron phosphate positive electrode material prepared in this embodiment is mixed with conductive carbon powder and PVDF binder in a mass ratio of 90:5:5, and after homogenization, it is coated on an aluminum foil sheet, rolled with a double roller machine after drying, and then a positive electrode sheet is obtained by a punching machine. The negative electrode sheet is a lithium sheet, and a CR2032 button battery is obtained after assembly.

[0043] Comparative Example 4 The difference from Example 1 is that the lithium manganese iron phosphate positive electrode material has no coating layer, and the preparation steps are as follows: S1. Preparation of lithium manganese iron phosphate particles: Lithium acetate, ferrous acetate, manganese acetate and phosphoric acid were mixed according to LiMn 0.6 Fe 0.4 The stoichiometric ratio of each element in PO4 is weighed and mixed, and the mixture is put into a ball mill at 500 r / min for 4 hours. After ball milling, the mixture is pre-sintered at 350° C. for 3 hours in an inert atmosphere, and then cooled to obtain lithium manganese iron phosphate particles.

[0044] S2, Lithium manganese iron phosphate positive electrode material: The lithium iron manganese phosphate particles were liquid-phase ball-milled in anhydrous ethanol medium on a planetary ball mill for 4 hours. The obtained slurry was dried and kept at 600° C. for 16 hours in an argon atmosphere furnace, and then cooled to room temperature with the furnace to obtain the lithium iron manganese phosphate positive electrode material.

[0045] The lithium manganese iron phosphate positive electrode material prepared in this embodiment is mixed with conductive carbon powder and PVDF binder in a mass ratio of 90:5:5, and after homogenization, it is coated on an aluminum foil sheet, rolled with a double roller machine after drying, and then a positive electrode sheet is obtained by a punching machine. The negative electrode sheet is a lithium sheet, and a CR2032 button battery is obtained after assembly.

[0046] The performance tests were performed on the batteries and positive electrode materials prepared in Examples 1 to 9 and Comparative Examples 1 to 3. The results are shown in Table 1:

[0047] As can be seen from Table 1, the positive electrode material prepared by the present invention has good electron / ion conductivity, so that the battery has excellent rate performance and cycle stability. Combining the data in Example 1 and Comparative Examples 1-4 in Table 1, it can be seen that the positive electrode material is prepared by coating lithium iron manganese phosphate with N and F dual-doped carbon material and Li3BO3 / carbon fiber, and the carbon material is doped with N and F elements to produce active defect sites, and the charge transfer resistance is reduced under the action of coordination bonds. The coating layer mixed with carbon material and Li3BO3 / carbon fiber can significantly inhibit manganese dissolution, improve electrical conductivity and lithium ion diffusion rate, and the electrochemical performance of the positive electrode material is significantly improved.

[0048] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0049] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. Double-doped mixed-coated lithium manganese iron phosphate positive electrode material, It is characterized in that The lithium iron manganese phosphate positive electrode material comprises lithium iron manganese phosphate particles and a coating layer on the surface of the lithium iron manganese phosphate particles; The coating layer is N, F double doped carbon material and Li 3 BO 3 / Carbon fiber.

2. The dual-doped mixed-coated lithium manganese iron phosphate positive electrode material according to claim 1, It is characterized in that The preparation steps of the N and F dual-doped carbon material are as follows: Completely dissolve citric acid and urea in DMF, add ammonium fluoride and mix evenly with ultrasonic method, put into a reactor and react at 180°C for 4 hours, add 1.2M sodium hydroxide aqueous solution and stir after cooling to room temperature, adjust the pH to neutral, and obtain N, F dual-doped carbon material after centrifugation, washing, filtration and freeze-drying.

3. The dual-doped mixed-coated lithium manganese iron phosphate positive electrode material according to claim 2, It is characterized in that The mass ratio of the citric acid to urea is 1.8-5.3:1, and the volume ratio of the total mass of the citric acid and urea to DMF is 3g:10mL.

4. The dual-doped mixed-coated lithium manganese iron phosphate positive electrode material according to claim 2, It is characterized in that The mass ratio of the ammonium fluoride to the citric acid is 1:48-87.

5. The dual-doped mixed-coated lithium manganese iron phosphate positive electrode material according to claim 1, It is characterized in that The Li 3 BO 3 / The preparation steps of carbon fiber are as follows: Polyvinyl alcohol was dissolved in deionized water to obtain a solution, wherein the mass concentration of polyvinyl alcohol in the solution was 20%, and the solution was fully dissolved at 90°C to obtain a spinning solution, and the spinning solution was prepared by electrospinning to obtain polyvinyl alcohol nanofibers, and the polyvinyl alcohol nanofibers were placed in a muffle furnace, oxygen was introduced into the muffle furnace, and the heating rate was set to 5°C / min, and the temperature was raised to 350°C and kept constant for 2h for pre-oxidation, and then placed in a tubular furnace and heated to 800°C under an inert atmosphere for carbonization treatment for 4h, and carbon fibers were obtained after cooling, and the carbon fibers were placed in a container, and a lithium carbonate aqueous solution with a mass concentration of 10% was added, and the mass ratio of lithium carbonate to carbon fibers was 0.3:1, and boric acid was added after heating to 80°C and ultrasonically mixed for 0.5h, and the molar ratio of boric acid to lithium carbonate was 2:3, and the mixture was stirred and heated to 200°C for dehydration, and then crystallized at a high temperature of 650°C to obtain Li 3 BO 3 / Carbon fiber.

6. A method for preparing a dual-doped mixed-coated lithium manganese iron phosphate positive electrode material as claimed in any one of claims 1 to 5, It is characterized in that The following steps are involved: S1. Preparation of lithium manganese iron phosphate precursor: The lithium source, iron source, manganese source and phosphorus source were prepared according to LiMn 0.6 Fe 0.4 PO 4 The stoichiometric ratio of each element is weighed and mixed, and the mixture is put into a ball mill at 500 r / min for 4 hours. After ball milling, the mixture is pre-sintered at 350° C. for 3 hours in an inert atmosphere, and then cooled to obtain lithium manganese iron phosphate particles. S2, coated lithium manganese iron phosphate particles: Li 3 BO 3 / Carbon fiber is mixed with N, F dual-doped carbon material to obtain a mixed material, the mixed material is mixed with lithium iron manganese phosphate particles, and liquid-phase ball milled in anhydrous ethanol medium on a planetary ball mill for 4 hours. The obtained slurry is dried and kept at 600-700°C in an argon atmosphere furnace for 10-16 hours, and cooled to room temperature with the furnace to obtain a dual-doped mixed-coated lithium iron manganese phosphate positive electrode material.

7. The method for preparing the dual-doped mixed-coated lithium manganese iron phosphate positive electrode material according to claim 6, It is characterized in that The lithium source includes one of lithium acetate, lithium carbonate and lithium hydroxide monohydrate; The iron source includes one of ferrous acetate, ferric acetate and ferric sulfate; The manganese source includes one of manganese acetate, manganese carbonate and manganese sulfate; The phosphorus source includes one or more of phosphoric acid, diammonium hydrogen phosphate and ammonium dihydrogen phosphate.

8. The method for preparing the dual-doped mixed-coated lithium manganese iron phosphate positive electrode material according to claim 6, It is characterized in that The N and F doped carbon material and Li 3 BO 3 / The mass ratio of carbon fiber is 1:0.5-1.

9. The method for preparing the dual-doped mixed-coated lithium manganese iron phosphate positive electrode material according to claim 6, It is characterized in that The mass ratio of the mixed material to the lithium iron manganese phosphate particles is 2-5:

100.

10. A lithium battery, It is characterized in that The positive electrode material of the lithium battery is the dual-doped mixed-coated lithium manganese iron phosphate positive electrode material as described in any one of claims 1 to 5.

Citation Information

Cited By

  • Preparation method of lithium iron manganese phosphate positive electrode material by coprecipitation method

    CN120463170A

  • Preparation method of lithium manganese iron phosphate cathode material by co-precipitation

    CN120463170B

  • High-conductivity lithium manganese iron phosphate positive electrode material and preparation method thereof

    CN120483086A

  • A difluoroborate-doped lithium manganese iron phosphate positive electrode material, a preparation method and application thereof

    CN122868521A