Metal oxide positive electrode material and preparation method and application thereof

By preparing a metal oxide positive electrode material with a specific chemical formula of NaxFekWzMn1-z-kO2, combined with heat treatment and external doping elements, the problem of poor air stability and circulation performance of sodium manganate positive electrode material is solved, and high performance and Low-cost positive electrode material applications.

CN119050339APending Publication Date: 2024-11-29GEM WUXI ENERGY MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411144973.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing sodium manganate positive electrode materials have problems with poor air stability and circulation performance in actual applications, which limits their commercial applications.

Method used

Using a metal oxide positive electrode material with a specific chemical formula of NaxFekWzMn1-z-kO2, it is prepared by the first and second heat treatment steps, including sodium manganate beta phase and sodium manganate P phase, and optionally external doping element M, Improve material stability and rate performance.

Benefits of technology

The high circulation performance, air stability and high first-time charging specific capacity of metal oxide positive electrode materials are achieved, while reducing costs, and controlling morphology and simple synthesis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050339A_ABST
    Figure CN119050339A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of sodium ion batteries, and particularly relates to a metal oxide positive electrode material and a preparation method and application thereof. According to the metal oxide positive electrode material provided by the invention, the chemical general formula of the metal oxide positive electrode material is Na < x > Fe < k > W < z > Mn < 1-z-k > O < 2 >, z < = 0.01, and 0.1 < = k < = 0.5. The specific metal oxide positive electrode material has the advantages of high first charge specific capacity, high rate capability, high cycle performance and high air stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to a metal oxide positive electrode material and a preparation method and application thereof. Background Art

[0002] Sodium-ion batteries have become one of the best candidates to replace lithium-ion batteries due to their wide distribution of sodium resources, and have received extensive research and attention in the global energy storage field. The cathode material of sodium-ion batteries plays a decisive role in the performance of sodium-ion batteries. The existing sodium manganate cathode material has received widespread attention due to its extremely low cost and extremely high theoretical capacity (244mAh / g). However, in practical applications, its poor air stability and cycle performance limit its further commercial application. Summary of the invention

[0003] Therefore, the technical problem to be solved by the present invention is to overcome the defects of the existing sodium manganate positive electrode material in terms of poor air stability and cycle performance, thereby providing a metal oxide positive electrode material and a preparation method and application thereof.

[0004] The present invention provides a metal oxide positive electrode material, the chemical formula of the metal oxide positive electrode material is Na x Fe k W z Mn 1-z-k O2, where 0.9≤x≤1, 0 <z≤0.01,0.1≤k≤0.5。

[0005] Optionally, the metal oxide positive electrode material includes β-phase sodium manganate and P-phase sodium manganate.

[0006] Preferably, the metal oxide positive electrode material further includes an external doping element M, and the chemical formula of the metal oxide positive electrode material is Na x Fe k M y W z Mn 1-z-y-k O2, where 0.9≤x≤1, 0 <z≤0.01,0<y≤0.09,0.1≤k≤0.5;

[0007] The external doping element M is selected from at least one of Ca, Zn, Al, Sn, Cu, K, Li, and Mg.

[0008] The present invention provides a method for preparing the above-mentioned metal oxide positive electrode material, comprising the following steps:

[0009] The sodium source, the iron source, the manganese source and the tungsten source are mixed in a stoichiometric ratio, and subjected to a first heat treatment and a second heat treatment to obtain the metal oxide positive electrode material.

[0010] Preferably, the sodium source is selected from at least one of sodium hydroxide, sodium oxalate and sodium carbonate;

[0011] The iron source is selected from at least one of ferrous oxide, ferrous oxalate, ferric oxalate, ferric hydroxide, ferric oxide, ferrous oxide, ferric nitrate, ferrous sulfate, and ferric sulfate;

[0012] The manganese source is selected from at least one of manganese dioxide, manganese nitrate, manganese sulfate, manganese acetate, and manganese trioxide;

[0013] The tungsten source is selected from at least one of ammonium metatungstate, ammonium paratungstate and tungsten trioxide.

[0014] Preferably, when the sodium source, the iron source, the manganese source and the tungsten source are mixed in a stoichiometric ratio, the step of adding an external doping element compound is also included;

[0015] The external doping element compound is selected from Ca oxide, Zn oxide, Al oxide, Sn oxide, Cu oxide, K oxide, Li oxide, Mg oxide, Ca hydroxide, Zn hydroxide, Al hydroxide, Sn hydroxide, Cu hydroxide, K hydroxide, Li hydroxide, Mg hydroxide, Ca carbonate, Zn carbonate, Al carbonate, Sn carbonate, Cu carbonate, K carbonate, Li carbonate, Mg carbonate At least one of salts of Ca, nitrates of Zn, nitrates of Al, nitrates of Sn, nitrates of Cu, nitrates of K, nitrates of Li, nitrates of Mg, sulfates of Ca, sulfates of Zn, sulfates of Al, sulfates of Sn, sulfates of Cu, sulfates of K, sulfates of Li, sulfates of Mg, organic acid salts of Ca, organic acid salts of Zn, organic acid salts of Al, organic acid salts of Sn, organic acid salts of Cu, organic acid salts of K, organic acid salts of Li, and organic acid salts of Mg.

[0016] Preferably, the external doping element compound is selected from at least one of Ca oxide, Zn oxide, Al oxide, Sn oxide, Cu oxide, K oxide, Li oxide, Mg oxide, Ca hydroxide, Zn hydroxide, Al hydroxide, Sn hydroxide, Cu hydroxide, K hydroxide, Li hydroxide, Mg hydroxide, Ca carbonate, Zn carbonate, Al carbonate, Sn carbonate, Cu carbonate, K carbonate, Li carbonate, Mg carbonate, organic acid salt of Ca, organic acid salt of Zn, organic acid salt of Al, organic acid salt of Sn, organic acid salt of Cu, organic acid salt of K, organic acid salt of Li, and organic acid salt of Mg.

[0017] Optionally, the external doping element compound is selected from at least one of aluminum oxide, copper oxide, magnesium oxide, zinc oxide, potassium oxide, lithium oxide, tin oxide, calcium oxide, copper carbonate, copper hydroxide, calcium oxalate, and aluminum oxalate.

[0018] Preferably, the first heat treatment temperature is 800-850°C, and the first heat treatment time is 2-4h;

[0019] Optionally, the first heat treatment is performed in an oxygen-containing atmosphere.

[0020] Optionally, the first heat treatment is performed in an air atmosphere.

[0021] Optionally, the first heat treatment temperature is 800° C., and the first heat treatment time is 4 hours.

[0022] Preferably, the second heat treatment temperature is 900-1100°C, and the second heat treatment time is 9-12h;

[0023] Optionally, the second heat treatment is performed in an oxygen-containing atmosphere.

[0024] Optionally, the second heat treatment is performed in an air atmosphere.

[0025] Optionally, the second heat treatment temperature is 1000° C., and the second heat treatment time is 10 hours.

[0026] Preferably, the mixing time is 5-30 min;

[0027] After the second heat treatment is completed, a cooling step is also included.

[0028] Preferably, the heating rate of the first heat treatment is 0.5-11°C;

[0029] The heating rate of the second heat treatment is 0.5-11°C.

[0030] The present invention also provides an application of the metal oxide positive electrode material described above or the metal oxide positive electrode material prepared by the preparation method described above in a sodium ion battery.

[0031] The technical solution of the present invention has the following advantages:

[0032] 1. The metal oxide positive electrode material provided by the present invention has a chemical formula of Na x Fe k W z Mn 1-z-kO₂, where 0.9 ≤ x ≤ 1, 0 < z ≤ 0.01, 0.1 ≤ k ≤ 0.5. In the metal oxide cathode material of the present invention, specific contents of Na, Fe, W, and Mn cooperate with each other. The specific content of Fe can cooperate with W to ensure that sodium manganate in the β-phase and sodium manganate in the P-phase in the cathode material always stably exist. The specific metal oxide cathode material of the present invention has the advantages of high cycle performance and strong air stability, and also maintains a high initial charge specific capacity and high rate performance.

[0033] 2. The metal oxide cathode material provided by the present invention, wherein the metal oxide cathode material further includes an externally doped element M; the chemical general formula of the metal oxide cathode material is Na x Fe k M y W z Mn 1-z-y-k O₂, where 0.9 ≤ x ≤ 1, 0 < z ≤ 0.01, 0 < y ≤ 0.09, 0.1 ≤ k ≤ 0.5; the externally doped element M is selected from at least one of Ca, Zn, Al, Sn, Cu, K, Li, and Mg. By adding an external metal element, the present invention can further improve the rate performance and cycle stability performance of the material.

[0034] 3. The metal oxide cathode material provided by the present invention is low in cost, controllable in morphology, and simple to synthesize. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following will briefly introduce the drawings required for use in the description of the specific embodiments or the prior art. Obviously, the following drawings are some embodiments of the present invention. For those of ordinary skill in the art, without creative efforts, other drawings can also be obtained based on these drawings.

[0036] Figure 1 XRD test chart of the cathode material of Example 1 of the present invention;

[0037] Figure 2 Voltage-specific capacity corresponding curve of the first charge and discharge of the cathode material of Example 1 of the present invention. DETAILED DESCRIPTION OF THE EMBODIMENTS

[0038] The following embodiments are provided to better further understand the present invention. They are not limited to the best embodiments, and do not limit the content and protection scope of the present invention. Any product that is the same as or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior art features falls within the protection scope of the present invention.

[0039] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0040] Example 1

[0041] This embodiment provides a method for preparing a metal oxide positive electrode material, comprising the following steps:

[0042] Sodium carbonate, ferric oxide, tungsten trioxide and manganese dioxide were weighed and mixed according to the molar ratio of sodium element, iron element, tungsten element and manganese element of 0.9:0.1:0.01:0.89, the mixture was mechanically mixed for 5 minutes, then put into a sagger and then placed in a box furnace, heated to 800°C at a heating rate of 2°C / min in an air atmosphere, calcined at 800°C for 4 hours, then heated to 1000°C at a heating rate of 2°C / min in an air atmosphere, calcined at 1000°C for 10 hours, and naturally cooled to room temperature to obtain the metal oxide positive electrode material (Na 0.9 Fe 0.1 W 0.01 Mn 0.89 O2).

[0043] The metal oxide positive electrode material obtained by the present invention is detected by XRD, including β-phase sodium manganate and P-phase sodium manganate. The XRD detection diagram is as follows: Figure 1 As shown, Figure 1 Also included are the XRD standard PDF card of β-phase sodium manganate (numbered 25-0844), the XRD standard PDF card of P-phase sodium manganate (numbered 70-3726), and the XRD standard PDF card of sodium tungstate (numbered 74-2369) for comparison.

[0044] Example 2

[0045] This embodiment provides a method for preparing a metal oxide positive electrode material, comprising the following steps:

[0046] Sodium carbonate, ferric oxide, tungsten trioxide and manganese dioxide were weighed and mixed according to the molar ratio of sodium element, iron element, tungsten element and manganese element of 1:0.1:0.01:0.89, the mixture was mechanically mixed for 5 minutes, then put into a sagger and then placed in a box furnace, heated to 800°C at a heating rate of 2°C / min in an air atmosphere, calcined at 800°C for 4 hours, then heated to 1000°C at a heating rate of 2°C / min in an air atmosphere, calcined at 1000°C for 10 hours, and naturally cooled to room temperature to obtain the metal oxide positive electrode material (NaFe 0.1 W 0.01 Mn 0.89 O2).

[0047] Example 3

[0048] This embodiment provides a method for preparing a metal oxide positive electrode material, comprising the following steps:

[0049] Sodium carbonate, ferric oxide, tungsten trioxide and manganese dioxide were weighed and mixed according to the molar ratio of sodium element, iron element, tungsten element and manganese element of 0.9:0.1:0.01:0.89, the mixture was mechanically mixed for 5 minutes, then put into a sagger and then placed in a box furnace, heated to 800°C at a heating rate of 5°C / min in an air atmosphere, calcined at 800°C for 4 hours, then heated to 1000°C at a heating rate of 5°C / min in an air atmosphere, calcined at 1000°C for 10 hours, and naturally cooled to room temperature to obtain the metal oxide positive electrode material (Na 0.9 Fe 0.1 W 0.01 Mn 0.89 O2).

[0050] Example 4

[0051] This embodiment provides a method for preparing a metal oxide positive electrode material, comprising the following steps:

[0052] Sodium carbonate, ferric oxide, tungsten trioxide and manganese dioxide were weighed and mixed according to a molar ratio of sodium element, iron element, tungsten element and manganese element of 0.9:0.1:0.01:0.89, the mixture was mechanically mixed for 5 minutes, then put into a sagger and then placed in a box furnace, heated to 850°C at a heating rate of 2°C / min in an air atmosphere, calcined at 850°C for 4 hours, then heated to 950°C at a heating rate of 2°C / min in an air atmosphere, calcined at 950°C for 10 hours, and naturally cooled to room temperature to obtain the metal oxide positive electrode material (Na 0.9 Fe 0.1 W 0.01 Mn 0.89 O2).

[0053] Example 5

[0054] This embodiment provides a method for preparing a metal oxide positive electrode material, comprising the following steps:

[0055] Sodium carbonate, ferric oxide, tungsten trioxide and manganese dioxide were weighed and mixed according to the molar ratio of sodium element, iron element, tungsten element and manganese element of 1:0.5:0.01:0.49, the mixture was mechanically mixed for 5 minutes, then put into a sagger and then placed in a box furnace, heated to 800°C at a heating rate of 2°C / min in an air atmosphere, calcined at 800°C for 4 hours, then heated to 1000°C at a heating rate of 2°C / min in an air atmosphere, calcined at 1000°C for 10 hours, and naturally cooled to room temperature to obtain the metal oxide positive electrode material (NaFe 0.5 W 0.01 Mn 0.49 O2).

[0056] Example 6

[0057] This embodiment provides a method for preparing a metal oxide positive electrode material, comprising the following steps:

[0058] Sodium carbonate, ferric oxide, aluminum oxide (Al2O3), tungsten trioxide and manganese dioxide were weighed and mixed according to the molar ratio of sodium element, iron element, aluminum element, tungsten element and manganese element of 0.9:0.1:0.03:0.01:0.86, the mixture was mechanically mixed for 5 minutes, then put into a sagger and then placed in a box furnace, heated to 800°C at a heating rate of 2°C / min in an air atmosphere, calcined at 800°C for 4 hours, then heated to 1000°C at a heating rate of 2°C / min in an air atmosphere, calcined at 1000°C for 10 hours, and naturally cooled to room temperature to obtain the metal oxide positive electrode material (Na 0.9 Fe 0.1 Al 0.03 W 0.01 Mn 0.86 O2).

[0059] Comparative Example 1

[0060] This comparative example provides a method for preparing a metal oxide positive electrode material, comprising the following steps:

[0061] Sodium carbonate, tungsten trioxide and manganese dioxide were weighed and mixed according to a molar ratio of sodium element, tungsten element and manganese element of 0.9:0.01:0.99, the mixture was mechanically mixed for 5 minutes, then put into a sagger and then placed in a box furnace, heated to 800°C at a heating rate of 2°C / min in an air atmosphere, calcined at 800°C for 4 hours, then heated to 1000°C at a heating rate of 2°C / min in an air atmosphere, calcined at 1000°C for 10 hours, and naturally cooled to room temperature to obtain the metal oxide positive electrode material (Na 0.9 W 0.01 Mn 0.99 O2).

[0062] Comparative Example 2

[0063] This comparative example provides a method for preparing a metal oxide positive electrode material, comprising the following steps:

[0064] Sodium carbonate, ferric oxide, tungsten trioxide and manganese dioxide were weighed and mixed according to the molar ratio of sodium element, iron element, tungsten element and manganese element of 0.9:0.05:0.01:0.94, the mixture was mechanically mixed for 5 minutes, then put into a sagger and then placed in a box furnace, and heated to 800°C at a heating rate of 2°C / min in an air atmosphere, calcined at 800°C for 4 hours, then heated to 1000°C at a heating rate of 2°C / min in an air atmosphere, calcined at 1000°C for 10 hours, and naturally cooled to room temperature to obtain the metal oxide positive electrode material (Na 0.9 Fe 0.05 W 0.01 Mn 0.94 O2).

[0065] Comparative Example 3

[0066] This comparative example provides a method for preparing a metal oxide positive electrode material, comprising the following steps:

[0067] Sodium carbonate, ferric oxide and manganese dioxide were weighed and mixed according to a molar ratio of sodium element, iron element and manganese element of 0.9:0.1:0.9, the mixture was mechanically mixed for 5 minutes, then put into a sagger and then placed in a box furnace, heated to 800°C at a heating rate of 2°C / min in an air atmosphere, calcined at 800°C for 4 hours, then heated to 1000°C at a heating rate of 2°C / min in an air atmosphere, calcined at 1000°C for 10 hours, and naturally cooled to room temperature to obtain the metal oxide positive electrode material (Na 0.9 Fe 0.1 Mn 0.9 O2).

[0068] Test Case

[0069] The positive electrode materials prepared in Examples 1-6 and Comparative Examples 1-3 were used as the positive electrode main materials to prepare positive electrode sheets, N-methylpyrrolidone was used as a dispersant, and the positive electrode main material: carbon black: PVDF (polyvinylidene fluoride): dispersant were mixed in a mass ratio of 95:2.5:2.5:120 to prepare a positive electrode slurry, and the same mass of the positive electrode slurry was evenly coated on an aluminum foil, compacted for the same time under the same pressure conditions, and then dried in an oven at 80°C for 2h to obtain a positive electrode sheet; metallic sodium was used as a negative electrode sheet, glass fiber was used as a diaphragm, and 1 mol / L NaPF6 ethylene carbonate (EC) / dimethyl carbonate (DMC) solution was used as an electrolyte (the volume ratio of EC and DMC was 1:1), and in an argon atmosphere of a glove box, the positive electrode sheet, the negative electrode sheet, the electrolyte, the diaphragm, the gasket and the spring were placed in a button battery shell to assemble a CR2032 button battery.

[0070] The button cell was placed in the blue power test system for electrical performance testing. The electrical performance test parameters were set as follows: voltage range 2.0V-4.0V, the first cycle was charged and discharged at 0.1C / 0.1C for charge and discharge specific capacity test, and then charged and discharged at 0.2C / 0.2C and 0.5C / 0.5C to test the charge and discharge specific capacity at different rates, and then charged and discharged at 1C / 1C for 50 cycles, and the discharge rate performance was evaluated by the value of the lower discharge specific capacity of the first cycle of the 1C / 1C charge and discharge cycle / the lower discharge specific capacity of the first cycle of 0.1C / 0.1C charge and discharge*100%; and the cycle performance was evaluated based on the discharge specific capacity retention rate of 50 cycles of 1C / 1C charge and discharge, and the cycle discharge specific capacity retention rate = the lower discharge specific capacity of the 50th cycle of 1C rate cycle / the discharge specific capacity of the first cycle of 1C rate cycle*100%. The test results of the discharge specific capacity, discharge rate performance and 1C / 1C cycle 50 cycle capacity retention rate of the first 0.1C / 0.1C charge and discharge are shown in Table 1. Among them, the voltage-specific capacity corresponding curve of the first charge and discharge cycle of the positive electrode material of Example 1 of the present invention is shown in Table 1. Figure 2 shown.

[0071] Table 1

[0072]

[0073] Test Example 2

[0074] The positive electrode materials prepared in Examples 1-6 and Comparative Examples 1-3 were placed in an environment with a temperature of 30°C and a relative humidity of more than 40% for 0 days, 3 days, 5 days, and 8 days, respectively, and their moisture content / ppm and surface pH were measured. The changes in moisture content and surface pH were used to measure their air stability. The test results are shown in Table 2.

[0075] Table 2

[0076]

[0077]

[0078] As can be seen from Table 2, the moisture content / ppm and surface pH of the inventive embodiment measured at 0 days, 3 days, 5 days and 8 days are lower than those of the comparative example. It can be seen that the specific positive electrode material of the present invention has higher air stability.

[0079] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A metal oxide positive electrode material, characterized in that: The chemical formula of the metal oxide positive electrode material is Na x Fe k W z Mn 1-z-k O2, where 0.9≤x≤1, 0 <z≤0.01,0.1≤k≤0.5。 2. The metal oxide positive electrode material according to claim 1, characterized in that: The metal oxide positive electrode material further includes an external doping element M. The general chemical formula of the metal oxide positive electrode material is Na x Fe k M y W z Mn 1-z-y-k O2, where 0.9≤x≤1, 0 <z≤0.01,0<y≤0.09,0.1≤k≤0.5; The external doping element M is selected from at least one of Ca, Zn, Al, Sn, Cu, K, Li, and Mg.

3. A method for preparing the metal oxide positive electrode material according to claim 1 or 2, characterized in that: The steps include: The sodium source, the iron source, the manganese source and the tungsten source are mixed in a stoichiometric ratio, and subjected to a first heat treatment and a second heat treatment to obtain the metal oxide positive electrode material.

4. The method for preparing the metal oxide positive electrode material according to claim 3, characterized in that: The sodium source is selected from at least one of sodium hydroxide, sodium oxalate and sodium carbonate; The iron source is selected from at least one of ferrous oxide, ferrous oxalate, ferric oxalate, ferric hydroxide, ferric tetroxide, ferrous oxide, ferric nitrate, ferrous sulfate, and ferric sulfate. The manganese source is selected from at least one of manganese dioxide, manganese nitrate, manganese sulfate, manganese acetate, and manganese trioxide; The tungsten source is selected from at least one of ammonium metatungstate, ammonium paratungstate and tungsten trioxide.

5. The method for preparing the metal oxide positive electrode material according to claim 3 or 4, characterized in that: When the sodium source, the iron source, the manganese source and the tungsten source are mixed in a stoichiometric ratio, the step of adding an external doping element compound is also included; The external doping element compound is selected from Ca oxide, Zn oxide, Al oxide, Sn oxide, Cu oxide, K oxide, Li oxide, Mg oxide, Ca hydroxide, Zn hydroxide, Al hydroxide, Sn hydroxide, Cu hydroxide, K hydroxide, Li hydroxide, Mg hydroxide, Ca carbonate, Zn carbonate, Al carbonate, Sn carbonate, Cu carbonate, K carbonate, Li carbonate, Mg carbonate At least one of salts of Ca, nitrates of Zn, nitrates of Al, nitrates of Sn, nitrates of Cu, nitrates of K, nitrates of Li, nitrates of Mg, sulfates of Ca, sulfates of Zn, sulfates of Al, sulfates of Sn, sulfates of Cu, sulfates of K, sulfates of Li, sulfates of Mg, organic acid salts of Ca, organic acid salts of Zn, organic acid salts of Al, organic acid salts of Sn, organic acid salts of Cu, organic acid salts of K, organic acid salts of Li, and organic acid salts of Mg.

6. The method for preparing the metal oxide positive electrode material according to any one of claims 3 to 5, characterized in that: The first heat treatment temperature is 800-850°C, and the first heat treatment time is 2-4h; Optionally, the first heat treatment is performed in an oxygen-containing atmosphere.

7. The method for preparing the metal oxide positive electrode material according to any one of claims 3 to 6, characterized in that: The second heat treatment temperature is 900-1100°C, and the second heat treatment time is 9-12h; Optionally, the second heat treatment is performed in an oxygen-containing atmosphere.

8. The method for preparing the metal oxide positive electrode material according to any one of claims 3 to 7, characterized in that: The mixing time is 5-30min; After the second heat treatment is completed, a cooling step is also included.

9. The method for preparing the metal oxide positive electrode material according to any one of claims 3 to 8, characterized in that: The heating rate of the first heat treatment is 0.5-11°C; The heating rate of the second heat treatment is 0.5-11°C.

10. Use of the metal oxide positive electrode material according to claim 1 or 2 or the metal oxide positive electrode material prepared by the preparation method according to any one of claims 3 to 9 in a sodium ion battery.