Water-based rechargeable zinc ion battery with double SEI and CEI layers and preparation method of water-based rechargeable zinc ion battery

By introducing DTPA-Na into the aqueous zinc ion battery to form a double-layer SEI and CEI layers, the problem of zinc negative electrode dendrite and hydrogen evolution reaction is solved, the cycle stability and self-discharge performance of the battery are significantly improved, and efficient zinc ions are achieved Battery application.

CN119050504APending Publication Date: 2024-11-29TSINGHUA SHENZHEN INTERNATIONAL GRADUATE SCHOOL
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411158055.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The zinc negative electrode has problems with dendrite formation, corrosion and hydrogen evolution reaction in aqueous zinc ion batteries, resulting in a decrease in battery performance and life, and the manganese-based positive electrode material has problems such as dissolution, capacity attenuation and poor self-discharge performance.

Method used

The aqueous zinc-ion battery is rechargeable by using a double-layer solid electrolyte interface mask (SEI) and a cathode electrolyte interface mask (CEI) layer. By adding diethylene triamine pentaacetate sodium salt (DTPA-Na) to the electrolyte as an additive, it is formed. The stable SEI layer and CEI layer inhibit the growth and side reaction of zinc dendrites, and improve the uniformity of zinc deposition and the stability of the positive electrode material.

Benefits of technology

Effectively inhibit the growth of zinc dendrites and the generation of by-products, improve the battery cycle stability and self-discharge performance, and the capacity retention rate after 720 hours of self-discharge is as high as 98.61%, significantly improving the stability of zinc negative electrode and the overall efficiency of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050504A_ABST
    Figure CN119050504A_ABST
Patent Text Reader

Abstract

A water-based rechargeable zinc ion battery with double SEI and CEI layers comprises a positive electrode, a negative electrode, a diaphragm and an electrolyte, and the positive electrode comprises a manganese-based oxide positive electrode material; the negative electrode comprises metal zinc; and the electrolyte is a zinc sulfate aqueous solution containing a diethylenetriamine pentaacetic acid sodium salt DTPA-Na additive. The preparation method of the aqueous rechargeable zinc ion battery comprises the following steps: preparing a manganese-based oxide positive electrode material through a hydrothermal method; metal zinc is used as a negative electrode material; dissolving DTPA-Na in a zinc sulfate aqueous solution to prepare an electrolyte; and sequentially assembling the prepared positive electrode, negative electrode and diaphragm, injecting electrolyte, and sealing the battery. And diethylenetriamine pentaacetic acid sodium salt DTPA-Na is introduced as an electrolyte additive. And the DTPA-Na can form a stable multi-layer SEI layer on the surface of the negative electrode, so that the hydrogen evolution reaction and the generation of byproducts are effectively inhibited, and uniform zinc deposition is promoted, thereby inhibiting dendritic crystal growth. Meanwhile, the DTPA-Na is also beneficial for forming a CEI layer on the positive electrode, so that the dissolution of active substances is reduced, and the cycling stability and the self-discharge performance of the battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of new energy materials, and in particular to an aqueous rechargeable zinc ion battery having a double-layer solid electrolyte interface (SEI) and a cathode electrolyte interface (CEI) and a preparation method thereof. Background Art

[0002] Rechargeable aqueous zinc-ion batteries (ZIBs) have become a potential alternative to traditional lithium-ion batteries due to their cost-effectiveness, environmental friendliness, and safety. However, challenges faced by zinc anodes, including dendrite formation, corrosion, and hydrogen evolution reaction, have hindered the widespread application of ZIBs. These problems can lead to decreased battery performance and lifespan. To overcome these obstacles, researchers have explored a variety of strategies to improve the stability and functionality of zinc anodes, such as using advanced anode materials or coatings, adjusting electrolyte composition, etc. However, most methods mainly focus on anode improvements, while ignoring the simultaneous improvement of anode and cathode performance. In particular, manganese-based cathode materials also have problems such as dissolution leading to capacity decay, shortened lifespan, and poor self-discharge performance.

[0003] It should be noted that the information disclosed in the above background technology section is only used for understanding the background of the present application, and therefore may include information that does not constitute prior art known to ordinary technicians in the field. Summary of the invention

[0004] The main purpose of the present invention is to solve the problems existing in the above-mentioned background technology and provide an aqueous rechargeable zinc ion battery with double SEI and CEI layers and a preparation method thereof.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] A water-based rechargeable zinc ion battery with a double-layer SEI and CEI layer comprises a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode comprises a manganese-based oxide positive electrode material; the negative electrode comprises metallic zinc; and the electrolyte is a zinc sulfate aqueous solution containing a diethylenetriaminepentaacetic acid sodium salt DTPA-Na additive.

[0007] Furthermore, the manganese-based oxide positive electrode material is MnOOH.

[0008] Furthermore, the concentration of the DTPA-Na is 0.1wt% to 1wt%.

[0009] Furthermore, the concentration of the DTPA-Na is 0.5wt%.

[0010] Furthermore, the diaphragm is a glass fiber diaphragm.

[0011] A method for preparing the aqueous rechargeable zinc ion battery comprises the following steps:

[0012] Positive electrode preparation: Manganese-based oxide positive electrode materials were prepared by hydrothermal method;

[0013] Negative electrode preparation: Use metallic zinc as the negative electrode material;

[0014] Preparation of electrolyte: dissolving DTPA-Na in an aqueous solution of zinc sulfate to prepare an electrolyte;

[0015] Battery assembly: Assemble the prepared positive electrode, negative electrode and separator in sequence, inject electrolyte, and seal the battery.

[0016] Furthermore, the hydrothermal method for preparing the MnOOH positive electrode material specifically includes: dissolving potassium permanganate and ammonium chloride in deionized water, stirring at room temperature and then transferring to a hydrothermal autoclave, first reacting at a constant temperature of 180° C., then reacting at a constant temperature of 140° C., cooling naturally, filtering and rinsing with deionized water and anhydrous ethanol, and drying the obtained solid and then grinding and sieving.

[0017] Further, 1 mM potassium permanganate and 1 mM ammonium chloride were dissolved in 50 ml of deionized water.

[0018] An electrolyte contains diethylenetriamine pentaacetic acid sodium salt DTPA-Na and zinc sulfate, wherein the concentration of DTPA-Na is 0.1wt% to 1wt%.

[0019] Furthermore, the concentration of the DTPA-Na is 0.5wt%.

[0020] The present invention has the following beneficial effects:

[0021] The present invention provides an aqueous rechargeable zinc ion battery having a double-layer solid electrolyte interface (SEI) and a cathode electrolyte interface (CEI) and a preparation method thereof, which can effectively inhibit zinc dendrite growth and side reactions and improve battery cycle stability and coulomb efficiency.

[0022] The present invention introduces diethylenetriamine pentaacetic acid sodium salt (DTPA-Na) as a unique electrolyte additive. DTPA-Na can not only form a stable SEI layer on the negative electrode, enhance corrosion resistance and reduce hydrogen evolution reaction, but also help to form a CEI layer on the positive electrode, thereby significantly reducing the generation of by-product zinc sulfate hydroxide (ZHS) and improving the overall battery efficiency.

[0023] The main advantages of the present invention are:

[0024] 1. By adding DTPA-Na, a multi-layer SEI layer can be formed on the surface of the zinc negative electrode, which effectively inhibits the hydrogen evolution reaction and the formation of ZHS by-products, promotes uniform zinc deposition, and thus inhibits dendrite growth.

[0025] 2. DTPA-Na changed the zinc deposition behavior, significantly inhibited dendrite formation, and improved the stability and reversibility of the zinc anode.

[0026] 3. The electrolyte containing DTPA-Na exhibits a lower nucleation overpotential, reduced charge transfer resistance, and promotes a uniform electric field, leading to more uniform Zn deposition and stripping.

[0027] 4. The Zn||MnOOH full battery prepared by the method of the present invention exhibits excellent cycle stability, and the capacity retention rate is as high as 98.61% after self-discharge for 720 hours.

[0028] This invention paves the way for practical applications of ZIBs in large-scale, low-cost energy storage solutions.

[0029] Other beneficial effects of the embodiments of the present invention will be further described below. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The DTPA-Na additive of the embodiment of the present invention is to Zn 2+ Regulatory role of the solvation sheath.

[0031] Figure 2 The present invention provides theoretical and experimental research on the inhibition of zinc negative electrode side reactions.

[0032] Figure 3 The structure and composition of the zinc negative electrode of the embodiment of the present invention are characterized.

[0033] Figure 4 The composition and microstructure of the SEI layer of the zinc negative electrode after cycling in the embodiment of the present invention.

[0034] Figure 5 The composition and morphology of the zinc negative electrode after different cycle times in the embodiments of the present invention.

[0035] Figure 6 The electrochemical performance of the embodiments of the present invention using ZSO and ZSO+DTPA-Na as electrolytes.

[0036] Figure 7 Graph showing the cycle performance of the Zn||MnOOH battery according to an embodiment of the present invention.

[0037] Figure 8 1 is the composition and microstructure of the positive electrode CEI layer of an embodiment of the present invention. DETAILED DESCRIPTION

[0038] The following is a detailed description of the embodiments of the present invention. It should be emphasized that the following description is only exemplary and is not intended to limit the scope and application of the present invention.

[0039] An embodiment of the present invention provides an aqueous rechargeable zinc ion battery with a double-layer SEI and CEI layer, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode comprises a manganese-based oxide positive electrode material; the negative electrode comprises metallic zinc; and the electrolyte is an aqueous solution of zinc sulfate containing a diethylenetriaminepentaacetic acid sodium salt DTPA-Na additive.

[0040] The preparation method of the aqueous rechargeable zinc ion battery comprises the following steps: positive electrode preparation: preparing a manganese-based oxide positive electrode material by a hydrothermal method; negative electrode preparation: using metal zinc as the negative electrode material; electrolyte preparation: dissolving DTPA-Na in a zinc sulfate aqueous solution to prepare an electrolyte; battery assembly: assembling the prepared positive electrode, negative electrode and diaphragm in sequence, injecting the electrolyte, and sealing the battery.

[0041] The embodiment of the present invention proposes an aqueous rechargeable zinc ion battery having a double-layer solid electrolyte interface film (SEI) and a cathode electrolyte interface film (CEI) and a preparation method thereof. In order to solve the problems of zinc negative electrode dendrite growth, corrosion and hydrogen evolution in aqueous zinc ion batteries, the present invention introduces diethylenetriamine pentaacetic acid sodium salt (DTPA-Na) as an electrolyte additive. DTPA-Na can form a stable multi-layer SEI layer on the negative electrode surface, effectively inhibit hydrogen evolution reaction and by-product generation, promote uniform zinc deposition, and thus inhibit dendrite growth. At the same time, DTPA-Na also helps to form a CEI layer at the positive electrode, reduce the dissolution of active substances, and improve the battery cycle stability and self-discharge performance. The Zn||MnOOH full battery prepared by the method shows excellent cycle stability, and the capacity retention rate after 720 hours of self-discharge is as high as 98.61%. The present invention provides a new idea for the practical application of high-performance aqueous zinc ion batteries.

[0042] The specific embodiments of the present invention are further described below.

[0043] A water-based rechargeable zinc ion battery with a double-layer SEI and CEI layer, comprising a positive electrode, a negative electrode, a separator and an electrolyte. The positive electrode comprises a manganese-based oxide positive electrode material, preferably MnOOH. The negative electrode comprises metallic zinc. The separator is a glass fiber separator. The electrolyte is an aqueous solution of zinc sulfate containing a DTPA-Na additive, wherein the concentration of DTPA-Na is preferably 0.1wt% to 1wt%, more preferably 0.5wt%.

[0044] A method for preparing the above-mentioned aqueous rechargeable zinc ion battery comprises the following steps:

[0045] Positive electrode preparation: MnOOH positive electrode material was prepared by hydrothermal method. The specific steps are as follows: 1mM potassium permanganate and 1mM ammonium chloride were dissolved in 50ml deionized water, stirred at room temperature for 60 minutes, and then transferred to a hydrothermal autoclave, reacted at 180°C for 16 hours, and then at 140°C for 8 hours. After natural cooling, filter and rinse with deionized water and anhydrous ethanol several times. The obtained solid was transferred to an oven and dried at 60°C. After drying, the material was ground through a 400 mesh sieve.

[0046] Negative electrode preparation: Commercially available zinc foil was used as the negative electrode material.

[0047] Preparation of electrolyte: DTPA-Na was dissolved in 2M zinc sulfate aqueous solution, and the concentration of DTPA-Na was 0.5 wt%.

[0048] Battery assembly: Assemble the positive electrode, negative electrode and separator in the CR2032 button battery shell in sequence, inject electrolyte and seal the battery.

[0049] Example 1

[0050] This embodiment provides a method for preparing an aqueous rechargeable zinc ion battery having a double-layer SEI and CEI layer, the method comprising:

[0051] 1. Preparation of positive electrode material: The MnOOH positive electrode material was prepared by the above-mentioned hydrothermal method.

[0052] 2. Preparation of negative electrode material: Commercially available zinc foil was used as the negative electrode material.

[0053] 3. Preparation of electrolyte: 0.5 wt % DTPA-Na was dissolved in 2 M zinc sulfate aqueous solution to prepare electrolyte.

[0054] 4. Battery assembly: The prepared MnOOH positive electrode, zinc foil negative electrode and glass fiber separator are assembled in sequence in a CR2032 button battery shell, the electrolyte is injected, and the battery is sealed.

[0055] Electrochemical performance test

[0056] The assembled battery was subjected to the following electrochemical performance tests:

[0057] 1. Cyclic voltammetry (CV): scan rate was 0.1 mV / s.

[0058] 2. Self-discharge test: measure the capacity retention rate of the battery after standing for 720 hours.

[0059] 3. Long cycle performance test: current density is 0.5A / g, and cycle is 5000 times.

[0060] Result analysis:

[0061] The electrochemical performance test results show that the Zn||MnOOH full battery with DTPA-Na exhibits excellent electrochemical performance, including:

[0062] 1. Excellent rate performance: It can maintain a high discharge capacity at different current densities.

[0063] 2. Extremely low self-discharge rate: After 720 hours of standing, the capacity retention rate is as high as 98.61%.

[0064] 3. Ultra-long cycle life: After 5000 cycles at a current density of 0.5A / g, there is no obvious capacity decay.

[0065] The above results show that the aqueous rechargeable zinc ion battery with double SEI and CEI layers and the preparation method thereof provided by the present invention can effectively improve the cycle stability, rate performance and self-discharge performance of the battery, and has good application prospects.

[0066] The above content is a further detailed description of the present invention in combination with specific / preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, without departing from the concept of the present invention, it can also make several substitutions or modifications to these described embodiments, and these substitutions or modifications should be regarded as belonging to the protection scope of the present invention. In the description of this specification, the description of the reference terms "an embodiment", "some embodiments", "preferred embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in combination with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily target the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In the absence of mutual contradiction, those skilled in the art can combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples. Although the embodiments of the present invention and their advantages have been described in detail, it should be understood that various changes, substitutions and modifications can be made herein without departing from the scope of protection of the patent application.

Claims

1. An aqueous rechargeable zinc ion battery having a double SEI layer and a CEI layer, comprising a positive electrode, a negative electrode, a separator and an electrolyte, characterized in that: The positive electrode comprises a manganese-based oxide positive electrode material; The negative electrode includes metallic zinc; The electrolyte is an aqueous solution of zinc sulfate containing a diethylenetriaminepentaacetic acid sodium salt DTPA-Na additive.

2. The aqueous rechargeable zinc ion battery according to claim 1, characterized in that: The manganese-based oxide positive electrode material is MnOOH.

3. The aqueous rechargeable zinc ion battery according to claim 3, characterized in that: The concentration of the DTPA-Na is 0.1 wt% to 1 wt%.

4. The aqueous rechargeable zinc ion battery according to claim 4, characterized in that: The concentration of the DTPA-Na is 0.5 wt %.

5. The aqueous rechargeable zinc ion battery according to any one of claims 1 to 4, characterized in that: The diaphragm is a glass fiber diaphragm.

6. A method for preparing an aqueous rechargeable zinc ion battery according to any one of claims 1 to 5, characterized in that: The following steps are involved: Positive electrode preparation: Manganese-based oxide positive electrode materials were prepared by hydrothermal method; Negative electrode preparation: Use metallic zinc as the negative electrode material; Preparation of electrolyte: dissolving DTPA-Na in an aqueous solution of zinc sulfate to prepare an electrolyte; Battery assembly: Assemble the positive electrode, negative electrode and separator, inject electrolyte, and seal the battery.

7. The preparation method according to claim 6, characterized in that: The hydrothermal method for preparing the MnOOH positive electrode material specifically includes: dissolving potassium permanganate and ammonium chloride in deionized water, stirring at room temperature and transferring to a hydrothermal autoclave, first reacting at a constant temperature of 180° C., then reacting at a constant temperature of 140° C., cooling naturally, filtering and washing with deionized water and anhydrous ethanol, and drying the obtained solid and grinding and sieving it.

8. The preparation method according to claim 7, characterized in that: Dissolve 1 mM potassium permanganate and 1 mM ammonium chloride in 50 ml of deionized water.

9. An electrolyte, characterized in that: The invention contains diethylenetriamine pentaacetic acid sodium salt DTPA-Na and zinc sulfate, wherein the concentration of DTPA-Na is 0.1wt% to 1wt%.

10. The electrolyte according to claim 9, characterized in that: The concentration of the DTPA-Na is 0.5 wt %.

Citation Information

Patent Citations

  • Electrolyte additive and application thereof, and non-aqueous electrolyte and battery comprising additive

    CN111430800A

  • High-nickel ternary lithium ion battery non-aqueous electrolyte and battery containing electrolyte

    CN112290090A

  • Flame-retardant lithium ion battery electrolyte and preparation method thereof

    CN113540565A

  • Novel phosphorus-containing high-safety electrolyte and lithium ion battery

    CN113675474A

  • Application of pentasodium diethylenetriamine pentaacetate in aqueous zinc ion battery electrolyte

    CN118412552A