Release agent as well as preparation method and application thereof

The mold release agent is prepared by heating with a combination of vegetable oil and water, and combined with emulsifier and wax, which solves the problem of poor stability of existing mold release agents, improves the mold release effect and shelf life, and reduces the defective rate and stratification risk.

CN119054902APending Publication Date: 2024-12-03ANGEL YEAST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411283059.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing mold release agent has poor stability in the electrode baking process, which is prone to mold growth and stratification, resulting in poor mold release effect and increasing the defective rate of bread.

Method used

Using a combination of vegetable oil, water, emulsifier, wax and alcohol, the mold release agent is prepared by mixing heating and cooling to ensure its stability and anticorrosion, and prevent delamination by polyglycerol fatty acid esters, carnauba wax prevents adhesion, alcohol Extend the shelf life.

Benefits of technology

It improves the stability and release effect of the mold release agent, increases the yield rate, prevents the product from adhesion with the mold, extends the shelf life, and reduces the risk of stratification and mold growth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005042867030000091
    Figure BDA0005042867030000091
  • Figure BDA0005042867030000101
    Figure BDA0005042867030000101
Patent Text Reader

Abstract

The invention belongs to the technical field of release agents, and particularly relates to a release agent and a preparation method and application thereof. The release agent comprises the following components in percentage by weight: 43-50% of vegetable oil, 40-50% of water, 1-5% of an emulsifier, 0.1-4% of wax and 0.1-6% of alcohol. The polyglycerol fatty acid ester and the wax are mixed through the vegetable oil, water and alcohol at the same temperature are added at a certain temperature, the prepared release agent is stable and not layered, and when the release agent is applied to preparation of electrode cured bread, the release effect is improved, and the yield is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of mold release agents, and in particular relates to a mold release agent and a preparation method and application thereof. Background Art

[0002] A release agent is a food processing aid, which is commonly used in the baking production of various Chinese and Western foods such as bread, cakes, moon cakes and biscuits. It can form an oil mold between the dough and the metal baking mold to prevent the dough from adhering to the mold during the baking process, which is beneficial for the demoulding of the finished product. It is an indispensable food processing aid in the industrial production of baked products.

[0003] In the process of baking bread in a bakery, a lot of bread crumbs stick to the mold when the bread is demoulded, which not only wastes manual cleaning but also increases the defective rate of bread. However, the ratio and combination of the main components of the water-based demoulding agent in the prior art are limited, resulting in poor demoulding effect in bread baked by the electrode method. Therefore, a new solution is needed to solve the above problems. Summary of the invention

[0004] The technical problem to be solved by the present invention is that the release agent in the prior art has poor stability and is prone to mold growth and stratification, resulting in poor demoulding effect in bread baked in the electrode method.

[0005] In view of the deficiencies in the prior art, one of the objects of the present invention is to provide a release agent, a second object of the present invention is to provide a method for preparing the release agent, and a third object of the present invention is to provide an application of the release agent in baked goods.

[0006] In view of the above technical problems, the present invention provides a release agent and a preparation method and application thereof.

[0007] Specifically, the present invention provides the following technical solutions:

[0008] In a first aspect, the present invention provides a release agent, which comprises, by weight of the release agent, 43-50% vegetable oil, 40-50% water, 1-5% emulsifier, 0.1-4% wax and 0.1-6% alcohol.

[0009] Preferably, based on the weight of the release agent, the vegetable oil is 45-50%; and / or water is 43-46%; and / or emulsifier is 2-5%; and / or wax is 0.5-4%; and / or alcohol is 2-5%.

[0010] Preferably, based on the weight of the release agent, the composition further comprises: 0.1-0.6% gum arabic, preferably 0.1-0.3% gum arabic.

[0011] Preferably, the vegetable oil is one or more of rapeseed oil, soybean oil, sunflower oil and palm oil; preferably, the vegetable oil is one or a combination of rapeseed oil and soybean oil.

[0012] Preferably, based on the weight of the release agent, rapeseed oil is 45-50%, and / or soybean oil is 43-50%.

[0013] Preferably, the wax is one or a combination of carnauba wax and sunflower wax.

[0014] Preferably, based on the weight of the release agent, the carnauba wax is 0.1-4%, and / or the sunflower wax is 0.1-4%.

[0015] Preferably, the emulsifier is polyglycerol fatty acid ester.

[0016] In a second aspect, the present invention provides a method for preparing the release agent, comprising the following preparation steps:

[0017] (1) mixing, heating and homogenizing vegetable oil, emulsifier and wax to obtain an oil solution;

[0018] (2) heating water and alcohol, mixing the mixture with the oil solution obtained in step (1), and cooling the mixture to obtain a release agent.

[0019] Preferably, the preparation comprises the following steps:

[0020] (1) mixing, heating and homogenizing vegetable oil, emulsifier and wax to obtain an oil solution;

[0021] (2) heating water, gum arabic and alcohol, mixing the mixture with the oil solution obtained in step (1), and cooling the mixture to obtain a release agent.

[0022] Preferably, in step (1), the homogenization pressure is 20-50 MPa.

[0023] Preferably, the heating temperature is 75-80°C.

[0024] Preferably, cooling is to 25-30°C.

[0025] In a third aspect, the present invention provides a release agent, which is prepared by the preparation method.

[0026] Preferably, the viscosity of the release agent is greater than or equal to 800 Pa·s and less than or equal to 900 mPa·s; and / or the demoulding rate of the release agent is greater than or equal to 95% and less than or equal to 100%; and / or the delamination rate of the release agent is greater than or equal to 0% and less than or equal to 10%.

[0027] In a fourth aspect, the release agent provided by the present invention is used in the field of baking, preferably in the field of bread baking.

[0028] Beneficial effects of the present invention:

[0029] (1) The present invention mixes polyglycerol fatty acid ester and wax with vegetable oil, and then adds water and alcohol at the same temperature at a certain temperature. The prepared release agent is stable and does not stratify. When used in the preparation of electrode cooked bread, the release effect is improved and the yield rate is increased.

[0030] (2) The present invention determines the smoke point and solidification point of the release agent by using vegetable oil, and prevents the product from sticking to the mold by adding wax, thereby improving the demoulding effect and increasing the yield rate.

[0031] (3) The present invention prevents the liquid from emulsifying and stratifying by adding polyglycerol fatty acid ester, which facilitates the spraying of the release agent equipment.

[0032] (4) The present invention prolongs the shelf life of the release agent by adding alcohol, making it less likely to grow mold, thereby achieving an anti-corrosion effect. DETAILED DESCRIPTION

[0033] In order to better understand the above technical solution, the technical solution of the present invention is clearly and completely explained in conjunction with the specific implementation method below. It should be noted that the content in the specific implementation method is only a specific implementation and explanation of the technical solution of the present invention, and should not be understood as limiting the scope of protection of the present invention.

[0034] The invention mixes polyglycerol fatty acid ester and wax by vegetable oil, adds water and alcohol at the same temperature at a certain temperature, stirs and rapidly cools down after emulsification to obtain a stable release agent, and also solves the problems of easy delamination and easy mold growth.

[0035] In some specific embodiments, the present invention provides a release agent, which comprises, based on the weight of the release agent, 43-50% vegetable oil, 40-50% water, 1-5% emulsifier, 0.1-4% wax and 0.1-6% alcohol.

[0036] In some specific embodiments, the emulsifier is a polyglycerol fatty acid ester. Polyglycerol fatty acid ester is mainly obtained by esterification reaction with polyglycerol and fatty acid as raw materials. The polyglycerol fatty acid ester used in the present invention includes: one or more of dipolyglycerol fatty acid ester, tripolyglycerol fatty acid ester, tetrapolyglycerol fatty acid ester, pentapolyglycerol fatty acid ester, hexapolyglycerol fatty acid ester, heptapolyglycerol fatty acid ester, octapolyglycerol fatty acid ester, ninepolyglycerol fatty acid ester and tenpolyglycerol fatty acid ester. Preferably, the polyglycerol fatty acid ester used in the present invention is one or more of dipolyglycerol fatty acid ester, tripolyglycerol fatty acid ester and tetrapolyglycerol fatty acid ester. More preferably, the polyglycerol fatty acid ester used in the present invention is one or more of dipolyglycerol monostearate, tripolyglycerol monostearate and tetrapolyglycerol monostearate, and further more preferably, the polyglycerol fatty acid ester used in the present invention is a mixture of any proportion of dipolyglycerol monostearate, tripolyglycerol monostearate and tetrapolyglycerol monostearate.

[0037] In some specific embodiments, the vegetable oil content can be 43%, 43.5%, 44%, 44.5%, 45%, 45.5%, 46%, 46.5%, 47%, 47.5%, 48%, 48.5%, 49%, 49.5% or 50% by weight of the release agent, or the vegetable oil content within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges as long as the release agent with the desired performance of the present invention can be obtained.

[0038] In some specific embodiments, the water content can be 40%, 40.5%, 41%, 41.5%, 42%, 42.5%, 43%, 43.5%, 44%, 44.5%, 45%, 45.5%, 46%, 46.5%, 47%, 47.5%, 48%, 48.5%, 49%, 49.5% or 50% by weight of the release agent, or a water content within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as a release agent with the desired performance of the present invention can be obtained.

[0039] In some specific embodiments, the emulsifier content can be 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5% by weight of the release agent, or the emulsifier content within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the release agent with the desired performance of the present invention can be obtained.

[0040] In some specific embodiments, the wax content can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.3%, 1.5%, 1.7%, 2%, 2.3%, 2.5%, 2.7%, 3, 3.3, 3.5%, 3.7% or 4% by weight of the release agent, or the wax content within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the release agent with the desired performance of the present invention can be obtained.

[0041] In some specific embodiments, the alcohol content can be 0.1%, 0.5%, 1%, 1.3%, 1.5%, 1.7%, 2%, 2.3%, 2.5%, 2.7%, 3%, 3.3%, 3.5%, 3.7%, 4%, 4.3%, 4.5%, 4.7%, 5%, 5.3%, 5.5%, 5.7% or 6% by weight of the release agent, or an alcohol content within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges as long as a release agent with the desired performance of the present invention can be obtained.

[0042] In order to better understand the technical solution of the present invention, the technical solution of the present invention is described in detail below in conjunction with specific embodiments.

[0043] Unless otherwise specified, the various reagents / instruments used in the examples and comparative examples of the present invention are conventional commercially available products. The experimental materials and instrument information used in the present invention are shown in the following table:

[0044] Table 1 Experimental materials / instruments and manufacturers

[0045] Reagents / Instruments Purity / Model Manufacturer / seller Rapeseed Oil Level 1 Yihai Kerry Golden Dragon Fish Cereals, Oils and Foodstuffs Co., Ltd. Soybean Oil Level 1 Yihai Kerry Golden Dragon Fish Cereals, Oils and Foodstuffs Co., Ltd. Polyglycerol fatty acid esters PGE55-M Danisco (China) Co., Ltd. Gum Arabic Sundar Biopolymers Ltd. Carnauba wax Shanghai Yiba Chemical Raw Materials Co., Ltd. Sunflower wax Guangzhou Hatsube Chemical Co., Ltd. Alcohol 99% Anhui Ante Food Co., Ltd. Heating mixing tank Guangzhou Sipuxin Light Industry Machinery Co., Ltd. High pressure homogenizer APV-1000 Shanghai Shunyi Experimental Equipment Co., Ltd. Viscometer Brookfield

[0046] Example 1

[0047] Example 1 provides a release agent, which includes: 45.8 g rapeseed oil, 45 g water, 3 g polyglycerol fatty acid ester, 1 g carnauba wax, 5 g alcohol and 0.2 g gum arabic.

[0048] The release agent is prepared by a method comprising the following steps:

[0049] (1) mixing the rapeseed oil, polyglycerol fatty acid ester and carnauba wax in the above mass ratio, heating the mixture to 80° C., and homogenizing the mixture under a pressure of 30 MPa to obtain an oil solution;

[0050] (2) heating the water, gum arabic and alcohol in the above mass proportion to 80° C., mixing them evenly with the oil solution obtained in step (1), and then cooling them to 30° C. to obtain a release agent.

[0051] Example 2

[0052] Example 2 provides a release agent, which includes: 45.8 g soybean oil, 45 g water, 3 g polyglycerol fatty acid ester, 1 g carnauba wax, 5 g alcohol and 0.2 g gum arabic.

[0053] The release agent is prepared by a method comprising the following steps:

[0054] (1) mixing the soybean oil, polyglycerol fatty acid ester and carnauba wax in the above mass ratio, heating to 78° C., and homogenizing under a pressure of 35 MPa to obtain an oil solution;

[0055] (2) heating the water, gum arabic and alcohol in the above mass proportion to 78° C., mixing them evenly with the oil solution obtained in step (1), and then cooling them to 30° C. to obtain a release agent.

[0056] Example 3

[0057] Example 3 provides a release agent, which includes: 44g soybean oil, 45g water, 3g polyglycerol fatty acid ester, 3g carnauba wax and 5g alcohol.

[0058] The release agent is prepared by a method comprising the following steps:

[0059] (1) mixing the soybean oil, polyglycerol fatty acid ester and carnauba wax in the above mass ratio, heating to 82° C., and homogenizing under a pressure of 40 MPa to obtain an oil solution;

[0060] (2) The water and alcohol in the above mass ratio are heated to 82° C., mixed evenly with the oil solution obtained in step (1), and then cooled to 30° C. to obtain a release agent.

[0061] Example 4

[0062] Example 4 provides a release agent, which includes: 45.8 g rapeseed oil, 47 g water, 3 g polyglycerol fatty acid ester, 1 g carnauba wax, 3 g alcohol and 0.2 g gum arabic.

[0063] The release agent is prepared by a method comprising the following steps:

[0064] (1) mixing the rapeseed oil, polyglycerol fatty acid ester and carnauba wax in the above mass ratio, heating the mixture to 85° C., and homogenizing the mixture under a pressure of 20 MPa to obtain an oil solution;

[0065] (2) heating the water, gum arabic and alcohol in the above mass proportion to 85° C., mixing the mixture evenly with the oil solution obtained in step (1), and cooling the mixture to 30° C. to obtain a release agent.

[0066] Example 5

[0067] Example 5 provides a release agent, which includes: 46g rapeseed oil, 45g water, 3g polyglycerol fatty acid ester, 0.5g carnauba wax, 5g alcohol and 0.5g gum arabic.

[0068] The release agent is prepared by a method comprising the following steps:

[0069] (1) mixing rapeseed oil, polyglycerol fatty acid ester and carnauba wax in the above mass ratio, heating to 75° C., and homogenizing under a pressure of 25 MPa to obtain an oil solution;

[0070] (2) heating the water, gum arabic and alcohol in the above mass proportion to 75° C., mixing the mixture evenly with the oil solution obtained in step (1), and cooling the mixture to 30° C. to obtain a release agent.

[0071] Example 6

[0072] Example 6 provides a release agent, which includes: 48g soybean oil, 45g water, 1g polyglycerol fatty acid ester, 1g carnauba wax and 5g alcohol.

[0073] The release agent is prepared by a method comprising the following steps:

[0074] (1) mixing the soybean oil, polyglycerol fatty acid ester and carnauba wax in the above mass ratio, heating the mixture to 80° C., and homogenizing the mixture under a pressure of 50 MPa to obtain an oil solution;

[0075] (2) heating the water and alcohol in the above mass ratio to 80° C., mixing the mixture evenly with the oil solution obtained in step (1), and then cooling the mixture to 30° C. to obtain a release agent.

[0076] Example 7

[0077] Example 7 provides a release agent, which includes: 48g soybean oil, 45g water, 1g polyglycerol fatty acid ester, 1g sunflower wax and 5g alcohol.

[0078] The release agent is prepared by a method comprising the following steps:

[0079] (1) mixing the soybean oil, polyglycerol fatty acid ester and sunflower wax in the above mass ratio, heating to 80° C., and homogenizing under a pressure of 50 MPa to obtain an oil solution;

[0080] (2) heating the water and alcohol in the above mass ratio to 80° C., mixing the mixture evenly with the oil solution obtained in step (1), and then cooling the mixture to 30° C. to obtain a release agent.

[0081] Comparative Example 1

[0082] Comparative Example 1 provides a release agent, which includes: 47 g rapeseed oil, 45 g water, 3 g polyglycerol fatty acid ester and 5 g alcohol.

[0083] The release agent is prepared by a method comprising the following steps:

[0084] (1) mixing rapeseed oil, polyglycerol fatty acid ester and carnauba wax in the above mass ratio, heating to 80° C., and homogenizing under a pressure of 45 MPa to obtain an oil solution;

[0085] (2) heating the water and alcohol in the above mass ratio to 80° C., mixing the mixture evenly with the oil solution obtained in step (1), and then cooling the mixture to 30° C. to obtain a release agent.

[0086] Comparative Example 2

[0087] Comparative Example 2 provides a release agent, which includes: 42g rapeseed oil, 45g water, 3g polyglycerol fatty acid ester, 5g carnauba wax and 5g alcohol.

[0088] The release agent is prepared by a method comprising the following steps:

[0089] (1) mixing rapeseed oil, polyglycerol fatty acid ester and carnauba wax in the above mass ratio, heating to 85° C., and homogenizing under a pressure of 35 MPa to obtain an oil solution;

[0090] (2) The water and alcohol in the above mass ratio are heated to 85° C., mixed evenly with the oil solution obtained in step (1), and then cooled to 30° C. to obtain a release agent.

[0091] Comparative Example 3

[0092] Comparative Example 3 provides a release agent, which includes: 45.5 g rapeseed oil, 45 g water, 3 g polyglycerol fatty acid ester, 1 g carnauba wax, 5 g alcohol and 0.5 g gum arabic.

[0093] The release agent is prepared by a method comprising the following steps:

[0094] (1) mixing rapeseed oil, polyglycerol fatty acid ester and carnauba wax in the above mass ratio, heating to 60° C., and homogenizing under a pressure of 30 MPa to obtain an oil solution;

[0095] (2) heating the water, gum arabic and alcohol in the above mass proportion to 60° C., mixing them evenly with the oil solution obtained in step (1), and then cooling them to 30° C. to obtain a release agent.

[0096] Comparative Example 4

[0097] Comparative Example 4 provides a release agent, which includes: 16g rapeseed oil, 75g water, 3g polyglycerol fatty acid ester, 1g carnauba wax and 5g alcohol.

[0098] The release agent is prepared by a method comprising the following steps:

[0099] (1) mixing the rapeseed oil, polyglycerol fatty acid ester and carnauba wax in the above mass ratio, heating the mixture to 85° C., and homogenizing the mixture under a pressure of 50 MPa to obtain an oil solution;

[0100] (2) The water and alcohol in the above mass ratio are heated to 85° C., mixed evenly with the oil solution obtained in step (1), and then cooled to 30° C. to obtain a release agent.

[0101] Technical effect evaluation

[0102] (1) The viscosity of the release agents obtained in the examples and comparative examples was measured. The viscosity measurement method was as follows: 250 g of the release agents obtained in the examples and comparative examples were taken respectively, placed in an environment of 25° C. for 48 hours, and then the viscosity of the release agents was measured using a viscometer. The results are shown in Table 2.

[0103] (2) The demoulding rate of the demoulding agent obtained in the embodiment and the comparative example is measured. The method for measuring the demoulding rate is as follows: flour, yeast, sugar, salt, eggs, water and butter are stirred until the gluten is fully expanded to obtain dough, a certain amount of demoulding oil is applied to the inner wall of the toast mold, the dough is divided and loaded into the toast mold, the dough is loaded, baked, demoulded, the number of toasts that are completely demoulded is observed, and the percentage is calculated by dividing it by the total number of toasts to obtain the demoulding rate. The results are shown in Table 2.

[0104] (3) The release agents obtained in the examples and comparative examples were subjected to stratification rate determination. The stratification rate determination method is as follows: the release agents obtained in the examples and comparative examples were allowed to stand for 48 hours, and then a ruler was used to measure the oil layer height of the upper stratification and the overall height of the liquid. The percentage obtained by dividing the oil layer height of the stratification by the overall height of the release agent was as shown in Table 2.

[0105] (4) The mold growth of the release agents obtained in the examples and comparative examples was determined by storing the release agents at a temperature of 35° C. and a humidity of 85% for one year, and observing the mold growth of each group of release agents within one year.

[0106] Table 2 Technical effect evaluation results

[0107]

[0108]

[0109] As shown in Table 2, the results show that the viscosity of the release agents obtained in Examples 1-7 is in the range of 800-900 mPa.s, while the moisture content in the release agent obtained in Comparative Example 4 is relatively high, so that the viscosity of the release agent prepared in Comparative Example 4 is relatively high, which is 1211 mPa.s. It should be noted that since the viscosity affects the wall hanging effect of the release agent, a viscosity of 600-1000 mPa.s is better. If it is too small, it will not hang on the wall and the demoulding effect is not good. If it is too large, it is not easy to spray and the equipment is not easy to operate.

[0110] The demoulding rates obtained in Examples 1-7 are in the range of 95%-100%, while the demoulding rate of the demoulding agent obtained in Comparative Example 1 without adding carnauba wax is lower, at 80%. The moisture content in the demoulding agent obtained in Comparative Example 4 is relatively high, resulting in a slightly lower demoulding rate of 90%. It should be noted that the demoulding rate reflects the demoulding effect of the demoulding agent, and the better the demoulding effect, the higher the demoulding rate, and the best is 100% demoulding rate.

[0111] The delamination rate of the release agent obtained in Examples 1-7 is in the range of 0-10%, while the delamination rate of Comparative Example 2 is 30%, which is because the content of carnauba wax in the release agent obtained in Comparative Example 2 is relatively high, and it is easy to delaminate. The delamination rate of Comparative Example 3 is 50%, which is because in the process of preparing the release agent in Comparative Example 3, the reaction is carried out at 60°C, which makes the emulsification of each component in the release agent uneven, resulting in easy delamination of the release agent. It should be noted that the delamination rate reflects the demolding effect of the release agent. The lower the delamination rate, the better the demolding effect of the release agent, and the best is 0% delamination rate.

[0112] The mold release agents obtained in Examples 1-7 did not grow mold within one year, while the mold release agent obtained in Comparative Example 4 had a high moisture content, which made the mold release agent prepared in Comparative Example 4 easy to grow mold.

[0113] In summary, the release agents obtained in Examples 1-7 are superior to those in Comparative Examples 1-4 in terms of comprehensive effects of viscosity, demoulding rate, delamination rate and mold growth.

[0114] Although the above describes the specific implementation methods of the present invention, it does not limit the scope of protection of the present invention. Based on the technical solution of the present invention, various modifications or variations that can be made by those skilled in the art without creative work are still within the scope of protection of the present invention.

Claims

1. A release agent, characterized in that The release agent comprises, by weight, 43-50% of vegetable oil, 40-50% of water, 1-5% of emulsifier, 0.1-4% of wax and 0.1-6% of alcohol.

2. The release agent according to claim 1 or 2, characterized in that Calculated by weight of the release agent, the vegetable oil is 45-50%; and / or water is 43-46%; and / or emulsifier is 2-5%; and / or wax is 0.5-4%; and / or alcohol is 2-5%.

3. The release agent according to claim 1 or 2, characterized in that Calculated by weight of the release agent, the present invention further comprises: 0.1-0.6% gum arabic, preferably 0.1-0.3% gum arabic.

4. The release agent according to claim 1, wherein The vegetable oil is one or more of rapeseed oil, soybean oil, sunflower oil and palm oil; preferably, the vegetable oil is one or a combination of rapeseed oil and soybean oil.

5. The release agent according to claim 4, characterized in that Based on the weight of the release agent, the rapeseed oil is 45-50%, and / or the soybean oil is 43-50%.

6. The release agent according to claim 1, wherein The wax is one or a combination of carnauba wax and sunflower wax.

7. The release agent according to claim 6, characterized in that Based on the weight of the release agent, 0.1-4% of carnauba wax and / or 0.1-4% of sunflower wax. The release agent according to claim 1 , wherein the emulsifier is polyglycerol fatty acid ester.

9. A method for preparing the release agent according to any one of claims 1 to 8, characterized in that: The method comprises the following preparation steps: (1) mixing, heating and homogenizing vegetable oil, emulsifier and wax to obtain an oil solution; (2) heating water and alcohol, mixing the mixture with the oil solution obtained in step (1), and cooling the mixture to obtain a release agent.

10. The preparation method according to claim 9, characterized in that: The method comprises the following preparation steps: (1) mixing, heating and homogenizing vegetable oil, emulsifier and wax to obtain an oil solution; (2) heating water, gum arabic and alcohol, mixing the mixture with the oil solution obtained in step (1), and cooling the mixture to obtain a release agent.

11. The preparation method according to claim 9 or 10, characterized in that: In step (1), the homogenization pressure is 20-50 MPa.

12. The preparation method according to any one of claims 9 to 11, characterized in that: The heating temperature is 75-80℃.

13. The preparation method according to any one of claims 9 to 12, characterized in that: Cool to 25-30°C.

14. A release agent, characterized in that The release agent is prepared by the preparation method according to any one of claims 9 to 13.

15. The release agent according to any one of claims 1 to 8 or the release agent according to claim 14, characterized in that: The viscosity of the release agent is greater than or equal to 800 Pa·s and less than or equal to 900 mPa·s; and / or the release rate of the release agent is greater than or equal to 95% and less than or equal to 100%; And / or the delamination rate of the release agent is greater than or equal to 0% and less than or equal to 10%.

16. Use of the release agent according to any one of claims 1 to 8 or the release agent according to claim 14 in the field of baking, preferably in the field of bread baking.