Composite solid electrolyte membrane, preparation method and lithium battery

Through the composite of polymer solid electrolytes, lithium salts and oxide solid electrolytes, ball milling and vacuum defoaming processes, the problem of uneven dispersion between oxide solid electrolytes and polymer electrolytes is solved, and the performance of composite solid electrolyte membranes is significantly improved and Cycling performance of lithium batteries.

CN119050467APending Publication Date: 2024-11-29ANHUI LEOCH PENEWABLE ENERGY DEV CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411236285.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The dispersion of oxide solid electrolytes and polymer electrolytes in the composite membrane is uneven, resulting in inconsistent performance.

Method used

A uniformly dispersed composite solid electrolyte membrane is prepared by using the composite method of polymer solid electrolyte, lithium salt and oxide solid electrolyte, through ball milling and vacuum defoaming processes.

Benefits of technology

The substance dispersion and circulation performance of the electrolyte membrane are improved, ensuring that the capacity retention rate of lithium batteries reaches more than 70% after 100 cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005027807320000071
    Figure BDA0005027807320000071
  • Figure BDA0005027807320000111
    Figure BDA0005027807320000111
Patent Text Reader

Abstract

The invention discloses a composite solid electrolyte membrane, a preparation method and a lithium battery, and relates to the technical field of electrolyte membranes. The composite solid electrolyte membrane is prepared from 30-50 wt% of a polymer solid electrolyte, 20 wt% of a lithium salt and 30-50 wt% of an oxide solid electrolyte. The preparation method of the composite solid electrolyte membrane comprises the following steps: S1, mixing a polymer solid electrolyte, a lithium salt and an oxide solid electrolyte, and carrying out ball milling to obtain a colloidal mixture; s2, carrying out vacuum defoaming on the prepared colloidal mixture; s3, the mixture obtained after defoaming is dried; and S4, carrying out hot rolling on the dried mixture to obtain the composite solid electrolyte membrane. The invention also provides a lithium battery comprising the electrolyte membrane. The polymer solid electrolyte, the lithium salt and the oxide solid electrolyte are compounded, and a ball milling process is matched with a defoaming technology, so that the substance dispersity in the composite solid electrolyte membrane can be effectively improved, and the cycle performance of the prepared battery is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of electrolyte membranes, and in particular to a composite solid electrolyte membrane, a preparation method, and a lithium battery. Background Art

[0002] Oxide solid electrolytes have good thermal stability, a wide electrochemical window, and high mechanical strength. However, their disadvantages are general conductivity, high brittleness, difficulty in processing, and poor interface contact. Existing technologies allow them to be compounded with polymers, which can significantly improve the toughness of the product, increase the conductivity of the product, and reduce the interface resistance.

[0003] However, since both oxide solid electrolytes and polymer electrolytes are solid and do not have good dispersibility, this will lead to uneven dispersion of oxide solid electrolytes and polymer electrolytes in the prepared electrolyte membrane and different performance, thus affecting the performance of the prepared electrolyte membrane. Summary of the Invention

[0004] In order to solve at least one of the above technical problems, an electrolyte membrane in which an oxide solid electrolyte and a polymer electrolyte can be evenly dispersed is developed. The present application provides a composite solid electrolyte membrane, a preparation method, and a lithium battery.

[0005] In one aspect, the present application provides a composite solid electrolyte membrane, which is prepared from the following components by weight percentage:

[0006] Polymer solid electrolyte 30-50wt%;

[0007] Lithium salt 20wt%;

[0008] Oxide solid electrolyte 30-50wt%.

[0009] Optionally, the polymer solid electrolyte is a combination of one or more of polyethylene oxide, polyvinylidene fluoride and polyacrylonitrile.

[0010] Optionally, the lithium salt is lithium bis(trifluoromethanesulfonyl)imide, lithium perchlorate, or a combination of the two.

[0011] Optionally, the oxide solid electrolyte is powdered lithium lanthanum titanate.

[0012] In a second aspect, the present application provides a method for preparing the above-mentioned composite solid electrolyte membrane, comprising the following steps:

[0013] S1. Mixing a polymer solid electrolyte, a lithium salt, and an oxide solid electrolyte, and ball-milling the mixture to obtain a colloidal mixture;

[0014] S2, vacuum degassing the obtained colloidal mixture;

[0015] S3, drying the deaerated mixture;

[0016] S4. Hot rolling the dried mixture to obtain a composite solid electrolyte membrane.

[0017] Optionally, the ball milling process in S1 is as follows: ball milling temperature is 100° C., ball milling speed is 600 r / min, and ball milling time is 8 h.

[0018] Optionally, the ball milling process in S1 is:

[0019] The first step is ball milling at a temperature of 100°C, a speed of 600 r / min, and a time of 2 to 4 h.

[0020] The first step is ball milling temperature of 25 ° C, ball milling speed of 600 r / min, and ball milling time of 5 to 10 minutes;

[0021] The first step is to set the ball milling temperature at 100°C, the ball milling speed at 600 r / min, and the ball milling time at 2 to 4 h.

[0022] Optionally, in S2, the drying temperature is 80°C.

[0023] Optionally, in S3, the hot rolling process is: double-roll hot rolling at a hot rolling temperature of 100°C.

[0024] In a third aspect, the present application provides a lithium battery comprising an electrolyte membrane, wherein the electrolyte membrane is the composite solid electrolyte membrane prepared according to claim 1, and the thickness of the composite solid electrolyte membrane is 20 to 100 μm.

[0025] In summary, the present application can effectively improve the dispersion of materials in the composite solid electrolyte membrane and effectively improve the cycle performance of the prepared battery by compounding polymer solid electrolyte, lithium salt and oxide solid electrolyte, and coordinating the ball milling process with defoaming technology. DETAILED DESCRIPTION

[0026] The present application is further described in detail below with reference to the embodiments.

[0027] In the following examples of this application, unless otherwise specified, all products were purchased from commercially available products.

[0028] Lithium lanthanum titanate: powder, particle size not exceeding 10μm.

[0029] Example 1

[0030] This embodiment is used to prepare a composite solid electrolyte membrane, which is prepared from 30 wt % PEO (polyethylene oxide), 20 wt % LiTFSI (lithium bis(trifluoromethanesulfonyl)imide) and 50 wt % LLTO (lithium lanthanum titanate).

[0031] According to the above formula, PEO, LiTFSI, and LLTO were weighed and added to a ball ink tank, and ball milled using a planetary ball mill. The ball ink temperature was 100°C, the ball mill speed was 600 r / min, and the ball milling time was 8 h to obtain a colloidal mixture.

[0032] The resulting colloidal mixture was placed in a vacuum degasser and degassed under stirring until the colloidal mixture was uniform and no bubbles were visible on the surface. The resulting colloidal mixture was then dried in a vacuum drying oven at 80°C overnight. Subsequently, the dried colloidal mixture was hot-rolled (hot-rolling temperature: 100°C) to obtain a composite solid electrolyte membrane with a thickness of 50 μm.

[0033] Example 2

[0034] This embodiment is used to prepare a composite solid electrolyte membrane, which is prepared from 35wt% PVDF (polyvinylidene fluoride), 20wt% LiTFSI (lithium bis(trifluoromethanesulfonyl)imide) and 45wt% LLTO (lithium lanthanum titanate).

[0035] According to the above formula, PVDF, LiTFSI, and LLTO were weighed respectively and added into a ball ink tank, and ball milled using a planetary ball mill. The ball ink temperature was 100°C, the ball mill speed was 600 r / min, and the ball milling time was 8 h to obtain a colloidal mixture.

[0036] The resulting colloidal mixture was placed in a vacuum degasser and degassed under stirring until the colloidal mixture was uniform and no bubbles were visible on the surface. The resulting colloidal mixture was then dried in a vacuum drying oven at 80°C overnight. Subsequently, the dried colloidal mixture was hot-rolled (hot-rolling temperature: 100°C) to obtain a composite solid electrolyte membrane with a thickness of 50 μm.

[0037] Example 3

[0038] This embodiment is used to prepare a composite solid electrolyte membrane, which is prepared from 40 wt % PAN (polyacrylonitrile), 20 wt % LiTFSI (lithium bis(trifluoromethanesulfonyl)imide) and 40 wt % LLTO (lithium lanthanum titanate).

[0039] According to the above formula, PAN, LiTFSI, and LLTO were weighed respectively and added into a ball ink tank, and ball milled using a planetary ball mill. The ball ink temperature was 100°C, the ball mill speed was 600 r / min, and the ball milling time was 8 h to obtain a colloidal mixture.

[0040] The resulting colloidal mixture was placed in a vacuum degasser and degassed under stirring until the colloidal mixture was uniform and no bubbles were visible on the surface. The resulting colloidal mixture was then dried in a vacuum drying oven at 80°C overnight. Subsequently, the dried colloidal mixture was hot-rolled (hot-rolling temperature: 100°C) to obtain a composite solid electrolyte membrane with a thickness of 50 μm.

[0041] Example 4

[0042] This embodiment is used to prepare a composite solid electrolyte membrane, which is prepared from 30wt% PEO (polyethylene oxide), 20wt% LiClO4 (lithium perchlorate) and 50wt% LLTO (lithium lanthanum titanate).

[0043] According to the above formula, PEO, LiClO4, and LLTO were weighed respectively and added into a ball ink tank, and ball milled using a planetary ball mill. The ball ink temperature was 100°C, the ball mill speed was 600 r / min, and the ball milling time was 8 h to obtain a colloidal mixture.

[0044] The resulting colloidal mixture was placed in a vacuum degasser and degassed under stirring until the colloidal mixture was uniform and no bubbles were visible on the surface. The resulting colloidal mixture was then dried in a vacuum drying oven at 80°C overnight. Subsequently, the dried colloidal mixture was hot-rolled (hot-rolling temperature: 100°C) to obtain a composite solid electrolyte membrane with a thickness of 50 μm.

[0045] Example 5

[0046] This embodiment is used to prepare a composite solid electrolyte membrane, which is prepared from 35wt% PVDF (polyvinylidene fluoride), 20wt% LiClO4 (lithium perchlorate) and 45wt% LLTO (lithium lanthanum titanate).

[0047] According to the above formula, PVDF, LiClO4, and LLTO were weighed respectively and added into a ball ink tank, and ball milled using a planetary ball mill. The ball ink temperature was 100°C, the ball mill speed was 600 r / min, and the ball milling time was 8 h to obtain a colloidal mixture.

[0048] The resulting colloidal mixture was placed in a vacuum degasser and degassed under stirring until the colloidal mixture was uniform and no bubbles were visible on the surface. The resulting colloidal mixture was then dried in a vacuum drying oven at 80°C overnight. Subsequently, the dried colloidal mixture was hot-rolled (hot-rolling temperature: 100°C) to obtain a composite solid electrolyte membrane with a thickness of 50 μm.

[0049] Example 6

[0050] This embodiment is used to prepare a composite solid electrolyte membrane, which is prepared from 40wt% PAN (polyacrylonitrile), 20wt% LiClO4 (lithium perchlorate) and 40wt% LLTO (lithium lanthanum titanate).

[0051] According to the above formula, PAN, LiClO4, and LLTO were weighed respectively and added into a ball ink tank, and ball milled using a planetary ball mill. The ball ink temperature was 100°C, the ball mill speed was 600 r / min, and the ball milling time was 8 h to obtain a colloidal mixture.

[0052] The resulting colloidal mixture was placed in a vacuum degasser and degassed under stirring until the colloidal mixture was uniform and no bubbles were visible on the surface. The resulting colloidal mixture was then dried in a vacuum drying oven at 80°C overnight. Subsequently, the dried colloidal mixture was hot-rolled (hot-rolling temperature: 100°C) to obtain a composite solid electrolyte membrane with a thickness of 50 μm.

[0053] Comparative Example 1

[0054] This comparative example is used to prepare an electrolyte membrane, which is prepared from 20 wt % of LiTFSI and 80 wt % of LLTO.

[0055] According to the above formula, LiTFSI and LLTO were weighed and added into a ball ink tank, and ball milled using a planetary ball mill. The ball ink temperature was 100°C, the ball mill speed was 600 r / min, and the ball milling time was 8 h to obtain a colloidal mixture.

[0056] The resulting colloidal mixture was placed in a vacuum degasser and degassed under stirring until the colloidal mixture was uniform and no bubbles were visible on the surface. The resulting colloidal mixture was then dried in a vacuum drying oven at 80°C overnight. Subsequently, the dried colloidal mixture was hot-rolled (hot-rolling temperature: 100°C) to obtain a composite solid electrolyte membrane with a thickness of 50 μm.

[0057] The electrolyte membranes prepared in the above Examples 1 to 6 and Comparative Example 1 were assembled into CR2032 button batteries 1 to 7 in the order of positive electrode sheet-electrolyte membrane-lithium sheet.

[0058] The CR2032 button cell was charged at a constant current and constant voltage of 0.5C to 3.95V, with a cut-off current of 0.05C, and then discharged at a constant current of 0.5C to 1.5V for 100 cycles. The test results are shown in Table 1.

[0059] Table 1

[0060]

[0061] It can be seen from Examples 1 to 6, Comparative Example 1 and Table 1 that the present application can effectively improve the dispersion of substances in the composite solid electrolyte membrane by compounding polymer solid electrolyte, lithium salt and oxide solid electrolyte, and coordinating the ball milling process with defoaming technology. The cycle performance of the prepared battery can achieve a capacity retention rate of more than 70% after 100 cycles.

[0062] Based on the above embodiments, the inventors improved the ball milling process and verified it through Examples 7 to 12.

[0063] Example 7

[0064] This embodiment is used to prepare a composite solid electrolyte membrane, which is prepared from 30 wt % PEO (polyethylene oxide), 20 wt % LiTFSI (lithium bis(trifluoromethanesulfonyl)imide) and 50 wt % LLTO (lithium lanthanum titanate).

[0065] According to the above formula, PEO, LiTFSI, and LLTO were weighed and added to a ball ink tank, and ball milled using a planetary ball mill. The ball milling process is as follows:

[0066] In the first step, the temperature of the spherical graphite is 100°C, the ball mill speed is 600 r / min, and the ball milling time is 2 h;

[0067] In the second step, the temperature of the spherical graphite is 25°C, the ball milling speed is 600 r / min, and the ball milling time is 10 min;

[0068] The third step is to set the spherical graphite temperature to 100°C, the ball mill speed to 600 r / min, and the ball milling time to 4 h.

[0069] The resulting colloidal mixture was placed in a vacuum degasser and degassed under stirring until the colloidal mixture was uniform and no bubbles were visible on the surface. The resulting colloidal mixture was then dried in a vacuum drying oven at 80°C overnight. Subsequently, the dried colloidal mixture was hot-rolled (hot-rolling temperature: 100°C) to obtain a composite solid electrolyte membrane with a thickness of 50 μm.

[0070] Example 8

[0071] This embodiment is used to prepare a composite solid electrolyte membrane, which is prepared from 35wt% PVDF (polyvinylidene fluoride), 20wt% LiTFSI (lithium bis(trifluoromethanesulfonyl)imide) and 45wt% LLTO (lithium lanthanum titanate).

[0072] According to the above formula, PVDF, LiTFSI, and LLTO were weighed and added to a ball ink tank, and ball milled using a planetary ball mill. The ball milling process is as follows:

[0073] In the first step, the temperature of the spherical graphite is 100°C, the ball mill speed is 600 r / min, and the ball milling time is 2 h;

[0074] In the second step, the temperature of the spherical graphite is 25°C, the ball milling speed is 600 r / min, and the ball milling time is 10 min;

[0075] The third step is to set the spherical graphite temperature to 100°C, the ball mill speed to 600 r / min, and the ball milling time to 4 h.

[0076] The resulting colloidal mixture was placed in a vacuum degasser and degassed under stirring until the colloidal mixture was uniform and no bubbles were visible on the surface. The resulting colloidal mixture was then dried in a vacuum drying oven at 80°C overnight. Subsequently, the dried colloidal mixture was hot-rolled (hot-rolling temperature: 100°C) to obtain a composite solid electrolyte membrane with a thickness of 50 μm.

[0077] Example 9

[0078] This embodiment is used to prepare a composite solid electrolyte membrane, which is prepared from 40 wt % PAN (polyacrylonitrile), 20 wt % LiTFSI (lithium bis(trifluoromethanesulfonyl)imide) and 40 wt % LLTO (lithium lanthanum titanate).

[0079] According to the above formula, PAN, LiTFSI, and LLTO were weighed and added to a ball ink tank, and ball milled using a planetary ball mill. The ball milling process is as follows:

[0080] In the first step, the temperature of the spherical graphite is 100°C, the ball mill speed is 600 r / min, and the ball milling time is 3 h;

[0081] In the second step, the temperature of the spherical graphite is 25°C, the ball milling speed is 600 r / min, and the ball milling time is 8 min;

[0082] The third step is to set the spherical graphite temperature to 100°C, the ball mill speed to 600 r / min, and the ball milling time to 3 h.

[0083] The resulting colloidal mixture was placed in a vacuum degasser and degassed under stirring until the colloidal mixture was uniform and no bubbles were visible on the surface. The resulting colloidal mixture was then dried in a vacuum drying oven at 80°C overnight. Subsequently, the dried colloidal mixture was hot-rolled (hot-rolling temperature: 100°C) to obtain a composite solid electrolyte membrane with a thickness of 50 μm.

[0084] Example 10

[0085] This embodiment is used to prepare a composite solid electrolyte membrane, which is prepared from 30wt% PEO (polyethylene oxide), 20wt% LiClO4 (lithium perchlorate) and 50wt% LLTO (lithium lanthanum titanate).

[0086] According to the above formula, PEO, LiClO4, and LLTO were weighed and added into the ball ink tank, and ball milled using a planetary ball mill. The ball milling process is as follows:

[0087] In the first step, the temperature of the spherical graphite is 100°C, the ball mill speed is 600 r / min, and the ball milling time is 3 h;

[0088] In the second step, the temperature of the spherical graphite is 25°C, the ball milling speed is 600 r / min, and the ball milling time is 8 min;

[0089] The third step is to set the spherical graphite temperature to 100°C, the ball mill speed to 600 r / min, and the ball milling time to 3 h.

[0090] The resulting colloidal mixture was placed in a vacuum degasser and degassed under stirring until the colloidal mixture was uniform and no bubbles were visible on the surface. The resulting colloidal mixture was then dried in a vacuum drying oven at 80°C overnight. Subsequently, the dried colloidal mixture was hot-rolled (hot-rolling temperature: 100°C) to obtain a composite solid electrolyte membrane with a thickness of 50 μm.

[0091] Example 11

[0092] This embodiment is used to prepare a composite solid electrolyte membrane, which is prepared from 35wt% PVDF (polyvinylidene fluoride), 20wt% LiClO4 (lithium perchlorate) and 45wt% LLTO (lithium lanthanum titanate).

[0093] According to the above formula, PVDF, LiClO4, and LLTO were weighed and added to the ball ink tank, and ball milled using a planetary ball mill. The ball milling process is as follows:

[0094] In the first step, the ball graphite temperature is 100°C, the ball mill speed is 600 r / min, and the ball milling time is 4 h;

[0095] In the second step, the temperature of the spherical graphite is 25°C, the ball milling speed is 600r / min, and the ball milling time is 5min;

[0096] The third step is to set the spherical graphite temperature to 100°C, the ball mill speed to 600 r / min, and the ball milling time to 2 h.

[0097] The resulting colloidal mixture was placed in a vacuum degasser and degassed under stirring until the colloidal mixture was uniform and no bubbles were visible on the surface. The resulting colloidal mixture was then dried in a vacuum drying oven at 80°C overnight. Subsequently, the dried colloidal mixture was hot-rolled (hot-rolling temperature: 100°C) to obtain a composite solid electrolyte membrane with a thickness of 50 μm.

[0098] Example 12

[0099] This embodiment is used to prepare a composite solid electrolyte membrane, which is prepared from 40wt% PAN (polyacrylonitrile), 20wt% LiClO4 (lithium perchlorate) and 40wt% LLTO (lithium lanthanum titanate).

[0100] According to the above formula, PAN, LiClO4, and LLTO were weighed and added to the ball ink tank, and ball milled using a planetary ball mill. The ball milling process is as follows:

[0101] In the first step, the ball graphite temperature is 100°C, the ball mill speed is 600 r / min, and the ball milling time is 4 h;

[0102] In the second step, the temperature of the spherical graphite is 25°C, the ball milling speed is 600r / min, and the ball milling time is 5min;

[0103] The third step is to set the spherical graphite temperature to 100°C, the ball mill speed to 600 r / min, and the ball milling time to 2 h.

[0104] The resulting colloidal mixture was placed in a vacuum degasser and degassed under stirring until the colloidal mixture was uniform and no bubbles were visible on the surface. The resulting colloidal mixture was then dried in a vacuum drying oven at 80°C overnight. Subsequently, the dried colloidal mixture was hot-rolled (hot-rolling temperature: 100°C) to obtain a composite solid electrolyte membrane with a thickness of 50 μm.

[0105] The electrolyte membranes prepared in the above Examples 7 to 12 were assembled into CR2032 button batteries 8 to 13 in the order of positive electrode sheet-electrolyte membrane-lithium sheet.

[0106] The CR2032 button cell was charged at a constant current and constant voltage of 0.5C to 3.95V, with a cutoff current of 0.05C, and then discharged at a constant current of 0.5C to 1.5V for 100 cycles. The test results are shown in Table 2.

[0107] Table 2

[0108]

[0109] As shown in Examples 7-12 and Table 2, this application further improves the ball milling process. By reducing the temperature of the intermediate ball milling process to room temperature during the initial ball milling process and the overall ball milling time, the resulting battery exhibits cycle performance with a capacity retention rate exceeding 80% after 100 cycles. The inventors speculate that this is because after stirring at 100°C for 2-4 hours, the polymer solid electrolyte material and the oxide solid electrolyte material form bridges to form larger particles. Cooling the mixture allows these bridged large particles to cool and form. These large particles are more easily displaced by mechanical stirring than the polymer solid electrolyte material and the oxide solid electrolyte material, resulting in better dispersion. This accelerates the mixing and dispersion of the polymer solid electrolyte material and the oxide solid electrolyte material. Further heating and stirring reduces the internal bonding force of these large particles, further enhancing the mixing of the materials between adjacent large particles. This reduces stirring time and improves dispersion, resulting in improved electrical properties of the resulting electrolyte membrane.

[0110] The above are all preferred embodiments of the present application, and are not intended to limit the scope of protection of the present application. Therefore, any equivalent changes made based on the structure, shape, and principle of the present application should be included in the scope of protection of the present application.

Claims

1. A composite solid electrolyte membrane, characterized in that: Prepared from the following components by weight percentage: Polymer solid electrolyte 30-50wt%; Lithium salt 20wt%; Oxide solid electrolyte 30-50wt%.

2. The composite solid electrolyte membrane according to claim 1, characterized in that: The polymer solid electrolyte is one or more combinations of polyethylene oxide, polyvinylidene fluoride and polyacrylonitrile.

3. The composite solid electrolyte membrane according to claim 1, characterized in that: The lithium salt is selected from lithium bis(trifluoromethanesulfonyl)imide and lithium perchlorate, or a combination of the two.

4. The composite solid electrolyte membrane according to claim 1, characterized in that: The oxide solid electrolyte uses powdered lithium lanthanum titanate.

5. A method for preparing the composite solid electrolyte membrane according to claim 1, characterized in that: The following steps are involved: S1, mixing a polymer solid electrolyte, a lithium salt, and an oxide solid electrolyte, and ball-milling the mixture to obtain a colloidal mixture; S2, vacuum degassing the obtained colloidal mixture; S3, drying the deaerated mixture; S4. The dried mixture is hot-rolled to obtain a composite solid electrolyte membrane.

6. The preparation method according to claim 5, characterized in that: The ball milling process in S1 is as follows: ball milling temperature is 100° C., ball milling speed is 600 r / min, and ball milling time is 8 h.

7. The preparation method according to claim 5, characterized in that: The ball milling process in S1 is: The first step is ball milling temperature of 100°C, ball milling speed of 600r / min, and ball milling time of 2 to 4h; The first step is ball milling temperature of 25°C, ball milling speed of 600r / min, and ball milling time of 5 to 10min; The first step is to set the ball milling temperature to 100°C, the ball milling speed to 600r / min, and the ball milling time to 2 to 4h.

8. The preparation method according to claim 5, characterized in that: In the step S2, the drying temperature is 80°C.

9. The preparation method according to claim 5, characterized in that: In S3, the hot rolling process is: hot rolling by double rolls at a hot rolling temperature of 100°C.

10. A lithium battery, characterized in that: The invention comprises an electrolyte membrane, wherein the electrolyte membrane adopts the composite solid electrolyte membrane prepared in claim 1, and the thickness of the composite solid electrolyte membrane is 20-100 μm.

Citation Information

Cited By

  • Organic-inorganic composite solid electrolyte membrane incorporated with redox mediator, method of preparing large-area membrane thereof, and lithium air battery comprising the same

    KR102906284B1