Mother glass plate and method for manufacturing mother glass plate
By using large-size table back flexural difference measurement and flexural difference change calculation on the production line of the hard drive mother glass plate, combined with optical interferometer measurement, the problem of long-term measurement of the shape accuracy of the mother glass plate is solved, achieving high efficiency, Accurate shape accuracy measurement and production, suitable for high-demand HDD substrate manufacturing.
Patent Information
- Application Number
- CN202380037566.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-07-13
- Filing Date
- 2023-07-03
- Publication Date
- 2024-11-29
AI Technical Summary
When manufacturing a glass substrate for hard disk drives (HDD substrate), the process of measuring the shape accuracy of the mother glass plate takes a lot of time and time, and the prior art is difficult to ensure high shape accuracy efficiently.
Through continuous production, extraction, measurement and determination processes on the production line of the mother glass plate, the flexural difference of the table back is measured using a larger size first evaluation area, and the change of the flexural difference between the two consecutive extractions is calculated, combined with optical The interferometer measures flatness, reduces the number and time of measuring objects, and improves the measurement efficiency.
On the basis of ensuring shape accuracy, the time and time required for measurement is significantly reduced, the shape accuracy and yield of the mother glass plate are improved, and it is suitable for high-demand HDD substrate manufacturing.
Smart Images

Figure CN119053561A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a mother glass plate and a method for manufacturing the mother glass plate. Background Art
[0002] An example of a glass plate that requires high flatness is a glass substrate for a hard disk drive (hereinafter referred to as an HDD substrate). Patent Document 1 discloses an example of an HDD substrate.
[0003] As an example of a method for manufacturing a HDD substrate, in the case of manufacturing a 3.5-inch HDD substrate, first, a plurality of small rectangular glass plates (about 100 mm square) are cut out from a large-area mother glass plate of, for example, 1300×1500 mm to 2400×2800 mm. Then, each of the rectangular glass plates is processed into a circular shape to manufacture an HDD substrate (also called a disc blank).
[0004] As a method for measuring the shape accuracy of the HDD substrate, there is a method in which a circular area of a rectangular glass plate before being processed into a round shape and corresponding to the HDD substrate is used as an object, and the flatness of the object is measured using an oblique incidence interferometer. Although this is an example, the flatness required for a 3.5-inch HDD substrate is strictly a flatness of 50 μm or less in a vertical state without the influence of gravity.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application No. 2020-510950 Summary of the invention
[0008] Problems to be solved by the invention
[0009] As described above, there is a strict requirement for the shape accuracy of the HDD substrate, and therefore, when manufacturing a mother glass plate to be a raw material of the HDD substrate, it is necessary to ensure the shape accuracy of the mother glass plate through, for example, the following steps.
[0010] First, a mother glass plate for inspection is extracted from a production line of mother glass plates. Next, the shape accuracy of the extracted mother glass plate for inspection is measured. Specifically, a plurality of rectangular glass plates (about 100 mm square) are cut out from the mother glass plate for inspection. The plurality of rectangular glass plates are arranged along the pulling direction and the width direction of the mother glass plate for inspection. Afterwards, the flatness of each of the cut rectangular glass plates is measured using an oblique incidence interferometer. Furthermore, if the flatness values of all the rectangular glass plates are within the allowable range, it is determined that the mother glass plate meets the shape accuracy benchmark for use as an HDD substrate, and the shape accuracy of the mother glass plate is guaranteed.
[0011] As described above, when ensuring the shape accuracy of the mother glass plate, the shape accuracy of the mother glass plate for inspection is measured by measuring the flatness of a plurality of rectangular glass plates. In summary, the above steps are as follows: if a plurality of rectangular glass plates corresponding to the size of the final product (HDD substrate) are actually cut out from the mother glass plate for inspection, and each of them satisfies the required shape accuracy, then the mother glass plate satisfies the standard of shape accuracy for use as an HDD substrate.
[0012] When the shape accuracy of the mother glass plate is ensured by the above steps, the number of rectangular glass plates cut from the mother glass plate for inspection will reach several hundred. For example, when a part of the mother glass plate for inspection with a size of 2200×2500 mm is used, 10 rows of rectangular glass plates are cut along the drawing direction of the mother glass plate for inspection and 25 rows of rectangular glass plates are cut along the width direction, totaling 250 sheets. Then, the shape accuracy needs to be measured for each of the 250 sheets. Therefore, there is a problem that the measurement of the shape accuracy of the mother glass plate for inspection consumes a lot of effort and time.
[0013] In view of the above, a technical problem to be solved is to reduce the effort and time required for measurement while ensuring the measurement accuracy when manufacturing a mother glass plate for an HDD substrate requiring high shape accuracy includes a step of measuring the shape accuracy of a mother glass plate for inspection.
[0014] Solutions to Solve Problems
[0015] (1) A method for manufacturing a mother glass plate for a hard disk drive, which is used to solve the above-mentioned problem, comprises: a production step of continuously producing mother glass plates in a production line; a picking step of picking up a mother glass plate for inspection from the production line; a measuring step of measuring the shape accuracy of the mother glass plate for inspection; and a pass / fail judging step of judging the pass / fail status of a plurality of mother glass plates produced in the production step based on the result of the measuring step, wherein the mother glass plate is in a rectangular shape having a first side along a plate pulling direction and a second side along a width direction orthogonal to the plate pulling direction, and the length of each of the first side and the second side is 1000 mm or more, and the mother glass plate is The thickness of the plate is greater than or equal to 0.3 mm and less than or equal to 0.7 mm, the extraction process is performed at predetermined intervals, and a plurality of rectangular first evaluation areas are arranged along the width direction of the effective portion in a manner that fills the entire width of the effective portion of the extracted inspection mother glass plate and are set with a side length of greater than or equal to 300 mm and less than or equal to 700 mm, the measuring process includes: a process of measuring the front and back deflection difference along the plate pulling direction and the width direction for each of the plurality of first evaluation areas; and a process of calculating the amount of change in the front and back deflection difference between the corresponding first evaluation areas between the inspection mother glass plates extracted in two consecutive extraction processes.
[0016] In the measurement process of the present manufacturing method, when measuring the shape accuracy of the mother glass plate for inspection, a process of measuring the front and back deflection difference along the pulling direction and the width direction for each of the plurality of first evaluation regions (hereinafter referred to as the front and back deflection difference measurement process) is performed. According to this measurement scheme, the shape accuracy can be measured more efficiently than when the shape accuracy of the mother glass plate for inspection is measured by measuring the flatness of a plurality of rectangular glass plates using an oblique incidence interferometer. This is based on the following reasons (A) and (B). (A) Since the size of each first evaluation region (the length of one side is 300 mm or more and 700 mm or less) can be made larger than the size of the rectangular glass plate when the oblique incidence interferometer is used, the number of measurement objects can be greatly reduced. That is, the number of first evaluation regions can be greatly reduced compared to the number of rectangular glass plates. (B) Even if the size of the first evaluation region is increased as described above, the shape accuracy of the mother glass plate for inspection can be accurately measured. That is, it is possible to accurately determine whether the mother glass plate for inspection meets the required shape accuracy standard. The reason is as follows. The mother glass plate (the mother glass plate for inspection) is not a mother glass plate whose shape changes locally in a small area, but a mother glass plate whose shape changes slowly in a large area. Therefore, if the shape accuracy of the first evaluation area (the shape accuracy obtained based on the front and back deflection difference) can be guaranteed, the shape accuracy when cut out with a size smaller than the first evaluation area (the size of the final product, etc.) can also be guaranteed. Due to the reasons (A) and (B) above, according to this measurement process, when measuring the shape accuracy of the mother glass plate for inspection, the number of measurement objects can be greatly reduced, and the measurement can be accurately performed. As a result, the effort and time required for the measurement can be reduced while ensuring the accuracy of the measurement.
[0017] In the measurement process of the present manufacturing method, in addition to the front and back deflection difference measurement process, a process of calculating the amount of change of the front and back deflection difference between the corresponding first evaluation areas between the mother glass sheets for inspection extracted in the two consecutive extraction processes (hereinafter referred to as the corresponding area deflection difference change calculation process) is also performed. Thereafter, a pass / fail judgment process of judging the pass / fail of the plurality of mother glass sheets produced in the production process based on the result of the measurement process is performed. In addition, in the present manufacturing method, the plurality of mother glass sheets can be judged as pass / fail when both the following [Condition 1] and [Condition 2] are satisfied. It should be noted that "a plurality of mother glass sheets" refers to a plurality of mother glass sheets sandwiched between the preceding inspection sheet and the following inspection sheet on the production line when the mother glass sheets for inspection extracted in the preceding extraction process and the following extraction process in the two consecutive extraction processes are respectively set as the preceding inspection sheet and the following inspection sheet. [Condition 1]: The mother glass sheets for inspection (the preceding inspection sheet and the following inspection sheet) extracted in the two consecutive extraction processes each meet the required standard of shape accuracy. Specifically, when the front and back deflection differences along the plate pulling direction and the width direction are measured for each of the plurality of first evaluation areas in both the preceding inspection plate and the following inspection plate (when the front and back deflection difference measuring step is performed), the values of the front and back deflection differences along the plate pulling direction and the width direction in all the first evaluation areas are within the allowable range. [Condition 2]: When the variation of the front and back deflection differences between the corresponding first evaluation areas between the inspection mother glass plates (between the preceding inspection plate and the following inspection plate) extracted in two consecutive extraction steps is calculated (when the variation calculation step of the deflection difference between the corresponding areas is performed), all the calculated values are within the allowable range. For example, when there are 7 first evaluation areas on a mother glass plate for inspection, the variation of the front and back deflection differences between the corresponding first evaluation areas in all the 7 must be within the allowable range. On the other hand, when either [Condition 1] or [Condition 2] is not satisfied, the plurality of mother glass plates described above can be judged as unqualified.
[0018] (2) In the manufacturing method of (1) above, preferably, the measuring step further includes the step of calculating the amount of change in the front and back deflection difference between first evaluation regions adjacent in the width direction for each inspection mother glass plate.
[0019] In this way, in the measurement process, based on the amount of change in the front and back deflection difference between the first evaluation areas adjacent in the width direction, the change in the shape of the mother glass plate for inspection along the width direction can be made clear. Therefore, the shape accuracy of the mother glass plate for inspection can be measured more accurately. This is advantageous in the case where a higher shape accuracy is required for the mother glass plate and a mother glass plate that meets the requirement is selected (determined as qualified in the pass / fail determination process). For example, if, in addition to satisfying both the above-mentioned conditions 1 and 2, the amount of change in the front and back deflection difference between the first evaluation areas adjacent in the width direction is calculated, and it is determined as qualified in the pass / fail determination process when all the calculated values are below the threshold, a mother glass plate with a higher shape accuracy can be obtained.
[0020] (3) In the manufacturing method of (1) or (2) above, it may be that, in the extraction process, second evaluation regions whose positions in the width direction are the same as those of the first evaluation regions and which are adjacent to the first evaluation regions in the plate pulling direction are further set corresponding to each of the plurality of first evaluation regions, and the measurement process further includes: a process of measuring the front and back deflection difference along the plate pulling direction and the width direction for each second evaluation region; and a process of calculating the change in the front and back deflection difference between the corresponding first evaluation region and the second evaluation region.
[0021] In this way, in the measurement process, based on the front and back deflection difference along the plate pulling direction and the width direction of the second evaluation area and the amount of change in the front and back deflection difference between the first evaluation area and the second evaluation area adjacent to each other in the plate pulling direction, the change in the shape of the mother glass plate for inspection along the plate pulling direction can be made clear. Therefore, the shape accuracy of the mother glass plate for inspection can be measured more accurately. Therefore, it is advantageous when a mother glass plate is required to have a higher shape accuracy and a mother glass plate that meets the requirement is selected (determined to be qualified in the pass / fail judgment process). For example, if, in addition to satisfying both the above-mentioned conditions 1 and 2, the front and back deflection difference along the plate pulling direction and the width direction of the second evaluation area and the amount of change in the front and back deflection difference between the first evaluation area and the second evaluation area adjacent to each other in the plate pulling direction are calculated, and when all the calculated values are below the threshold, it is determined to be qualified in the pass / fail judgment process, a mother glass plate with a higher shape accuracy can be obtained.
[0022] (4) In any one of the manufacturing methods described in (1) to (3) above, in the extraction step, a plurality of third evaluation regions may be set for the width direction end regions in the effective portion of the extracted inspection mother glass plate, and the width of the width direction end regions may be less than 30% of the length of the second side. The measuring step may further include a step of measuring the flatness of each of the plurality of third evaluation regions using an optical interferometer.
[0023] In the width direction end region of the effective part of the mother glass plate for inspection, the shape of the mother glass plate for inspection is prone to change, such as warping. Therefore, for the width direction end region, in addition to the measurement of the front and back deflection difference of the first evaluation region mentioned above, if the flatness of the plurality of third evaluation regions is measured respectively by using an optical interferometer on the basis of setting a plurality of third evaluation regions, the shape accuracy of the mother glass plate for inspection can be measured more accurately. It should be noted that the plurality of third evaluation regions are set in the width direction end region of the effective part of the mother glass plate for inspection, and should not be set in the entire effective part of the mother glass plate for inspection. Therefore, the increase in the number of measurement objects caused by setting a plurality of third evaluation regions is suppressed to a minimum, so that the risk of hindering the efficient measurement of the shape accuracy of the mother glass plate for inspection can be eliminated.
[0024] (5) In the manufacturing method of (4) above, the third evaluation region may be in a rectangular shape with a side being 50 mm or more and 150 mm or less.
[0025] In this way, the size of the third evaluation area corresponds to the size of the HDD substrate (2.5-inch size, 3.5-inch size). Specifically, the size of the third evaluation area is based on the size of the rectangular glass plate before being processed into a round shape. Therefore, it is advantageous in terms of ensuring the shape accuracy of the mother glass plate for the HDD substrate.
[0026] (6) In the manufacturing method of (4) or (5) above, preferably, the third evaluation region is a part of the first evaluation region.
[0027] In this way, when both the front and back deflection difference measurement of the first evaluation region and the flatness measurement of the third evaluation region using an optical interferometer are performed, it is not necessary to cut out the first evaluation region and the third evaluation region from different regions of the mother glass plate for inspection. In addition, since the flatness measurement is performed on the third evaluation region in addition to the front and back deflection difference measurement performed on the first evaluation region serving as the raw material of the third evaluation region, the shape accuracy of the mother glass plate for inspection can be measured more accurately.
[0028] (7) In any one of the manufacturing methods described in (1) to (6) above, the mother glass plate may have a defect inside, and the manufacturing method of the mother glass plate may further include: a defect depth measuring step of measuring the depth from the main surface of the mother glass plate to the defect; and a defect evaluation step of evaluating the defect based on the measured depth.
[0029] In the manufacturing process of manufacturing HDD substrates from a mother glass plate, there is a case where the main surface of a glass plate cut out from the mother glass plate in small pieces is mechanically ground. Therefore, even if the mother glass plate has defects such as foreign matter and bubbles inside, if the depth from the main surface of the mother glass plate to the defect is below a specified value, the defect can be removed by grinding. The mother glass plate from which the defect can be removed by a post-process in this way can be used instead of being discarded as a defective product. Therefore, by executing a defect depth measurement process and a defect evaluation process, the defects are classified into qualified defects (defects that can be removed) with a depth below a specified value and unqualified defects with a depth greater than a specified value, and the mother glass plate is evaluated based on the number, size and type of unqualified defects, thereby improving the yield of the mother glass plate.
[0030] (8) In addition, the mother glass plate that can be manufactured by the above-mentioned manufacturing method is a mother glass plate for a hard disk drive, the mother glass plate is a rectangular shape having a first side along a plate pulling direction and a second side along a width direction orthogonal to the plate pulling direction, and the length of each of the first side and the second side is greater than 1000 mm, and the thickness of the mother glass plate is greater than 0.3 mm and less than 0.7 mm, wherein a plurality of rectangular first evaluation areas are set in a manner to fill the entire width of the effective portion of the mother glass plate, the sides of the plurality of first evaluation areas in the plate pulling direction are 500 mm, and the sides of the plurality of first evaluation areas in the width direction are 400 mm, and when the front and back deflection differences along the plate pulling direction and the width direction are measured for each of the first evaluation areas in all the first evaluation areas, the values of the front and back deflection differences all fall within the range of ±0.5 mm, and the values of the front and back deflection differences are values when converted to a square size of 350 mm.
[0031] In the present mother glass plate, when converted to a 350 mm square size, the values of the front and back deflection differences along the drawing direction and the width direction of all the first evaluation areas fall within the range of ±0.5 mm, ensuring high shape accuracy. Therefore, the present mother glass plate is suitable as a mother glass plate for HDD substrates requiring high shape accuracy.
[0032] (9) In the mother glass sheet of (8) above, preferably, each of the changes in the front and back deflection differences between first evaluation regions adjacent to each other in the width direction of the mother glass sheet is 0.3 mm or less.
[0033] In this way, the change in shape of the mother glass plate along the width direction is small, and thus the mother glass plate is more suitable as a mother glass plate for an HDD substrate that requires high shape accuracy.
[0034] (10) In the mother glass plate of (8) or (9) above, preferably, the mother glass plate is further provided with second evaluation areas corresponding to each of the plurality of first evaluation areas, the second evaluation areas having the same width direction position as the first evaluation areas and being adjacent to the first evaluation areas in the plate pulling direction, and when the front and back deflection differences along the plate pulling direction and the width direction are measured for each second evaluation area, the values of the front and back deflection differences all fall within the range of ±0.5 mm, and the changes in the front and back deflection differences between the corresponding first evaluation areas and the second evaluation areas are each less than 0.3 mm.
[0035] In this way, the change in shape of the mother glass plate along the pulling direction is small, and thus the mother glass plate is more suitable as a mother glass plate for an HDD substrate that requires high shape accuracy.
[0036] (11) In any of the mother glass sheets described in (8) to (10) above, preferably, a plurality of third evaluation areas having a rectangular shape are set in the mother glass sheet in a range where the distance from the first side is less than 30% of the length of the second side, and each side of the third evaluation area is 100 mm. When the flatness of each of the third evaluation areas is measured using an optical interferometer, the flatness is less than 50 μm.
[0037] Thus, the size of the third evaluation area corresponds to the size of the HDD substrate (specifically, the size of the rectangular glass plate before being processed into a round shape). In addition, the flatness of all the third evaluation areas is 50 μm or less, ensuring high flatness. Therefore, it is suitable as a mother glass plate for an HDD substrate.
[0038] (12) In any one of the mother glass sheets described in (8) to (11) above, it is preferred that the longitudinal elastic modulus of the mother glass sheet is 80 GPa or more.
[0039] If the longitudinal elastic modulus has such a value, it is more suitable as a mother glass plate of an HDD substrate.
[0040] (13) In any of the mother glass sheets described in (8) to (12) above, the mother glass sheet may have a defect inside, and preferably the depth of the defect from the main surface of the mother glass sheet is 25 μm or less.
[0041] If the depth of the defect of the mother glass plate is less than 25 μm from the main surface, the defect can be removed by mechanically grinding the main surface in the manufacturing process of the HDD substrate from the mother glass plate. In this way, even if the mother glass plate contains a defect inside, if the depth of the defect is less than 25 μm from the main surface, it will not be discarded as a defective product and can be used as a glass plate for HDD substrates, thereby improving the yield rate.
[0042] Effects of the Invention
[0043] According to the method for manufacturing a mother glass plate of the present invention, when manufacturing a mother glass plate of an HDD substrate requiring high shape accuracy, in the case of including a step of measuring the shape accuracy of the mother glass plate for inspection, the labor and time required for the measurement can be reduced while ensuring the measurement accuracy. In addition, the mother glass plate of the present invention is suitable as a mother glass plate of an HDD substrate requiring high shape accuracy. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 is a top view showing a mother glass plate.
[0045] Figure 2 is a top view showing a mother glass plate.
[0046] Figure 3 is a top view showing a mother glass plate.
[0047] Figure 4 is a top view showing a mother glass plate.
[0048] Figure 5 It is a plan view showing an enlarged view of the periphery of the first evaluation region in the mother glass plate.
[0049] Figure 6 This is a diagram for explaining a method for measuring the difference in front and back deflection.
[0050] Figure 7 It is a graph showing the measurement results of the front and back deflection differences along the pulling direction of a plurality of first evaluation areas.
[0051] Figure 8 It is a diagram showing the measurement results of the front and back deflection differences along the width direction of a plurality of first evaluation areas.
[0052] Fig. 9 It is a graph showing the measurement results of the front and back deflection differences along the pulling direction of a plurality of second evaluation areas.
[0053] Fig.10 It is a diagram showing the measurement results of the front and back deflection differences along the width direction of a plurality of second evaluation areas.
[0054] Fig.11 The diagram shows the measurement results of the front and back deflection difference along the plate pulling direction of the first evaluation area and the measurement results of the front and back deflection difference along the plate pulling direction of the second evaluation area.
[0055] Fig.12 The diagram shows the measurement results of the front and back deflection difference along the width direction of the first evaluation area and the measurement results of the front and back deflection difference along the width direction of the second evaluation area.
[0056] Fig.13ais a cross-sectional view schematically showing a mother glass plate.
[0057] Fig.13b is a cross-sectional view schematically showing a glass plate cut out from a mother glass plate.
[0058] Fig.14 It is a cross-sectional view showing a production process in a method for manufacturing a mother glass plate.
[0059] Fig.15 It is a schematic diagram which shows the extraction process in the manufacturing method of a mother glass plate.
[0060] Fig.16 It is a figure which shows the measurement result of a part of the measurement process in the manufacturing method of a mother glass plate.
[0061] Fig.17 It is a figure which shows the measurement result of a part of the measurement process in the manufacturing method of a mother glass plate. DETAILED DESCRIPTION
[0062] Hereinafter, a mother glass sheet and a method for manufacturing the mother glass sheet according to an embodiment will be described with reference to the drawings. First, the mother glass sheet will be described.
[0063] exist Figure 1 1 shows a mother glass plate 1. The mother glass plate 1 is a glass cut from a glass ribbon formed by a down-draw method or a float method. The mother glass plate 1 is a mother glass of a product glass plate that is required to have high shape accuracy. When manufacturing a product glass plate, the product glass plate is assembled from the mother glass plate 1. In detail, the mother glass plate 1 of this embodiment is a mother glass of a 3.5-inch HDD substrate (a glass substrate for a hard disk drive). Of course, it is not limited to this, and the mother glass plate 1 can also be a mother glass of a HDD substrate of other sizes (for example, 2.5 inches).
[0064] The mother glass sheet 1 is in a rectangular shape having a first side 2 along a drawing direction and a second side 3 along a width direction orthogonal to the drawing direction. Here, the "drawing direction" of the mother glass sheet 1 refers to a direction that is consistent with the drawing direction of the glass ribbon when the glass ribbon is formed. On the other hand, the "width direction" of the mother glass sheet 1 refers to a direction that is consistent with the width direction of the glass ribbon. The drawing direction can be observed as a stripe pattern by, for example, irradiating light from a light source (such as a xenon lamp) while adjusting the angle of the mother glass sheet 1 in a dark room and projecting the transmitted light onto a screen. Therefore, the drawing direction and the width direction can also be distinguished in the mother glass sheet 1 cut from the glass ribbon.
[0065] The longitudinal elastic modulus of the mother glass plate 1 is 80 GPa or more. The thickness of the mother glass plate 1 is 0.3 mm or more and 0.7 mm or less. The length 2y of the first side 2 and the length 3x of the second side 3 are both 1000 mm or more. Here, in this embodiment, the mother glass plate 1 is G8.5 size, the length 2y of the first side 2 is 2200 mm, and the length 3x of the second side 3 is 2500 mm. Of course, it is not limited to this, and the mother glass plate 1 may also be other sizes such as G6 size.
[0066] The mother glass plate 1 is preferably alkali-free glass or alkali-aluminosilicate glass.
[0067] In the case of alkali-free glass, the glass composition preferably contains, by mol%, 60 to 75% SiO2, 5 to 20% Al2O3, 0 to 15% B2O3, 0 to 1% Li2O+Na2O+K2O (the total amount of Li2O, Na2O and K2O) or more and less than 1%, 0 to 10% MgO, 0 to 15% CaO, 0 to 10% SrO, and 0 to 10% BaO. The following glass composition example (1) or (2) is particularly preferred.
[0068] (1) The glass composition preferably contains, in mol %, 62 to 72% SiO2, 9.5 to 16% (particularly 11 to 15%) Al2O3, 1 to 8% (particularly 2 to 4%) B2O3, 0 to less than 1% (particularly 0 to 0.5%) Li2O+Na2O+K2O, 1 to 9% (particularly 4 to 8%) MgO, 2 to 10% (particularly 3 to 8%) CaO, 0.1 to 5% (particularly 1 to 3%) SrO, and 0.1 to 5% (particularly 1 to 3%) BaO.
[0069] (2) The glass composition preferably contains, in mol %, 67 to 77% of SiO2, 9 to 14% of Al2O3, 0 to 3% (particularly 0 to less than 1%) of B2O3, 0 to less than 1% (particularly 0 to 0.5%) of Li2O+Na2O+K2O, 0 to 5% (particularly 2 to 5%) of MgO, 0 to 10% (particularly 6 to 9%) of CaO, 0 to 5% of SrO, and 0 to 7% (particularly 3 to 6%) of BaO.
[0070] In the case of alkali aluminosilicate glass, the glass composition preferably contains, by mol%, 50 to 75% SiO2, 10 to 30% Al2O3, 0 to 12% B2O3, 0 to 10% Li2O, 2 to 18% Na2O, and 0 to 5% K2O. The following glass composition examples (3) or (4) are particularly preferred.
[0071] (3) The glass composition preferably contains, by mol%, 60 to 70% of SiO2, 10 to 14% of Al2O3, 0 to 3% of B2O3, 0 to 1% of Li2O, 12 to 18% of Na2O, and 0 to 2% of K2O.
[0072] (4) The glass composition preferably contains, by mol%, 65 to 75% of SiO2, 10 to 30% of Al2O3, 0 to 12% of B2O3, 5 to 10% of Li2O, 2 to 10% of Na2O, and 0 to 3% of K2O.
[0073] In the mother glass plate 1, the entire region (entire area) thereof becomes the effective portion. Here, the "effective portion" refers to the region of the mother glass plate 1 that will later become the product glass plate. It should be noted that in the present embodiment, the entire region of the mother glass plate 1 becomes the effective portion, but the present invention is not limited thereto. In the case where only a portion of the region of the mother glass plate 1 will later become the product glass plate, the portion becomes the effective portion.
[0074] In the mother glass plate 1, a plurality of rectangular first evaluation regions 41 (in Figure 1 Indicated by double-dotted lines). It should be noted that "setting multiple first evaluation areas 41 in a manner that fills the entire width of the effective part" means that all parts in the width direction of the effective part are included in the width of a first evaluation area 41 among the multiple first evaluation areas 41. The multiple first evaluation areas 41 have the same size as each other. In each first evaluation area 41, the size 41ay of the longitudinal side 41a extending in the pulling direction and the size 41bx of the transverse side 41b extending in the width direction are respectively greater than 300 mm and less than 700 mm. In the present embodiment, the size 41ay of the longitudinal side 41a is 500 mm, and the size 41bx of the transverse side 41b is 400 mm. Here, the size of the first evaluation area 41 is larger than the size of the product glass plate (here, a 3.5-inch HDD substrate).
[0075] In the present embodiment, there are seven first evaluation regions 41. It should be noted that the number of the first evaluation regions 41 is not limited to seven, and for example, the number of the first evaluation regions 41 may be appropriately increased or decreased according to the size of the mother glass plate 1. In the following description, the seven first evaluation regions 41 are sometimes distinguished by being recorded as first evaluation regions A, B, ..., F, G in the order in which they are arranged.
[0076] Among the seven first evaluation regions 41, five first evaluation regions B to F near the center in the width direction of the mother glass plate 1 are arranged in a row without gaps along the width direction of the mother glass plate 1. On the other hand, the two first evaluation regions A and G located at both ends in the width direction of the mother glass plate 1 are located at positions offset in the plate pulling direction relative to the five first evaluation regions B to F. It should be noted that the first evaluation region A and the first evaluation region B, and the first evaluation region F and the first evaluation region G are offset in the plate pulling direction, but a part of the region in the width direction overlaps.
[0077] In this embodiment, there are seven first evaluation regions 41 near the center of the mother glass sheet 1 in the pulling direction, but the present invention is not limited thereto. The positions of the seven first evaluation regions 41 can be any positions in the pulling direction. That is, the positions of the first evaluation regions 41 can be any positions in the pulling direction. Figure 1 Therefore, as a form of setting the first evaluation area 41 for the mother glass sheet 1, it is also possible to adopt Figure 2 , Figure 3 The form shown. Figure 2 In the embodiment shown, the seven first evaluation areas 41 are arranged in a zigzag pattern. Figure 3 In the illustrated embodiment, all of the seven first evaluation regions 41 are arranged in a row without any gap in the width direction.
[0078] In this embodiment, if Figure 4 As shown, corresponding to each of the seven first evaluation regions 41, a second evaluation region 42 (in Figure 4 The second evaluation region 42 may be set on the upper side of the first evaluation region 41 along the plate pulling direction, or may be set on the lower side of the first evaluation region 41 along the plate pulling direction. In addition, the dimension 42ay of the longitudinal side 42a extending along the plate pulling direction and the dimension 42bx of the transverse side 42b extending along the width direction of the second evaluation region 42 are preferably the same as the dimension 41ay of the longitudinal side 41a and the dimension 41bx of the transverse side 41b of the first evaluation region 41 (for the dimension 41ay and the dimension 41bx, refer to Figure 1 Here, in the following description, the seven second evaluation areas 42 are sometimes distinguished by being recorded as second evaluation areas H, I, ..., M, N in the order in which they are arranged.
[0079] In the mother glass plate 1, a width direction end region 5 (at Figure 1 to Figure 4). The width direction end regions 5 are respectively set at one end side and the other end side of the mother glass plate 1 in the width direction. The width dimension 5x of the width direction end region 5 is a dimension with 30% of the length 3x of the second side 3 as the upper limit. That is, the width direction end region 5 corresponds to a range in which the distance from the first side 2 in the mother glass plate 1 is less than 30% of the length 3x of the second side 3. In the width direction end region 5, warping is easily generated in the mother glass plate 1 (especially in the range up to 300 mm from the first side 2). It should be noted that when the glass ribbon is formed, a thick-walled ear portion is formed further outside the width direction of the width direction end region 5.
[0080] like Figure 5 As shown, a plurality of rectangular third evaluation areas 6 are set in the width direction end area 5 (in Figure 5 ). In detail, a plurality of third evaluation regions 6 are set in the region overlapping with the first evaluation region 41 in the width direction end region 5. That is, each of the plurality of third evaluation regions 6 becomes a part of the first evaluation region 41. However, it is not limited thereto, and the third evaluation region 6 may also be set in a region different from the first evaluation region 41 (a region not overlapping with the first evaluation region 41) in the width direction end region 5. In addition, as long as the third evaluation region 6 is set in the width direction end region 5, the position in the pulling direction may be arbitrary. It should be noted that the width direction end region 5 is respectively set at one end side and the other end side in the width direction of the mother glass plate 1, and therefore, the plurality of third evaluation regions 6 are also respectively set at one end side and the other end side in the width direction of the mother glass plate 1.
[0081] In the present embodiment, 5 columns of the third evaluation areas 6 are arranged without gaps along the plate pulling direction at one end side and the other end side in the width direction, respectively, and 2 columns of the third evaluation areas 6 are arranged without gaps along the width direction. Therefore, in the present embodiment, the total number of the third evaluation areas 6 set in the mother glass plate 1 is 20. The number of columns of the third evaluation areas 6 along the plate pulling direction and the width direction can be appropriately increased or decreased. As an example, it can be set to 5 to 10 columns along the plate pulling direction and 1 to 3 columns along the width direction. Here, regardless of the number of columns of the third evaluation areas 6 along the plate pulling direction and the width direction, the third evaluation area 6 located on the outermost side in the width direction is preferably the width direction end edge (edge) of the mother glass plate 1 (effective part) included in the area.
[0082] Each side of the third evaluation area 6 is greater than 50 mm and less than 150 mm. The third evaluation area 6 of the present embodiment is a square of 100 mm square. It should be noted that, in a case where the product glass plate is a 2.5-inch HDD substrate different from the present embodiment, the third evaluation area 6 may be set to a square of 75 mm square, for example.
[0083] In the present mother glass sheet 1 described above, when seven first evaluation regions 41 are cut out from the mother glass sheet 1 , the following [shape accuracy criterion A] and [shape accuracy criterion B] are satisfied.
[0084] [Shape accuracy criterion A]: When the front-back deflection difference d1 of the two sides along the pulling direction (two longitudinal sides 41a) and the two sides along the width direction (two transverse sides 41b) are measured for each of the seven first evaluation areas 41 (first evaluation areas A to G) (when a total of 28 front-back deflection differences d1 are measured), the values of the front-back deflection difference d1 are all within the range of ±0.5 mm. It should be noted that it is more preferred if the value of the front-back deflection difference d1 falls within the range of ±0.3 mm, further preferred if it falls within the range of ±0.2 mm, and most preferred if it falls within the range of ±0.1 mm.
[0085] [Shape accuracy criterion B]: The first evaluation areas 41, 41 adjacent in the width direction are regarded as one group, and in all 6 groups (group A, B, group B, C, ... group E, F, group F, G), when the change Δd1 of the front and back deflection difference d1 between the first evaluation areas 41, 41 along the pulling direction (two longitudinal sides 41a) and along the width direction (two transverse sides 41b) is calculated (when a total of 24 changes Δd1 are calculated), the calculated values are each less than 0.3 mm. It should be noted that it is more preferred if the calculated value of the change Δd1 is less than 0.2 mm, and even more preferred if it is less than 0.1 mm. Here, "adjacent in the width direction" not only includes Figure 3 The case where two first evaluation areas 41, 41 are adjacent to each other in the positive transverse direction as in the group A and B of FIG. Figure 1 as well as Figure 2 In the case where the two first evaluation regions 41, 41 are located at positions offset along the plate pulling direction, as in the group A and B in FIG. It should be noted that the calculation of the change Δd1 of the front and back deflection difference d1 on both sides along the plate pulling direction may be omitted, and only the change Δd1 of the front and back deflection difference d1 on both sides along the width direction may be calculated. In this case (the case where a total of 12 changes Δd1 are calculated), the calculated values are preferably 0.3 mm or less, more preferably 0.2 mm or less, and even more preferably 0.1 mm or less.
[0086] Furthermore, in the present mother glass sheet 1 , when seven second evaluation regions 42 are cut out in addition to the seven first evaluation regions 41 , the following “shape accuracy criterion C” and “shape accuracy criterion D” are satisfied.
[0087] [Shape accuracy criterion C]: When the front-back deflection difference d2 of the two sides along the pulling direction (two longitudinal sides 42a) and the two sides along the width direction (two transverse sides 42b) are measured for each of the 7 second evaluation areas 42 (second evaluation areas H to N) (when a total of 28 front-back deflection differences d2 are measured), the values of the front-back deflection difference d2 all fall within the range of ±0.5 mm. It should be noted that it is more preferred if the value of the front-back deflection difference d2 falls within the range of ±0.3 mm, further preferred if it falls within the range of ±0.2 mm, and most preferred if it falls within the range of ±0.1 mm.
[0088] [Shape accuracy criterion D]: Taking the corresponding first evaluation area 41 and the second evaluation area 42 as one group, in all 7 groups (groups A and H, groups B and I, ... groups F and M, groups G and N), when calculating the change Δd2 between the front and back deflection difference d1 of the four sides (two longitudinal sides 41a and two transverse sides 41b) of the first evaluation area 41 and the front and back deflection difference d2 of the corresponding four sides (two longitudinal sides 42a and two transverse sides 42b) of the corresponding second evaluation area 42 (when calculating a total of 28 changes Δd2), the calculated values are each 0.3 mm or less. It should be noted that it is more preferred if the calculated value of the change Δd2 is 0.2 mm or less, and it is even more preferred if it is 0.1 mm or less. It should be noted that it is also possible to calculate only the change Δd2 between the front and back deflection difference d1 of the two sides along the pull plate direction of the first evaluation area 41 and the front and back deflection difference d2 of the two sides along the pull plate direction of the second evaluation area 42. That is, the calculation of the variation Δd2 of the front-back deflection difference d1 of the two sides extending in the width direction of the first evaluation area 41 and the front-back deflection difference d2 of the two sides extending in the width direction of the second evaluation area 42 may be omitted. In this case, the calculated values (when a total of 14 variations Δd2 are calculated) are preferably 0.3 mm or less, more preferably 0.2 mm or less, and even more preferably 0.1 mm or less.
[0089] Furthermore, in the present mother glass sheet 1 , when all the third evaluation regions 6 are cut out from each of the seven first evaluation regions 41 , the following “shape accuracy criterion E” is satisfied.
[0090] [Shape accuracy criterion E]: When the flatness is measured for all third evaluation regions 6 using an optical interferometer (when a total of 20 flatness values are measured), the flatness values are all 50 μm or less. It should be noted that a flatness value of 30 μm or less is more preferred, 20 μm or less is further preferred, and 10 μm or less is most preferred.
[0091] The following describes in detail [Shape Accuracy Standard A] to [Shape Accuracy Standard E].
[0092] When determining whether the [shape accuracy criterion A] and [shape accuracy criterion B] are satisfied, the front-back deflection difference d1 is measured by the following steps. It should be noted that, as described above, the front-back deflection difference d1 is measured in both the plate pulling direction and the width direction for each of the seven first evaluation regions 41, but here the case of measuring the front-back deflection difference d1 along the plate pulling direction of the first evaluation region A is taken as an example.
[0093] like Figure 6 As shown, by measuring the deflection W1 when the surface of the front and back of the first evaluation area A is set to the upper side (in the case shown by the solid line) and the deflection W2 when the back is set to the upper side (in the case shown by the single-dot chain line), and finding W1-W2, the front and back deflection difference d1 (d1=W1-W2) is measured. At this time, the first evaluation area A is supported by two supporting members 7, 7 extending in parallel with a distance L. In this embodiment, the distance L is 350mm. Here, in order to measure the deflection along the pulling direction, the longitudinal side 41a of the first evaluation area A is set between the two supporting members 7, 7. Of course, when measuring the front and back deflection difference d1 along the width direction, when measuring the deflection along the width direction, the horizontal side 41b of the first evaluation area A is set between the two supporting members 7, 7. Here, the deflection W1 and the deflection W2 are measured for each of the two sides (two longitudinal sides 41a) extending in the pulling direction, and the front and back deflection difference d1 is measured for each of the two sides extending in the pulling direction. Figure 6 In the measurement scheme shown, two measurement values of the front-back deflection difference d1 of one of the two longitudinal sides 41 a and the front-back deflection difference d1 of the other are obtained.
[0094] When the measurement procedure of the front-back deflection difference d1 is imitated, the front-back deflection difference d1 of the two sides along the pulling direction (two longitudinal sides 41a) and the two sides along the width direction (two transverse sides 41b) of each of the 7 first evaluation areas 41 is measured, and a total of 28 measurement values are obtained as the value of the front-back deflection difference d1. It should be noted that since the values of the deflection W1 and the deflection W2 change according to the length of the above-mentioned distance L, the value of the front-back deflection difference d1 may also change. Therefore, when the distance L is not 350 mm, the value of the front-back deflection difference d1 is converted into the value when the distance L is 350 mm (d1 = (W1-W2) × 350 / L). Here, Figure 7 The measurement results of the front and back deflection differences d1 of the seven first evaluation areas 41 (first evaluation areas A to G) along the plate pulling direction are shown in FIG. Figure 8 The measurement results of the front and back deflection difference d1 of both sides along the width direction are shown in FIG. Figure 7 as well as Figure 8 In the figure, one of the measurement results on the two sides is connected by a solid line, and the other measurement result on the two sides is connected by a dashed-dotted line.
[0095] As in Figure 7 as well as Figure 8 As shown in the measurement results shown in the example, the total of 28 (14 in the pulling direction and 14 in the width direction) measured values of the front and back deflection differences d1 all fall within the range of ±0.5 mm (-0.5 mm ≤ d1 ≤ 0.5 mm). Therefore, [Shape Accuracy Criteria A] is satisfied.
[0096] In addition, a total of 24 (12 in the pulling direction and 12 in the width direction) changes Δd1 (in Figure 7 as well as Figure 8 The calculated values (in each case, only one of the 12 calculated changes Δd1) are 0.3 mm or less (|Δd1|≤0.3 mm). Thus, [Shape Accuracy Criteria B] is satisfied.
[0097] When determining whether the [Shape Accuracy Criteria C] and [Shape Accuracy D] are satisfied, the procedure for measuring the front-back deflection difference d2 of the two sides along the plate pulling direction (two longitudinal sides 42a) and the two sides along the width direction (two transverse sides 42b) of the second evaluation area 42 is the same as the procedure for measuring the front-back deflection difference d1 described above. Fig. 9 The measurement results of the front and back deflection differences d2 of the seven second evaluation areas 42 (second evaluation areas H to N) along the pulling direction are shown as examples. Fig.10 4 shows the measurement results of the front and back deflection differences d2 of the seven second evaluation areas 42 (second evaluation areas H to N) along the width direction. Fig. 9 as well as Fig.10 In the figure, one of the measurement results on the two sides is connected by a solid line, and the other measurement result on the two sides is connected by a dashed-dotted line.
[0098] As in Fig. 9 as well as Fig.10 As shown in the measurement results shown in the example, a total of 28 (14 in the pulling direction and 14 in the width direction) measured values of the front and back deflection differences d2 all fall within the range of ±0.5 mm (-0.5 mm ≤ d2 ≤ 0.5 mm). Therefore, [Shape Accuracy Criteria C] is satisfied.
[0099] The measurement results of the front-back deflection difference d1 of one side (one of the two longitudinal sides 41a) along the pulling direction of the seven first evaluation areas 41 (first evaluation areas A to G) and the measurement results of the front-back deflection difference d2 of the corresponding side (one of the two longitudinal sides 42a) of the seven second evaluation areas 42 (second evaluation areas H to N) are shown together. Fig.11 (d1 is represented by a solid line, and d2 is represented by a dashed line). In addition, the measurement results of the front-back deflection difference d1 of one side (one of the two lateral sides 41b) along the width direction of the seven first evaluation areas 41 (second evaluation areas A to G) and the measurement results of the front-back deflection difference d2 of the corresponding side (one of the two lateral sides 42b) of the seven second evaluation areas 42 (second evaluation areas H to N) are shown together. Fig.12 (d1 is represented by a solid line, and d2 is represented by a dot-dash line). A total of 14 (7 in the pulling direction and 7 in the width direction) changes Δd2 (in Fig.11 as well as Fig.12 The calculated values of only one of the seven calculated changes Δd2 are 0.3 mm or less (|Δd2|≤0.3 mm). Thus, [Shape Accuracy Criteria D] is satisfied.
[0100] When determining whether the [Shape Accuracy Criteria E] is satisfied, the flatness of each third evaluation area 6 is measured by the following method. That is, using an oblique incidence interferometer (product name: FT-17 or FT-900) manufactured by Nidec Corporation, the flatness is measured on the basis of setting each third evaluation area 6 to an upright state. Specifically, the flatness of the circular area corresponding to the HDD substrate in each third evaluation area 6 is measured. Of course, other oblique incidence interferometers can also be used. And, the value of the flatness in the upright state is set as the value of the flatness of each third evaluation area 6. The total of 20 flatness values obtained are all below 50μm. Thus, the [Shape Accuracy Criteria E] is satisfied.
[0101] By satisfying the above-mentioned [Shape Accuracy Criteria A] to [Shape Accuracy Criteria E], the shape accuracy of the mother glass plate 1 is ensured. It should be noted that when ensuring the shape accuracy of the mother glass plate 1, there is a case where the [Shape Accuracy Criteria A] must be satisfied, and whether or not to satisfy the [Shape Accuracy Criteria B], [Shape Accuracy Criteria C], [Shape Accuracy Criteria D], and [Shape Accuracy Criteria E] is arbitrary. That is, there is a case where the change Δd1 of the front-back deflection difference d1 of the first evaluation area 41, the front-back deflection difference d2 of the second evaluation area 42, the change Δd2 between the front-back deflection difference d1 of the first evaluation area 41 and the front-back deflection difference d2 of the second evaluation area 42, and the flatness of the third evaluation area 6 are not considered.
[0102] like Fig.13a As shown, there is a case where the mother glass plate 1 has defects 1d represented by foreign matter, bubbles, etc. inside. In this case, if the depth of the defect 1d from the main surface (the front surface 1a or the back surface 1b) of the mother glass plate 1 is less than a predetermined value, the defect 1d is removed in the process of manufacturing the HDD substrate from the mother glass plate 1, and the defect 1d does not remain in the finally obtained HDD substrate.
[0103] Specifically, in the process of manufacturing the HDD substrate, the main surface of each of the plurality of glass plates 1X (glass plates that become the raw materials of the HDD substrate) cut out as small pieces from the mother glass plate 1 is sometimes mechanically polished. Fig.13a The defect 1d (the portion indicated by the diagonal lines in FIG. 1 ) is removed from the glass plate 1X by mechanical grinding (in FIG. Fig.13b ). Therefore, no defect 1d remains in the HDD substrate.
[0104] Here, the depth of the defect 1d from the main surface (the front surface 1a or the back surface 1b) of the mother glass plate 1 is preferably 25 μm or less, more preferably 20 μm or less, further preferably 15 μm or less, and most preferably 10 μm or less. If the defect 1d exists in this depth range, it can be appropriately removed by mechanical polishing.
[0105] Hereinafter, a method for manufacturing the above-mentioned mother glass plate 1 will be described.
[0106] The manufacturing method includes: production process P1 ( Fig.14 ), the mother glass plate 1 is continuously produced in the production line; the extraction process P2 ( Fig.15), extracting the inspection mother glass plate 8 from the production line; a measuring step of measuring the shape accuracy of the inspection mother glass plate 8; and a pass / fail judging step of judging the pass / fail status of the plurality of mother glass plates 1 produced in the production step P1 based on the result of the measuring step. And, each of the plurality of mother glass plates 1 that pass in the pass / fail judging step is obtained as a mother glass with guaranteed shape accuracy (in this embodiment, a mother glass of a 3.5-inch HDD substrate).
[0107] <Production process>
[0108] like Fig.14 As shown, a manufacturing device 9 is used in the execution of the production process P1. The manufacturing device 9 is a device for continuously forming a glass ribbon Gr. The manufacturing device 9 includes: a forming furnace 10, which forms the glass ribbon Gr; an annealing furnace 11, which anneals the glass ribbon Gr (annealing treatment); a cooling area 12, which cools the glass ribbon Gr to near room temperature; and a pair of rollers 13, which are respectively arranged in multiple stages in the forming furnace 10, the annealing furnace 11 and the cooling area 12.
[0109] A forming body 14 for forming a glass ribbon Gr from molten glass Gm by an overflow down-draw method is arranged in the internal space of the forming furnace 10. The molten glass Gm supplied to the forming body 14 overflows to both sides from a groove (not shown) formed at the top 14a of the forming body 14. The overflowing molten glass Gm flows along the two side surfaces 14b of the wedge-shaped forming body 14 and merges at the lower end of the forming body 14, thereby continuously forming the glass ribbon Gr. The glass ribbon Gr is in a longitudinal posture (preferably a vertical posture), and the direction Q is the drawing direction.
[0110] The inner space of the annealing furnace 11 tends downward and has a predetermined temperature gradient. The glass ribbon Gr is annealed in such a manner that the temperature decreases as the glass ribbon Gr moves downward in the inner space of the annealing furnace 11. By this annealing, the internal strain of the glass ribbon Gr is reduced. The temperature gradient of the inner space of the annealing furnace 11 can be adjusted by a heating device (such as a heater, etc.) provided on the inner surface of the annealing furnace 11.
[0111] The plurality of roller pairs 13 clamp the ends of the glass ribbon Gr in the longitudinal posture in the width direction from both the front and back sides. It should be noted that, in the internal space of the annealing furnace 11, a roller pair that does not clamp the ends may be included in the plurality of roller pairs 13. In other words, the interval between the rollers constituting the roller pair 13 may be larger than the thickness of the ends, and the ends may pass between the rollers.
[0112] It should be noted that, in the present embodiment, the outer side of the wall portion 15 that divides the forming furnace 10, the annealing furnace 11, and the cooling area 12 is surrounded by an outer enclosure 16 (e.g., a building, etc.). In the space between the wall portion 15 and the outer enclosure 16, partitions 17 and 18 (e.g., the floor surfaces of each floor of the building, etc.) are respectively provided at positions corresponding to the upper end and the lower end of the cooling area 12. Under the action of these partitions 17 and 18, the space between the wall portion 15 and the outer enclosure 16 is divided into a chamber R1 that surrounds the annealing furnace 11 and a chamber R2 that surrounds the cooling area 12.
[0113] The manufacturing device 9 includes a cutting device 19 below the cooling zone 12. The cutting device 19 is configured to sequentially cut out glass sheets Gs (glass to be the raw material of the mother glass sheet 1) from the glass ribbon Gr by cutting the vertical glass ribbon Gr in the width direction at predetermined length intervals.
[0114] The cutting device 19 includes: a cutter wheel (not shown) that moves on one surface of the glass ribbon Gr descending from the cooling area 12 to form a score line S along the width direction of the glass ribbon Gr; a contact portion 20 that supports the area where the score line S is formed from the other surface side of the glass ribbon Gr; and a holding portion 21 that performs an action (action in the V direction) for applying a bending stress to the periphery of the score line S while holding the glass ribbon Gr at a portion corresponding to the glass sheet Gs.
[0115] The cutter wheel is structured to form a scoring line S in the entire width or a part of the width direction of the glass ribbon Gr while following the descending glass ribbon Gr. In the present embodiment, the scoring line S is also formed at the end including the ear portion having a relatively large thickness, but the scoring line S may not be formed at the end. It should be noted that the scoring line S may also be formed by irradiation of a laser or the like. In addition, since the end including the ear portion is cut off and removed from the glass sheet Gs in a subsequent process, no ear portion remains in the produced mother glass sheet 1.
[0116] The contact portion 20 is composed of a long bar that contacts the entire width or a part of the width direction of the glass ribbon Gr while following the descending glass ribbon Gr. The contact surface of the contact portion 20 that contacts the glass ribbon Gr may be a flat surface or a curved surface that curves in the width direction.
[0117] The holding part 21 is composed of a clamp that clamps the end of the glass ribbon Gr in the width direction from both sides. A plurality of holding parts 21 are provided at intervals along the length direction of the glass ribbon Gr. The holding parts 21 are provided for one end and the other end in the width direction of the glass ribbon Gr. The plurality of holding parts 21 for the one end are all held by the same arm (not shown). Similarly, the plurality of holding parts 21 for the other end are all held by the same arm (not shown). Under the action of the action of these arms, the plurality of holding parts 21 for the one end and the other end follow the glass ribbon Gr in the process of descending, and perform an action (action in the V direction) to bend the glass ribbon Gr with the contact part 20 as a fulcrum. Thus, a bending stress is applied to the periphery of the score line S, and the glass ribbon Gr is broken and cut along the score line S. Accompanying this breaking and cutting, a glass sheet Gs is cut out from the glass ribbon Gr. And, by repeating this breaking and cutting, a glass sheet Gs is continuously cut out from the glass ribbon Gr. In addition, the holding part 21 is not limited to the form which clamps and holds the edge part of the glass ribbon Gr, For example, it may be a form which adsorbs and holds any one of the front and back surfaces of the glass ribbon Gr.
[0118] Each glass sheet Gs cut out from the glass ribbon Gr includes a rectangular effective portion that will later become the mother glass sheet 1 and ends that sandwich the effective portion and exist on both sides in the width direction. The ends include thick-walled ears. When the mother glass sheet 1 is produced, the effective portion is cut out by cutting off the ends from the glass sheet Gs. When the effective portion is cut out, for example, by forming a score line along the drawing direction of the glass sheet Gs (formed along the boundary between the effective portion and the end) and breaking and cutting along the score line, the ends at both ends in the width direction of the glass sheet Gs are cut off. In this way, the effective portion is cut out from the glass sheet Gs to obtain the mother glass sheet 1.
[0119] Here, the glass ribbon Gr is appropriately annealed by annealing in the above-mentioned annealing furnace 11, so that the predetermined shape accuracy can be obtained in the glass ribbon Gr and the mother glass sheet 1 obtained from the glass ribbon Gr. At this time, when the ambient temperature of the glass ribbon Gr changes over time in the annealing temperature region, the shape accuracy of the glass ribbon Gr (mother glass sheet 1) is affected. Therefore, the temperature in the annealing furnace 11 is kept constant by suppressing the change in the differential pressure between the chamber R1 surrounding the annealing furnace 11 and the cooling area 12 (the internal space of the cooling area 12 divided by the wall 15). Specifically, the fluctuation range of the differential pressure between the chamber R1 surrounding the annealing furnace 11 and the cooling area 12 is set to 0.5Pa to 1.5Pa. It should be noted that the "fluctuation range of the differential pressure" means the difference between the maximum value and the minimum value of the differential pressure between the chamber R1 surrounding the annealing furnace 11 and the cooling area 12 during the production of the mother glass sheet 1.
[0120] <Extraction process>
[0121] exist Fig.15 In the figure, a plurality of mother glass sheets 1 are arranged in the order in which they were produced in the production process P1. The mother glass sheets 1 that are arranged to the right are the mother glass sheets 1 that were produced earlier in the time series. From these mother glass sheets 1, the inspection mother glass sheets 8 that are to be measured for shape accuracy in the measurement process are extracted. The extraction process P2 is performed at predetermined intervals (e.g., 2 to 24 hours). That is, Fig.15 The left side of the two inspection mother glass plates 8 shown is the inspection mother glass plate 8 extracted after a predetermined time of the right side. Here, in the following description, there is a case where the inspection mother glass plate 8 on the right side extracted first is recorded as the previous inspection plate 8a, and the inspection mother glass plate 8 on the left side extracted later is recorded as the subsequent inspection plate 8b for distinction.
[0122] It should be noted that, when the forming conditions of the glass ribbon Gr are changed in the above-mentioned production process P1, it is preferable to make the time interval for executing the extraction process P2 shorter than the time interval before the change of the forming conditions. In addition, the number of sheets of the mother glass plate 8 for inspection (the number of sheets of the preceding inspection plate 8a and the number of sheets of the subsequent inspection plate 8b) extracted in one extraction process P2 may be one sheet as in the present embodiment, or may be a plurality of sheets.
[0123] <Measurement process>
[0124] In the measurement process, first, the previous inspection plate 8a is used as the object and Figure 1 As shown in FIG. 1 , a plurality of (seven in this embodiment) first evaluation regions 41 and width direction end regions 5 are set, and Figure 4 As shown in FIG. 1 , a plurality of (seven in this embodiment) second evaluation areas 42 are set, and Figure 5 A plurality of third evaluation areas 6 are set similarly to those shown in FIG. 1 (in this embodiment, 10 are set at one end side and the other end side in the width direction, for a total of 20). Figure 2 as well as Figure 3 A plurality of first evaluation areas 41 are set similarly as shown.
[0125] Next, the following [Step 1] to [Step 5] are performed on the previous inspection plate 8a.
[0126] [Step 1]: The front-back deflection difference d1 along the plate pulling direction and the width direction is measured for each of the seven first evaluation areas 41 (first evaluation areas A to G). The specific measurement procedure of the front-back deflection difference d1 is the same as the procedure described above. Thus, a total of 28 (14 in the plate pulling direction and 14 in the width direction) front-back deflection differences d1 are measured for one previous inspection plate 8a.
[0127] [Process 2]: The adjacent first evaluation areas 41, 41 are regarded as one group, and the change amount Δd1 of the front and back deflection difference d1 along the plate pulling direction and the width direction between the first evaluation areas 41, 41 is calculated in all 6 groups (group A, B, group B, C, ... group E, F, group F, G). The scheme for calculating the change amount Δd1 is the same as the scheme described above. Thus, a total of 24 (12 in the plate pulling direction and 12 in the width direction) changes Δd1 are calculated for a sheet of the previous inspection plate 8a. However, in [Process 2], only the change amount Δd1 of the front and back deflection difference d1 along the width direction may be calculated.
[0128] [Step 3]: The front-back deflection difference d2 along the plate pulling direction and the width direction is measured for each of the seven second evaluation areas 42 (second evaluation areas H to N). The specific measurement procedure of the front-back deflection difference d2 is the same as the procedure described above. Thus, a total of 28 (14 in the plate pulling direction and 14 in the width direction) front-back deflection differences d2 are measured for one previous inspection plate 8a.
[0129] [Process 4]: The corresponding first evaluation area 41 and the second evaluation area 42 are regarded as one group, and in all 7 groups (groups A and H, groups B and I, ... groups F and M, groups G and N), the change amount Δd2 of the front and back deflection difference d1 of the four sides of the first evaluation area 41 and the front and back deflection difference d2 of the corresponding four sides of the second evaluation area 42 is calculated. The scheme for calculating the change amount Δd2 is the same as the scheme described above. Thus, a total of 28 changes Δd2 are calculated for a sheet 8a for prior inspection. However, in [Process 4], only the change amount Δd2 of the front and back deflection difference d1 of the two sides along the pulling direction of the first evaluation area 41 and the front and back deflection difference d2 of the two sides along the pulling direction of the corresponding second evaluation area 42 can be calculated.
[0130] [Step 5]: The flatness of all third evaluation regions 6 is measured using an optical interferometer. The method for measuring the flatness is the same as that described above. Thus, a total of 20 flatness values are measured for one previous inspection plate 8a.
[0131] The above-mentioned measurement of the front and back deflection differences d1 and d2, calculation of the changes Δd1 and Δd2, and measurement of the flatness are performed for each of the plurality of inspection plates 8a when there are a plurality of plates.
[0132] Next, the subsequent inspection plate 8b is taken as the object, and the above-mentioned [Process 1] to [Process 5] are performed on the basis of setting the first evaluation area 41, the width direction end area 5, the second evaluation area 42, and the third evaluation area 6 in the same manner as the previous inspection plate 8a. Thus, for one subsequent inspection plate 8b, a total of 28 front and back deflection differences d1, a total of 28 front and back deflection differences d2, a total of 24 changes Δd1, a total of 28 changes Δd2, and a total of 20 flatness values are measured and calculated. Of course, in the case of a plurality of subsequent inspection plates 8b, the front and back deflection differences d1 and d2 are measured, the changes Δd1 and Δd2 are calculated, and the flatness is measured for each of the plurality of sheets.
[0133] Next, perform the following [Step 6].
[0134] [Step 6]: Calculate the change Δd3 of the front and back deflection difference d1 along the pulling direction and the width direction of the corresponding first evaluation areas 41, 41 (first evaluation areas A, between A, B, between B, ..., F, between F, G, between G) between the inspection mother glass plates 8, 8 (between the previous inspection plate 8a and the subsequent inspection plate 8b) extracted in the two consecutive extraction steps P2.
[0135] Here, in Fig.16 (the result of one of the two sides extending in the pulling direction) and Fig.17 An example of the change amount Δd3 is shown in (the result of one of the two sides extending in the width direction). Fig.16 as well as Fig.17 The solid line in the figure shows the measurement result of the front-back deflection difference d1 of the previous inspection plate 8a, and the dashed line in the figure shows the measurement result of the corresponding front-back deflection difference d1 of the subsequent inspection plate 8b. It should be noted that only the change Δd3 between the corresponding first evaluation areas A and A is shown in the two figures. When there is one sheet of the previous inspection plate 8a and one sheet of the subsequent inspection plate 8b, a total of 28 changes Δd3 are calculated (14 in the pulling direction and 14 in the width direction).
[0136] <Pass / Fail Judgment Process>
[0137] In the pass / fail judgment process, if all of the following [Criteria 1] to [Criteria 6] are met, the Fig.15The plurality of mother glass plates 1 within the range Z shown (the plurality of mother glass plates 1 sandwiched between the preceding inspection plate 8a and the subsequent inspection plate 8b) are deemed acceptable. That is, they are glass plates that satisfy the quality of the mother glass plate 1 as an HDD substrate. On the other hand, if any one of [reference 1] to [reference 6] is not satisfied, the plurality of mother glass plates 1 within the range Z are deemed unacceptable. That is, they are glass plates that do not satisfy the quality of the mother glass plate 1 as an HDD substrate.
[0138] [Criteria 1]: In both the preceding inspection plate 8a and the subsequent inspection plate 8b, the total front and back deflection differences d1 measured in [Process 1] fall within the range of ±0.5 mm (-0.5 mm ≤ d1 ≤ 0.5 mm). It should be noted that it is more preferred if the total front and back deflection differences d1 fall within the range of ±0.3 mm, further preferred if they fall within the range of ±0.2 mm, and most preferred if they fall within the range of ±0.1 mm.
[0139] [Criteria 2]: In both the preceding inspection plate 8a and the following inspection plate 8b, the total amount of change Δd1 calculated in [Process 2] is 0.3 mm or less (|Δd1|≤0.3 mm). It should be noted that it is more preferable if the total amount of change Δd1 is 0.2 mm or less, and even more preferable if it is 0.1 mm or less.
[0140] [Criteria 3]: In both the preceding inspection plate 8a and the subsequent inspection plate 8b, the total front and back deflection differences d2 measured in [Process 3] fall within the range of ±0.5 mm (-0.5 mm ≤ d2 ≤ 0.5 mm). It should be noted that it is more preferred if the total front and back deflection differences d2 fall within the range of ±0.3 mm, further preferred if they fall within the range of ±0.2 mm, and most preferred if they fall within the range of ±0.1 mm.
[0141] [Criteria 4]: In both the preceding inspection plate 8a and the following inspection plate 8b, the total amount of change Δd2 calculated in [Process 4] is 0.3 mm or less (|Δd2|≤0.3 mm). It should be noted that it is more preferable if the total amount of change Δd2 is 0.2 mm or less, and even more preferable if it is 0.1 mm or less.
[0142] [Criteria 5]: For both the preceding inspection plate 8a and the subsequent inspection plate 8b, the total flatness values measured in [Step 5] are 50 μm or less. It is more preferred that the total flatness values are 30 μm or less, more preferred that they are 20 μm or less, and most preferred that they are 10 μm or less.
[0143] [Criterion 6]: The total amount of change Δd3 calculated in [Step 6] is 0.3 mm or less (|Δd3|≤0.3 mm). It is more preferable that the total amount of change Δd3 is 0.2 mm or less, and even more preferable that it is 0.1 mm or less.
[0144] Here, in the present embodiment, all of [Step 1] to [Step 6] are executed in the measurement process, but the present invention is not limited thereto. Alternatively, only [Step 1] and [Step 6] may be required, and whether or not to execute the other [Step 2], [Step 3], [Step 4], and [Step 5] may be set to be optional. For example, [Step 2], [Step 3], [Step 4], and [Step 5] may be executed only when the forming conditions of the glass ribbon Gr in the production process P1 are changed, when the shape accuracy of the produced mother glass sheet 1 is considered to have a tendency to deteriorate (for example, when the absolute value |d1| of the front and back deflection difference d1 and the change amount Δd3 tend to increase).
[0145] It is possible that, in the measurement process, only [Process 1] and [Process 6] are set as required. In the pass / fail judgment process, if only [Criteria 1] and [Criteria 6] are satisfied, Fig.15 A plurality of mother glass plates 1 within the range Z shown are qualified. That is, the mother glass plates 1 can be glass plates satisfying the quality of the mother glass plates 1 as HDD substrates.
[0146] In addition, the present manufacturing method may further include a defect depth measuring step of measuring the depth of the defect 1d from the main surface (front surface 1a or back surface 1b) of the mother glass plate 1, and a defect evaluation step of evaluating the defect 1d based on the measured depth, for defects 1d represented by foreign matter, bubbles, etc. contained in the mother glass plate 1. When these two steps are performed, only the mother glass plates 1 that are further determined to be qualified according to the results of the defect evaluation step among the plurality of mother glass plates 1 that are determined to be qualified in the above-mentioned pass / fail judging step can be treated as glass plates that meet the quality of the mother glass plate 1 of the HDD substrate.
[0147] <Defect Depth Measurement Process>
[0148] In the defect depth measurement step, the depth of the defect 1d can be measured using various known measurement methods. For example, an image in which the defect 1d is most focused can be selected from images obtained by photographing the mother glass sheet 1 at multiple focal lengths, and the depth of the defect 1d from the main surface (the depth along the thickness direction of the mother glass sheet 1) can be calculated based on the focal position of the image.
[0149] <Defect evaluation process>
[0150] In the defect evaluation process, if the depth of the defect 1d measured in the defect depth measurement process is less than a specified value (for example, less than 25 μm, less than 20 μm, less than 15 μm, less than 10 μm, etc.), the defect 1d is determined to be a qualified defect regardless of the size and type of the defect 1d. At this time, a defect whose depth from one main surface is less than a specified value may be determined as a qualified defect, but it is preferred that a defect whose depth from one main surface is less than a specified value is determined as a qualified defect, and a defect whose depth from the other main surface is less than a specified value is determined as a qualified defect. In the case where the mother glass plate 1 has only a qualified defect, the mother glass plate 1 is determined to be qualified. On the other hand, in the case where the depth of the defect 1d is greater than a specified value, the defect 1d is determined to be a non-qualified defect. Thereafter, the pass or fail of the mother glass plate 1 is determined based on the number, size and type of non-qualified defects contained in the mother glass plate 1, and the mother glass plate 1 determined to be non-qualified is discarded. By performing such a defect evaluation step, it is possible to determine that the mother glass plate 1 having only acceptable defects satisfies the quality of the mother glass plate 1 as an HDD substrate, and the yield of the mother glass plate 1 can be improved.
[0151] Description of Reference Numerals
[0152] 1 Mother glass plate
[0153] 1a Surface (main surface)
[0154] 1b Back side (main side)
[0155] 1d Defect
[0156] 2 The first side of the mother glass
[0157] 3 Second side of the mother glass
[0158] 41 First evaluation area
[0159] 42 Second evaluation area
[0160] 5 Width end area
[0161] 6 The third evaluation area
[0162] 8 Mother glass plate for inspection
[0163] 8a Prior inspection board
[0164] 8b Subsequent inspection board
[0165] d1 Case and back deflection difference
[0166] Δd1 Change in the deflection difference between the front and back
[0167] d2 Differential deflection of case and back
[0168] Δd2 Change in the difference in deflection between the front and back
[0169] Δd3 Change in the difference in deflection between the front and back
[0170] P1 Production Process
[0171] P2 extraction process.
Claims
1. A method for manufacturing a mother glass plate, which is a method for manufacturing a mother glass plate for a hard disk drive, and comprises: The production process continuously produces mother glass sheets in a production line; An extraction step of extracting the mother glass plate for inspection from the production line; a measuring step of measuring the shape accuracy of the inspection mother glass sheet; and a pass / fail judging step of judging the pass / fail of the plurality of mother glass sheets produced in the production step based on the result of the measuring step, in, The mother glass plate is in a rectangular shape having a first side along a plate pulling direction and a second side along a width direction orthogonal to the plate pulling direction, and the length of each of the first side and the second side is greater than or equal to 1000 mm, and the thickness of the mother glass plate is greater than or equal to 0.3 mm and less than or equal to 0.7 mm, The extraction step is performed at predetermined intervals, and a plurality of rectangular first evaluation areas are arranged in a width direction of the effective portion and each of which has a side length of 300 mm or more and 700 mm or less, so as to fill the entire width of the effective portion of the extracted mother glass plate for inspection. The measuring process includes: a process of measuring the front and back deflection difference along the pulling direction and the width direction for each of the first evaluation areas among the multiple first evaluation areas; and a process of calculating the change amount of the front and back deflection difference between the corresponding first evaluation areas between the inspection mother glass plates extracted in two consecutive extraction processes.
2. The method for manufacturing a mother glass sheet according to claim 1, wherein: The measuring step further includes the step of calculating the amount of change in the front and back deflection difference between the first evaluation regions adjacent to each other in the width direction for each of the inspection mother glass plates.
3. The method for manufacturing a mother glass sheet according to claim 1 or 2, wherein: In the extraction step, a second evaluation region is further set corresponding to each of the plurality of first evaluation regions, the second evaluation region having the same width direction position as the first evaluation region and adjacent to the first evaluation region in the plate pulling direction. The measuring step further includes: measuring the front and back deflection difference along the plate pulling direction and the width direction for each second evaluation area; and calculating the change amount of the front and back deflection difference between the corresponding first evaluation area and the second evaluation area.
4. The method for manufacturing a mother glass sheet according to claim 1 or 2, wherein: In the extraction step, a plurality of third evaluation regions are further set for the width direction end regions in the extracted effective portion of the mother glass plate for inspection, and the width of the width direction end regions is less than 30% of the length of the second side. The measuring step further includes a step of measuring the flatness of each of the plurality of third evaluation regions using an optical interferometer.
5. The method for manufacturing a mother glass sheet according to claim 4, wherein: The third evaluation region has a rectangular shape with a side being not less than 50 mm and not more than 150 mm.
6. The method for manufacturing a mother glass sheet according to claim 4, wherein: The third evaluation area is a part of the first evaluation area.
7. The method for manufacturing a mother glass sheet according to claim 1 or 2, wherein: The mother glass sheet has defects inside, The method for manufacturing the mother glass sheet further includes: a defect depth measuring step of measuring a depth from a main surface of the mother glass sheet to the defect; and a defect evaluating step of evaluating the defect based on the measured depth.
8. A mother glass plate for a hard disk drive, wherein the mother glass plate is in a rectangular shape having a first side along a plate pulling direction and a second side along a width direction orthogonal to the plate pulling direction, wherein the first side and the second side are each longer than 1000 mm, and the thickness of the mother glass plate is greater than or equal to 0.3 mm and less than or equal to 0.7 mm. in, A plurality of rectangular first evaluation areas are set on the mother glass plate so as to fill the entire width of the effective portion of the mother glass plate. The sides of the plurality of first evaluation regions in the pulling direction are 500 mm and the sides of the plurality of first evaluation regions in the width direction are 400 mm, When the front and back deflection differences along the plate pulling direction and the width direction are measured for each of the first evaluation regions in all the first evaluation regions, the values of the front and back deflection differences are all within the range of ±0.5 mm, The above-mentioned difference in front and back deflection is a value converted into a 350 mm square size.
9. The mother glass sheet according to claim 8, wherein: The amount of change in the front and back deflection difference between the first evaluation regions adjacent to each other in the width direction of the mother glass sheet is 0.3 mm or less.
10. The mother glass sheet according to claim 8 or 9, wherein: The mother glass sheet further has second evaluation regions corresponding to each of the plurality of first evaluation regions, the second evaluation regions being located at the same width direction as the first evaluation regions and adjacent to the first evaluation regions in the pulling direction. When the front and back deflection differences along the plate pulling direction and the width direction are measured for each of the second evaluation regions, the values of the front and back deflection differences are all within the range of ±0.5 mm, The amount of change in the front and back deflection difference between the corresponding first evaluation area and the second evaluation area is 0.3 mm or less.
11. The mother glass sheet according to claim 8 or 9, wherein: In the mother glass plate, a plurality of third evaluation areas having a rectangular shape are set in a range where the distance from the first side is not more than 30% of the length of the second side. Each side of the third evaluation area is 100 mm. When the flatness of each of the third evaluation regions is measured using an optical interferometer, the flatness is 50 μm or less.
12. The mother glass sheet according to claim 8 or 9, wherein: The longitudinal elastic modulus of the mother glass plate is 80 GPa or more.
13. The mother glass sheet according to claim 8 or 9, wherein: The mother glass sheet has defects inside. The depth of the defect from the main surface of the mother glass plate is 25 μm or less.