Electromagnetic wave shielding material and method for producing same
By plating the shielding layer composed of zinc, nickel and chromium on the substrate of automotive electrical components, the existing electromagnetic wave shielding materials are solved, and the lightweight and efficient electromagnetic wave shielding effect is achieved. Automotive electrical components.
Patent Information
- Application Number
- CN202380034026.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-28
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-29
AI Technical Summary
The existing electromagnetic wave shielding materials have problems such as heavy weight and high manufacturing difficulty, especially in automotive electrical components, which are difficult to achieve lightweight and efficient shielding.
A shielding layer composed of zinc, nickel and chromium is plated on the substrate, and a multi-layer structure is formed by magnetron sputtering method, and the atomic ratio and thickness of zinc, nickel and chromium are controlled to achieve excellent electromagnetic wave shielding performance.
It realizes a lightweight electromagnetic wave shielding material, which is suitable for various materials, can effectively shield electromagnetic waves, reduce processing difficulty, and improve corrosion resistance and shielding performance.
Smart Images

Figure CN119054424A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an electromagnetic wave shielding material and a method for manufacturing the same, and in particular to an electromagnetic wave shielding material capable of shielding electromagnetic waves generated inside and outside a vehicle to prevent abnormal operation of electrical components used in the vehicle and a method for manufacturing the same. Background Art
[0002] Electromagnetic wave shielding is to prevent the noise generated inside electronic components from flowing out, or to shield electromagnetic wave noise from flowing in from electromagnetic waves generated by sunlight or pedestrians.
[0003] In particular, in order to prevent malfunction of electronic components that are sensitive to external electromagnetic waves, electromagnetic wave shielding is required, and various electromagnetic wave shielding technologies have been developed for this purpose.
[0004] In addition, with the development of the automobile industry, the number of electrical components installed in automobiles has continued to increase, but research and development of electromagnetic wave shielding technology that can prevent malfunction of electrical components that may cause safety accidents to drivers and pedestrians is still insufficient.
[0005] Such electrical components include automobile controllers, automobile motor housings, and air control valves (ACV) of hydrogen vehicles.
[0006] At present, in order to shield electromagnetic waves, domestic and foreign automobile manufacturers have developed the following technology: metal wires such as iron or aluminum, carbon nanotubes or carbon materials such as asphalt are included in the shell to shield electromagnetic waves generated inside and outside the vehicle. However, this technology has the disadvantages of increasing the weight of the entire shell and requiring processing such as corrosion protection.
[0007] In addition, when manufacturing a composite material capable of shielding electromagnetic waves by dispersing conductive fillers in a polymer matrix, it is difficult to evenly disperse the fillers in the polymer matrix, and the fillers increase the rigidity of the composite material, so there is a problem of increased difficulty in subsequent processing. Summary of the invention
[0008] Technical issues
[0009] The present invention is made to solve the problem that the existing electromagnetic wave shielding materials are heavy and difficult to manufacture, and its purpose is to provide an electromagnetic wave shielding material and a manufacturing method thereof that can achieve light weight and excellent compatibility with other materials.
[0010] Technical means
[0011] In order to achieve the above-mentioned purpose, the electromagnetic wave shielding material according to the present invention includes: a substrate; and a shielding layer plated on the surface of the substrate.
[0012] The shielding layer may include at least one selected from the group consisting of zinc (Zn), nickel (Ni), and chromium (Cr).
[0013] The shielding layer may be configured to contain zinc in an amount of 53 atomic % or more and 63 atomic % or less based on the total atomic number.
[0014] The shield layer may be configured to include 37 atomic % or more and 47 atomic % or less of nickel and chromium with respect to the total atomic number, and the atomic ratio of the nickel to the chromium may be 1:1.
[0015] The shielding layer may have a thickness of 0.1 μm or more and 5 μm or less.
[0016] The shielding layer may exhibit electromagnetic wave shielding of 40 dB / μm or more and 55 dB / μm or less at 0.5 GHz.
[0017] In addition, the manufacturing method of the electromagnetic wave shielding material of the present invention is a method of plating an electromagnetic wave shielding layer on the surface of a substrate, comprising: a substrate placement step of placing the substrate in a reaction chamber; and a shielding layer formation step of laminating the shielding layer on the outer peripheral surface of the substrate.
[0018] The shield layer forming step may include: a first metal lamination step of sputtering a substance from a first target including zinc toward the substrate; and a second metal lamination step of sputtering a substance from a second target including nickel and chromium toward the substrate.
[0019] The second target material may be configured such that the atomic ratio of nickel to chromium is 1:1.
[0020] The shielding layer may be configured to contain zinc in an amount of 53 atomic % or more and 63 atomic % or less based on the total atomic number.
[0021] The shield layer may be configured to include 37 atomic % or more and 47 atomic % or less of nickel and chromium with respect to the total atomic number, and the atomic ratio of the nickel to the chromium may be 1:1.
[0022] In the first metal lamination step, a power of 240 W or more and 250 W or less may be applied to the first target.
[0023] In the second metal lamination step, power of 160 W or more and 190 W or less may be applied to the second target.
[0024] Effects of the Invention
[0025] The electromagnetic wave shielding material and the method for producing the same according to the present invention as described above can effectively shield electromagnetic waves flowing out of or into electrical components, and can achieve overall lightness and be applicable to various materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a schematic diagram showing a state in which a filler made of a conductive material is dispersed in a polymer matrix in a conventional electromagnetic wave shielding material.
[0027] Figure 2 is a schematic diagram of a cross section of an electromagnetic wave shielding material according to a first embodiment of the present invention.
[0028] Figure 3 This is a photograph of a cross section of the electromagnetic wave shielding material according to the first embodiment of the present invention taken with a scanning electron microscope (SEM).
[0029] Figure 4 This is a flowchart for explaining a method for producing an electromagnetic shielding material according to a second embodiment of the present invention. DETAILED DESCRIPTION
[0030] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings.
[0031] The present invention can be subjected to various modifications and can have a variety of embodiments, and specific embodiments are illustrated in the drawings and specifically described in the detailed description. It should be interpreted that this is not intended to limit the present invention to a specific embodiment, including all changes, equivalents and substitutes included in the concept and technical scope of the present invention.
[0032] When describing the present invention, although the terms "first" and "second" are used when describing various components, the above components may not be limited to the above terms. The purpose of the above terms is only to distinguish one component from other components. For example, without departing from the scope of the present invention, the first component may be named as the second component, and similarly, the second component may also be named as the first component.
[0033] The term "and / or" may include a combination of a plurality of related items or any one of the plurality of related items.
[0034] When a certain component is described as being “connected” or “connected” to another component, it may be directly connected or connected to the other component, but it can be understood that other components may exist in between. Conversely, when a certain component is described as being “directly connected” or “directly connected” to another component, it can be understood that other components do not exist in between.
[0035] The terms used in this application are used only to describe specific embodiments and are not intended to limit the present invention. Unless the context clearly indicates a different meaning, a single expression may also include a plurality of expressions.
[0036] In the present application, terms such as "including" or "having" are used to specify the existence of features, numbers, steps, actions, constituent elements, parts or combinations thereof recorded in the specification, and can be understood as not excluding in advance the possibility of the existence or addition of one or more other features or numbers, steps, actions, constituent elements, parts or combinations thereof.
[0037] Unless defined differently, all terms used herein, including technical or scientific terms, may have the same meaning as generally understood by those skilled in the art. Terms that are the same as terms defined in generally used dictionaries may be interpreted as having the same meaning as that in the context of the relevant technology, and may not be interpreted as having an ideal or overly formal meaning unless explicitly defined in this application.
[0038] The following embodiments are provided for more complete description to those skilled in the art. For a clearer description, the shapes and sizes of elements in the drawings may be exaggerated.
[0039] Figure 1 This is a schematic diagram showing a state in which a filler made of a conductive material is dispersed in a polymer matrix in a conventional electromagnetic wave shielding material.
[0040] Reference Figure 1 The existing electromagnetic wave shielding material is composed of a polymer matrix 1 such as polyethylene (PE), polypropylene (PP), polycarbonate (PC) and the like, filled with fillers 2 such as metal nanowires, carbon black, and carbon nanotubes.
[0041] However, there are problems in that it is difficult to uniformly disperse the filler 2 inside the polymer matrix 1 and when the filler 2 is reinforced in the polymer matrix 1 , the processability of the polymer matrix 1 is deteriorated.
[0042] Figure 2is a schematic diagram of a cross section of an electromagnetic wave shielding material according to a first embodiment of the present invention. Figure 3 This is a photograph of a cross section of the electromagnetic wave shielding material according to the first embodiment of the present invention taken with a scanning electron microscope (SEM).
[0043] See also Figure 2 An electromagnetic wave shielding material according to an embodiment of the present invention includes a substrate 10 and a shielding layer 20 plated on a surface of the substrate 10 .
[0044] The shielding layer 20 includes at least one selected from the group consisting of zinc (Zn), nickel (Ni), and chromium (Cr). The most preferred shielding layer 20 includes Zn-NiCr which is lightweight and has excellent shielding performance.
[0045] Specifically, in order to prevent electromagnetic waves from flowing into the substrate 10 from the outside or flowing out from the inside of the substrate 10 to the outside, a shielding layer 20 is plated on one side of the substrate 10, thereby providing an electromagnetic wave shielding material having a multi-layer structure.
[0046] Although the substrate 10 is shown as a flat surface in the first embodiment, it is not limited thereto and may include various shapes such as a curved surface corresponding to the shape of an automotive electrical component.
[0047] The material of the substrate 10 may be plastic such as polyethylene (PE), polypropylene (PP), polycarbonate (PC), or ceramic such as glass, alumina, zeolite, or a composite material thereof, but is not limited thereto.
[0048] At this time, the shielding layer 20 can be formed by a physical deposition method, preferably a physical vapor deposition (PVD) method.
[0049] The above-mentioned physical vapor deposition method can be achieved by using various methods such as arc ion plating (AIP), sputtering, laser evaporation (PLD) using laser, etc. In this embodiment, magnetron sputtering is used, but it is not limited to this. The above-mentioned shielding layer 20 can be formed using existing physical vapor deposition methods.
[0050] For example, as in the embodiment of the present invention, a sputtering voltage is applied to a zinc target by a PVD device using magnetron sputtering, and the sputtered zinc atoms are deposited on the substrate 10 .
[0051] After the zinc atoms are deposited on the substrate 10 , a sputtering voltage is applied to the nickel-chromium target by using the magnetron sputtering PVD equipment, and the sputtered nickel atoms and chromium atoms are deposited on the substrate 10 to form a Zn—NiCr shielding layer 20 .
[0052] The nickel-chromium target material has a composition of nickel and chromium in an atomic ratio of 1:1.
[0053] The shielding layer 20 contains zinc in an amount of 53 atomic % or more and 63 atomic % or less based on the total atomic number.
[0054] When the content of zinc in the shielding layer 20 is less than 53 atomic % relative to the total atomic number, the shielding performance of the shielding layer 20 is reduced and it cannot fully shield electromagnetic waves incident from the outside, which may cause malfunction of internal electrical components.
[0055] In addition, when the content of zinc in the shield layer 20 is greater than 63 atomic % relative to the total atomic number, although the shielding performance of the shield layer 20 is improved, the corrosion resistance to the external environment is reduced, so there is a problem of reduced long-term shielding stability.
[0056] The shield layer 20 includes nickel and chromium in an amount of 37 atomic % or more and 47 atomic % or less based on the total atomic number, and the atomic ratio of the nickel to the chromium is 1:1.
[0057] In the shielding layer 20, when the content of nickel and chromium is less than 37 atomic % relative to the total atomic number, the corrosion potential decreases, and the tendency to be corroded in the external environment increases, resulting in a decrease in the long-term electromagnetic wave shielding characteristics.
[0058] On the other hand, when the content of nickel and chromium exceeds 47 atomic % based on the total atomic number, the corrosion potential increases and the corrosion resistance improves, but the ability to shield electromagnetic waves flowing in from the outside decreases.
[0059] When the thickness of the shielding layer 20 is formed to be not less than 0.1 μm and not more than 5 μm, it is the thickness in the optimal range for shielding electromagnetic waves entering from the outside while maintaining the weight.
[0060] When the thickness of the shielding layer 20 is less than 0.1 μm, the attenuation of electromagnetic waves flowing in from the outside or electromagnetic waves moving from the inside to the outside is reduced, which may cause malfunction of internal electrical components.
[0061] In addition, when the thickness of the shielding layer 20 is greater than 5 μm, the electromagnetic wave shielding effect is slightly increased, the plating time required to form the shielding layer 20 is increased, a brittle columnar structure is formed, and the residual stress in the layer is increased.
[0062] The shielding layer 20 exhibits electromagnetic wave shielding of 40 dB / μm or more and 55 dB / μm or less at 0.5 GHz.
[0063] According to the electromagnetic absorption rate (SAR) standard stipulated in Announcement No. 2019-4 issued by the Ministry of Science, Technology and Information Communications, the electromagnetic waves radiated to ordinary people in the range of 100kHz to 10GHz are stipulated as follows: 0.08W / kg for the whole body, 1.6W / kg for the head and trunk, and less than 4W / kg for the limbs, and the measurement was carried out at 0.5GHz as an arbitrary value within the range.
[0064] When the shielding layer 20 shows a shielding performance of less than 40 dB / μm at 0.5 GHz, it may cause malfunction of electrical components inside the electromagnetic wave shielding material, and the electromagnetic waves radiated from the electrical components cannot be sufficiently reduced, which may have a bad effect on the health of ordinary people.
[0065] In addition, when the shielding layer 20 shows a performance greater than 55 dB / μm at 0.5 GHz, the further electromagnetic wave shielding effect is very small, the amount of electromagnetic wave shielding material consumed increases, and the economic efficiency deteriorates.
[0066] Below, refer to Figure 4 , a method for manufacturing an electromagnetic wave shielding material based on the second embodiment of the present invention is described in accordance with each step.
[0067] Reference Figure 4 In order to laminate the shielding layer 20 on the surface of the substrate 10, the method for manufacturing the electromagnetic wave shielding material based on the second embodiment of the present invention includes: a substrate placing step (S10) of placing the above-mentioned substrate 10 inside the reaction chamber; and a shielding layer forming step (S50) of laminating the shielding layer 20 on the outer peripheral surface of the above-mentioned substrate 10.
[0068] In the substrate placement step ( S10 ), the substrate 10 is placed in a reaction chamber of a PVD device using magnetron sputtering. The substrate 10 can be placed using a jig (not shown) for placing the substrate 10 .
[0069] Specifically, the base material 10 may be fixed by applying an attractive force based on a magnetic field to the base material 10 formed of a metal material using a jig equipped with a magnet.
[0070] The shielding layer forming step (S50) includes: a first metal lamination step (S51) of sputtering a substance from a first target including zinc toward the substrate 10; and a second metal lamination step (S52) of sputtering a substance from a second target including nickel and chromium toward the substrate 10.
[0071] In the second target material, the atomic ratio of nickel to chromium is 1:1.
[0072] The shielding layer 20 contains zinc in an amount of 53 atomic % or more and 63 atomic % or less based on the total atomic number.
[0073] When the content of zinc in the shielding layer 20 is less than 53 atomic % relative to the total atomic number, the shielding performance of the shielding layer 20 is reduced and electromagnetic waves incident from the outside cannot be sufficiently shielded, which may cause malfunction of internal electrical components.
[0074] In addition, when the content of zinc in the shield layer 20 is greater than 63 atomic % relative to the total atomic number, although the shielding performance of the shield layer 20 is improved, the corrosion resistance to the external environment is reduced, so there is a problem of reduced long-term shielding stability.
[0075] The shield layer 20 includes nickel and chromium in an amount of 37 atomic % or more and 47 atomic % or less based on the total atomic number, and the atomic ratio of the nickel to the chromium is 1:1.
[0076] In the shielding layer 20, when the content of nickel and chromium is less than 37 atomic % relative to the total atomic number, the corrosion potential decreases, and the tendency to be corroded in the external environment increases, resulting in a decrease in the long-term electromagnetic wave shielding characteristics.
[0077] In addition, when the solder content of nickel and chromium is greater than 47 atomic % relative to the total atomic number, the corrosion potential increases and the corrosion resistance improves, but the ability to shield electromagnetic waves flowing in from the outside decreases.
[0078] In the first metal lamination step ( S51 ), a power of 240 W or more and 250 W or less is applied to the first target.
[0079] When the amount of electric power applied to the first target is less than 240 W, the amount of zinc sputtered from the first target is reduced, and the shielding amount of the shield layer 20 against electromagnetic waves flowing in from the outside is reduced.
[0080] When the amount of electric power applied to the first target is greater than 250 W, the amount of zinc sputtered from the first target increases, and the electromagnetic wave shielding capability of the shielding layer 20 increases, but the corrosion resistance decreases.
[0081] In addition, in the second metal lamination step (S52), an electric power of 160 W or more and 190 W or less is applied to the second target.
[0082] When the amount of electric power applied to the second target is less than 160 W, the amount of nickel and chromium sputtered from the second target is reduced, and there is a problem that the corrosion resistance of the shield layer 20 is reduced.
[0083] When the amount of power applied to the second target is greater than 190 W, the amount of nickel and chromium sputtered from the second target increases, the corrosion resistance of the shielding layer 20 increases, but the shielding amount against electromagnetic waves flowing from the outside decreases.
[0084] In addition, the manufacturing method of the electromagnetic wave shielding material based on the second embodiment of the present invention, after the above-mentioned substrate placement step (S10), also includes: a vacuum forming step (S20), in which the internal atmosphere of the above-mentioned reaction chamber is maintained in a vacuum state when the above-mentioned substrate 10 is arranged inside the above-mentioned reaction chamber; a plasma forming step (S30), in which Ar gas is injected into the interior of the above-mentioned reaction chamber to increase the temperature of the chamber to form a plasma state for generating Ar ions; and a cleaning step (S40), in which the above-mentioned Ar ions collide with the surface of the above-mentioned substrate 10 to clean the surface of the above-mentioned substrate 10.
[0085] In the vacuum forming step ( S20 ), a jig carrying the substrate 10 is disposed inside the reaction chamber to form and maintain the internal atmosphere of the reaction chamber in a vacuum state.
[0086] Next, in the plasma forming step (S30), argon (Ar) gas is supplied as a process gas, and the temperature is increased by a constant temperature device to form a plasma state in which Ar ions are formed inside the reaction chamber.
[0087] Thereafter, in the cleaning step ( S40 ), a bias voltage is applied to the bias electrode to accelerate Ar ions and cause them to collide with the surface of the substrate 10 , thereby cleaning the surface of the substrate 10 .
[0088] This is to preferentially perform an etching step for removing an oxide layer and impurities naturally formed on the surface of the substrate 10 , thereby improving adhesion between the electromagnetic wave shielding layer 20 and the substrate 10 .
[0089] In this case, the bias voltage can be maintained in the range of 200 V to 400 V. If the bias voltage is less than 200 V, the acceleration voltage of Ar ions decreases, and the hardness of the shielding material decreases. If the bias voltage exceeds 400 V, the lattice arrangement becomes irregular, which may cause the problem of reduced adhesion of the shielding material.
[0090] Hereinafter, the comparison results of physical property evaluation between Examples produced by the method for producing an electromagnetic shielding material according to the present invention will be described.
[0091] Example
[0092] First, a flat plate-shaped substrate 10 is placed inside a reaction chamber of a sputtering device. While maintaining a vacuum inside the reaction chamber, an Ar gas is used to create a plasma state, and the inside of the chamber is heated to 80°C to activate the surface of the substrate formed of SUS440C stainless steel. Then, a bias voltage of 300V is applied to cause Ar ions to collide with the surface of the substrate 10, thereby cleaning the surface of the substrate 10.
[0093] After the surface of the substrate 10 is cleaned, a first metal lamination step ( S51 ) is performed in which a predetermined power is applied to a first target including zinc by magnetron sputtering to sputter metal atoms including zinc toward the substrate 10 .
[0094] After executing the above-mentioned first metal stacking step (S51), the second metal stacking step (S52) is executed to manufacture Examples 1 to 7. In the second metal stacking step (S52), a predetermined electric power is applied to a second target material containing nickel and chromium (the atomic ratio of nickel to chromium is 1:1) by magnetron sputtering, and metal atoms containing nickel and chromium are sputtered onto the above-mentioned substrate 10.
[0095] Table 1 shows the power applied to form and accelerate plasma in the first target and the second target and the composition ratio (Zn—NiCr) of the shield layer 20 .
[0096]
Table 1
[0097]
[0098]
[0099] Shielding performance evaluation
[0100] First, in order to evaluate the surface resistance of the shielding layer 20 , measurement was performed using a four-point probe.
[0101] Generally, the surface resistance can be obtained by applying a certain voltage to the sample and measuring the current flowing through the sample. The surface resistance is proportional to the applied voltage (V) and the length (L) of the sample, and inversely proportional to the current flowing through the sample (I) and the width (W) of the sample. The detailed measurement method can refer to the known technology, so the detailed description is omitted.
[0102] Then, in order to evaluate the shielding performance of the shielding layer, the shielding performance of the shielding layer 20 of Examples 1 to 7 was compared at 0.5 GHz according to the international standard for automotive narrowband radiation (CISPR25) established by the International Special Committee on Radio Interference (CISPR).
[0103] Corrosion resistance evaluation
[0104] Furthermore, in order to evaluate the corrosion resistance of the shield layer 20, the corrosion potential and the corrosion current density were evaluated using a constant potential / constant current device (AMETEK PARSTAT4000A).
[0105] Specifically, using an AgCl / KCl electrode as a reference electrode and Pt as a counter electrode, the measurement was performed in a 3.5 mass % sodium chloride solution at an injection rate of 1 mV / s in a range of -0.8 V to 0.4 V.
[0106]
Table 2
[0107]
[0108]
[0109] According to the shielding performance evaluation results in Table 2 above, it was confirmed that as the zinc ratio in the shielding layer 20 increased, the resistivity decreased from 2.7Ω / sq. (Example 1) to 0.6Ω / sq. (Example 7), while the shielding performance increased from 37dB (Example 1) to 52dB (Example 7).
[0110] In addition, the corrosion resistance evaluation results confirmed that as the zinc ratio in the shielding layer 20 increased, the corrosion potential relative to the reference electrode (Ag / AgCl) decreased from -0.383 V (Example 1) to -0.481 V (Example 7), while the corrosion current density increased from 0.59 μA (Example 1) to 14.93 μA (Example 7).
[0111] The results show that the shielding layer 20 containing more than 53 atomic % and less than 63 atomic % of zinc and more than 37 atomic % and less than 47 atomic % of nickel-chromium (the atomic ratio of nickel and chromium is 1:1) not only has sufficient shielding performance but also has significantly improved corrosion resistance.
[0112] Although the present invention has been described in detail above through specific embodiments, this is for the purpose of specifically illustrating the present invention and the present invention is not limited thereto. It is clear that the present invention can be modified or improved by those skilled in the art within the technical concept of the present invention.
[0113] Simple modifications and changes of the present invention are within the scope of the present invention, and the specific protection scope of the present invention will be clarified by the claims.
Claims
1. An electromagnetic wave shielding material, in, The electromagnetic wave shielding material comprises: substrate; and A shielding layer plated on the surface of the substrate, The shielding layer includes at least one selected from the group consisting of zinc (Zn), nickel (Ni), and chromium (Cr).
2. The electromagnetic wave shielding material according to claim 1, in, The shielding layer contains zinc in an amount of 53 atomic % or more and 63 atomic % or less based on the total number of atoms.
3. The electromagnetic wave shielding material according to claim 1, in, The shielding layer contains nickel and chromium in an amount of 37 atomic % or more and 47 atomic % or less relative to the total atomic number, and the atomic ratio of the nickel to the chromium is 1:
1.
4. The electromagnetic wave shielding material according to claim 1, in, The shielding layer has a thickness of 0.1 μm or more and 5 μm or less.
5. The electromagnetic wave shielding material according to claim 1, in, The shielding layer exhibits electromagnetic wave shielding of 40 dB / μm or more and 55 dB / μm or less at 0.5 GHz.
6. A method for producing an electromagnetic wave shielding material, which comprises plating an electromagnetic wave shielding layer on the surface of a substrate. include: A substrate placement step of placing the substrate in a reaction chamber; as well as A shield layer forming step is to laminate a shield layer on the outer peripheral surface of the substrate.
7. The method for producing an electromagnetic wave shielding material according to claim 6, in, The shielding layer forming step comprises: A first metal layering step of sputtering a substance from a first target comprising zinc toward the substrate; and A second metal deposition step of sputtering a substance toward the substrate from a second target comprising nickel and chromium.
8. The method for producing an electromagnetic wave shielding material according to claim 7, in, The atomic ratio of nickel to chromium in the second target is 1:
1.
9. The method for producing an electromagnetic wave shielding material according to claim 6, in, The shielding layer contains zinc in an amount of 53 atomic % or more and 63 atomic % or less based on the total number of atoms.
10. The method for producing an electromagnetic wave shielding material according to claim 6, in, The shielding layer contains nickel and chromium in an amount of 37 atomic % or more and 47 atomic % or less relative to the total atomic number, and the atomic ratio of the nickel to the chromium is 1:
1.
11. The method for producing an electromagnetic wave shielding material according to claim 7, in, In the first metal lamination step, a power of 240 W or more and 250 W or less is applied to the first target.