Preparation method of solid oxide fuel cell sealing material
Through the casting forming method based on glass-based materials, the problem of insufficient sealing performance of flat-panel solid oxide fuel cell is solved, and sealing gaskets with high airtightness and thermal stability are prepared, which simplifies the production process and reduces the Cost, suitable for large-scale production.
Patent Information
- Application Number
- CN202411117521.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The sealing problem of flat-panel solid oxide fuel cell stacks is due to the harsh working environment, which leads to challenges in structural design and sealing performance. The existing sealing methods are highly complex, costly, and airtight.
The sealing material is prepared by casting molding method based on glass-based materials. The gas discharge is prepared by mixing glass powder, organic solvent, dispersant, plasticizer and binder with ball milling, filtering and vacuum defoaming. Sealing gasket with good density, thermal stability, chemical stability and mechanical properties.
It realizes sealing gaskets with high airtightness, thermal stability and mechanical properties, simplifies production processes, reduces costs, and improves sealing performance, and is suitable for large-scale production.
Smart Images

Figure CN119050402A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of sealing materials, and in particular to a method for preparing a sealing material for a solid oxide fuel cell. Background Art
[0002] With the rapid development of economy, energy depletion and environmental pollution have become the key factors restricting the sustainable development of society. Therefore, the development of efficient and clean new energy conversion technology has become an important issue facing all countries today. Solid oxide fuel cells (SOFCs) are a kind of all-solid-state energy conversion device that can directly convert the chemical energy stored in the fuel into electrical energy through electrochemical reaction. They have the advantages of high energy conversion efficiency, wide fuel adaptability, clean and pollution-free, and low cost. They are considered to be one of the most promising fuel cells at present.
[0003] Planar SOFCs have the best application prospects in the field of fuel cells, with advantages such as high power density, simple production process and low cost. Planar SOFCs stack is a stacked structure with single cells, sealing materials and metal connectors as units; however, the working environment of planar SOFCs stack is harsh, including high working temperature (600-800℃), strong oxidizing and reducing atmosphere and repeated hot and cold cycles. The structural design and working environment of planar SOFCs stack make the stack sealing problem one of the main problems restricting its development.
[0004] At present, the sealing methods of flat-plate SOFCs stacks mainly include: pressure sealing and hard sealing. Pressure sealing is a method of sealing by deforming the sealing material with the help of external pressure. Pressure sealing achieves the sealing effect through physical bonding, so the sealing material and the adjacent components do not need to meet the precise matching of thermal expansion coefficients, and the repair of the stack is simple and convenient; however, the introduction of external pressure in pressure sealing increases the complexity and manufacturing cost of the system, and the airtightness of pressure sealing needs to be improved. Hard sealing is a method of sealing through the bonding effect between the sealing material and the adjacent components. Among them, the glass-based sealing material has a simple sealing method and good airtightness; its required performance can be achieved by adjusting the composition; in addition, its production process is simple, the cost is low, and it is easy to achieve large-scale preparation. Summary of the invention
[0005] The present invention provides a method for preparing a solid oxide fuel cell sealing material. The method is based on a glass-based material, develops a slurry suitable for tape casting, and prepares a sealing gasket with good air tightness, thermal stability, chemical stability and mechanical properties through tape casting.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A first aspect of the present invention provides a method for preparing a solid oxide fuel cell sealing material, comprising the following steps:
[0008] The glass powder, the organic solvent and the dispersant are mixed and ball-milled once, and then a plasticizer and a binder are added and ball-milled twice to obtain a sealing slurry; the sealing slurry is filtered and vacuum-defoamed in turn, and then tape-casted to obtain a green blank; the green blank is dried and cut to obtain the solid oxide fuel cell sealing material;
[0009] The glass powder components include a network former, a network modifier, an intermediate oxide and an additive, and the molar ratio of the network former, the network modifier, the intermediate oxide and the additive is (40-65): (20-45): (2-10): (2-10).
[0010] Preferably, the network former is at least one of SiO2 and B2O3; the network modifier is at least one of BaO, SrO, CaO, and MgO; the intermediate oxide is Al2O3; and the additive is at least one of NiO, TiO2, ZnO, Y2O3, ZrO2, and La2O3.
[0011] Preferably, the preparation method of the glass powder comprises the following steps: weighing the raw materials of the glass powder according to the molar ratio of the network former, the network modifier, the intermediate oxide and the additive, mixing and ball-milling the raw materials, then placing the mixture in a crucible, first heating the temperature to 800-1000°C at 1-3°C / min and keeping it for 2-4h, then heating the temperature to 1300-1550°C at 3-5°C / min and melting it for 2-4h, then placing it in deionized water for quenching to obtain a glass frit; finally, drying the glass frit, crushing it, and ball-milling it to obtain a glass powder.
[0012] Preferably, based on 100wt% of the total mass of the sealing slurry, the glass powder content is 30-60wt%, the organic solvent content is 30-60wt%, the dispersant content is 1-10wt%, the plasticizer content is 1-10wt%, and the binder content is 1-10wt%.
[0013] Preferably, the organic solvent is at least one of alcohols, ketones, and benzenes; the dispersant is at least one of BYK dispersant, triethyl phosphate, and triolein; the plasticizer is at least one of polyethylene glycol, diethyl phthalate, and dibutyl phthalate; the binder includes polyvinyl butyral; specifically, the alcohol is ethanol; the ketone is butanone; and the benzene is xylene.
[0014] Preferably, the rotation speed of the first ball milling is 200-300 rpm, and the first ball milling time is 10-20 h; the rotation speed of the second ball milling is 200-300 rpm, and the second ball milling time is 15-30 h.
[0015] Preferably, during the tape casting process, the temperature in the tape casting chamber is 40-70° C., the bottom mold moving speed is 0.1-1 m / min, and the thickness of the solid oxide fuel cell sealing material is controlled by the height of the scraper.
[0016] The second aspect of the present invention provides a solid oxide fuel cell sealing gasket, which is prepared by the preparation method of the solid oxide fuel cell sealing material; the solid oxide fuel cell sealing gasket has a thickness of 50-300 μm.
[0017] The third aspect of the present invention provides a sealing method for a solid oxide fuel cell, comprising the following steps: placing the solid oxide fuel cell sealing gasket at the location to be sealed of the solid oxide fuel cell, first raising the temperature to 400-600°C at a heating rate of 1-5°C / min, and keeping it warm for 2-6 hours to remove organic matter in the sealing gasket; then raising the temperature to 800-900°C at a heating rate of 1-5°C / min, and keeping it warm for 0.5-5 hours to achieve sealing of the solid oxide fuel cell.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] Based on glass-based materials, a slurry suitable for tape casting has been developed, and a sealing gasket with good air tightness, thermal stability, chemical stability and mechanical properties has been prepared through tape casting. The sealing gasket is suitable for solid oxide fuel cell stacks. In addition, the process of preparing sealing gaskets by tape casting can be operated continuously, with high production efficiency, easy to realize automation, and can be mass-produced. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Leakage rate of the sealing gasket prepared in Example 1 under different ventilation (nitrogen) pressures;
[0021] Figure 2 The leakage rate of the sealing gasket prepared in Example 2 under different ventilation (nitrogen) pressures. DETAILED DESCRIPTION
[0022] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0023] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.
[0024] The composition ratio (molar percentage) of the glass powder in the following embodiments is shown in Table 1:
[0025] Table 1
[0026]
[0027] Example 1
[0028] (1) Preparation of glass powder: SiO2, H3BO3, BaCO3, CaCO3, Al2O3, NiO and La2O3 were weighed according to the ratio of various components of glass powder in Table 1, and were ball-milled on a planetary ball mill for 4 h, then taken out and dried to obtain a mixture; the mixture was placed in a platinum crucible and heated to 800°C at 2°C / min and kept at this temperature for 4 h, then heated to 1500°C at 3°C / min and melted for 3 h, and then the crucible was taken out of the furnace and quenched in deionized water to obtain a glass frit; the glass frit was dried and then crushed, and was ball-milled on a planetary ball mill for 6 h, then taken out and dried, and passed through a 200-mesh sieve to obtain glass powder.
[0029] (2) Preparation of sealing slurry: First, 100 g of glass powder, 55 g of ethanol, 45 g of butanone, and 5 g of DISPERBYK were placed in a ball mill and milled on a planetary ball mill for 12 h at a speed of 250 rpm. Then, 2 g of polyethylene glycol 200, 4.5 g of dibutyl phthalate, and 10 g of polyvinyl butyral were added and the mixture was milled on a planetary ball mill for 18 h at a speed of 250 rpm to obtain sealing slurry.
[0030] (3) Preparation of sealing gasket: The slurry prepared in step (2) is taken out and filtered and vacuum-defoamed in sequence, and then the slurry is poured onto a bottom mold for tape casting. The temperature in the tape casting chamber is 55°C, and the bottom mold moving speed is 0.35 m / min to obtain a blank. The blank is then dried and cut to obtain a solid oxide fuel cell sealing gasket. The thickness of the sealing gasket is controlled to 200 μm by using a scraper height.
[0031] Place the sealing gasket at the place to be sealed of the stainless steel connector. First, increase the temperature to 550°C at a heating rate of 2°C / min and keep it warm for 6 hours to remove organic matter in the sealing gasket; then increase the temperature to 850°C at a heating rate of 2°C / min and keep it warm for 2 hours to achieve the sealing of the stainless steel connector and for the air tightness test of the sealing gasket.
[0032] Figure 1 The leakage rate of the sealing gasket prepared in Example 1 under different ventilation (nitrogen) pressures; the test temperature is 750°C, and the loading pressure is 0.1 MPa; the leakage rates are all less than 0.04 sccm / cm, meeting the SOFC sealing requirements.
[0033] Example 2
[0034] (1) Preparation of glass powder: SiO2, H3BO3, BaCO3, SrCO3, CaCO3, Al2O3, Y2O3 and ZrO2 were weighed according to the ratio of various components of glass powder in Table 1, and were ball-milled on a planetary ball mill for 4 h, then taken out and dried to obtain a mixture; the mixture was placed in a platinum crucible and heated to 1000°C at 2°C / min and kept at this temperature for 2 h, then heated to 1550°C at 5°C / min and melted for 3 h, and then the crucible was taken out of the furnace and quenched in deionized water to obtain a glass frit; the glass frit was dried and then crushed, and was ball-milled on a planetary ball mill for 6 h, then taken out and dried, and passed through a 200-mesh sieve to obtain glass powder.
[0035] (2) Preparation of sealing slurry: First, 100 g of glass powder, 58 g of ethanol, 42 g of butanone, 2 g of triethyl phosphate, and 4.5 g of DISPERBYK were placed in a ball mill and milled on a planetary ball mill for 12 h at a speed of 250 rpm. Then, 2 g of polyethylene glycol 200, 4 g of dibutyl phthalate, and 10 g of polyvinyl butyral were added and the mixture was milled on a planetary ball mill for 18 h at a speed of 250 rpm to obtain sealing slurry.
[0036] (3) Preparation of sealing gasket: The slurry prepared in step (2) is taken out and filtered and vacuum-defoamed in sequence, and then the slurry is poured onto a bottom mold for tape casting. The temperature in the tape casting chamber is 55°C, and the bottom mold moving speed is 0.35 m / min to obtain a blank. The blank is then dried and cut to obtain a solid oxide fuel cell sealing gasket. The thickness of the sealing gasket is controlled to 200 μm by using a scraper height.
[0037] Place the sealing gasket at the place to be sealed of the stainless steel connector. First, increase the temperature to 550°C at a heating rate of 1°C / min and keep it warm for 4 hours to remove organic matter in the sealing gasket; then increase the temperature to 850°C at a heating rate of 1°C / min and keep it warm for 2 hours to achieve the sealing of the stainless steel connector and for the air tightness test of the sealing gasket.
[0038] Figure 2 The leakage rate of the sealing gasket prepared in Example 2 under different ventilation (nitrogen) pressures; the test temperature is 750°C, and the loading pressure is 0.1 MPa; the leakage rates are all less than 0.04 sccm / cm, meeting the SOFC sealing requirements.
[0039] Example 3
[0040] (1) The preparation process of the glass powder in this embodiment refers to that in Embodiment 2.
[0041] (2) Preparation of sealing slurry: First, 100 g of glass powder, 77 g of ethanol, 48 g of butanone, 2 g of triethyl phosphate, and 3 g of DISPERBYK were placed in a ball mill and milled on a planetary ball mill for 12 h at a speed of 250 rpm. Then, 4 g of polyethylene glycol 200, 2 g of dibutyl phthalate, and 12 g of polyvinyl butyral were added and the mixture was milled on a planetary ball mill for 20 h at a speed of 250 rpm to obtain sealing slurry.
[0042] (3) Preparation of sealing gasket: The slurry prepared in step (2) is taken out and filtered and vacuum-defoamed in sequence, and then the slurry is poured onto a bottom mold for tape casting. The temperature in the tape casting chamber is 65°C, and the bottom mold moving speed is 0.40 m / min to obtain a blank. The blank is then dried and cut to obtain a solid oxide fuel cell sealing gasket. The thickness of the sealing gasket is controlled to be 150 μm by using a scraper height.
[0043] Place the sealing gasket at the place to be sealed of the stainless steel connector. First, increase the temperature to 600°C at a heating rate of 2°C / min and keep it warm for 4 hours to remove organic matter in the sealing gasket; then increase the temperature to 850°C at a heating rate of 1°C / min and keep it warm for 1 hour to achieve sealing of the stainless steel connector.
[0044] Example 4
[0045] (1) The preparation process of the glass powder in this embodiment refers to that in Embodiment 2.
[0046] (2) Preparation of sealing slurry: First, 100 g of glass powder, 120 g of ethanol, and 5 g of triethyl phosphate were placed in a ball mill, and ball milled on a planetary ball mill for 12 h at a speed of 250 rpm; then 4.5 g of polyethylene glycol 200, 2 g of dibutyl phthalate, and 12 g of polyvinyl butyral were added, and the mixture was ball milled on a planetary ball mill for 20 h at a speed of 250 rpm to obtain sealing slurry.
[0047] (3) Preparation of sealing gasket: The slurry prepared in step (2) is taken out and filtered and vacuum-defoamed in sequence, and then the slurry is poured onto a bottom mold for tape casting. The temperature in the tape casting chamber is 65°C, and the bottom mold moving speed is 0.40 m / min to obtain a blank. The blank is then dried and cut to obtain a solid oxide fuel cell sealing gasket. The thickness of the sealing gasket is controlled to be 150 μm by using a scraper height.
[0048] Place the sealing gasket at the place to be sealed of the stainless steel connector. First, increase the temperature to 600°C at a heating rate of 1°C / min and keep it warm for 2 hours to remove organic matter in the sealing gasket; then increase the temperature to 850°C at a heating rate of 1°C / min and keep it warm for 0.5 hours to achieve sealing of the stainless steel connector.
[0049] Example 5
[0050] (1) The preparation process of the glass powder in this embodiment refers to that in Embodiment 2.
[0051] (2) Preparation of sealing slurry: First, 100 g of glass powder, 55 g of ethanol, 45 g of butanone, and 5 g of DISPERBYK were placed in a ball mill and milled on a planetary ball mill for 15 h at a speed of 200 rpm. Then, 6.0 g of polyethylene glycol 200, 5.5 g of diethyl phthalate, and 12 g of polyvinyl butyral were added and milled on a planetary ball mill for 24 h at a speed of 200 rpm to obtain sealing slurry.
[0052] (3) Preparation of sealing gasket: The slurry prepared in step (2) is taken out and filtered and vacuum-defoamed in sequence, and then the slurry is poured onto a bottom mold for tape casting. The temperature in the tape casting chamber is 55°C, and the bottom mold moving speed is 0.35 m / min to obtain a blank. The blank is then dried and cut to obtain a solid oxide fuel cell sealing gasket. The thickness of the sealing gasket is controlled to be 250 μm by using a scraper height.
[0053] Place the sealing gasket at the place to be sealed of the stainless steel connector. First, increase the temperature to 600°C at a heating rate of 1°C / min and keep it warm for 6 hours to remove organic matter in the sealing gasket; then increase the temperature to 850°C at a heating rate of 1°C / min and keep it warm for 2 hours to achieve sealing of the stainless steel connector.
[0054] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.
Claims
1. A method for preparing a solid oxide fuel cell sealing material, characterized in that: The following steps are involved: The glass powder, the organic solvent and the dispersant are mixed and ball-milled once, and then a plasticizer and a binder are added and ball-milled twice to obtain a sealing slurry; the sealing slurry is filtered and vacuum-defoamed in turn, and then tape-casted to obtain a green blank; the green blank is dried and cut to obtain the solid oxide fuel cell sealing material; The glass powder components include a network former, a network modifier, an intermediate oxide and an additive, and the molar ratio of the network former, the network modifier, the intermediate oxide and the additive is (40-65): (20-45): (2-10): (2-10).
2. The method for preparing a solid oxide fuel cell sealing material according to claim 1, characterized in that: The network former is at least one of SiO2 and B2O3; the network modifier is at least one of BaO, SrO, CaO, and MgO; the intermediate oxide is Al2O3; and the additive is at least one of NiO, TiO2, ZnO, Y2O3, ZrO2, and La2O3.
3. The method for preparing a solid oxide fuel cell sealing material according to claim 1, characterized in that: The preparation method of the glass powder comprises the following steps: weighing the raw materials of the glass powder according to the molar ratio of the network former, the network modifier, the intermediate oxide and the additive, mixing and ball-milling the raw materials, placing the mixture in a crucible, heating the mixture to 800-1000°C at 1-3°C / min and keeping the temperature for 2-4h, heating the mixture to 1300-1550°C at 3-5°C / min and melting the mixture for 2-4h, placing the mixture in deionized water for quenching to obtain a glass frit; and finally drying the glass frit, crushing it and ball-milling it to obtain a glass powder.
4. The method for preparing a solid oxide fuel cell sealing material according to claim 1, characterized in that: Based on 100wt% of the total mass of the sealing slurry, the glass powder content is 30-60wt%, the organic solvent content is 30-60wt%, the dispersant content is 1-10wt%, the plasticizer content is 1-10wt%, and the binder content is 1-10wt%.
5. The method for preparing a solid oxide fuel cell sealing material according to claim 1, characterized in that: The organic solvent is at least one of alcohols, ketones, and benzenes; the dispersant is at least one of BYK dispersant, triethyl phosphate, and triolein; the plasticizer is at least one of polyethylene glycol, diethyl phthalate, and dibutyl phthalate; and the binder includes polyvinyl butyral.
6. The method for preparing a solid oxide fuel cell sealing material according to claim 1, characterized in that: The rotation speed of the first ball milling is 200-300 rpm, and the first ball milling time is 10-20 hours; the rotation speed of the second ball milling is 200-300 rpm, and the second ball milling time is 15-30 hours.
7. The method for preparing a solid oxide fuel cell sealing material according to claim 1, characterized in that: During the tape casting process, the temperature in the tape casting chamber is 40-70° C., the bottom mold moving speed is 0.1-1 m / min, and the thickness of the solid oxide fuel cell sealing material is controlled by the height of the scraper.
8. A solid oxide fuel cell sealing gasket, characterized in that: The solid oxide fuel cell sealing gasket is prepared by the preparation method of the solid oxide fuel cell sealing material according to any one of claims 1 to 7; the thickness of the solid oxide fuel cell sealing gasket is 50-300 μm.
9. A method for sealing a solid oxide fuel cell, characterized in that: The method comprises the following steps: placing the solid oxide fuel cell sealing gasket described in claim 8 at the location to be sealed of the solid oxide fuel cell, first raising the temperature to 400-600°C at a heating rate of 1-5°C / min, and keeping the temperature for 2-6 hours to remove organic matter in the sealing gasket; then raising the temperature to 800-900°C at a heating rate of 1-5°C / min, and keeping the temperature for 0.5-5 hours to achieve sealing of the solid oxide fuel cell.
Citation Information
Patent Citations
Solid oxide fuel cell composite sealing material as well as preparation method and application thereof
CN112521011A
High-strength stable sealing material for solid oxide fuel cell and application of high-strength stable sealing material
CN115838248A
High-strength sealing material for medium-high temperature solid oxide fuel cell and preparation method of high-strength sealing material
CN116063001A
Sealant for solid oxide fuel cell and method for manufacturing the same
KR1020120075240A
Method for producing a solder glass green seal
US20160072137A1