Perovskite solar cell and preparation method thereof

By using conductive carbon slurry coating and hot-pressure packaging technology in perovskite solar cells, the problem of solvent dissolving functional layer in the coating method is solved, the photoelectric conversion efficiency and conductivity of the battery are improved, and the cost is reduced. Industrialized production.

CN119053218APending Publication Date: 2024-11-29BYD CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310618472.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-29
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

When the carbon electrode is prepared by coating in existing perovskite solar cells, the solvent dissolves the functional layer, affecting the photoelectric conversion rate of the battery, and the high content of binder in the coating method leads to poor conductivity of the electrode.

Method used

The conductive carbon slurry is coated on the packaging base plate for annealing to form a carbon electrode, and the functional layer and the carbon electrode are closely combined through hot-pressure packaging technology to avoid contact with the solvent and the functional layer and improve conductivity.

Benefits of technology

It improves the photoelectric conversion efficiency of solar cells, enhances the bonding between carbon electrodes and wires, reduces production costs, simplifies process conditions, is suitable for industrial development, and improves the bending resistance of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119053218A_ABST
    Figure CN119053218A_ABST
Patent Text Reader

Abstract

In order to solve the problems that in an existing perovskite solar cell, a coating method is adopted for preparing a carbon electrode, a solvent dissolves a functional layer, and the photoelectric conversion rate of the cell is influenced, the flexible carbon electrode perovskite solar cell and the preparation method thereof are provided, and the preparation method comprises the steps that the functional layer is prepared on a substrate to obtain a first combination layer; coating a packaging bottom plate with the conductive carbon slurry, carrying out first annealing treatment, and forming a carbon electrode on the packaging bottom plate to obtain a second combination layer; and hot-pressing and packaging the first combined layer and the second combined layer, and abutting one side, far away from the substrate, of the functional layer against the carbon electrode to obtain the flexible carbon electrode perovskite solar cell. According to the preparation method provided by the invention, by utilizing the characteristics of porous structure and excellent mechanical property of the carbon material, the direct contact between each functional layer material and the organic solvent in the carbon paste can be avoided, the function of protecting the functional layer is achieved, and the photoelectric conversion efficiency of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of solar cells, and in particular relates to a preparation method and application of a flexible carbon electrode perovskite solar cell. Background Art

[0002] The principle of perovskite solar cells is to use perovskite-type organic metal halide semiconductors as solar cells that absorb light. Perovskite solar cells have attracted much attention due to their high photoelectric conversion efficiency and low cost. Flexible perovskite solar cells are bendable, portable, lightweight, and have a wide range of application scenarios, making them a promising candidate for development in future flexible wearable electronic devices and aerospace. Carbon electrodes are widely used due to their excellent hydrophobic properties, low cost, and simple preparation methods.

[0003] Perovskite solar cells generally consist of a transparent electrode, a transmission layer, a perovskite absorption layer, a metal electrode or a carbon electrode. Traditional flexible perovskite solar cells are generally prepared by a deposition method to prepare a metal electrode or a coating method to prepare a carbon electrode. The deposition method is generally to evaporate the metal material onto the perovskite functional layer under high temperature and low pressure conditions. This method is costly and wastes a lot of materials. The coating method is to coat the carbon material in the form of carbon paste on the transmission layer or the perovskite layer. The carbon paste in this method generally contains an organic solvent with low polarity (such as a solvent including one or more of ethanol, methanol, isopropanol, n-propanol, n-butanol, acetone, n-hexane, acetonitrile, and 3-methoxypropionitrile), but such solvents will dissolve the functional layer material (the functional layer is the transmission layer or the perovskite layer) material, causing irreversible damage to the transmission layer or the perovskite layer material, resulting in a decrease in device performance; there is also a technology that uses a coating method to pre-coat the carbon paste on the substrate to form a carbon film, and then covers the carbon film on the functional layer. The carbon electrode binder prepared by this method (such as a binder including one or more of acrylic resin, polyvinylidene fluoride, polyvinyl acetate, ethylene-vinyl acetate copolymer, polymethyl methacrylate, polycarbonate, polyamide and polystyrene) has a high content and poor electrode conductivity. Summary of the invention

[0004] In view of the problem that the carbon electrode is prepared by a coating method in the existing perovskite solar cell, the solvent dissolves the functional layer, and the photoelectric conversion rate of the cell is affected, the present application provides a flexible carbon electrode perovskite solar cell and a preparation method thereof.

[0005] In order to solve the above problems, the present application provides a method for preparing a flexible carbon electrode perovskite solar cell, comprising the following steps:

[0006] preparing a functional layer on a substrate to obtain a first composite layer;

[0007] Coating a conductive carbon slurry on the packaging bottom plate, and performing a first annealing treatment to form a carbon electrode on the packaging bottom plate to obtain a second composite layer;

[0008] The first combined layer and the second combined layer are heat-pressed and packaged, and the side of the functional layer away from the substrate is in contact with the carbon electrode to obtain a flexible carbon electrode perovskite solar cell.

[0009] Preferably, the conductive carbon paste comprises a carbon material, a binder and a solvent, the solvent is a low-viscosity system solvent, and the viscosity of the solvent is 1 to 20 mPa·s.

[0010] Preferably, the solvent includes one or more of water, ethanol, terpineol, ethylene glycol methyl ether, ethylene glycol 19.9, glycerol, glycerol methyl ether, N-methyl pyrrolidone, butyl acetate, butyl acetate, diethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, isophorone, and alkanes;

[0011] The carbon material includes one or more of Ketjen black, acetylene black, carbon nanotubes, graphene, and carbon black;

[0012] The binder includes one or more of acrylic resin, polyvinylidene fluoride, polyvinyl acetate, ethylene-vinyl acetate copolymer, polymethyl methacrylate, polycarbonate, polyamide and polystyrene.

[0013] Preferably, the mass ratio of the carbon material to the binder is 1:(0.05-0.5).

[0014] Preferably, the mass ratio of the carbon material to the binder is 1:(0.05-0.15).

[0015] Preferably, the solid content of the conductive carbon slurry is 10% to 50%.

[0016] Preferably, in the first annealing step, the first annealing temperature is 50° C. to 200° C., and the first annealing time is 10 s to 30 min.

[0017] Preferably, the first annealing temperature is 70° C. to 120° C., and the first annealing time is 5 min to 15 min.

[0018] Preferably, the carbon electrode has a thickness of 0.05 μm to 500 μm.

[0019] Preferably, in the step of hot-pressing and packaging the first combined layer and the second combined layer, the hot-pressing temperature is 50° C. to 200° C., and the hot-pressing pressure is 1 KPa to 200 KPa.

[0020] Preferably, before preparing the functional layer on the substrate, the substrate is pre-treated, and the pre-treatment comprises the following steps: firstly ultrasonically cleaning the substrate with a cleaning solvent, drying, and then ozone treating for 5 to 20 minutes;

[0021] The cleaning solvent includes one or more of detergent water, water, ethanol, and isopropanol.

[0022] Preferably, the functional layer includes an electron transport layer and a perovskite layer, and preparing the functional layer on the substrate includes the following steps:

[0023] The electron transport layer is deposited on the substrate, and after drying, a perovskite precursor solution is deposited on the electron transport layer, and an anti-solvent or vacuum treatment is performed, and then a second annealing treatment is performed to obtain the perovskite layer.

[0024] Preferably, the electron transport layer includes one or more of titanium nitride, tin oxide, titanium oxide, nickel oxide, C60, and PCBM, and the thickness of the electron transport layer is 2 nm to 200 nm.

[0025] Preferably, the perovskite precursor solution comprises perovskite and a solvent.

[0026] The structure of the perovskite is A x A' (1-x) BX3,

[0027] Wherein 0<x<1, A includes one or more of formamidine and methylamine; A' is one or more of cesium, potassium, sodium, calcium, and rubidium; B includes one or more of lead and tin; and X is one or more of iodine, bromine, chlorine, and fluorine;

[0028] The solvent includes one or more of N,N-dimethylformamide, N-methylpyrrolidone, dimethyl sulfoxide, γ-hydroxybutyrolactone, isopropanol, diphenyl sulfoxide, and ethyl acetate.

[0029] Preferably, x is 0.5 to 0.99.

[0030] Preferably, the thickness of the perovskite layer is 100 nm to 1000 nm.

[0031] Preferably, the anti-solvent includes one or more of chlorobenzene, acetonitrile, ethanol, isopropanol, ethyl acetate, and ether; in the vacuum treatment step, the vacuum degree is 50-5000 Pa, and the vacuum treatment time is 10s-1000s; in the second annealing treatment step, the second annealing temperature is 50-200°C, and the second time is 5-500min.

[0032] Preferably, the functional layer further comprises a hole transport layer, and preparing the functional layer on the substrate further comprises the following steps: depositing the hole transport layer on the surface of the perovskite layer away from the resistance transport layer;

[0033] The thickness of the hole transport layer is 20nm-200nm;

[0034] The hole transport layer includes one or more of Spiro-OMeTAD, PTAA, PEDOT:PSS, CuOx, and NiOx.

[0035] Preferably, the substrate comprises a transparent electrode and a flexible substrate, the flexible substrate comprises one or more of glass, a first polymer material, and a first metal film; the packaging base plate comprises a packaging base plate body and a packaging layer arranged on the packaging base plate body, the base plate body comprises a second polymer material or a second metal film; the first polymer material and the second polymer material are each independently selected from one or more of polyethylene naphthalate and polyethylene terephthalate;

[0036] The transparent electrode comprises one or more of indium tin oxide, fluorine-doped tin oxide, carbon nanotubes, and graphene;

[0037] The encapsulation layer includes one or more of ethylene-octene polymer, butyl rubber, metal oxide, and metal nitride.

[0038] On the other hand, the present application provides a flexible carbon electrode perovskite solar cell, which is prepared by the above-mentioned method for preparing a flexible carbon electrode perovskite solar cell.

[0039] The method for preparing a flexible carbon electrode perovskite solar cell provided in the present application comprises coating a conductive carbon slurry on a packaging substrate, annealing to form a carbon electrode to obtain a second combination layer, and then hot-pressing and packaging the first combination layer and the second combination layer to form a battery, which has the following effects: first, by utilizing the porous structure and excellent mechanical properties of the carbon material, the functional layer materials can be prevented from directly contacting with the organic solvent in the conductive carbon slurry, thereby protecting the functional layer and improving the photoelectric conversion efficiency of the battery; second, the conductive carbon slurry is coated and annealed on the wire of the packaging substrate to obtain the first combination layer, which is conducive to close fitting with the wire, improving the overall conductivity of the device, and is similar to the conductive carbon slurry prepared on the substrate. The preparation of the functional layer and the second combination layer can be carried out simultaneously, which greatly saves production time; third, the conductive carbon slurry contains carbon material, the carbon material has stable performance, and the coating and annealing process of the conductive carbon slurry can be carried out completely in the atmospheric atmosphere, and the process conditions are mild; fourth, the preparation method provided in the present application can adopt a simpler annealing process to prepare the carbon electrode, which is conducive to industrial development; fifth, the conductive carbon slurry has a variety of solvent choices, and a low-viscosity solvent system or even an aqueous solution can be selected for preparation, which enhances the fit between the carbon electrode and the wire, promotes the carrier transmission effect, and compared with high-viscosity solvents, it has the advantages of excellent anti-bending performance, reduced cost, energy saving and environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 It is a schematic diagram of the structure of a perovskite solar cell before hot pressing packaging provided by an embodiment of the present invention.

[0041] The reference numerals in the drawings of the specification are as follows:

[0042] 1. Substrate; 2. Functional layer; 3. Carbon electrode; 4. Packaging base plate; 41. Base plate body; 42. Packaging layer. DETAILED DESCRIPTION

[0043] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0044] like Figure 1 As shown, an embodiment of the present invention provides a method for preparing a flexible carbon electrode 3 perovskite solar cell, comprising the following steps:

[0045] A functional layer 2 is prepared on a substrate 1 to obtain a first composite layer;

[0046] Coating the conductive carbon slurry on the packaging bottom plate 4 and performing a first annealing treatment to form a carbon electrode 3 on the packaging bottom plate 4 to obtain a second composite layer;

[0047] The first and second combined layers are hot-pressed and packaged, and the side of the functional layer 2 away from the substrate 1 is in contact with the carbon electrode 3 to obtain a flexible carbon electrode 3 perovskite solar cell. The preparation method of the flexible carbon electrode 3 perovskite solar cell provided in the present application is to coat the conductive carbon slurry on the packaging base plate 4, form the carbon electrode 3 through annealing to obtain the second combined layer, and then hot-press the first and second combined layers to form a battery, which has the following effects: First, the porous structure and excellent mechanical properties of the carbon material can be used to avoid direct contact between the functional layer 2 materials and the organic solvent in the conductive carbon slurry, thereby protecting the functional layer 2 and improving the photoelectric conversion efficiency of the battery; second, the conductive carbon slurry is coated and annealed on the wire of the packaging base plate 4 to obtain the first combined layer, which is conducive to close fitting with the wire, improving the overall conductivity of the device, and on the substrate 1 The preparation of the functional layer 2 and the preparation of the second combination layer can be carried out simultaneously, which greatly saves production time; third, the conductive carbon slurry contains carbon material, the carbon material has stable performance, and the coating and annealing process of the conductive carbon slurry can be carried out completely in the atmospheric atmosphere, and the process conditions are mild; fourth, the preparation method provided in the present application can adopt a simpler annealing process to prepare the carbon electrode, which is conducive to industrial development; fifth, the conductive carbon slurry has a variety of solvent choices, and a low-viscosity solvent system or even an aqueous solution can be selected for preparation, which enhances the adhesion between the carbon electrode 3 and the wire, promotes the carrier transmission effect, and compared with high-viscosity solvents, it has the advantages of excellent anti-bending performance, reduced cost, energy saving and environmental protection.

[0048] In some embodiments, the conductive carbon slurry includes a carbon material, a binder and a solvent, and the carbon material includes but is not limited to the following types: one or more of Ketjen black, acetylene black, carbon nanotubes, graphene, carbon black, and carbon fibers; the binder includes but is not limited to the following types: one or more of acrylic resin, polyvinylidene fluoride, polyvinyl acetate, ethylene-vinyl acetate copolymer, polymethyl methacrylate, polycarbonate, polyamide, sodium carboxymethyl cellulose, and polystyrene; the solvent is a low-viscosity system solvent.

[0049] The present application first applies the conductive carbon paste on the packaging base plate 4, and performs the first annealing treatment to form the carbon electrode 3, and obtains the second combination layer, and then the first combination layer and the second combination layer are hot-pressed and packaged to obtain a battery, and the porous structure and excellent mechanical properties of the carbon material can be used to avoid direct contact between the materials of each functional layer 2 and the organic solvent in the conductive carbon paste. The structure of the carbon material determines its excellent performance, and the above-mentioned carbon material has good conductivity, hydrophobicity, chemical stability, etc.

[0050] In some embodiments, the solvent is a low viscosity system solvent, the viscosity of the solvent is 1 to 20 mPa·s, and the solvent includes but is not limited to the following types: water, ethanol, terpineol, ethylene glycol methyl ether, ethylene glycol, glycerol, glycerol methyl ether, N-methylpyrrolidone, butyl acetate, butyl acetate, diethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, isophorone, and one or more of alkanes.

[0051] Specifically, if the existing carbon paste is coated on the functional layer, the photoelectric conversion efficiency of the solar cell is low. This is because the carbon paste containing a low-viscosity solvent will quickly infiltrate the functional layer during the coating process, directly contact the perovskite, decompose the perovskite, and reduce the photoelectric conversion efficiency of the solar cell. The solar cell preparation method provided by the present application coats the conductive carbon paste on the packaging base plate. The solvent in the conductive carbon paste adopts a low-viscosity system solvent, which can enhance the fit between the carbon electrode and the wire, promote the carrier transmission effect, and improve the conductivity of the carbon electrode. At the same time, the carbon electrode prepared by the low-viscosity system solvent in the present application has the advantage of anti-bending performance. The conductive carbon paste is not directly coated on the functional layer, which effectively avoids the decomposition of the perovskite by the low-viscosity solvent of the conductive carbon paste during the coating process, plays a role in protecting the functional layer, and improves the photoelectric conversion rate of the solar cell.

[0052] The above-mentioned alkane solvents are organic compounds containing carbon and hydrogen elements, including cycloalkane and chain alkane organic solvents. The chain alkane organic solvents satisfy the structural formula C n H 2n+2 , cycloalkane organic solvents satisfy the structural formula C n H2 n .

[0053] In some preferred embodiments, the solvent includes at least one of water and ethanol. Further preferably, the solvent is a mixed solution of water and ethanol, and the mixing ratio of hydrated ethanol is 1:(0.5-5); more preferably, the mixed solvent of water and ethanol is 1:1.

[0054] Compared with the existing method of using low-viscosity organic solvents as solvents for carbon slurries, the conductive carbon slurry of the present application can use water or a mixed solution of water and ethanol as a solvent, which can reduce the cost of solar cells without reducing the electrical performance of solar cells. This is because in the preparation method provided by the present application, during the first annealing treatment, the first annealing temperature can be higher than 100°C. After the conductive carbon slurry is subjected to the first annealing treatment, water and ethanol can be completely evaporated, and the formed carbon electrode 3 does not contain water and ethanol, and does not affect the electrical performance of the solar cell.

[0055] In some embodiments, the conductive carbon paste includes a carbon material, a binder, and a solvent, and the mass ratio of the carbon material to the binder is 1:(0.05-0.5).

[0056] The carbon electrode 3 prepared in the present application does not need to be bonded to the functional layer 2 by a binder, so the mass content of the binder can be controlled in a lower range of 1: (0.05-0.5) of the mass ratio of the carbon material to the binder. The reduction in the mass content of the binder helps to improve the conductivity of the carbon electrode 3 and reduce the production cost of the battery. Specifically, the mass ratio of the carbon material to the binder can be 1: 0.05, 1: 0.1, 1: 0.015, 1: 0.2, 1: 0.25, 1: 0.3, 1: 0.35, 1: 0.4, 1: 0.45, 1: 0.5, etc., as long as the mass ratio of the carbon material to the binder is within the range of 1: (0.05-0.5).

[0057] In some preferred embodiments, the mass ratio of the carbon material to the binder is 1:(0.05-0.15).

[0058] The mass ratio of carbon material to binder in the conductive carbon paste is within the above range, the content of binder in the conductive carbon paste is low, and the conductive carbon paste can be coated on the wire on the packaging base plate 4 to form a carbon electrode 3. The carbon electrode 3 has a good bonding effect with the wire, and can also promote the transmission of carriers, thereby improving the conductivity of the carbon electrode 3 and reducing the preparation cost of the carbon electrode 3.

[0059] In some embodiments, the solid content of the conductive carbon slurry is 10% to 50%.

[0060] The solid content of the conductive carbon slurry is the mass proportion of the carbon material and the binder in the entire conductive carbon slurry. If the solid content of the conductive carbon slurry is higher than 50%, the solvent content is low, and the viscosity of the slurry is high, which affects the coating of the conductive carbon slurry on the surface of the wire on the packaging base plate 4, and weakens the adhesion between the carbon electrode 3 and the wire. If the solid content of the conductive carbon slurry is lower than 10%, the carbon material content is low, which reduces the conductivity of the carbon electrode 3.

[0061] In some preferred embodiments, the solid content of the conductive carbon slurry is 20% to 30%.

[0062] The solid content of the conductive carbon paste is within the preferred range of 20 to 30%, which makes it easier for the conductive carbon paste to be coated on the packaging base plate 4, thereby enhancing the fit between the carbon electrode 3 and the wire, promoting the carrier transmission effect, and improving the conductivity of the carbon electrode 3. The prepared carbon electrode 3 has better anti-bending performance.

[0063] In some embodiments, the viscosity of the conductive carbon paste is 1000-30000 mPa·s.

[0064] The viscosity of the conductive carbon slurry prepared in the present application is a low-viscosity slurry system with good fluidity, which is conducive to coating the conductive carbon slurry on the wire of the packaging base plate 4. The formed carbon electrode 3 can better fit the wire and improve the conductivity of the carbon electrode 3.

[0065] In some preferred embodiments, the viscosity of the conductive carbon paste is 5000-15000 mPa·s.

[0066] The viscosity of the conductive carbon paste is within the above preferred range, which is more conducive to coating the conductive carbon paste on the wires of the packaging base plate 4, so that the carbon electrode 3 can better fit the wires and improve the conductivity of the carbon electrode 3.

[0067] In some embodiments, in the first annealing step, the first annealing temperature is 50° C. to 200° C., and the first annealing time is 10 s to 30 min.

[0068] Specifically, after the conductive carbon paste is coated on the packaging base plate 4, a conductive carbon layer is formed on the packaging base plate 4, and then the conductive carbon layer is subjected to a first annealing treatment to remove the solvent in the conductive carbon layer, thereby obtaining a carbon electrode 3. The first annealing temperature is 50°C to 200°C. The selection of the first annealing temperature needs to meet the temperature that can volatilize the solvent in the conductive carbon paste, that is, the first annealing temperature is greater than or equal to the solvent volatilization temperature. The appropriate first annealing temperature can be selected according to the solvent in the selected conductive carbon paste. Specifically, the first annealing temperature can be 50°C, 70°C, 100°C, 120°C, 150°C, 180°C, 200°C, etc., as long as the first annealing temperature is between 50 and 200°C. For the selection of annealing time, when the annealing temperature is low, the corresponding annealing time is longer. If the annealing time is short, the low-viscosity system solvent contained in the carbon electrode 3 will decompose the perovskite, causing the battery to fail.

[0069] In some preferred embodiments, the first annealing temperature is 70° C. to 120° C., and the first annealing time is 5 min to 15 min.

[0070] Compared with the prior art, the conductive carbon paste in the present application is coated on the packaging base plate 4. The conductive carbon paste uses a low-viscosity solvent and has an annealing temperature of 70°C to 120°C, which is generally higher than the annealing temperature of the existing carbon paste. The first annealing temperature is increased, the annealing time is shortened, the process time is saved, and the decomposition of the perovskite is avoided.

[0071] In some embodiments, the carbon electrode 3 has a thickness of 0.05 μm to 500 μm.

[0072] The carbon electrode 3 provided in the present application has hole transport and conductive functions. The thickness of the carbon electrode 3 is controlled between 50nm and 500μm, has good conductive and hole transport functions, is easy to assemble, and has a suitable thickness for the prepared solar cell device.

[0073] In some embodiments, in the step of hot pressing and packaging the first combined layer and the second combined layer, the hot pressing temperature is 50° C. to 200° C., and the hot pressing pressure is 1 KPa to 200 KPa.

[0074] Specifically, the first combined layer and the second combined layer are hot pressed, and the first combined layer is stacked on the second combined layer, and the side of the functional layer 2 away from the substrate 1 is adjacent to the carbon electrode 3. After hot pressing, the following structure is obtained from top to bottom: from top to bottom, there are substrate 1, functional layer 2, carbon electrode 3, and packaging base plate 4.

[0075] The hot pressing temperature is between 50°C and 200°C, and the hot pressing pressure is between 1KPa and 200KPa. Under the above hot pressing temperature and hot pressing pressure, the first composite layer and the second composite layer can be pressed together at a lower hot pressing temperature and hot pressing pressure to prepare a solar cell device.

[0076] In some embodiments, before preparing the functional layer 2 on the substrate 1, the substrate 1 is pretreated, and the pretreatment includes the following steps: the substrate 1 is first ultrasonically cleaned with a cleaning solvent, dried, and then ozone treated for 5 to 20 minutes; the cleaning solvent includes but is not limited to the following types: one or more of water, ethanol, and isopropanol.

[0077] The specific steps are as follows: ultrasonically clean the substrate 1 with detergent water, deionized water, ethanol, and isopropanol for 10 minutes respectively, then blow dry with a nitrogen air gun, and perform ozone treatment for 5 to 20 minutes. The substrate 1 is first ultrasonically cleaned with a cleaning solvent, and the ozone treatment is to wash away impurities on the surface of the substrate 1 and reduce the internal resistance of the battery.

[0078] In some embodiments, the functional layer 2 includes an electron transport layer and a perovskite layer, and the preparation of the functional layer 2 on the substrate 1 includes the following steps: depositing the electron transport layer on the substrate 1, transferring to a dry atmosphere for drying after the deposition is completed, the dry atmosphere should be RH <30%, after drying, depositing the perovskite precursor solution on the electron transport layer, and performing an anti-solvent or vacuum treatment, and then performing a second annealing treatment to obtain the perovskite layer. The dry atmosphere is specifically an environment in which the RH is <30%.

[0079] Specifically, the perovskite layer acts as a light-absorbing layer, and after being irradiated by sunlight, electron-hole pairs are generated, and then the electrons and holes are separated. The electrons flow to the transparent electrode in the substrate 1 through the electron transport layer, and the holes flow to the anode of the battery through the hole transport layer or the carbon electrode 3. The anode of the battery is the carbon electrode 3. It should be noted that the carbon electrode 3 has the function of transporting holes and conducting electricity.

[0080] Methods for depositing the electron transport layer on the substrate 1 include hydrothermal method, coating method, spray pyrolysis method, etc.

[0081] Anti-solvent treatment is to replace the solvent in the perovskite precursor solution with a more volatile solvent, and improve the uniformity of the perovskite film formation, pre-crystallization and other functions. Anti-solvent treatment or vacuum treatment is the process of crystallization of the perovskite precursor solution, thereby forming a uniform perovskite film layer. The second annealing treatment promotes solvent volatilization to form a uniform and complete perovskite layer.

[0082] In some embodiments, the electron transport layer includes but is not limited to the following: titanium nitride, tin oxide, titanium oxide, nickel oxide, C 60 , PCBM, and the thickness of the electron transport layer is 2nm to 200nm.

[0083] The electron transport layer has the function of transporting electrons. The thickness of the electron transport layer is controlled between 2nm and 200nm, which can not only ensure that the solar cell has a thinner thickness, but also play the role of electron transport.

[0084] Specifically, when the electron transport layer is titanium nitride, the deposition method of titanium nitride is one of magnetron sputtering, thermal evaporation, electron beam evaporation, screen printing, doctor blade coating, slit coating or spraying.

[0085] In some embodiments, the perovskite precursor solution includes perovskite and a solvent, and the structure of the perovskite is A x A' (1-x) BX3, wherein 0<x<1, A includes one or more of formamidine and methylamine; A' is one or more of cesium, potassium, sodium, calcium, and rubidium; B includes one or more of lead and tin, and X is one or more of iodine, bromine, chlorine, and fluorine; the solvent includes one or more of N,N-dimethylformamide, N-methylpyrrolidone, dimethyl sulfoxide, γ-hydroxybutyrolactone, isopropanol, diphenyl sulfoxide, and ethyl acetate.

[0086] Furthermore, the solvent is preferably one or more of N-methylpyrrolidone, N,N-dimethylformamide, diphenyl sulfoxide, and γ-hydroxybutyrolactone.

[0087] In some preferred embodiments, x is 0.5-0.99.

[0088] The specific value range of x is 0.5 to 0.99, and the corresponding value range of 1-x is 0.01 to 0.5.

[0089] In some preferred embodiments, the thickness of the perovskite layer is 100 nm to 1000 nm.

[0090] If the thickness of the perovskite layer is less than 100nm, the perovskite content in the perovskite layer is low, and the generated electron-hole pairs are few, which reduces the battery performance. If the thickness of the perovskite layer is greater than 1000nm, the thickness of the solar cell device increases, affecting the battery performance.

[0091] In some embodiments, the anti-solvent includes but is not limited to the following types: one or more of chlorobenzene, acetonitrile, ethanol, isopropanol, ethyl acetate, and ether; in the vacuum treatment step, the vacuum degree is 50-5000Pa, and the vacuum treatment time is 10s-1000s; in the second annealing treatment step, the second annealing temperature is 50-200°C, and the second annealing time is 5-500min.

[0092] Furthermore, the anti-solvent includes one or more of isopropanol, acetonitrile, and chlorobenzene. Furthermore, in the vacuum treatment step, the vacuum degree is 500Pa to 5000Pa.

[0093] In some embodiments, the functional layer 2 also includes a hole transport layer, and the preparation of the functional layer 2 on the substrate 1 also includes the following steps: depositing a hole transport layer on the surface of the perovskite layer away from the resistance transport layer; the thickness of the hole transport layer is 20nm-200nm; the hole transport layer includes one or more of Spiro-OMeTAD, PTAA, PEDOT:PSS, CuOx, and NiOx.

[0094] The hole transport layer has the function of transporting holes. The perovskite layer is irradiated by sunlight to generate electron-hole pairs. The electron transport layer transports electrons to the transparent electrode in the substrate 1, and the hole transport layer transports them to the carbon electrode 3 to form a conductive path. Methods for depositing the hole transport layer on the surface of the perovskite layer away from the resistance transport layer include hydrothermal method, coating method, spray pyrolysis method, etc.

[0095] In some embodiments, the substrate 1 includes a transparent electrode and a flexible substrate, the flexible substrate includes one or more of glass, a first polymer material, and a first metal film; the packaging base plate 4 includes a base plate body 41 and a packaging layer 42 arranged on the base plate body 41, and the base plate body 41 includes a second polymer material or a second metal film; the first polymer material and the second polymer material are each independently selected from one or more of polyethylene naphthalate and polyethylene terephthalate; the transparent electrode includes but is not limited to the following types: one or more of indium tin oxide, fluorine-doped tin oxide, carbon nanotubes, and graphene; the packaging layer 4 includes but is not limited to the following types: one or more of ethylene-octene polymer, butyl rubber, metal oxides, and metal nitrides.

[0096] The first metal film and the second metal film include, but are not limited to, one or more of the following materials: aluminum, copper, silver, aluminum oxide, copper oxide, and copper oxide.

[0097] Specifically, the substrate 1 is generally a substrate 1 having a transparent electrode covering a flexible substrate, the transparent electrode has a conductive function, and the flexible substrate carries the transparent electrode. The width of the substrate 1 is 1 to 200 cm.

[0098] The conductive carbon slurry is coated on the packaging base plate 4. The coating methods that can be used include slit coating, blade coating, gravure coating, etc. For example, when slit coating is selected, the following coating parameters can be selected: the width of the coating head is 5-50 cm, the coating speed is 0.5-50 mm / s, the liquid output is 0.2-20 mL / s, and the coating head height is 0.1-10 mm. More preferred coating parameters are a coating head width of 15-20 cm, a coating speed of 5-10 mm / s, a liquid output of 0.5-2 mL / s, and a coating head height of 2-5 mm.

[0099] On the other hand, the present application provides a flexible carbon electrode 3 perovskite solar cell, which is prepared by the above-mentioned method for preparing a flexible carbon electrode 3 perovskite solar cell.

[0100] Compared with the prior art, the flexible carbon electrode 3 perovskite solar cell provided in the present application is obtained by coating the carbon electrode 3 on the packaging base plate 4 and performing a first annealing treatment to obtain the carbon electrode 3, and then hot-pressing and packaging the first combined layer containing the functional layer 2 and the substrate 1 and the second combined layer containing the carbon electrode 3. The porous structure and excellent mechanical properties of the carbon material can prevent the materials of each functional layer 2 from directly contacting the organic solvent in the carbon slurry, thereby protecting the functional layer 2 and improving the photoelectric conversion efficiency of the battery.

[0101] The present invention is further described in detail below by way of examples.

[0102] Example 1

[0103] This embodiment is used to illustrate the preparation method of the flexible carbon electrode 3 perovskite solar cell disclosed in the present invention, which includes the following steps:

[0104] 1) Preparation of the first composite layer: An electron transport layer SnO2 is coated on a substrate 1 having a transparent electrode indium tin oxide and a polymer material polyethylene naphthalate, and the thickness of the electron transport layer is 20nm. Then it is transferred to a dry atmosphere (RH < 30%), and the perovskite precursor solution is coated on the surface of the electron transport layer away from the substrate 1, and an anti-solvent treatment and a second annealing treatment are performed to obtain a perovskite layer, and the thickness of the perovskite layer is 500nm. A hole transport layer Spiro-OMeTAD is coated on the surface of the perovskite layer away from the electron transport layer, and the thickness of the hole transport layer is 70nm.

[0105] The chemical formula of perovskite in the perovskite precursor solution is FA 0.85 MA 0.1 Cs 0.05 PbI 2.7 Br 0.3 The solvent in the perovskite precursor solution is N,N-dimethylformamide and N-methylpyrrolidone, and the anti-solvent is chlorobenzene. The second annealing treatment temperature is 120°C and the annealing time is 10 minutes.

[0106] 2) Preparation of conductive carbon slurry: Carbon black is used as the carbon material, N-methylpyrrolidone is used as the solvent, and polyvinylidene fluoride is used as the binder. A mixture of carbon material and binder in a mass ratio of 90:10 is mixed with solvent N-methylpyrrolidone to obtain conductive carbon slurry. The solid content of the prepared conductive carbon slurry is 15%, and the viscosity of the conductive carbon slurry is 24000mPa·s. Among them, the viscosity of the solvent N-methylpyrrolidone in the conductive carbon slurry is 1.65mPa·s.

[0107] 3) Preparation of the second composite layer: The conductive carbon paste is coated on the flexible polymer packaging substrate 4 covered with the wire and the packaging layer 42, and then subjected to the first annealing treatment to obtain the carbon electrode 3, the thickness of the carbon electrode 3 is 1 μm. The first annealing temperature is 70° C., and the first annealing time is 15 min.

[0108] 4) Hot pressing packaging: The first combined layer is placed on the carbon electrode 3 of the second combined layer, and the carbon electrode 3 is in contact with the hole transport layer, and then the first combined layer and the second combined layer are hot pressed to obtain a perovskite solar cell. The hot pressing temperature is 100°C and the hot pressing pressure is 50KPa.

[0109] Example 2

[0110] The difference between Example 2 and Example 1 is that the preparation of the first combination layer is different and the hot pressing packaging is different. Specifically, in the preparation step of the first combination layer, there is no hole transport layer in Example 2, and the rest is the same as Example 1. In the hot pressing assembly step, when the first combination layer is placed on the carbon electrode 3 of the second combination layer in Example 2, the side of the carbon electrode 3 away from the packaging bottom plate 4 is in contact with the perovskite layer, and the rest is the same as Example 1.

[0111] Example 3

[0112] The difference between Example 3 and Example 1 is that the conductive carbon slurry in Example 3 is prepared differently, the solvent in the conductive carbon slurry in Example 3 is water, the binder is sodium carboxymethyl cellulose, and the rest is the same as Example 1. The viscosity of the water used is 1 mPa·s, the solid content of the prepared conductive carbon slurry is 10%, and the viscosity of the conductive carbon slurry is 10000 mPa·s.

[0113] When the first annealing treatment is performed, the first annealing temperature and the first annealing time are different from those in Example 1. Specifically, the first annealing temperature is 70° C., and the first annealing time is 5 minutes.

[0114] Example 4

[0115] The difference between Example 4 and Example 1 is that the conductive carbon slurry in Example 3 is prepared differently, the solvent in the conductive carbon slurry in Example 3 is a mixture of water and ethanol, the mixing ratio of water to ethanol is 1:1, and the rest is the same as Example 1. The viscosity of the water used is 1 mPa·s, the viscosity of ethanol is 1.2 mPa·s, the solid content of the prepared conductive carbon slurry is 10%, and the viscosity of the conductive carbon slurry is 10000 mPa·s.

[0116] When the first annealing treatment is performed, the first annealing temperature and the first annealing time are different from those in Example 1. Specifically, the first annealing temperature is 70° C., and the first annealing time is 5 minutes.

[0117] Example 5

[0118] Compared with Example 1, Example 5 has a different preparation method for the conductive carbon slurry. The mass ratio of the carbon material to the binder in Example 5 is 80:20, and the rest is the same as Example 1. The viscosity of the conductive carbon slurry prepared is 28000 mPa·s

[0119] Example 6

[0120] Compared with Example 1, Example 6 differs in that the first annealing temperature and the first annealing time in Example 6 are different, and the rest are the same as Example 1.

[0121] Specifically, the first annealing temperature in Example 6 is 40° C., and the first annealing time is 60 min.

[0122] Example 7

[0123] The difference between Example 7 and Example 1 is that the mass ratio of carbon material to binder in the conductive carbon slurry in Example 7 is 1:1, and the rest is the same as Example 1. The viscosity of the prepared conductive carbon slurry is 36000 mPa·s

[0124] Comparative Example 1

[0125] The difference between Comparative Example 1 and Example 1 is that the preparation of the first combination layer is different, the preparation of the conductive carbon paste is different, there is no preparation of the second combination layer, the hot pressing packaging is different, and the rest is the same as Example 1.

[0126] Specifically, in the preparation of the first combination layer, in Comparative Example 1, after the preparation of the first combination layer of Example 1, a conductive carbon slurry is coated on the surface of the hole transport layer away from the perovskite layer; and then a vacuum annealing treatment is performed to obtain a conductive carbon layer, and the thickness of the conductive carbon layer is 1 μm. The treatment conditions are vacuum degree -0.1 MPa, annealing temperature 70°C, and annealing time 5 min.

[0127] The preparation of the conductive carbon slurry is different. In Comparative Example 1, the mass ratio of the carbon material to the binder in the conductive carbon slurry is 90:10, and the solvent is N-methylpyrrolidone, and the rest is the same as in Example 1. The viscosity of the solvent N-methylpyrrolidone is 1.65 mPa·s. The hot pressing packaging step is different, and the packaging material is directly placed on the surface of the carbon electrode 3 for hot pressing packaging, and the hot pressing packaging conditions are the same as in Example 1.

[0128] Comparative Example 2

[0129] The difference between Comparative Example 2 and Comparative Example 1 is that there is no hole transport layer in Comparative Example 2, and the conductive carbon slurry is directly coated on the perovskite layer, and the rest is the same as Comparative Example 1.

[0130] Comparative Example 3

[0131] The difference between Comparative Example 3 and Comparative Example 1 is that the conductive carbon layer is subjected to a non-vacuum annealing treatment, and the annealing conditions are the same as those of Example 1, and the rest are the same as Comparative Example 1.

[0132] Comparative Example 4

[0133] The preparation method of the first combination layer is the same as that of Example 1; then, a carbon electrode film layer is prepared according to the conductive carbon slurry in Example 1, and then the carbon electrode film layer is adhered to the side of the functional layer away from the substrate through an adhesive, and then the first combination layer + carbon electrode film layer and the packaging base plate are hot-pressed and packaged according to the hot-pressing packaging method of Example 1 to obtain a solar cell.

[0134] The open circuit voltage, short circuit current, fill factor and photoelectric conversion efficiency of the batteries prepared in the above Examples 1-7 and Comparative Examples 1-4 were tested. The test results are shown in Table 1.

[0135] Table 1 Performance test table of various embodiments and comparative examples

[0136]

[0137]

[0138] It can be seen from Table 1 above that, compared with Example 1 and Comparative Example 3, Comparative Example 3 directly coats the conductive carbon slurry on the hole transport layer, and the battery prepared in Comparative Example 3 has low open circuit voltage, low short circuit current, low photoelectric conversion rate, and low filling factor. Compared with Example 2 and Comparative Example 2, in the absence of a hole transport layer, the battery performance of Comparative Example 2 is also poor, indicating that coating the carbon slurry on the packaging base plate 4 can avoid direct contact between the functional layer materials and the organic solvent in the conductive carbon slurry, thereby protecting the functional layer and improving the photoelectric conversion efficiency of the battery. At the same time, the use of low-viscosity conductive carbon slurry enhances the adhesion between the carbon electrode and the wire, promotes the carrier transport effect, and improves the conductivity of the carbon electrode. Comparative Example 1 is compared with Example 1. The annealing condition of Comparative Example 1 is vacuum annealing. Compared with Comparative Example 3, although the short-circuit current, open-circuit voltage and fill factor in Comparative Example 1 are improved, the photoelectric conversion efficiency of the battery is still poor, which shows that coating the carbon slurry on the packaging base plate 4 can avoid direct contact between the functional layer materials and the organic solvent in the conductive carbon slurry, thereby protecting the functional layer and improving the photoelectric conversion efficiency of the battery.

[0139] In Comparative Example 4, the carbon electrode is directly pasted onto the functional layer. Although it can also play a conductive role, compared with Example 1, the photoelectric conversion efficiency of the battery is poor, indicating that the solar cell preparation method provided in the present application has the effect of improving the photoelectric conversion efficiency of the battery.

[0140] Comparing Example 1 with Example 2, there is no hole transport layer, and the photoelectric conversion rate of the battery is poor, indicating that although the carbon electrode 3 can play the role of transporting holes, the photoelectric conversion rate of the battery without a hole transport layer is still poor. In Example 3, the conductive carbon slurry solvent is water, and in Example 4, the conductive carbon slurry solvent is a mixture of water and ethanol. Comparing Examples 1, 3, and 4, the conductive carbon slurry solvent is a mixture of water and ethanol. The carbon material is better dispersed in the carbon slurry, which can make the conductive carbon slurry fit more closely with the wire, improve carrier transmission, and the prepared carbon electrode 3 has higher conductivity and higher battery photoelectric conversion efficiency. Comparing Examples 1, 5, and 7, the ratio of the two in Example 7 is not within the scope of the present application, the binder content is high, and the photoelectric conversion efficiency of the battery is low; the mass ratio of the carbon material to the binder in Example 5 is in the range of 1:(0.05-0.5), but is not in the preferred range, and the battery photoelectric conversion efficiency is low; the mass ratio of the carbon material to the binder in Example 1 is in the range of 1:(0.05-0.15), and the battery photoelectric conversion efficiency is high compared with Example 5, indicating that the mass ratio of the carbon material and the binder is between 1:(0.05-0.5), which can improve the battery photoelectric conversion rate, and the more preferred mass ratio of the carbon material and the binder is in the range of 1:(0.05-0.15), and the battery has a higher battery photoelectric conversion efficiency.

[0141] Compared with Example 1 and Example 6, Example 6 adopts low-temperature and long-term annealing to volatilize N-methylpyrrolidone, but the carbon electrode prepared at low temperature has poor conductivity, which makes the battery photoelectric conversion efficiency low; it shows that at a lower first annealing temperature, although the first annealing time is extended to volatilize the solvent in the conductive carbon slurry, the carbon electrode 3 prepared by low-temperature annealing has poor conductivity and the battery photoelectric conversion efficiency is high, indicating that the first annealing temperature is between 50-200°C and the first annealing time is between 10s-30min, and the carbon electrode 3 has a higher conductivity, which improves the battery photoelectric conversion efficiency. Compared with Example 1 and Examples 3-4, the first annealing temperature is between 70-120°C and the first annealing time is between 5-15min, and the conductivity of the carbon electrode 3 is higher, and the battery photoelectric conversion efficiency is higher.

[0142] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a flexible carbon electrode perovskite solar cell, It is characterized in that The following steps are involved: preparing a functional layer on a substrate to obtain a first composite layer; Coating a conductive carbon slurry on the packaging bottom plate, and performing a first annealing treatment to form a carbon electrode on the packaging bottom plate to obtain a second composite layer; The first combined layer and the second combined layer are heat-pressed and packaged, and the side of the functional layer away from the substrate is in contact with the carbon electrode to obtain a flexible carbon electrode perovskite solar cell.

2. The method for preparing a flexible carbon electrode perovskite solar cell according to claim 1, It is characterized in that The conductive carbon paste comprises a carbon material, a binder and a solvent. The solvent is a low-viscosity system solvent, and the viscosity of the solvent is 1 to 20 mPa·s.

3. The method for preparing a flexible carbon electrode perovskite solar cell according to claim 2, It is characterized in that The solvent includes one or more of water, ethanol, terpineol, ethylene glycol methyl ether, ethylene glycol 19.9, glycerol, glycerol methyl ether, N-methyl pyrrolidone, butyl acetate, butyl acetate, diethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, isophorone, and alkanes; The carbon material includes one or more of Ketjen black, acetylene black, carbon nanotubes, graphene, and carbon black; The binder includes one or more of acrylic resin, polyvinylidene fluoride, polyvinyl acetate, ethylene-vinyl acetate copolymer, polymethyl methacrylate, polycarbonate, polyamide, sodium carboxymethyl cellulose, and polystyrene.

4. The method for preparing a flexible carbon electrode perovskite solar cell according to claim 2, It is characterized in that The mass ratio of the carbon material to the binder is 1:(0.05-0.5).

5. The method for preparing a flexible carbon electrode perovskite solar cell according to claim 4, It is characterized in that The mass ratio of the carbon material to the binder is 1:(0.05-0.15).

6. The method for preparing a flexible carbon electrode perovskite solar cell according to claim 1 or 2, It is characterized in that The solid content of the conductive carbon slurry is 10% to 50%.

7. The method for preparing a flexible carbon electrode perovskite solar cell according to claim 1, It is characterized in that In the first annealing step, the first annealing temperature is 50° C. to 200° C., and the first annealing time is 10 s to 30 min.

8. The method for preparing a flexible carbon electrode perovskite solar cell according to claim 7, It is characterized in that The first annealing temperature is 70° C. to 120° C., and the first annealing time is 5 min to 15 min.

9. The method for preparing a flexible carbon electrode perovskite solar cell according to claim 1, It is characterized in that The thickness of the carbon electrode is 0.05 μm to 500 μm.

10. The method for preparing a flexible carbon electrode perovskite solar cell according to claim 1, It is characterized in that In the step of hot-pressing and packaging the first combined layer and the second combined layer, the hot-pressing temperature is 50° C. to 200° C., and the hot-pressing pressure is 1 KPa to 200 KPa.

11. The method for preparing a flexible carbon electrode perovskite solar cell according to claim 1, It is characterized in that Before preparing the functional layer on the substrate, the substrate is pre-treated, and the pre-treatment includes the following steps: firstly ultrasonically cleaning the substrate with a cleaning solvent, drying, and then ozone treating for 5 to 20 minutes; The cleaning solvent includes one or more of detergent water, water, ethanol, and isopropanol.

12. The method for preparing a flexible carbon electrode perovskite solar cell according to claim 1, It is characterized in that The functional layer includes an electron transport layer and a perovskite layer, and preparing the functional layer on the substrate includes the following steps: The electron transport layer is deposited on the substrate, and after drying, a perovskite precursor solution is deposited on the electron transport layer, and an anti-solvent or vacuum treatment is performed, and then a second annealing treatment is performed to obtain the perovskite layer.

13. The method for preparing a flexible carbon electrode perovskite solar cell according to claim 12, It is characterized in that The electron transport layer includes one or more of titanium nitride, tin oxide, titanium oxide, nickel oxide, C60, and PCBM, and the thickness of the electron transport layer is 2nm to 200nm.

14. The method for preparing a flexible carbon electrode perovskite solar cell according to claim 12, It is characterized in that The perovskite precursor solution comprises perovskite and a solvent, The structure of the perovskite is A x A' (1-x) BX 3 , Wherein 0<x<1, A includes one or more of formamidine and methylamine; A' is one or more of cesium, potassium, sodium, calcium, and rubidium; B includes one or more of lead and tin; and X is one or more of iodine, bromine, chlorine, and fluorine; The solvent includes one or more of N,N-dimethylformamide, N-methylpyrrolidone, dimethyl sulfoxide, γ-hydroxybutyrolactone, isopropanol, diphenyl sulfoxide, and ethyl acetate.

15. The method for preparing a flexible carbon electrode perovskite solar cell according to claim 14, It is characterized in that x is 0.5 to 0.

99.

16. The method for preparing a flexible carbon electrode perovskite solar cell according to claim 12, It is characterized in that The thickness of the perovskite layer is 100nm-1000nm.

17. The method for preparing a flexible carbon electrode perovskite solar cell according to claim 12, It is characterized in that The anti-solvent includes one or more of chlorobenzene, acetonitrile, ethanol, isopropanol, ethyl acetate, and ether; in the vacuum treatment step, the vacuum degree is 50-5000 Pa, and the vacuum treatment time is 10s-1000s; in the second annealing treatment step, the second annealing temperature is 50-200°C, and the second time is 5-500min.

18. The method for preparing a flexible carbon electrode perovskite solar cell according to claim 12, It is characterized in that The functional layer further includes a hole transport layer, and preparing the functional layer on the substrate further includes the following steps: depositing the hole transport layer on the surface of the perovskite layer away from the resistance transport layer; The thickness of the hole transport layer is 20nm-200nm; The hole transport layer includes one or more of Spiro-OMeTAD, PTAA, PEDOT:PSS, CuOx, and NiOx.

19. The method for preparing a flexible carbon electrode perovskite solar cell according to claim 1, It is characterized in that The substrate includes a transparent electrode and a flexible substrate, wherein the flexible substrate includes one or more of glass, a first polymer material, and a first metal film; the packaging base plate includes a packaging base plate body and a packaging layer arranged on the packaging base plate body, and the base plate body includes a second polymer material or a second metal film; the first polymer material and the second polymer material are each independently selected from one or more of polyethylene naphthalate and polyethylene terephthalate; The transparent electrode comprises one or more of indium tin oxide, fluorine-doped tin oxide, carbon nanotubes, and graphene; The encapsulation layer includes one or more of ethylene-octene polymer, butyl rubber, metal oxide, and metal nitride.

20. A flexible carbon electrode perovskite solar cell, It is characterized in that The flexible carbon electrode perovskite solar cell is prepared by the preparation method of any one of claims 1 to 19.

Citation Information

Cited By

  • Perovskite solar cell and preparation method thereof

    CN119855450A