Bonded body manufacturing method, bonded body, and electrical / electronic component

By configuring component materials and thermoplastic film A on a support substrate, and utilizing the bonding between thermoplastic film A and resin B, the problems of long bonding time and poor sealing in the process of bonding dissimilar materials are solved, realizing a fast, strong and thermally resistant bonding method for manufacturing a bond.

CN119053433APending Publication Date: 2024-11-29RESONAC CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202380035207.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-12-19
Filing Date
2023-11-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing technologies for bonding dissimilar materials suffer from problems such as long bonding time, poor sealing, insufficient leakage resistance, and easy peeling during thermal cycling. In particular, it is difficult to achieve a strong and tight bond when using liquid adhesives and surface roughening treatments.

Method used

The method involves placing component materials and thermoplastic film A on a support substrate. By bonding thermoplastic film A with resin B, and utilizing the melting and curing of thermoplastic film A, rapid sealing of dissimilar materials is achieved. The thermoplastic properties of thermoplastic film A are used to alleviate stress and improve the sealing performance.

Benefits of technology

It enables rapid and robust bonding of dissimilar materials, improves adhesion and peel resistance, adapts to stress changes during thermal cycling, and reduces the bonding process time and operational complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119053433A_ABST
    Figure CN119053433A_ABST
Patent Text Reader

Abstract

A method for producing a bonded body in which a support substrate, an element material, a thermoplastic film A, and a resin B are arranged in this order and bonded, the method comprising the following steps in this order: a step 1 in which the element material is arranged on the support substrate; and a step (2) in which the resin (B) is bonded to at least a portion of the element material in a state in which the element material is disposed on the support substrate with the thermoplastic film (A) interposed therebetween, and the element material and the thermoplastic film (A) are sealed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a joined body in which dissimilar materials are firmly joined together, the joined body, and an electric and electronic component. Background Art

[0002] In recent years, from the perspective of product lightweighting and high performance, the use of multiple materials has been developing in various fields such as automotive parts, medical equipment, and home appliances. The so-called multi-materialization is a method of achieving lightweight and high strength of materials by using materials with different functions and materials (hereinafter referred to as "heterogeneous materials"). In order to achieve multi-materialization, technology to firmly join heterogeneous materials is indispensable.

[0003] As an example of a product that uses components that must be made of multiple materials, a semiconductor package can be cited. The semiconductor package has electrical conductive components such as a lead frame, an IC chip, or a wire on a substrate, and the electrical conductive components are sealed with a sealing material. In particular, electronic devices often fail due to minute moisture or dust, and the sealing portion is required to have a high degree of tightness.

[0004] For example, it is known to use a resin material as a sealing material to seal the periphery of a metal terminal by insert molding such as injection molding. However, if the resin material is sealed to the metal by insert molding, there is a possibility that it will leak out from the gap. In particular, when the resin material is sealed in a manner that covers the periphery of a metal terminal, etc., a better leakage resistance is required.

[0005] As a method of sealing a metal terminal with a resin material, for example, a method of sealing the metal terminal with a resin material by insert molding after applying a liquid adhesive or varnish on the metal terminal has been studied. Specifically, a technique is known in which a seal is formed by applying an in-situ polymerizable composition on an electrode body and polymerizing it to provide a primer layer (Patent Document 1, etc.). In addition, a technique is known in which an external terminal is immersed in a bath filled with a cationic epoxy resin electrodeposition coating, and a terminal adhesive layer is provided by applying electricity to form a seal member (Patent Document 2, etc.).

[0006] In addition, a method of roughening the surface of a metal terminal and then sealing it with a resin material by insert molding has been studied. Specifically, there is a known technique of mechanically polishing the joint surface of the metal terminal with the sealing resin by sandblasting, shot peening, grinding, barrel processing, etc., or polishing the surface layer by chemical polishing (Patent Document 3, etc.).

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2021-157887

[0010] Patent Document 2: Japanese Patent Application Publication No. 2020-88137

[0011] Patent Document 3: Japanese Patent Application Publication No. 2016-126989 Summary of the invention

[0012] Inventions should solve problems

[0013] However, in the technology of applying liquid adhesive, bonding sometimes takes time, which easily leads to problems such as application time (usable time) and trouble. In addition, sometimes leakage resistance is damaged due to insufficient or uneven coating operation, or pollution risk is generated due to excessive coating amount, resulting in poor workability.

[0014] In addition, when using a liquid thermosetting adhesive, when the metal terminal is repeatedly exposed to high and low temperatures (hot and cold cycles), the metal terminal and the sealing resin are misaligned due to the difference in linear expansion coefficient between the metal terminal and the sealing resin, and the adhesive layer is subjected to stress. Moreover, if the stress is not relieved, the adhesive layer will peel off, which is likely to cause leakage. This is because the thermosetting adhesive layer does not have thermoplasticity and will quickly break when it reaches the plastic deformation area.

[0015] In addition, by roughening the surface of the metal terminal, the bonding strength with the sealing material is improved. On the other hand, a gap is easily formed between the rough surface of the metal terminal and the sealing material, which has the risk of insufficient leakage resistance. Moreover, during the aforementioned hot and cold cycles, since there is no layer that can relieve stress, it is easy to peel off. Therefore, the sealing material is not only required to be firmly bonded to the interface of heterogeneous materials such as lead frames, IC chips or metal wires, but also difficult to peel off, so excellent adhesion is required.

[0016] Therefore, an object of the present invention is to provide a method for producing a joined body in which the joining process time is short, dissimilar materials are firmly joined and the adhesion is excellent, a joined body and an electric and electronic component.

[0017] Solution

[0018] The present inventors have found that the above-mentioned problems can be solved by disposing a predetermined thin film on a device material on a substrate and then sealing the device material and the thin film with a resin.

[0019] That is, the present invention is as follows.

[0020] [1] A method for manufacturing a bonded body, wherein the bonded body is formed by arranging and bonding a supporting substrate, an element material, a thermoplastic film A, and a resin B in this order, the method comprising the following steps in sequence:

[0021] Step 1 of disposing the element material on the support substrate; and

[0022] Step 2 of bonding the resin B to at least a portion of the device material disposed on the support substrate via the thermoplastic film A to seal the device material and the thermoplastic film A.

[0023] [2] The method for producing a joined body according to [1], wherein the thermoplastic film A has adhesion to the element material.

[0024] [3] A method for manufacturing a joined body as described in [1] or [2], wherein in step 2, after the thermoplastic film A is joined to the resin B, the thermoplastic film A in a state of being joined to the resin B is brought into contact with the element material arranged on the supporting substrate (i.e., brought into surface-to-surface contact), and the thermoplastic film A is melted and then solidified, thereby joining the resin B and sealing the element material and the thermoplastic film A.

[0025] [4] A method for manufacturing a joined body as described in [1] or [2], wherein in the step 2, after the thermoplastic film A is joined to the element material arranged on the supporting substrate, the resin B is brought into contact with the thermoplastic film A, and the thermoplastic film A is melted and then solidified, thereby joining the resin B and sealing the element material and the thermoplastic film A.

[0026] [5] A method for manufacturing a bonded body as described in [1] or [2], wherein in step 2, the element material, the thermoplastic film A and the resin B are arranged in this order on the supporting substrate, and then the thermoplastic film A is melted and solidified, thereby bonding the resin B and sealing the element material and the thermoplastic film A.

[0027] [6]. A method for manufacturing a joined body as described in any one of [1] to [5], wherein in step 2, joining is performed by at least one selected from contact heating, hot air heating, hot pressing, infrared heating, hot plate fusion, ultrasonic fusion, vibration fusion and high-frequency induction fusion.

[0028] [7] The method for producing a joined body according to any one of [1] to [6], wherein in step 2, joining is performed at a temperature of 100 to 300°C at the joining portion.

[0029] [8] The method for producing a joined body according to any one of [1] to [7], wherein the thickness of the thermoplastic film A is not less than 10 μm and not more than 3 mm.

[0030] [9]. The method for producing a joined body according to any one of [1] to [8], wherein the thermoplastic film A contains more than 50% by mass of an amorphous thermoplastic resin.

[0031]

[10] . The method for producing a joined body according to [9], wherein the amorphous thermoplastic resin is at least one of a thermoplastic epoxy resin and a phenoxy resin.

[0032]

[11] . The method for producing a joined body according to any one of [1] to

[10] , wherein the thermoplastic film A is a thermoplastic resin having an epoxy equivalent of 1600 g / eq. or more or containing no epoxy group.

[0033]

[12] . The method for producing a joint according to any one of [1] to

[11] , wherein the element material is a metal.

[0034]

[13] . The method for producing a joined body according to any one of [1] to

[12] , wherein the resin B is a thermosetting resin.

[0035]

[14] . An electric or electronic component comprising a bonded body obtained by the method for producing a bonded body according to any one of [1] to

[13] .

[0036] Effects of the Invention

[0037] According to the present invention, it is possible to provide a method for producing a joined body in which the joining process time is short, dissimilar materials are firmly joined and the adhesion is excellent, a joined body, and an electric and electronic component. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is a schematic cross-sectional view schematically showing an example of an embodiment of a bonded body. DETAILED DESCRIPTION

[0039] Hereinafter, embodiments of the present invention will be described in detail.

[0040] In this specification, "joining" means connecting objects together, and adhesion and fusion are subordinate concepts. The so-called "bonding" refers to the use of organic materials such as tapes or adhesives (thermosetting resins or thermoplastic resins, etc.) to make two bonded materials (materials to be bonded together) into a joined state. "Fusion" means that the surface of thermoplastic resins, etc. is melted by heat, and the molecular diffusion caused by cooling process causes entanglement and compatibility, so that they are in a joined state. "Adhesion" refers to the property of having an adhesive strength that can connect objects to objects. "Adhesion" refers to the property of having a strength that allows objects to be tightly attached to each other. "Adhesion" and "adhesion" are different properties.

[0041] In this specification, the "bonding process time" refers to the time from the start point when the element material constituting the bonded body comes into contact with the film to the end point when the production of the bonded body is completed.

[0042] In this specification, the description "A to B" indicating a numerical range indicates a numerical range including endpoints A and B. That is, it means "A or more and B or less" (when A < B) or "A or less and B or more" (when A > B).

[0043] <Method for producing a bonded body>

[0044] The method for manufacturing a bonded body of the present embodiment is formed by arranging and bonding a supporting substrate, a component material, a thermoplastic film A, and a resin B in this order, and the manufacturing method sequentially comprises the following steps:

[0045] Step 1 of disposing the element material on the support substrate; and

[0046] Step 2 of bonding the resin B to at least a portion of the device material disposed on the support substrate via the thermoplastic film A to seal the device material and the thermoplastic film A.

[0047] By providing the thermoplastic film A between the element material on the support substrate and the resin B as the sealing material, the support substrate and the element material are firmly bonded to the resin B. Moreover, since the thermoplastic film A can be directly brought into contact with the element material on the support substrate, it can be said that this is an effective operation in shortening the bonding process compared to the case where a liquid bonding agent is applied. In addition, by using the thermoplastic film A having a uniform thickness, compared to the case where a liquid bonding agent is applied, uneven portions such as incomplete coating or dripping are not generated, and different materials can be firmly bonded, exhibiting excellent adhesion.

[0048] The reasons why the effects of the present invention can be obtained are examined in more detail below.

[0049] By providing a thermoplastic resin that has completed a chemical reaction such as polymerization between the element material on the support substrate and the resin B, it is possible to quickly solidify by utilizing the phase change between solid and liquid, thereby shortening the bonding process. In addition, by using the thermoplastic resin in a film form, there is no trouble of handling the liquid, compared with applying an amorphous liquid bonding agent, and the bonding process time is shortened.

[0050] In addition, if it is a thermoplastic resin, since it also has thermoplasticity at high temperatures, it can relax stress, and can readjust stress in each cycle during hot and cold cycles, thereby preventing peeling. Therefore, by using the thermoplastic film A, plastic deformation can be performed, and stress can be effectively relaxed, so that a bonded body that is difficult to peel off during hot and cold cycles and has excellent adhesion can be formed. In addition, by softening the thermoplastic film A when the bonded body is exposed to high temperatures, stress can be more effectively relaxed, so peeling resistance and adhesion are excellent.

[0051] Furthermore, as an example of a preferred embodiment, when an amorphous thermoplastic film A is used as the thermoplastic film A, the film is less likely to rapidly decrease in viscosity when heated, and thus can maintain a shape for maintaining the peel resistance and adhesion of the bonded body when exposed to high temperatures.

[0052] [Process 1]

[0053] In step 1, the element material is arranged on the support substrate. The element material may be arranged on the support substrate and temporarily fixed after applying an adhesive within a range that does not hinder the effect of the present invention. As the adhesive, a commercially available product can be used.

[0054] [Support substrate]

[0055] The shape of the support substrate may be, for example, a flat plate. The flat plate-shaped support substrate may include, for example, a recessed portion large enough to accommodate the element material, the thermoplastic film A, the resin B, and the like.

[0056] As the material of the support substrate, an appropriate material can be used according to the physical properties required for the application of the bonded body, etc. As an example of a material suitable for the support substrate, the same materials as those of the element material described later can be cited.

[0057] (Component Materials)

[0058] As the material of the element material, for example, metals and inorganic substances can be mentioned. As the material of the element material, one kind may be used alone, or two or more kinds may be used in combination.

[0059] From the viewpoint of heat resistance and strength, the element material is preferably metal.

[0060] When the material of the element material is a resin, the material of the resin must have a melting point or a glass transition temperature at which it does not deform at the temperature at the time of bonding in step 2 .

[0061] The metal is not particularly limited, and examples thereof include aluminum, iron, copper, magnesium, and titanium.

[0062] In addition, in this embodiment, the term "iron" is used to include iron and its alloys. As iron alloys, steel, stainless steel, etc. can be listed. Similarly, copper, aluminum, magnesium, and titanium are also used to include their monomers and their alloys.

[0063] The inorganic substance is not particularly limited, and examples thereof include glass, ceramics, and carbon molded bodies.

[0064] As glass, for example, in addition to general glass, it can also be heat-resistant glass, fire-resistant glass, fire-resistant glass, chemically strengthened glass for protecting smartphones, etc. Specifically, soda lime glass, lead glass, borosilicate glass can be listed. As ceramics, for example, fine ceramics used in semiconductors, automobiles, industrial equipment, etc. can be listed. Specifically, oxide-based ceramics such as aluminum oxide, zirconium oxide, and barium titanate; hydroxide-based ceramics such as hydroxyapatite, carbide-based ceramics such as silicon carbide; nitride-based ceramics such as silicon nitride, etc. can be listed.

[0065] Examples of the resin used as the material of the element include glass fiber reinforced thermosetting resins, cured products of thermosetting resins such as epoxy resins, vinyl ester resins, and unsaturated polyesters, and highly heat-resistant engineering plastics such as polyimide resins, polyetherimide, and polyethersulfone.

[0066] A pretreatment suitable for the component material may also be implemented. As the pretreatment, a pretreatment for cleaning the surface or a pretreatment for forming unevenness on the surface is preferred. Specifically, when the component material is composed of aluminum, ceramic or iron, at least one of degreasing treatment, UV ozone treatment, sandblasting, grinding treatment, plasma treatment and etching treatment is preferably selected. When the component material is composed of FRP, polypropylene, polycarbonate, polymethyl methacrylate, polyetherimide, polyamide or polybutylene terephthalate, at least one of degreasing treatment, UV ozone treatment, sandblasting, grinding treatment, plasma treatment and corona discharge treatment is preferably selected.

[0067] Only one type of pretreatment may be performed, or two or more types may be performed. As specific methods of these pretreatments, known methods can be used.

[0068] [Process 2]

[0069] In step 2, the resin B is bonded to at least a portion of the element material disposed on the support substrate via the thermoplastic film A, so that the element material and the thermoplastic film A are sealed.

[0070] Here, “at least a portion of the device material disposed on the support substrate” refers to the entirety or a portion of the surface of the device material that is not in contact with the support substrate.

[0071] In the method for producing a bonded body of the present embodiment, examples of methods for bonding the element material, the thermoplastic film A, and the resin B disposed on a supporting substrate in this order include the following methods a, b, and c.

[0072] 〔Method a〕

[0073] Method a is a method in which after bonding a thermoplastic film A to a resin B, the thermoplastic film A bonded to the resin B is brought into contact with a device material disposed on a supporting substrate, and the thermoplastic film A is melted and then solidified, thereby bonding the resin B and sealing the device material and the thermoplastic film A.

[0074] In method a, first, as step a1, thermoplastic film A and resin B are bonded in advance. For example, thermoplastic film A and resin B may be bonded by injecting resin B into the cavity while thermoplastic film A is provided on the wall surface of the cavity of the mold.

[0075] By bonding the thermoplastic film A and the resin B in advance, it is possible to bond the element material disposed on the support substrate and the resin B with high accuracy. In this case, the thermoplastic film A may have adhesiveness.

[0076] Next, as step a2, the thermoplastic film A bonded to the resin B is brought into contact with the device material disposed on the supporting substrate, and the thermoplastic film A is melted and then solidified.

[0077] The element material disposed on the supporting substrate may be pressed against the molten thermoplastic film A so that the thermoplastic film A follows the element material.

[0078] By melting the thermoplastic film A, at least the interface portion of the resin B in contact with the thermoplastic film A can be melted and solidified together with the thermoplastic film A. The thermoplastic film A can be solidified after being melted, so that the element material arranged on the supporting substrate can be bonded to the resin B. As a result, the resin B can seal the element material arranged on the supporting substrate and the thermoplastic film A.

[0079] When the thermoplastic film A is brought into contact with the element material disposed on the support substrate and the thermoplastic film A is melted, it is preferred to melt the thermoplastic film A by heating at a temperature equal to or higher than the melting point of at least one of the thermoplastic film A and the resin B in order to obtain a high bonding strength. By heating at a temperature equal to or higher than the melting point of at least one of the thermoplastic film A and the resin B, the thermoplastic film A and the resin B are compatible, and a stronger bonding strength is easily obtained.

[0080] In the method a, the method of melting the thermoplastic film A and then solidifying it is as described in the "melting and solidifying" below.

[0081] [Method b]

[0082] Method b is a method in which a thermoplastic film A is bonded to an element material disposed on a supporting substrate, and then resin B is brought into contact with the thermoplastic film A, and the thermoplastic film A is melted and then solidified, thereby bonding resin B and sealing the element material and the thermoplastic film A.

[0083] In the method b, first, as step b1, the thermoplastic film A is bonded to the element material disposed on the support substrate in advance. For example, the thermoplastic film A may be bonded to the element material disposed on the support substrate by melting the thermoplastic film A and then solidifying the thermoplastic film A in a state where the thermoplastic film A is in contact with the element material disposed on the support substrate.

[0084] By bonding the thermoplastic film A and the element material disposed on the support substrate in advance, it is possible to bond the element material disposed on the support substrate with high precision to the resin B. In this case, the thermoplastic film A may have adhesiveness.

[0085] Next, as step b2, the thermoplastic film A bonded to the element material disposed on the supporting substrate is brought into contact with the resin B, and the thermoplastic film A is melted and then solidified.

[0086] The resin B may be pressed onto the molten thermoplastic film A so that the thermoplastic film A follows the element material.

[0087] By bringing the molten thermoplastic film A into contact with the resin B, at least the contacting portion of the resin B in contact with the thermoplastic film A can be melted and solidified together with the thermoplastic film A. The thermoplastic film A can be solidified after being melted, so that the element material disposed on the supporting substrate can be bonded to the resin B. As a result, the resin B can seal the element material disposed on the supporting substrate and the thermoplastic film A.

[0088] In addition, the insert molding method can also be applied in the b2 step. As a specific method, first, a thermoplastic film A is provided on the wall surface in the cavity of the mold to be bonded to the element material disposed on the support substrate. At this time, the wall surface in the cavity of the mold is provided to be in contact with the support substrate. Next, by injecting resin B into the cavity, the thermoplastic film A is brought into contact with the resin B, and the thermoplastic film A is melted and then solidified. By this method, the resin B can also seal the element material disposed on the support substrate and the thermoplastic film A.

[0089] When the thermoplastic film A is melted in a state where the thermoplastic film A and the resin B are in contact with each other, it is preferred to melt the thermoplastic film A by heating at a temperature higher than the melting point of at least one of the thermoplastic film A and the resin B in order to obtain a high bonding strength. By heating at a temperature higher than the melting point of at least one of the thermoplastic film A and the resin B, the thermoplastic film A and the resin B are compatibilized, and a stronger bonding strength is easily obtained.

[0090] In the method b, the method of melting the thermoplastic film A and then solidifying it is as described later in "melting and solidifying".

[0091] 〔Method C〕

[0092] Method c is a method in which the element material, thermoplastic film A and resin B are arranged in this order on a supporting substrate, and then the thermoplastic film A is melted and then solidified to bond the resin B and seal the element material and the thermoplastic film A.

[0093] In the c method, first, as step c1, the element material, thermoplastic film A, and resin B arranged on a supporting substrate are stacked in this order to form a laminate. The laminate is formed by stacking the element material, thermoplastic film A, and resin B arranged on a supporting substrate, which are independent of each other and are not bonded to any of the groups of thermoplastic film A and resin B. At this time, the thermoplastic film A may also have adhesiveness.

[0094] Next, as step c2, the thermoplastic film A in the laminate is melted and then solidified.

[0095] The thermoplastic film A may be made to follow the device material by applying force toward the thermoplastic film A from the support substrate side, the resin B side, or both the support substrate side and the resin B side to press the molten thermoplastic film A.

[0096] By melting the thermoplastic film A, at least the interface portion of the resin B in contact with the thermoplastic film A can be melted and solidified together with the thermoplastic film A. The thermoplastic film A can be solidified after being melted, so that the element material arranged on the supporting substrate can be bonded to the resin B. As a result, the resin B can seal the element material arranged on the supporting substrate and the thermoplastic film A.

[0097] When melting the thermoplastic film A in the laminate, it is preferred to melt the thermoplastic film A by heating at a temperature equal to or higher than the melting point of at least one of the thermoplastic film A and the resin B, from the viewpoint of obtaining high bonding strength. By heating at a temperature equal to or higher than the melting point of at least one of the thermoplastic film A and the resin B, the thermoplastic film A and the resin B become compatible, and a stronger bonding strength is easily obtained.

[0098] In method c, the method of melting the thermoplastic film A and then solidifying it is the same as the "melting and solidifying" described later.

[0099] [combination]

[0100] The method for producing a bonded body according to the present embodiment may include a combination of at least two steps selected from the group consisting of step a1 in the method a, step b1 in the method b, and step c1 in the method c.

[0101] As an example, a combination of step a1 and step b1 can be cited.

[0102] Specifically, a bonded body a in which a thermoplastic film A is bonded to a resin B in step a1 is bonded to a bonded body b in which a thermoplastic film A is bonded to a device material disposed on a support substrate in step b1. The bonded body a and the bonded body b are brought into contact with each other in a face-to-face manner (face-to-face contact), and the two thermoplastic films A are melted and then solidified. At this time, while the thermoplastic film A is melted, a force may be applied to the thermoplastic film A from the bonded body a side, from the bonded body b side, or from both the bonded body a side and the bonded body b side to press the thermoplastic film A, thereby making the thermoplastic film A follow the device material. That is, the method for manufacturing a bonded body having a combination of step a1 and step b1 can bond the device material and the resin B disposed on a support substrate using two thermoplastic films A.

[0103] Furthermore, as another example, a combination of step a1 and step c1 can be cited.

[0104] Specifically, in the c1 step, a bonded body a formed by bonding a thermoplastic film A and a resin B in the a1 step is arranged instead of the resin B. At this time, the thermoplastic film A bonded to the bonded body a is made to face another independent thermoplastic film A. That is, the element material, the thermoplastic film A, and the bonded body a in a state arranged on the supporting substrate are arranged in this order and stacked to form a laminate. Next, the two thermoplastic films A in the laminate are melted and then solidified. At this time, in a state where the thermoplastic film A is melted, a force may be applied to the thermoplastic film A from the bonded body a side, or from the supporting substrate side, or from both the bonded body a side and the supporting substrate side to press, thereby making the thermoplastic film A follow the element material. That is, the method for manufacturing a bonded body having a combination of the a1 step and the c1 step can bond the element material and the resin B in a state arranged on the supporting substrate using two thermoplastic films A.

[0105] Furthermore, as another example, a combination of step b1 and step c1 can be cited.

[0106] Specifically, in the c1 step, a bonded body b formed by bonding a thermoplastic film A to the element material disposed on the support substrate in the b1 step is disposed instead of the element material disposed on the support substrate. At this time, the thermoplastic film A bonded to the bonded body b is opposed to another independent thermoplastic film A. That is, a laminated body is formed in which the bonded body b, the thermoplastic film A and the resin B are disposed in this order and stacked. Next, the two thermoplastic films A in the laminated body are melted and then solidified. At this time, in the state where the thermoplastic film A is melted, a force may be applied to the thermoplastic film A from the resin B side, from the bonded body b side, or from both the resin B side and the bonded body b side to press the thermoplastic film A, thereby making the thermoplastic film A follow the element material. That is, the method for manufacturing a bonded body having a combination of the b1 step and the c1 step can bond the element material disposed on the support substrate and the resin B using two thermoplastic films A.

[0107] Melting and Solidification

[0108] In step 2, the bonding is preferably performed by melting the thermoplastic film A by at least one selected from contact heating, hot air heating, heat pressing, infrared heating, hot plate fusion, ultrasonic fusion, vibration fusion, and high-frequency induction fusion.

[0109] Among them, heat pressing or high-frequency induction welding is preferred from the viewpoint of ease of production and shortening of the joining process.

[0110] When the thermoplastic film A is melted by heating, the temperature of the joint between the element material disposed on the support substrate and the thermoplastic film A can be determined in consideration of the heat resistance temperature of the material of the support substrate and the element material, but is preferably 100 to 300° C., more preferably 120 to 250° C., and further preferably 150 to 220° C. By performing the joining at 100 to 300° C., the thermoplastic film A is effectively deformed and melted, and effectively wets and spreads on the joining surface, so that a high joining force can be obtained.

[0111] As a method for solidifying the melted thermoplastic film A, there can be listed a method of cooling at room temperature or a method of cooling using a cooling device. In addition, "room temperature" refers to a general room temperature in the range of 5 to 30° C. Among them, the method of cooling at room temperature is preferred from the viewpoint of ease of production.

[0112] In the present specification, "solidified" means being solid at room temperature, that is, having no fluidity at 23°C and in a non-pressurized state.

[0113] [Thermoplastic film A]

[0114] The thermoplastic film A preferably contains a thermoplastic resin as a main component. In addition, the thermoplastic film A preferably has adhesiveness to the element material.

[0115] In this specification, "main component" means the component with the highest content among the resin components in the thermoplastic film A. The thermoplastic film A preferably contains more than 50% by mass of the resin component, more preferably 70% by mass or more, further preferably 80% by mass or more, and particularly preferably 90% by mass or more.

[0116] The “film” mentioned above refers to a resin composition containing a thermoplastic resin as a main component formed into a thin film.

[0117] 《Y℃-X℃》

[0118] When the thermoplastic resin used in the thermoplastic film A has a melting point, the melting point of the thermoplastic film A is set to X°C, or when the thermoplastic resin used in the thermoplastic film A does not have a melting point, the temperature obtained by adding 70°C to the glass transition temperature is set to X°C, and the resin temperature of the resin B during bonding is set to Y°C. The value obtained by subtracting X°C from Y°C (Y°C-X°C) is preferably 0 to 300°C, more preferably 50 to 250°C, further preferably 100 to 250°C, and further preferably 125 to 210°C. In particular, when the resin B is a thermoplastic resin, the above Y°C-X°C is preferably within the range of 0 to 300°C, because the thermoplastic film A is efficiently melted by heating when bonding with the resin B, and is effectively wetted and spread on the bonding surface, so that high adhesion can be obtained.

[0119] In this specification, the melting point of a thermoplastic resin refers to the endothermic peak temperature due to melting measured by DSC. In addition, when the endothermic peak due to melting cannot be obtained or the heat of melting is 15 J / g or less, the temperature obtained by adding 70°C to the glass transition temperature is regarded as the melting point. The glass transition temperature refers to the temperature at which the DSC curve of the second cycle of heating to 200°C, cooling to 40°C or less, and then heating to 200°C in DSC begins to decrease. Specifically, it is a value measured by the method described in the Examples.

[0120] 《Amorphous Thermoplastic Resins》

[0121] The thermoplastic film A preferably contains more than 50% by mass of an amorphous thermoplastic resin.

[0122] From the viewpoint of sufficiently imparting the properties of the amorphous thermoplastic resin to the thermoplastic film A, the content of the amorphous thermoplastic resin in the resin component in the thermoplastic film A is more preferably 60 mass % or more, further preferably 70 mass % or more, further preferably 80 mass % or more, and most preferably 90 mass % or more.

[0123] The amorphous thermoplastic resin refers to a resin that has no crystals or has a small amount of crystals even if it has crystals and has a heat of fusion of 15 J / g or less.

[0124] The heat of fusion is calculated based on the area of ​​the endothermic peak of DSC (differential scanning calorimeter) and the weight of the thermoplastic resin component. When the film contains an inorganic filler, etc., it is calculated based on the weight of the thermoplastic resin component after removing the inorganic filler. Specifically, 2 to 10 mg of the sample can be weighed, placed in an aluminum pan, and heated from 23°C to 200°C or above at 10°C / min using DSC (DSC8231 manufactured by Rigaku Co., Ltd.) to obtain a DSC curve, and then calculated based on the area of ​​the endothermic peak during melting obtained from the DSC curve and the weighed value.

[0125] The heat of fusion of the amorphous thermoplastic resin is more preferably 11 J / g or less, more preferably 7 J / g or less, and further preferably 4 J / g or less. It is particularly preferred that the endothermic peak due to melting is below the detection limit.

[0126] By using a thermoplastic film A mainly composed of an amorphous thermoplastic resin having a melting heat of 15 J / g or less, the viscosity does not drop sharply when heated as in conventional hot melt adhesives, and the film does not reach a low viscosity (0.001 to 100 Pa·s) state even in a high temperature range exceeding 200° C. Therefore, the thermoplastic film A does not flow out between the element material and the resin B disposed on the supporting substrate even in a molten state, and the thickness of the thermoplastic film A can be stably ensured, and a high bonding strength can be stably obtained.

[0127] In addition, from the viewpoint of airtightness and toughness, the amorphous thermoplastic resin is preferably at least one of a thermoplastic epoxy resin and a phenoxy resin.

[0128] Among them, from the viewpoint of airtightness and toughness, the thermoplastic film A more preferably contains an amorphous thermoplastic resin which is at least one of a thermoplastic epoxy resin and a phenoxy resin as a main component. In addition, from the viewpoint of airtightness and toughness, the thermoplastic film A is further preferably an amorphous thermoplastic resin which is at least one of a thermoplastic epoxy resin and a phenoxy resin, and contains an amorphous thermoplastic resin having an epoxy equivalent of 1600 g / eq. or more and a heat of fusion of 15 J / g or less as a main component.

[0129] Since thermoplastic epoxy resins and phenoxy resins have low cohesive force within the resin and may have hydroxyl groups, they interact strongly with the supporting substrate, device material, and resin B, and can be expected to bond dissimilar materials with higher bonding strength than conventional crystalline hot melt adhesives.

[0130] Among them, from the viewpoint of storage properties, the thermoplastic film A is preferably a thermoplastic resin having an epoxy equivalent of 1600 g / eq. or more or containing no epoxy group.

[0131] The epoxy equivalent is more preferably 2000 g / eq. or more, further preferably 5000 g / eq. or more, and even more preferably 9000 g / eq. or more, and particularly preferably above the detection limit, with substantially no epoxy group detected. In addition, the epoxy equivalent being above the detection limit means that no epoxy group is detected when the epoxy equivalent is measured based on JIS K 7236:2001 described below.

[0132] The epoxy equivalent (weight of the thermoplastic resin containing 1 mol of epoxy groups) mentioned here is the value of the epoxy equivalent of the thermoplastic resin contained in the thermoplastic film A before bonding, and is a value measured by the method specified in JIS-K7236:2001 (unit "g / eq."). Specifically, a potentiometric titration apparatus is used, tetraethylammonium bromide acetic acid solution is added, and a 0.1 mol / L perchloric acid-acetic acid solution is used. For solvent-diluted products (resin varnishes), it is a value calculated as a solid content conversion value based on the non-volatile component. In addition, in the case of a mixture of two or more resins, it can also be calculated based on their respective contents and epoxy equivalents.

[0133] 《Thermoplastic Epoxy Resin》

[0134] The thermoplastic epoxy resin is preferably a polymer of (a) a bifunctional epoxy resin monomer or oligomer and (b) a bifunctional compound having two identical or different functional groups selected from phenolic hydroxyl groups, carboxyl groups, mercapto groups, isocyanate groups and cyanate groups.

[0135] By using this compound, the polymerization reaction to form a linear polymer proceeds preferentially, and a thermoplastic epoxy resin having desired properties can be obtained.

[0136] (a) The bifunctional epoxy resin monomer or oligomer refers to an epoxy resin monomer or oligomer having two epoxy groups in the molecule.

[0137] (a) Specific examples of the bifunctional epoxy resin monomer or oligomer include, for example, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bifunctional phenol novolac type epoxy resin, bisphenol AD ​​type epoxy resin, biphenyl type epoxy resin, bifunctional naphthalene type epoxy resin, bifunctional alicyclic epoxy resin, bifunctional glycidyl ester type epoxy resin (e.g., diglycidyl phthalate, diglycidyl tetrahydrophthalate, diglycidyl dimer acid diglycidyl ester, etc.), bifunctional glycidyl amine type epoxy resin (e.g., diglycidyl aniline, diglycidyl toluidine, etc.), bifunctional heterocyclic epoxy resin, bifunctional diaryl sulfone type epoxy resin, hydroquinone type epoxy resin (e.g., hydroquinone diglycidyl ether, diglycidyl ether, 2,5-di-tert-butylhydroquinone diglycidyl ether, resorcinol diglycidyl ether, etc.), bifunctional alkylene glycidyl ether compounds (e.g., butanediol diglycidyl ether, butenediol diglycidyl ether, butynediol diglycidyl ether, etc.), bifunctional glycidyl group-containing hydantoin compounds (e.g., 1,3-diglycidyl-5,5-dialkylhydantoin, 1-glycidyl-3-(glycidyloxyalkyl)-5,5-dialkylhydantoin, etc.), bifunctional glycidyl group-containing siloxanes (e.g., 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane, α,β-bis(3-glycidyloxypropyl)polydimethylsiloxane, etc.), and modified products thereof. Among them, bisphenol A type epoxy resin, bisphenol F type epoxy resin, and biphenyl type epoxy resin are preferred from the viewpoint of reactivity and handleability.

[0138] Examples of the (b) bifunctional compound having a phenolic hydroxyl group include mononuclear aromatic dihydroxy compounds having one benzene ring, such as catechol, resorcinol, and hydroquinone; bisphenols such as bis(4-hydroxyphenyl)propane (i.e., bisphenol A), bis(4-hydroxyphenyl)methane (i.e., bisphenol F), and bis(4-hydroxyphenyl)ethane (bisphenol AD); compounds having a condensed ring, such as dihydroxynaphthalene; bifunctional phenol compounds into which an allyl group has been introduced, such as diallylresorcinol, diallylbisphenol A, and triallyldihydroxybiphenyl; and dibutylbisphenol A.

[0139] Specific examples of the carboxyl group-containing compound (b) include adipic acid, succinic acid, malonic acid, cyclohexanedicarboxylic acid, phthalic acid, isophthalic acid, and terephthalic acid.

[0140] Examples of the bifunctional compound having a mercapto group (b) include ethylene glycol bis(thioglycolate) and ethylene glycol bis(thiopropionate).

[0141] Specific examples of the isocyanate group-containing bifunctional compound (b) include diphenylmethane diisocyanate (MDI), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HMDI), and toluene diisocyanate (TDI).

[0142] Specific examples of the bifunctional compound containing a cyanate group (b) include 2,2-bis(4-cyanatephenyl)propane, 1,1-bis(4-cyanatephenyl)ethane, and bis(4-cyanatephenyl)methane.

[0143] Among the bifunctional compounds (b), from the viewpoint of obtaining a thermoplastic polymer, a bifunctional compound having two phenolic hydroxyl groups is preferred. From the viewpoint of heat resistance and bonding properties, a bifunctional compound having two phenolic hydroxyl groups and a bisphenol structure or a biphenyl structure is preferred. From the viewpoint of heat resistance and cost, bisphenol A, bisphenol F or bisphenol S is preferred.

[0144] When (a) is a bisphenol A type epoxy resin, a bisphenol F type epoxy resin, a bisphenol S type epoxy resin, or a biphenyl type epoxy resin, and (b) is bisphenol A, bisphenol F, or bisphenol S, the polymer obtained by polymerization of (a) and (b) has the following structure: a main chain having a paraphenylene structure and an ether bond as the main skeleton, which are connected by an alkylene group, and hydroxyl groups generated by addition polymerization are arranged on the side chains.

[0145] The mechanical strength of the polymer after polymerization can be improved by the linear structure composed of the p-phenylene skeleton, and the adhesion to the substrate can be improved by the hydroxyl group arranged on the side chain. As a result, high bonding strength can be achieved while maintaining the workability of the thermosetting resin. Furthermore, in the case of a thermoplastic resin, it can be recycled and repaired by softening and melting with heat, and the recyclability and repairability, which are problematic points in thermosetting resins, can be improved.

[0146] 《Phenoxy resin》

[0147] Phenoxy resin is a polyhydroxy polyether synthesized from bisphenols and epichlorohydrin, and has thermoplasticity. In the manufacture of phenoxy resin, it is known that there are methods for direct reaction of divalent phenols with epichlorohydrin, and methods for addition polymerization of diglycidyl ethers of divalent phenols with divalent phenols, but the phenoxy resin used in this embodiment can be obtained by any preparation method. In the case of direct reaction of divalent phenols with epichlorohydrin, as divalent phenols, phenols such as bisphenol A, bisphenol F, bisphenol S, biphenol, biphenyl glycol, and fluorene diphenyl can be listed; aliphatic diols such as ethylene glycol, propylene glycol, and diethylene glycol. Among them, from the viewpoint of cost, bonding, viscosity, and heat resistance, bisphenol A, bisphenol F, and bisphenol S are preferred. They can be used alone or in combination of two or more.

[0148] The phenoxy resin has a chemical structure similar to that of the epoxy resin, and has a main chain having a p-phenylene structure and an ether bond as main skeletons, connecting them, and has a structure in which hydroxyl groups are arranged in side chains.

[0149] 《Physical properties of thermoplastic epoxy resin and phenoxy resin》

[0150] Thermoplastic epoxy resin and phenoxy resin preferably have a polystyrene conversion value measured by GPC (gel permeation chromatography), that is, a weight average molecular weight of 10000 to 500000, more preferably 18000 to 300000, and further preferably 20000 to 200000. The weight average molecular weight is calculated based on the dissolution peak position detected by GPC, and is the value of the molecular weight converted by standard polystyrene. When the weight average molecular weight is within the range of this value, the balance between thermoplasticity and heat resistance is good, and the heat resistance of the bonded body is also increased by efficiently melting. When the weight average molecular weight is 10000 or more, the heat resistance is excellent, and when the weight average molecular weight is 500000 or less, the viscosity during melting is low, and the bonding property is high.

[0151] 《Components other than resin components in thermoplastic film A》

[0152] If necessary, the thermoplastic film A may contain fillers or additives as components other than the resin component within a range that does not hinder the purpose of the present embodiment.

[0153] Examples of the filler include inorganic fillers and organic fillers (resin powders and the like).

[0154] Examples of the inorganic filler include spherical fused silica, metal powders such as iron, silica sand, talc, calcium carbonate, mica, acid clay, diatomaceous earth, kaolin, quartz, titanium oxide, silicon dioxide, phenolic resin microspheres, and glass spheres.

[0155] When the thermoplastic film A contains a filler, the content of the filler in 100% by volume of the total amount of the thermoplastic film A is preferably 50% by volume or less, more preferably 30% by volume or less, further preferably 20% by volume or less, and most preferably 10% by volume or less. The volume of the filler can be obtained by dividing the weight of the filler contained in the thermoplastic film A by the apparent specific gravity of the filler.

[0156] The content of the resin component in 100% by volume of the total amount of the thermoplastic film A is preferably 10% by volume or more, more preferably 20% by volume or more, further preferably 30% by volume or more, further preferably 50% by volume or more, in one embodiment, 80% by volume or more, in another embodiment, 90% by volume or more, and in another embodiment, 99% by volume or more.

[0157] Examples of the additives include defoaming agents, coupling agents such as silane coupling agents, pigments, and tackifier resins, and these may be contained alone or in combination of two or more.

[0158] The content of the additive in the thermoplastic film A is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less.

[0159] The content of the resin component in the thermoplastic film A is preferably 10% by mass or more, more preferably 20% by mass or more, further preferably 30% by mass or more, more preferably 50% by mass or more, 80% by mass or more in one embodiment, 90% by mass or more in another embodiment, and 99% by mass or more in another embodiment.

[0160] 《Morphology of thermoplastic film A》

[0161] The thermoplastic film A is in the form of a sheet.

[0162] The thickness of the thermoplastic film A is preferably not less than 10 μm and not more than 3 mm.

[0163] From the viewpoint of obtaining a firmly bonded body in a short bonding process time, the thickness of the thermoplastic film A is more preferably 1 mm or less, further preferably 0.5 mm or less, further preferably 0.3 mm or less, particularly preferably 0.2 mm or less, and most preferably 0.1 mm or less. In addition, from the viewpoint of further improving the adhesion and peeling resistance, the thickness of the thermoplastic film A is more preferably 20 μm or more, further preferably 30 μm or more, and further preferably 40 μm or more.

[0164] When the thickness of the thermoplastic film A is within the above numerical range, the bonding surface with the element material disposed on the supporting substrate can be effectively expanded by heating or the like, and high bonding strength and adhesion can be obtained.

[0165] The thermoplastic film A may be a single layer or a laminate composed of a plurality of layers. However, from the viewpoint of ease of production and improvement of bonding strength, the thermoplastic film A is preferably a single layer.

[0166] In addition, within the scope of not hindering the effect of the present invention, the thermoplastic film A may also have viscosity as described above. The imparting of viscosity may be by mixing a tackifying resin in the thermoplastic resin constituting the thermoplastic film A, or by applying an adhesive on the surface of the thermoplastic film A. The imparting of viscosity may be single-sided or double-sided, but if it is single-sided, only the surface in contact with the element material in the state configured on the supporting substrate may be made viscous, and it is difficult to expose the adhesive surface on the outside, so it is more preferred. In addition, the coating area of ​​the adhesive may be the entire surface, or it may be a part of stripe, dot, grid, tile (a plurality of quadrilaterals have a shape arranged with gaps), etc. If the coating area is small, the adhesive is difficult to extend outward from the end surface of the thermoplastic film A and expose, and the adhesion is difficult to decrease, so it is preferred. In addition, the imparting of viscosity may also be a small imparting that can prevent slipping. That is, when the thermoplastic film A is brought into contact with the element material disposed on the support substrate, the thermoplastic film A may not be attached to the element material disposed on the support substrate, or the film may be attached to a degree that resistance becomes large (difficult to slide) when a shearing force is applied. The film with low viscosity is preferred because the adhesive force is easy to increase, and the peeling resistance and adhesion are excellent.

[0167] 《Method for producing thermoplastic film A》

[0168] The method for producing the thermoplastic film A is not particularly limited. For example, a monomer or oligomer of a bifunctional epoxy compound may be heated to polymerize to obtain a resin composition, a solvent may be added to the obtained resin composition as needed, the composition may be coated on a release film or the like, cured and dried, and pressurized as needed to obtain the thermoplastic film A. The polymerization reaction may be carried out after coating on a release film or after removing the solvent to obtain a film shape, or a combination of these methods may be used.

[0169] 〔Resin B〕

[0170] In this embodiment, resin B is used as a sealing material.

[0171] Resin B is not particularly limited as long as it is a resin that can be insert molded, and is preferably composed of one selected from thermoplastic resins, thermosetting resins, and fiber reinforced plastics (FRP). Among them, resin B is preferably a thermosetting resin from the viewpoint of bonding strength, cost, and ease of molding.

[0172] However, the resin B and the resin constituting the thermoplastic film A are different in components.

[0173] Examples of the thermosetting resin include epoxy resins, silicone resins, polyurethane resins, polyimide resins, urea resins, melamine resins, and unsaturated polyester resins. These thermosetting resins may be used alone or in combination of two or more.

[0174] The thermosetting resin preferably includes an epoxy resin. As the epoxy resin, for example, a bifunctional epoxy resin and a trifunctional or higher multifunctional epoxy resin can be listed. As the bifunctional epoxy resin, for example, bisphenol A type epoxy resin, bisphenol F type epoxy resin, modified bisphenol A type epoxy resin, modified bisphenol F type epoxy resin and biphenyl type epoxy resin can be listed. As the trifunctional or higher multifunctional epoxy resin, for example, phenol novolac type epoxy resin, cresol novolac type epoxy resin, trihydroxyphenylmethane type epoxy resin, tetraphenol ethane type epoxy resin and dicyclopentadiene type epoxy resin can be listed. These epoxy resins can be used alone or in combination of two or more. As the epoxy resin, it is preferred to use a bifunctional epoxy resin, and it is more preferred to use one or more selected from bisphenol F type epoxy resin and bisphenol A type epoxy resin.

[0175] When using epoxy resin, the thermosetting resin preferably contains a phenolic resin as a curing agent for epoxy resin. As the phenolic resin, preferably a novolac type phenolic resin is used. As the novolac type phenolic resin, for example, phenol novolac resin, phenol aralkyl resin, trihydroxyphenylmethane novolac resin, cresol novolac resin, tert-butylphenol novolac resin and nonylphenol novolac resin can be listed. These phenolic resins can be used alone or in combination of two or more.

[0176] As thermoplastic resins, for example, polyolefins and acid-modified products thereof, polystyrene, polymethyl methacrylate, AS resin, ABS resin, thermoplastic aromatic polyesters such as polyethylene terephthalate or polybutylene terephthalate, polycarbonate, polyimide, polyamide, polyamide-imide, polyetherimide, polyethersulfone, polyphenylene ether and modified products thereof, polyphenylene sulfide, polyoxymethylene, polyarylate, polyetherketone, polyetheretherketone, polyetherketoneketone, thermoplastic epoxy resin and fiber-reinforced materials thereof, etc. can be cited. In addition, as thermosetting resins, for example, one or more selected from epoxy resins, vinyl ester resins, phenolic resins, polyurethane resins, etc. can be used. From the viewpoints of heat resistance, bonding strength, cost, ease of molding, etc., it is preferably composed of at least one selected from polycarbonate, glass fiber reinforced polyamide, glass fiber reinforced polybutylene terephthalate, and glass fiber reinforced polyphenylene sulfide.

[0177] The molding temperature (resin temperature) of resin B is preferably 100 to 400° C., more preferably 150 to 350° C., and further preferably 180 to 300° C. By molding at a temperature within a range of 100 to 400° C., the thermoplastic film A is effectively deformed and melted by heating, and effectively wets and spreads on the bonding surface, thereby obtaining a high bonding strength.

[0178] The combination of the material of the support substrate and the material of the element material and the resin B is not particularly limited.

[0179] In the bonded body of the present embodiment, the thickness of the resin B (sealing material) is not particularly limited, and can be appropriately set according to the intended use within a range in which the bonding strength and the adhesiveness are excellent.

[0180] <Joint body>

[0181] use Figure 1 An example of a bonded body produced by the method for producing a bonded body according to the present embodiment will be described.

[0182] Figure 1 It is a schematic cross-sectional view schematically showing an example of an embodiment of a bonded body. Figure 1 1-1 to 1-4 are all examples of embodiments of the conjugate.

[0183] like Figure 1 As shown in Figure 1-1, the bonded body is formed by sealing the element material 3 arranged on the supporting substrate 4 with the resin B1 via the thermoplastic film A2. The element material 3 arranged on the supporting substrate 4 and the resin B1 have excellent bonding strength and excellent adhesion via the thermoplastic film A2. Since the element material 3 arranged on the supporting substrate 4 and the thermoplastic film A2 are firmly sealed by the resin B1, the resin B1 is difficult to peel off and has excellent adhesion.

[0184] In addition, if Figure 1 As shown in FIG. 1 - 1 , as long as the element material 3 is sealed by the resin B through the thermoplastic film A2 without being exposed to the outside air, the element material 3 , the thermoplastic film A2 , and the resin B may be located in the concave portion of the support substrate 4 .

[0185] In addition, if Figure 1 As shown in FIG. 1 - 2 , as long as the element material 3 is sealed by the resin B through the thermoplastic film A2 without being exposed to the outside air, the element material 3 , the thermoplastic film A2 and the resin B may be located on the flat support substrate 4 .

[0186] In addition, as long as the element material 3 is sealed by the resin B through the insulating thermoplastic film A2 without being exposed to the outside air, at least a part or all of the side surface (thickness direction) of the element material 3 may be in contact with the supporting substrate ( Figure 11-1), at least a part or all of the side surface (thickness direction) of the element material 3 may be in contact with the thermoplastic film A2 ( Figure 1 1-2), at least a part or all of the side surface (thickness direction) of the element material 3 may be in contact with the resin B ( Figure 1 1-3 and 1-4).

[0187] In addition, as long as the element material 3 is sealed by the resin B through the thermoplastic film A2 so as not to be exposed to the outside air, the entire surface of the element material 3 that is not in contact with the support substrate 4 may be in contact with the thermoplastic film A2 ( Figure 1 1-2), a portion of the surface of the element material 3 that is not in contact with the supporting substrate 4 may also be in contact with the thermoplastic film A2 ( Figure 1 1-3 and 1-4). In addition, Figure 1 1-3 means that the surface (upper side) opposite to the surface (lower side) of the element material 3 in contact with the support substrate 4 is in contact with the thermoplastic film A2. Figure 1 1-4 indicates that a part of the surface (upper side) opposite to the surface (lower side) in contact with the support substrate 4 of the element material 3 is in contact with the thermoplastic film A2.

[0188] The joint body of this embodiment, even if it is a joint body of heterogeneous materials, also shows excellent joint strength. Regarding the joint strength, in addition to the strength of the interface interaction between the thermoplastic film A and the element material in the state configured on the supporting substrate, and between the thermoplastic film A and the resin B, it is also affected by many factors such as the thickness of the thermoplastic film A, the molecular weight of the polymer constituting the thermoplastic film A, the chemical structure, mechanical properties, and viscoelastic properties, so the joint body of this embodiment is more preferably a embodiment of the joint body, and the thermoplastic film A is mainly composed of an amorphous thermoplastic resin as at least one of a thermoplastic epoxy resin and a phenoxy resin. Although the details of the mechanism of the more preferred embodiment showing more excellent joint strength and adhesion are unclear, it can be inferred that it is due to the low cohesive force in the amorphous thermoplastic resin, and in the case of the presence of hydroxyl groups in the resin, the main reason is that chemical bonds or intermolecular forces such as hydrogen bonds or van der Waals forces are formed at the interface between the thermoplastic film A and the element material in the state configured on the supporting substrate, and at the interface between the thermoplastic film A and the resin B.

[0189] However, in the bonded body of the present embodiment, the state or characteristics of the interface between the thermoplastic film A and the element material disposed on the supporting substrate, and the state or characteristics of the interface between the thermoplastic film A and the resin B are extremely thin chemical structures below the nanometer level, and are difficult to analyze. Therefore, it is impossible or impractical with current technology to distinguish the state or characteristics of the interface from the case where the thermoplastic film A is not used by determining the state or characteristics of the interface.

[0190] The bonded body of this embodiment has excellent adhesion because the element material disposed on the support substrate is firmly bonded to the resin B, and can be suitably used for applications that can take advantage of this property. For example, an electric or electronic component including the bonded body of this embodiment can be provided.

[0191] Example

[0192] Hereinafter, the present embodiment will be specifically described using Examples and Comparative Examples, but the present embodiment is not limited thereto.

[0193] <Materials>

[0194] The following materials were used in Examples and Comparative Examples.

[0195] 《Supporting substrate》

[0196] ·Glass fiber epoxy board (50mm long x 50mm wide x 2mm thick)

[0197] 《Component Materials》

[0198] ·Copper (C1100 (electrolytic copper (Tough-Pitch Copper)) 18mm in length × 45mm in width × 1.5mm in thickness)

[0199] 《Resin B》

[0200] ·PPS: Polyphenylene sulfide (manufactured by DIC Corporation, FZ-1130-D5)

[0201] An injection molded article (45 mm in length×10 mm in width×3 mm in thickness) obtained by injection molding the PPS (resin temperature: 300° C., mold temperature: 140° C.) was used. However, in the case of the method a described below, the PPS was used instead of the injection molded article.

[0202] Epoxy resin: (Epoxy sealing resin (CEL-420HFC) manufactured by Showa Denko Materials

[0203] The epoxy resin was subjected to compression molding (mold temperature 180°C, curing heating time 90 seconds) to form a plate with a thickness of 3 mm, and then heated in an oven at 200°C for 6 hours to complete the curing of the resin, and the compression molded body (45 mm in length × 10 mm in width × 3 mm in thickness) obtained by cutting the plate was used. However, in the case of the method a described later, the epoxy resin is used instead of the compression molded body.

[0204] 《Adhesive (thermoplastic film A)》

[0205] Adhesives A1 to A8 produced in Examples 1 to 8.

[0206] 《Adhesive (for comparative example)》

[0207] Adhesives B1 to B5 produced in Comparative Examples 1 to 5.

[0208] <Measurement method>

[0209] The physical properties of the bonding agents used in Examples and Comparative Examples were measured by the following methods.

[0210] (Weight average molecular weight)

[0211] The thermoplastic epoxy resin and the phenoxy resin were dissolved in tetrahydrofuran, and the results were measured under the following conditions using Prominence 501 (manufactured by Showa Science Corporation) and Detector: Shodex (registered trademark) RI-501 (manufactured by Showa Denko K.K.).

[0212] Chromatographic column: LF-804 manufactured by Showa Denko K.K. × 2

[0213] Column temperature: 40°C

[0214] Sample: 0.4 mass% tetrahydrofuran solution of resin

[0215] Flow rate: 1ml / min

[0216] Eluent: Tetrahydrofuran

[0217] Calibration method: Standard polystyrene conversion

[0218] (Heat of Fusion and Melting Point)

[0219] 2 to 10 mg of the adhesive used in the examples and comparative examples were weighed, placed in an aluminum pan, and heated from 23°C to 200°C at 10°C / min using a DSC (DSC8231 manufactured by Rigaku Co., Ltd.) to obtain a DSC curve. The heat of fusion was calculated based on the endothermic peak area during melting in the DSC curve and the weighed value. In addition, the endothermic peak temperature caused by melting of the obtained DSC curve was taken as the melting point. In addition, when the endothermic peak caused by melting cannot be obtained or is 15 J / g or less, for a thermoplastic resin (amorphous resin) that melts by heating, the temperature after adding 70°C to the glass transition temperature is taken as the melting point. In this region, the thermoplastic resin melts and has fluidity. The glass transition temperature is measured by the DSC curve of the second cycle of heating to 200°C by DSC, cooling to below 40°C, and then heating to 200°C. In addition, for a thermosetting resin that does not melt by heating, it is considered to have no melting point.

[0220] (Epoxy Equivalent Weight)

[0221] The value was measured according to JIS K-7236: 2001 and converted into a value of resin solid content. In the case of a simple mixture without accompanying reaction, it was calculated based on the respective epoxy equivalents and contents.

[0222] <Evaluation Method>

[0223] The bonded bodies obtained in Examples and Comparative Examples were evaluated by the following methods.

[0224] (Shear joint strength)

[0225] The bonded bodies obtained in Examples and Comparative Examples were used as test pieces, and a tensile shear bond strength test was performed in an atmosphere of 23° C. and 80° C. in accordance with ISO 19095 (lap joint) to measure the shear bond strength (MPa).

[0226] The shear bonding strength test was performed using a tensile testing machine (universal testing machine autograph "AG-X plus" (manufactured by Shimadzu Corporation) with a load cell of 10 kN and a tensile speed of 10 mm / min.

[0227] (Adhesion (sealing))

[0228] The same test piece as in the shear bonding strength test was placed in a thermal cycle tester (TSA-71L manufactured by Espec) and subjected to a thermal cycle of -40°C and 125°C (maintaining time at each temperature for 15 minutes). The test piece was observed after 1000 cycles and the adhesion was evaluated based on the following criteria.

[0229] ○: There was no change in the appearance of the joint surface of the test piece, and there was no peeling on the joint surface.

[0230] △: The appearance of the joint surface of the test piece was slightly changed.

[0231] ×: The bonding surface of the test piece peeled off.

[0232] (Joining process time)

[0233] The joining process time was measured as follows.

[0234] The time from the start point to the end point was measured, with the time when the supporting substrate or resin B on which the element materials constituting the bonded body were placed contacting the bonding agent being the start point and the time when the bonded body was completed being the end point.

[0235] <Examples 1-1, 1-2 and 1-3>

[0236] (Manufacturing of Solid Adhesive A1)

[0237] In a reaction apparatus equipped with a stirrer, a circulation cooler, a gas introduction pipe and a thermometer, 1.0 equivalent (203 g) of jER (registered trademark) 1007 (manufactured by Mitsubishi Chemical Corporation, bisphenol A type epoxy resin, weight average molecular weight of about 10,000), 1.0 equivalent (12.5 g) of bisphenol S, 2.4 g of triphenylphosphine and 1000 g of methyl ethyl ketone were added, and the mixture was heated to 100° C. while stirring under a nitrogen atmosphere. Dissolution was visually confirmed, and the mixture was cooled to 40° C. to obtain a resin composition P-1 having a solid content of about 20% by mass. The solvent was then removed to obtain a solid. A non-adhesive fluorine-based resin film (ニトフロン (registered trademark), NO.900UL, manufactured by Nitto Denko Corporation) is provided on the upper plate and the lower plate of the press, and after the aforementioned solid is arranged on the non-adhesive fluorine-based resin film of the lower plate, the press is heated to 160°C, and the resin composition P-1 is heated and compressed for 2 hours to obtain a thin film-like solid adhesive A1 having a solid content of 100% by mass and a thickness of 100 μm.

[0238] The weight average molecular weight was about 37000. The epoxy equivalent was above the detection limit. No melting heat peak (melting peak) was detected in DSC.

[0239] Table 1 shows the measurement results of various physical properties of the obtained solid bonding agent A1.

[0240] (Manufacturing of a joint body)

[0241] In Examples 1-1, 1-2 and 1-3, two types of bonded bodies ("PPS / Cu" and "epoxy resin / Cu") were respectively manufactured using the solid bonding agent A1. In addition, Example 1-1 adopted the following (c method), Example 1-2 adopted the following (b method), and Example 1-3 adopted the following (a method).

[0242] (C method (one-step method)

[0243] The element material is arranged at the center portion of the supporting substrate.

[0244] Next, the solid adhesive A1 (10 mm in length×15 mm in width×100 μm in thickness) was placed on the element material arranged on the support substrate, and an injection-molded body of PPS as the resin B was stacked thereon so that the surface was in contact with the solid adhesive A1.

[0245] Next, a high-frequency induction welding machine (manufactured by Seidensha Electronics Co., Ltd., oscillator UH-2.5K, press machine JIIP30S) was used to heat the metal by high-frequency induction, and to heat and pressurize the metal, thereby joining the injection molded body of resin B, the sealing element material, and the solid bonding agent A1. The pressure was 110N (pressure 2.2MPa), and the oscillation frequency was 900kHz. The oscillation time was 10 seconds. In this way, a bonded body (PPS / Cu) was prepared.

[0246] Furthermore, a compression-molded body of epoxy resin was used as resin B, and a bonded body (epoxy resin / Cu) was prepared in the same manner as in the case of using the injection-molded body of PPS.

[0247] (Method b (two-step method)

[0248] The element material is arranged at the center portion of the supporting substrate.

[0249] Next, the solid bonding agent A1 (10 mm in length × 15 mm in width × 100 μm in thickness) was placed on the element material in a state configured on the support substrate, placed on a hot plate heated to 200°C, and pressed at 110 N to integrate the bonding agent A1 with the element material in a state configured on the support substrate. An injection molded body of PPS as resin B was placed thereon, and bonding was performed under the same conditions as in method c (one-step method). In this way, a bonded body (PPS / Cu) was prepared.

[0250] Furthermore, a compression-molded body of epoxy resin was used as resin B, and a bonded body (epoxy resin / Cu) was prepared in the same manner as in the case of using the injection-molded body of PPS.

[0251] (a method (film insertion method)

[0252] The element material is arranged at the center portion of the supporting substrate.

[0253] The solid bonding agent A1 (10 mm in length × 15 mm in width × 100 μm in thickness) is placed in the cavity of a preheated mold (material: HPM38, cavity size: 45 mm in length × 18 mm in width × 1.5 mm in height) and the mold is closed. The bonding agent A1 is bonded to the resin B by injection molding BPPS as a resin in the mold. It is placed on the component material in a state configured on the supporting substrate and bonded under the same conditions as in the c method (1-step method). In this way, a bonded body (PPS / Cu) is prepared.

[0254] Also, epoxy resin was used as the resin B, and a bonded body (epoxy resin / Cu) was prepared in the same manner as in the case of using the above-mentioned PPS.

[0255] <Example 2>

[0256] (Manufacturing of Solid Adhesive A2)

[0257] In a reaction apparatus equipped with a stirrer, a circulating cooler, a gas introduction tube and a thermometer, 20 g of フェノトート (registered trademark) YP-50S (manufactured by Nippon Tetsu Chemical & Material Co., Ltd., a phenoxy resin with a weight average molecular weight of about 50,000) and 80 g of cyclohexanone were added, and the temperature was raised to 60°C while stirring, and the dissolution was visually confirmed, and then cooled to 40°C to obtain a resin composition P-2 with a solid content of 20% by mass. The solvent was removed therefrom to obtain a film-like solid adhesive A2 (7 mm in length × 10 mm in width × 100 μm in thickness) with a solid content of 100% by mass. The weight average molecular weight was 50,000, and the epoxy equivalent was above the detection limit. No melting heat peak was detected in DSC.

[0258] Table 1 shows the measurement results of various physical properties of the obtained solid bonding agent A2.

[0259] (Manufacturing of a joint body)

[0260] A bonded body was produced in the same manner as in Example 1-1 except that the solid bonding agent A2 was used instead of the solid bonding agent A1.

[0261] Table 1 shows the evaluation results of the obtained bonded product.

[0262] <Example 3>

[0263] (Manufacturing of Solid Adhesive A3)

[0264] The solid adhesive A2 was mixed with crystalline epoxy resin YSLV-80XY (manufactured by Nippon Steel Chemika & Material Co., Ltd.) at a mass ratio of 98:2, pressed and cut to obtain a solid adhesive A3 (7 mm in length × 10 mm in width × 100 μm in thickness). The weight average molecular weight was 36,000, the epoxy equivalent was 9,600 g / eq, and the heat of fusion was 2 J / g.

[0265] Table 1 shows the measurement results of various physical properties of the obtained solid bonding agent A3.

[0266] (Manufacturing of a joint body)

[0267] A bonded body was produced in the same manner as in Example 1-1 except that the solid bonding agent A3 was used instead of the solid bonding agent A1.

[0268] Table 1 shows the evaluation results of the obtained bonded product.

[0269] <Example 4>

[0270] (Manufacturing of Solid Adhesive A4)

[0271] Solid adhesive A4 (7 mm in length × 10 mm in width × 100 μm in thickness) was obtained in the same manner as solid adhesive A3 except that the solid adhesive A2 and crystalline epoxy resin YSLV-80XY (manufactured by Nippon Steel Chemika & Material Co., Ltd.) were mixed in a mass ratio of 94 to 6. The weight average molecular weight was 35,000, the epoxy equivalent was 2,100 g / eq, and the heat of fusion was 4 J / g.

[0272] Table 1 shows the measurement results of various physical properties of the obtained solid bonding agent A4.

[0273] (Manufacturing of a joint body)

[0274] A bonded body was produced in the same manner as in Example 1-1 except that the solid bonding agent A4 was used instead of the solid bonding agent A1.

[0275] Table 1 shows the evaluation results of the obtained bonded product.

[0276] <Example 5>

[0277] (Manufacturing of Solid Adhesive A5)

[0278] Solid adhesive A5 (7 mm in length × 10 mm in width × 100 μm in thickness) was obtained in the same manner as solid adhesive A3 except that the solid adhesive A2 and crystalline epoxy resin YSLV-80XY (manufactured by Nippon Steel Chemical & Material Co., Ltd.) were mixed in a mass ratio of 89 to 11. The weight average molecular weight was 33,000, the epoxy equivalent was 1,745 g / eq, and the heat of fusion was 11 J / g.

[0279] Table 1 shows the measurement results of various physical properties of the obtained solid bonding agent A5.

[0280] (Manufacturing of a joint body)

[0281] A bonded body was produced in the same manner as in Example 1-1 except that the solid bonding agent A5 was used instead of the solid bonding agent A1.

[0282] Table 1 shows the evaluation results of the obtained bonded product.

[0283] <Example 6>

[0284] (Manufacturing of Solid Adhesive A6)

[0285] In a reaction apparatus equipped with a stirrer, a circulation cooler, a gas introduction pipe and a thermometer, 1.0 equivalent (203 g) of jER (registered trademark) 1007 (manufactured by Mitsubishi Chemical Corporation, bisphenol A type epoxy resin, molecular weight about 4060), 0.6 equivalent (12.5 g) of bisphenol S (molecular weight 250), 2.4 g of triphenylphosphine and 1000 g of methyl ethyl ketone were added, and the mixture was heated to 100° C. while stirring under a nitrogen atmosphere. Dissolution was visually confirmed, and the mixture was cooled to 40° C. to obtain a resin composition P-3 having a solid content of about 20% by mass. The solvent was then removed to obtain a solid. A non-adhesive fluorine resin film (NO.900UL, manufactured by Nitto Denko Corporation) was set on the upper and lower plates of the press, and after the solid was arranged on the non-adhesive fluorine resin film of the lower plate, the press was heated to 160°C, and the resin composition P-3 was heated and compressed for 2 hours to obtain a thin film solid adhesive A6 (7 mm in length × 10 mm in width × 100 μm in thickness) with a solid content of 100% by mass. The weight average molecular weight was about 30,000, and the epoxy equivalent was above the detection limit. No melting heat peak was detected in DSC.

[0286] Table 1 shows the measurement results of various physical properties of the obtained solid bonding agent A6.

[0287] (Manufacturing of a joint body)

[0288] A bonded body was produced in the same manner as in Example 1-1 except that the solid bonding agent A6 was used instead of the solid bonding agent A1.

[0289] Table 1 shows the evaluation results of the obtained bonded product.

[0290] <Example 7>

[0291] (Manufacturing of Solid Adhesive A7)

[0292] As the solid bonded body A7 (7 mm in length×10 mm in width×100 μm in thickness), an amorphous polycarbonate film (Uriplon (registered trademark) FE2000, manufactured by Mitsubishi Engineering Plastics Co., Ltd.) was used. No melting heat peak was detected in DSC.

[0293] Table 1 shows the measurement results of various physical properties of the solid bonding agent A7.

[0294] (Manufacturing of a joint body)

[0295] A bonded body was produced in the same manner as in Example 1-1 except that the solid bonding agent A7 was used instead of the solid bonding agent A1.

[0296] Table 1 shows the evaluation results of the obtained bonded product.

[0297] <Example 8>

[0298] (Manufacturing of Solid Adhesive A8)

[0299] As the solid adhesive, a crystalline polyamide hot melt adhesive film NT-120 (manufactured by Nippon Matai Co., Ltd., thickness 100 μm) was used as a solid bonded body A8 (7 mm in length×10 mm in width×100 μm in thickness). The heat of fusion was 60 J / g.

[0300] Table 1 shows the measurement results of various physical properties of the solid bonding agent A8.

[0301] (Manufacturing of a joint body)

[0302] A bonded body was produced in the same manner as in Example 1-1 except that the solid bonding agent A8 was used instead of the solid bonding agent A1.

[0303] Table 1 shows the evaluation results of the obtained bonded product.

[0304] <Comparative Example 1>

[0305] (Manufacturing of Solid Adhesive B1)

[0306] Two liquids of thermosetting liquid epoxy adhesive E-250 (manufactured by Conisy Co., Ltd., a two-component type of bisphenol epoxy resin and amine curing agent) were mixed, applied on a release film, and cured at 100°C for 1 hour. The mixture was then cooled and peeled off from the release film to obtain a thin film of solid adhesive B1 (7 mm in length × 10 mm in width × 100 μm in thickness).

[0307] Table 2 shows the measurement results of various physical properties of the solid bonding agent B1.

[0308] (Manufacturing of a joint body)

[0309] A bonded body was produced in the same manner as in Example 1-1 except that the solid bonding agent B1 was used instead of the solid bonding agent A1.

[0310] Table 2 shows the evaluation results of the obtained bonded product.

[0311] <Comparative Example 2>

[0312] (Manufacturing of Solid Adhesive B2)

[0313] Crystalline epoxy resin YSLV-80XY (manufactured by Nippon Tetsu Chemical & Material Co., Ltd.) was pressed at a pressure of 5 MPa to obtain a sheet, which was then cut to obtain a thin film of solid adhesive B2 (7 mm in length×10 mm in width×100 μm in thickness).

[0314] Table 2 shows the measurement results of various physical properties of the solid bonding agent B2.

[0315] (Manufacturing of a joint body)

[0316] A bonded body was produced in the same manner as in Example 1-1 except that the solid bonding agent B2 was used instead of the solid bonding agent A1.

[0317] Table 2 shows the evaluation results of the obtained bonded product.

[0318] <Comparative Example 3>

[0319] (Liquid adhesive B3)

[0320] As the adhesive B3, a thermosetting liquid epoxy adhesive E-250 (manufactured by Conisy Co., Ltd., a two-component type of a bisphenol epoxy resin and an amine curing agent) was used.

[0321] Table 2 shows the measurement results of various physical properties of the liquid adhesive B3.

[0322] (Manufacturing of a joint body)

[0323] The two liquids of the liquid adhesive B3 are mixed, and the mixture of the two liquids is applied to the surface of the component material in a state where it is arranged on the supporting substrate in an area of ​​7 mm in length and 10 mm in width. The component material in a state where it is arranged on the supporting substrate and the injection molded body of PPS as resin B are attached in such a way that the overlapping area is 5 mm in length and 10 mm in width within 1 minute after the coating. Then, while being fixed with a clamp, it is allowed to stand in an oven at 100°C for 1 hour to solidify the adhesive B3 with a thickness of 0.1 mm. Then, it is cooled to room temperature. In this way, a joint body (PPS / Cu) is prepared.

[0324] A compression-molded body of epoxy resin was used as the resin B, and a bonded body (epoxy resin / Cu) was prepared in the same manner as in the case of using the injection-molded body of PPS.

[0325] Table 2 shows the evaluation results of the obtained bonded product.

[0326] <Comparative Example 4>

[0327] (Manufacturing of Adhesive B4)

[0328] 1.0 equivalent (203 g) of jER (registered trademark) 1007 (manufactured by Mitsubishi Chemical Corporation, bisphenol A type epoxy resin, weight average molecular weight of about 10,000), 1.0 equivalent (12.5 g) of bisphenol S, 2.4 g of triphenylphosphine and 1000 g of methyl ethyl ketone were added to a flask and stirred at room temperature to obtain a liquid resin composition having a solid content of about 20% by mass. The liquid resin composition was applied to the injection molded body of resin B by a bar, dried at room temperature for 30 minutes, and then allowed to stand in an oven at 160° C. for 2 hours, thereby forming a solid thermoplastic epoxy resin polymer coating of 7 mm in length × 10 mm in width × 100 μm in thickness on the surface of the injection molded body of resin B. This coating was used as adhesive B4.

[0329] Table 2 shows the measurement results of various physical properties of bonding agent B4.

[0330] (Manufacturing of a joint body)

[0331] A bonded body was produced in the same manner as in Example 1-1 except that the coating layer on the injection-molded body of the resin B was superposed on the element material disposed on the supporting substrate.

[0332] Table 2 shows the evaluation results of the obtained bonded product.

[0333] <Comparative Example 5>

[0334] (Manufacturing of Adhesive B5)

[0335] In a reaction device equipped with a stirrer, a circulating cooler, a gas introduction pipe and a thermometer, 20 g of Fennotote (registered trademark) YP-50S (manufactured by Nippon Steel Chemica & Materia Co., Ltd., a phenoxy resin with a weight average molecular weight of about 50,000) and 80 g of cyclohexanone were added, and the temperature was raised to 60°C while stirring. The solution was visually confirmed, and the mixture was cooled to 40°C to obtain a liquid resin composition with a solid content of 20% by mass. The liquid resin composition was applied to the element material in a state arranged on the supporting substrate by a rod, and the mixture was allowed to stand in an oven at 70°C for 30 minutes, thereby forming a phenoxy resin coating with a length of 7 mm × a width of 10 mm × a thickness of 100 μm on the surface of the element material in a state arranged on the supporting substrate. The coating was used as bonding agent B5.

[0336] Table 2 shows the measurement results of various physical properties of bonding agent B5.

[0337] (Manufacturing of a joint body)

[0338] A bonded body was produced in the same manner as in Example 1-1 except that the coating layer on the element material disposed on the supporting substrate was superposed on the injection-molded body of the resin B.

[0339] Table 2 shows the evaluation results of the obtained bonded product.

[0340]

[0341]

[0342] Industrial Availability

[0343] The manufacturing method and the bonded body of the present embodiment are used for applications such as sealing components of power modules and electric and electronic components such as semiconductor packages, but are not particularly limited to these exemplified applications.

[0344] Description of the accompanying drawings

[0345] 1. Resin B

[0346] 2. Thermoplastic film A

[0347] 3. Component materials

[0348] 4. Support substrate

Claims

1. A method for producing a bonded body, wherein the bonded body is formed by arranging and bonding a supporting substrate, an element material, a thermoplastic film A, and a resin B in this order, the method comprising the following steps in sequence: Step 1 of disposing the element material on the support substrate; and Step 2 of bonding the resin B to at least a portion of the device material disposed on the support substrate via the thermoplastic film A to seal the device material and the thermoplastic film A. 2 . The method for producing a joined body according to claim 1 , wherein the thermoplastic film A has adhesiveness to the element material.

3. The method for manufacturing a joined body according to claim 1 or 2, wherein in the step 2, after the thermoplastic film A is joined to the resin B, the thermoplastic film A in a state of being joined to the resin B is brought into contact with the element material in a state of being arranged on the supporting substrate, and the thermoplastic film A is melted and then solidified, thereby joining the resin B and sealing the element material and the thermoplastic film A.

4. The method for manufacturing a joined body according to claim 1 or 2, wherein in the step 2, after the thermoplastic film A is joined to the element material disposed on the support substrate, the resin B is brought into contact with the thermoplastic film A, and the thermoplastic film A is melted and then solidified, thereby joining the resin B and sealing the element material and the thermoplastic film A.

5. The method for manufacturing a bonded body according to claim 1 or 2, wherein in the step 2, the thermoplastic film A is melted and then solidified in a state where the element material, the thermoplastic film A and the resin B are arranged in this order on the supporting substrate, thereby bonding the resin B and sealing the element material and the thermoplastic film A.

6. The method for manufacturing a joint body according to claim 1 or 2, wherein in step 2, the joining is performed by at least one selected from contact heating, hot air heating, hot pressing, infrared heating, hot plate fusion, ultrasonic fusion, vibration fusion and high-frequency induction fusion.

7. The method for producing a bonded body according to claim 1 or 2, wherein in the step 2, bonding is performed at a temperature of a bonding portion of 100 to 300°C. 8 . The method for producing a joined body according to claim 1 , wherein the thermoplastic film A has a thickness of 10 μm or more and 3 mm or less. 9 . The method for producing a joined body according to claim 1 , wherein the thermoplastic film A contains more than 50% by mass of an amorphous thermoplastic resin. 10 . The method for producing a bonded body according to claim 9 , wherein the amorphous thermoplastic resin is at least one of a thermoplastic epoxy resin and a phenoxy resin.

11. The method for producing a joined body according to claim 1 or 2, wherein the thermoplastic film A is a thermoplastic resin having an epoxy equivalent of 1600 g / eq. or more or containing no epoxy group.

12. The method for producing a bonded body according to claim 1 or 2, wherein the element material is metal. 13 . The method for producing a joined body according to claim 1 , wherein the resin B is a thermosetting resin.

14. An electric and electronic component comprising a bonded body obtained by the method for producing a bonded body according to claim 1 or 2.

Citation Information

Patent Citations

  • Method for producing joined body, transient liquid phase sintering composition, sintered body, and joined body

    CN110050047A

  • Metal / fiber-reinforced resin material composite body, method for producing same and bonding sheet

    CN110121413A

  • Semiconductor device and mounting method therefor

    JP2001185582A

  • Laminating device, laminating method, and method of manufacturing illuminating device

    JP2012187782A

  • Heat welding film, laminate, dissimilar material joined body, and method for producing dissimilar material joined body

    JP2019217699A