Drying system and pole piece production method

By using air guides and multiple heating zones in the drying system during the battery pole manufacturing process, the problem of folding of the pole sheet during the drying process is solved, the product quality and efficiency are improved, and the application speed is achieved stable drying effect.

CN119056716APending Publication Date: 2024-12-03REPT BATTERO ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411433087.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-14
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

During the manufacturing process of battery electrode sheets, the electrode sheets are prone to folding during drying, resulting in uneven thickness of the film surface, affecting product quality and safety.

Method used

Design a drying system. By setting air guides at the air outlet of the drying box, the airflow is guided between two adjacent drying boxes to form a vortex, improving the stability and uniformity of the airflow and reducing the wind field The pole sheet is disturbed, and multiple heating zones are set up in the drying box to regularly change the circulating air frequency to ensure that the pole sheet remains stable under the high-speed coating state.

Benefits of technology

Effectively reduce the folding of the pole piece, improve the yield rate, significantly increase production capacity, and maintain the same energy consumption level.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056716A_ABST
    Figure CN119056716A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of battery manufacturing, and discloses a drying system and a pole piece production method.The drying system comprises a plurality of drying boxes arranged at intervals in the preset direction, and air outlets facing pole pieces are formed in the two sides of the air outlet ends of the drying boxes; the air guide part is assembled and connected to the position, close to the air outlet, of the air outlet end, the air guide part is arranged at the air outlet of the drying box, the air guide part can guide airflow blown out of the air outlet to the position between the two adjacent drying boxes, and the airflow blown out of the drying boxes on the two sides intersects at the position to form vortex, so that the airflow is blown out of the air outlet, and the vortex is formed; the air flow can act on the pole piece more evenly while the stability of the air flow is improved, disturbance of a wind field to the moving process of the pole piece can be greatly reduced, the pole piece can still keep a stable state when moving at a high coating speed, and the good yield is still achieved while the coating efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery manufacturing, and in particular to a drying system and a pole piece production method. Background Art

[0002] With the continuous development of the battery industry, the quality control in the battery manufacturing process has become more and more stringent. According to the current quality monitoring points, in the battery manufacturing process, the battery pole piece manufacturing cannot meet the requirement of zero defect in membrane surface quality. In order to further improve the product yield and improve the membrane surface quality, it is also necessary to continuously optimize the manufacturing process of the battery pole piece. The membrane surface refers to the surface of the battery pole piece coated with the electrode active slurry.

[0003] At present, in the coating production process of battery pole pieces, after the electrode active material slurry is coated on the foil surface of the pole piece, it needs to be dried in an oven. Under the action of the wind field in the oven, the tape running state of the pole piece will be in an unstable state, and the position of the pole piece close to the pole ear will float up and down under the action of the wind field. The corresponding position of the pole piece and the pole ear is prone to folding and forming "dark marks". After drying, the thickness of the pole piece at the folding position will be different from the thickness of the middle area of ​​the membrane surface. This thickness difference cannot be eliminated after rolling. After such pole pieces are assembled, during the battery cycle process, metal ions (such as lithium ions in lithium batteries and sodium ions in sodium batteries) will not be fully embedded due to the longer transmission path, resulting in metal precipitation at this position, which will seriously affect product safety. Summary of the invention

[0004] In view of this, the present invention provides a drying system and an electrode production method to solve the problem that folding is easily occurred in the existing electrode production process and affects the product quality.

[0005] In a first aspect, the present invention provides a drying system, which is applied to the production process of battery pole pieces, wherein the moving direction of the pole pieces is a preset direction, and comprises: a plurality of drying boxes, which are arranged at intervals along the preset direction, wherein one end of the drying box close to the pole piece forms an air outlet end, and both sides of the air outlet end have air outlets arranged toward the pole piece; an air guide member, which is assembled and connected to a position of the air outlet end close to the air outlet, the air guide member comprises a blocking section and a guiding section, the lower part of the blocking section is connected to a side of the air outlet away from an adjacent drying box, the guiding section is connected to an upper part of the blocking section, the guiding section extends in a direction close to the adjacent drying box, and the air guide member is suitable for guiding the airflow at the air outlet to between two adjacent drying boxes.

[0006] An air guide is provided at the air outlet of the drying box, which can guide the airflow blown out from the air outlet to between two adjacent drying boxes. The airflow blown out from the drying boxes on both sides will meet at this position and form a vortex, which can improve the airflow stability and make the airflow act on the electrode more evenly, and can greatly reduce the disturbance of the wind field on the movement process of the electrode, so that the electrode can still maintain a stable state when moving at a higher coating speed, improve the coating efficiency and still have a good yield rate, and can achieve the advantage of increased production capacity while using the same energy consumption level, and effectively solve the problem of folding easily occurring in the existing electrode production process and affecting product quality.

[0007] In an optional embodiment, the air guide member includes a shielding section, and the shielding section is arranged obliquely downward at one end of the guide section away from the blocking section; the shielding section can guide the airflow to between two adjacent drying boxes, further reducing the situation where the airflow directly blows the pole piece through the gap between the two adjacent guide sections, thereby ensuring the reliability and stability of the airflow guidance.

[0008] In an optional embodiment, the length of the air guide is the same as the length of the air outlet. This type of air guide can effectively cover the air outlet, ensuring the reliability and stability of airflow guidance.

[0009] In an optional embodiment, at least one heating system is included, and the heating system includes multiple drying boxes. The heating system is used to perform drying operations during the primary coating process or the secondary coating process of the electrode. The drying boxes in the same heating system have a preset circulating wind frequency, and the circulating wind frequencies of the multiple drying boxes gradually increase along the preset direction. This form of setting the circulating wind frequency of the drying boxes can make the circulating wind frequency change more regularly, and can reduce the difference in circulating wind frequencies of adjacent drying boxes, thereby reducing the degree of chaos of the wind field along the preset direction, so that when the electrode moves at a higher coating speed, it can still maintain a stable state during the drying process, thereby improving the coating efficiency while still having a good yield rate.

[0010] In an optional embodiment, the drying system forms a plurality of first heating zones in sequence along a preset direction, and the plurality of first heating zones form a heating system. The first heating zone is used to perform a drying operation during a coating process of the electrode piece. Each first heating zone has at least two drying boxes. The plurality of first heating zones are a first preheating zone, a first drying zone, a first drying zone, and a first cooling zone in sequence along the preset direction. The first preheating zone and the first drying zone form a first high temperature zone, the first drying zone forms a first medium temperature zone, and the first cooling zone forms a first low temperature zone. The temperature of the first high temperature zone is higher than the temperature of the first medium temperature zone, and the temperature of the first low temperature zone is less than or equal to the temperature of the first medium temperature zone. The temperature of the temperature zone, and / or, the drying system forms multiple second heating zones in sequence along the preset direction, and the multiple second heating zones form a heating system. The second heating zone is used for drying operations during the secondary coating process. Each second heating zone has at least two drying boxes. The multiple second heating zones are sequentially a second preheating zone, a second drying zone, a second drying zone, and a second cooling zone along the preset direction. The second drying zone and the second drying zone form a second high temperature zone, the second preheating zone forms a second medium temperature zone, and the second cooling zone forms a second low temperature zone. The temperature of the second high temperature zone is higher than the temperature of the second medium temperature zone, and the temperature of the second low temperature zone is less than or equal to the temperature of the second medium temperature zone. The first heating zone is arranged in accordance with the characteristics of the primary coating process of the electrode piece, so that the primary coating process of the electrode piece can be dried more reliably. The second heating zone is arranged in accordance with the characteristics of the secondary coating process of the electrode piece, so that the secondary coating process of the electrode piece can be dried more reliably.

[0011] In an optional embodiment, the temperature of the drying box in the first preheating zone remains consistent or gradually decreases along a preset direction; the temperature of the drying box in the first drying zone gradually decreases along a preset direction or first decreases and then increases; the temperature of the drying box in the first drying zone remains consistent or gradually decreases along a preset direction; the temperature of the drying box in the first cooling zone gradually decreases along a preset direction. Corresponding to the drying requirements of the electrode one-time coating process, the temperature changes of the drying boxes in each first heating zone are set specifically, which can effectively improve the drying reliability and stability of the electrode one-time coating process.

[0012] In an optional embodiment, the temperature of the drying box in the second preheating zone remains consistent or gradually increases along a preset direction; the temperature of the drying box in the second drying zone gradually increases along a preset direction or first increases and then decreases; the temperature of the drying box in the second drying zone remains consistent or gradually decreases along a preset direction; the temperature of the drying box in the second cooling zone gradually decreases along a preset direction. Corresponding to the drying requirements of the secondary coating process of the electrode, the temperature changes of the drying boxes in each second heating zone are set in a targeted manner, which can effectively improve the drying reliability and stability of the secondary coating process of the electrode.

[0013] In the second aspect, the present invention also provides a method for producing pole pieces, which uses the above-mentioned drying system and is used to produce pole pieces, and the moving direction of the pole pieces is a preset direction, which includes: guiding the airflow blown out of the drying box to between two adjacent drying boxes through an air guide; and performing coating production.

[0014] By guiding the airflow in the drying box, the electrode can be dried stably and reliably under high-speed coating conditions, reducing the possibility of electrode folding, so that the electrode still has a high yield rate at a higher coating speed, and can significantly increase production capacity at the same energy consumption level.

[0015] In an optional embodiment, before the step of coating production, the process further comprises:

[0016] Check the amount of foil collapse used in electrode production; if the collapse is greater than the preset collapse, replace the foil until the collapse is less than or equal to the preset collapse.

[0017] This step can ensure that the foil's sag meets usage requirements. Since a large sag is prone to creases, choosing a foil with a smaller sag can reduce the occurrence of creases.

[0018] In an optional embodiment, after the step of replacing the foil material if the settling amount is greater than the preset settling amount until the settling amount of the foil material is less than or equal to the preset settling amount, the method further includes:

[0019] The foil is dried in an empty foil state through a drying system; the number of stripes of the dried foil is obtained; and the lower pulling tension of the coating machine is adjusted according to the number of stripes until the number of stripes of the dried foil is zero.

[0020] This step can intuitively and quantifiably evaluate the stability of the foil's running state, and can avoid folding caused by problems with the foil itself and the coating machine's lower traction tension.

[0021] In an optional embodiment, before the step of coating production, the process further comprises:

[0022] Conduct coating production tests;

[0023] Obtaining the surface density of the film surface of the electrode after the coating production test;

[0024] If the surface density is greater than the preset qualified surface density; increase the temperatures of the first high temperature zone, the first cooling zone, the second high temperature zone and the second cooling zone and perform the coating production test again;

[0025] Until the surface density is less than or equal to the preset qualified surface density.

[0026] In order to further improve the compatibility of this solution, an additional step is added to confirm whether the surface density exceeds the upper limit. If the surface density exceeds the upper limit, adjustments can be made as described in the solution to ensure the membrane surface drying effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 A schematic diagram of the arrangement of a drying system according to an embodiment of the present invention;

[0029] Figure 2 for Figure 1 The front view of the drying box side of the drying system after being assembled with the air guide member is shown;

[0030] Figure 3 for Figure 2 A side view of the drying system shown;

[0031] Figure 4 A schematic diagram of the main process of a pole piece production method according to an embodiment of the present invention;

[0032] Figure 5 for Figure 4 Schematic diagram of the entire process of the electrode production method shown.

[0033] Description of reference numerals:

[0034] 1. Drying box; 101. Air outlet; 2. Air guide; 201. Blocking section; 202. Guide section; 203. Shielding section; 3. Pole piece. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0036] Combine the following Figures 1 to 5 , describing an embodiment of the present invention.

[0037] In the related technology, during the coating production process, the battery pole piece needs to be dried in an oven. Under the influence of the wind field in the oven, the conveying state of the pole piece in the oven will be in an unstable state. The position of the pole piece close to the pole ear will float up and down under the influence of the wind field. This phenomenon will cause the corresponding position of the pole piece to be easily folded, resulting in unstable conveying state of the pole piece.

[0038] In order to solve this problem, the hot air blown out from the oven air outlet is generally guided to the pole piece in the related technology. The way to guide the hot air blown out from the oven air outlet is to set a guide plate inside the oven air outlet, so that the hot air blowing direction of the oven air outlet is deflected, increasing the distance from the hot air outlet to the pole piece 3, thereby reducing the impact of the hot air on the pole piece 3. However, in this form, the hot air blown out from the air outlet will still pass through the guide plate and directly impact the pole piece 3 in the moving process. This solution can only be applied to coating speeds less than or equal to 60m / min, but as the coating speed is further increased, especially when the coating speed reaches 70m / min and above, it is found in the production process that this solution cannot effectively solve the problem of electrode folding. The electrode will still be folded during the production process. When the coating speed is high, the defective rate of the electrode is still high, which will seriously affect the production efficiency and production cost of the electrode. Therefore, in order to ensure the yield rate of the electrode, production can only be carried out at a coating speed of less than or equal to 60m / min, which seriously affects the upper limit of the production capacity of the electrode in the industry.

[0039] According to an embodiment of the present invention, on the one hand, a drying system is provided, which is applied to the production process of the electrode 3 of the battery, the moving direction of the electrode 3 is a preset direction, and the drying system comprises: a plurality of drying boxes 1 and an air guide 2, the plurality of drying boxes 1 are arranged at intervals along the preset direction, an air outlet is formed at one end of the drying box 1 close to the electrode 3, both sides of the air outlet have air outlets 101 arranged toward the electrode 3, the air guide 2 is assembled and connected to the position of the air outlet close to the air outlet 101, the air guide 2 comprises a blocking section 201 and a guiding section 202, the lower part of the blocking section 201 is connected to the side of the air outlet 101 away from the adjacent drying box 1, the guiding section 202 is connected to the upper part of the blocking section 201, the guiding section 202 extends in the direction close to the adjacent drying box 1, and the air guide 2 is suitable for guiding the airflow at the air outlet 101 to between two adjacent drying boxes 1.

[0040] In the drying system of the present embodiment, an air guide 2 is provided at the air outlet 101 of the drying box 1. The air guide 2 can guide the airflow blown out from the air outlet 101 to between two adjacent drying boxes 1. The airflow blown out from the drying boxes 1 on both sides will meet at this position and form a vortex, which can improve the airflow stability and make the airflow act on the electrode 3 more evenly, and can greatly reduce the disturbance of the wind field on the movement process of the electrode 3, so that when the electrode 3 moves at a higher coating speed, such as 70 to 100 m / min, it can still maintain a stable state during the drying process, improve the coating efficiency and still have a good yield rate, and can achieve the advantage of significantly increasing production capacity while using the same energy consumption level, effectively solving the problem of folding easily occurring in the existing electrode production process and affecting product quality.

[0041] In addition, in the production process of the electrode sheet 3, the electrode active material slurry is usually first coated on one surface of the foil, and the electrode active material slurry on the surface is dried, which corresponds to a primary coating process, and then the electrode active slurry is coated on the other surface, and the electrode active material on the other surface is dried, which corresponds to a secondary coating process. Figure 1 As shown, the pole piece 3 here includes various states in the entire production process, including both the state when the foil is dried during the first coating process and the state when the foil is dried during the second coating process.

[0042] In a possible implementation, Figure 2 and Figure 3 As shown, the air guide member 2 includes a shielding section 203. The shielding section 203 is arranged obliquely downward at one end of the guide section 202 away from the blocking section 201. The shielding section 203 can guide the airflow to between two adjacent drying boxes 1, further reducing the situation where the airflow directly blows the pole piece 3 through the gap between the two adjacent guide sections 202, thereby ensuring the reliability and stability of the airflow guidance.

[0043] In a possible implementation, Figure 3 As shown, the length of the air guide member 2 is the same as the length of the air outlet 101. This type of air guide member 2 can effectively cover the air outlet 101, ensuring the reliability and stability of airflow guidance.

[0044] Specifically, the length of the air guide 2 is consistent with the length of the air outlet 101, and can be 1200 mm, 1600 mm, or other sizes.

[0045] It should be noted that the length direction of the air outlet 101 is the width direction of the pole piece 3 , and the length direction of the air outlet 101 is perpendicular to the moving direction of the pole piece 3 .

[0046] Furthermore, there is no limitation on the material and thickness of the air guide member 2, which may be a member made of metal, ceramic or plastic, and the thickness may be flexibly selected according to the use requirements, as long as the use requirements are met.

[0047] Preferably, if Figure 2 As shown, the air guide member 2 is made by bending a 1 mm thick stainless steel plate, the guide section 202 is horizontally arranged, the angle A between the guide section 202 and the air outlet 101 is 45°, and the angle B between the shielding section 203 and the guide section 202 is 135°. This form of air guide member 2 has a more reliable guiding effect and is more durable during use, and is not easy to deform or shake under the impact of airflow.

[0048] In one possible embodiment, the drying system includes at least one heating system, which includes multiple drying boxes 1. The heating system is used to perform drying operations during the primary coating process or the secondary coating process of the electrode. The drying boxes 1 in the same heating system have a preset circulating wind frequency. The circulating wind frequencies of the multiple drying boxes 1 gradually increase along the moving direction of the electrode 3. Setting the circulating wind frequency of the drying box 1 in this form can make the circulating wind frequency change more regularly, reduce the difference in circulating wind frequencies between adjacent drying boxes, and thus reduce the degree of chaos of the wind field along the preset direction, so that when the electrode moves at a higher coating speed, it can still maintain a stable state during the drying process, thereby improving the coating efficiency while still having a good yield rate.

[0049] Among them, it should be noted that the circulating air frequency of multiple drying boxes 1 is set to gradually increase along the moving direction of the pole piece 3, which means that the circulating air frequency of a single drying box 1 remains unchanged. Along the moving direction of the pole piece 3, among the two adjacent drying boxes 1, the circulating air frequency of the upstream drying box 1 is less than or equal to the circulating air frequency of the downstream drying box 1, and the circulating air frequency of the most downstream drying box 1 is greater than the circulating air frequency of the most upstream drying box 1. It does not mean that the circulating air frequency of each drying box 1 gradually increases along the moving direction of the pole piece 3.

[0050] In the related art, the change of the circulating wind frequency of the oven generally adopts a "low-high-low" scheme, that is, the circulating wind frequency of the oven increases first and then decreases along the preset direction. The change of the wind field under this circulating wind frequency fluctuates greatly and only considers the drying effect, and does not consider the influence of the circulating wind frequency on the folding during the drying process of the electrode 3. Under the high-speed coating state, the poor mechanical stability of the electrode 3 under high-speed conditions and the large change of the oven wind field are likely to affect the quality of the electrode. The high-speed moving electrode 3 is more susceptible to disturbance. Although the impact of the hot air is weakened, the direct hot air and the fluctuating wind field will still cause the electrode 3 to float up and down;

[0051] In addition, since the electrode 3 will continue to move during the drying process, the overall mass of the electrode 3 will gradually decrease over time during the drying process. If it is set according to the circulating wind frequency change form in the relevant technology, there will be a situation where the circulating wind frequency and the force on the electrode 3 are contradictory. This is because as the drying time increases, the solvent in the electrode 3 will be more difficult to evaporate. If the circulating wind frequency is further reduced, the solvent evaporation rate in the electrode 3 will be slower, and the corresponding mass of the electrode 3 will decrease more and more slowly. That is, as the electrode 3 moves, the mass change of the electrode 3 per unit time varies greatly (that is, the tape running consistency is poor), which can easily cause uneven force on the electrode 3 during the drying process, and then cause creases on the membrane surface of the electrode 3.

[0052] In the drying system of this embodiment, the air guide 2 is arranged outside the drying box 1 and the fluctuation of the wind field is improved. The blocking section 201 of the air guide 2 can prevent the airflow at the air outlet 101 from moving in a direction away from the adjacent drying box 1, and the guiding section 202 can guide the airflow at the air outlet 101 to between two adjacent drying boxes 1, forming a vortex while avoiding the airflow from directly impacting the pole piece 3 after passing through the air guide 2; and the circulating wind frequency of multiple drying boxes 1 gradually increases along the moving direction of the pole piece 3. Compared with the "low-high-low" solution, The fluctuation of the wind field change can be made smaller, and the fluctuation generated when the pole piece 3 moves in the wind field formed by the gradually increasing circulating wind frequency is also smaller. The gradually increasing circulating wind frequency can ensure that the increasing gradient of the circulating wind frequency is more matched with the drying rate of the pole piece 3, thereby ensuring the stability of the drying of the pole piece 3 under high-speed moving state; in addition, the total amount of solvent in the pole piece 3 will continue to decrease with the drying process, and the gradually increasing circulating wind frequency can make the volatilization rate of the solvent in the pole piece 3 during the drying process relatively uniform, so that the pole piece 3 has better walking consistency in the drying system.

[0053] In a possible embodiment, the drying system further includes a blocking piece, which is used to block the air outlet 101 of the drying box 1. Since the drying box 1 has a variety of arrangements with different spacing distances, when some of the drying boxes 1 have a large number of air outlets 101, which will significantly affect the stability of the wind field during the drying process, the air outlet 101 can be blocked.

[0054] Specifically, there is no limitation on the size and shape of the blocking piece, as long as it can block the air outlet 101 .

[0055] In a possible embodiment, the drying system forms a plurality of first heating zones in sequence along a preset direction, and the plurality of first heating zones form a heating system. The first heating zone is used for drying during the one-time coating process of the electrode 3. Each first heating zone has at least two drying boxes 1. The plurality of first heating zones are the first preheating zone, the first drying zone, the first drying zone and the first cooling zone in sequence along the preset direction. The first preheating zone and the first drying zone form a first high temperature zone, the first drying zone forms a first medium temperature zone, and the first cooling zone forms a first low temperature zone. The temperature of the first high temperature zone is higher than the temperature of the first medium temperature zone, and the temperature of the first low temperature zone is less than or equal to the temperature of the first medium temperature zone. During the one-time coating process of the electrode 3, the first heating zone is arranged correspondingly according to the characteristics of the one-time coating, so that the one-time coating process of the electrode can be dried more reliably. It should be noted that the high temperature, medium temperature and low temperature in this application do not correspond to a specific temperature range, but reflect the relative temperature between different heating zones.

[0056] In a possible embodiment, the temperature of the drying box 1 in the first preheating zone remains consistent or gradually decreases along a preset direction; the temperature of the drying box 1 in the first drying zone gradually decreases along a preset direction or first decreases and then increases; the temperature of the drying box 1 in the first drying zone remains consistent or gradually decreases along a preset direction; the temperature of the drying box 1 in the first cooling zone gradually decreases along a preset direction. Corresponding to the drying requirements of the one-time coating process of the electrode 3, the temperature change of the drying box 1 in each first heating zone is set specifically, which can effectively improve the drying reliability and stability of the one-time coating process of the electrode 3.

[0057] In a possible embodiment, the drying system forms a plurality of second heating zones in sequence along a preset direction, the second heating zones are used for drying during the secondary coating process of the electrode piece, each second heating zone has at least two drying boxes 1, and the plurality of second heating zones are a second preheating zone, a second drying zone, a second drying zone and a second cooling zone in sequence along the preset direction, the second drying zone and the second drying zone form a second high temperature zone, the second preheating zone forms a second medium temperature zone, and the second cooling zone forms a second low temperature zone, the temperature of the second high temperature zone is higher than the temperature of the second medium temperature zone, and the temperature of the second low temperature zone is less than or equal to the temperature of the second medium temperature zone, and the second heating zones are arranged in accordance with the characteristics of the secondary coating process of the electrode piece 3, so that the secondary coating process of the electrode piece can be dried more reliably.

[0058] In a possible embodiment, the temperature of the drying box 1 in the second preheating zone remains consistent or gradually increases along a preset direction; the temperature of the drying box 1 in the second drying zone gradually increases along a preset direction or first increases and then decreases; the temperature of the drying box 1 in the second drying zone remains consistent or gradually decreases along a preset direction; the temperature of the drying box 1 in the second cooling zone gradually decreases along a preset direction. Corresponding to the drying requirements of the secondary coating process of the electrode piece 3, the temperature change of the drying box 1 in each second heating zone is set in a targeted manner, which can effectively improve the drying reliability and stability of the secondary coating process of the electrode piece 3.

[0059] Preferably, the preheating zone (including the first preheating zone and the second preheating zone) has two drying boxes 1 to ensure uniform preheating of the electrode; the drying zone (including the first drying zone and the second drying zone) has six drying boxes 1 as a constant speed drying zone, and multiple circulating wind frequencies are used to ensure constant speed drying; the drying zone (including the first drying zone and the second drying zone) has two drying boxes 1 as the final drying zone to ensure that the weight loss rate of the electrode is qualified after leaving the oven; for the cooling zone (including the first cooling zone and the second cooling zone), the electrode has two drying boxes 1 in this temperature zone, the main function of which is to ensure that the temperature of the electrode 3 after leaving the oven is reduced to below the preset temperature, so as to avoid wrinkling of the electrode 3 due to excessive temperature difference;

[0060] Among them, since the electrode 3 gradually changes from a wet film state to a semi-solid state in the preheating zone and the drying zone, the amount of solvent volatilization in the electrode 3 will increase exponentially in this stage. Therefore, the weight difference of the electrode 3 at different positions in the preheating zone and the drying zone will cause the force on the electrode 3 to be different, thereby causing the electrode to operate in an unstable state.

[0061] The wind frequency variation law and the temperature setting method of the drying box 1 of this embodiment fully consider the weight change of the electrode 3 during the drying process, and can effectively improve the operation stability of the electrode 3 in the preheating zone and the drying zone, and avoid the generation of folds when the electrode 3 is dried in this area. Among them, since the electrode 3 is first coated with the electrode active material slurry to one surface of the foil to form a first slurry layer during the coating process, and after being dried in the drying box 1, the electrode active material is coated on the other surface of the foil to form a second slurry layer, and in the first coating and drying process, there is only a single layer of slurry, the overall weight of the electrode 3 is relatively light, and the two sides of the foil are unevenly stressed, which is easy to form folds, and in the second coating and drying process, there are slurry layers on both sides of the electrode 3, the overall weight is large and the two sides are evenly stressed, which is relatively difficult to form folds, so the temperature settings of the multiple first heating zones are more matched with the drying rate of the electrode 3 to reduce the generation of folds, and the temperature settings of the multiple second heating zones are more mainly considered to be drying efficiency.

[0062] It is particularly noted that the temperature of each first heating zone refers to the average temperature of the interval. For example, in some embodiments, the temperature of individual drying boxes in the first medium temperature zone may be greater than the temperature of individual drying boxes in the first high temperature zone; similarly, the temperature of each second heating zone refers to the average temperature of the interval. For example, the temperature of individual drying boxes in the second low temperature zone may be greater than the temperature of individual drying boxes in the second medium temperature zone. In addition, the temperature of each first heating zone refers to the preset temperature, and the actual temperature of the oven may fluctuate due to the influence of the environment, etc. Moreover, the average temperature of multiple second heating zones is usually greater than the average temperature of multiple first heating zones, because it is preferred not to completely dry the first slurry layer during one coating process, and in the secondary coating process, heat can be transferred to the first slurry layer to further dry the first slurry layer.

[0063] According to an embodiment of the present invention, on the other hand, a pole piece production method is provided, which uses the above-mentioned drying system and is used to produce a pole piece 3, wherein the moving direction of the pole piece 3 is a preset direction, and comprises:

[0064] The airflow blown out of the drying box 1 is guided to between two adjacent drying boxes 1 through the air guide 2; the circulating wind frequency of the multiple drying boxes 1 is set to gradually increase along a preset direction; and the electrode coating production is carried out.

[0065] By guiding the airflow of the drying box 1, the battery electrode 3 can still be stably and reliably dried under high-speed coating conditions, reducing the possibility of folding of the electrode 3, so that the coating speed of the electrode 3 is increased while still having a high yield rate, which is far higher than the industry level and can increase production capacity at the same energy consumption level.

[0066] In a possible implementation manner, before the step of coating production, the method further includes:

[0067] The drying system has a first preheating zone, a first drying zone, a first drying zone and a first cooling zone in sequence along a preset direction, which are used to perform drying operations during a coating process of the electrode 3, and the frequency of the plurality of drying boxes 1 in the first preheating zone, the first drying zone, the first drying zone and the first cooling zone gradually increases along the preset direction.

[0068] The first preheating zone is set as the first high temperature zone, and the temperature of the drying box 1 therein is set to remain constant or gradually decrease along a preset direction;

[0069] The first drying zone is set as the first medium temperature zone, and the temperature of the drying box 1 therein is set to gradually decrease along a preset direction or to first decrease and then increase;

[0070] The first drying zone is set as the first high temperature zone, and the temperature of the drying box 1 therein is set to remain constant or gradually decrease along a preset direction;

[0071] The first temperature reduction zone is set as the first low temperature zone, and the temperature of the drying box 1 therein is set to gradually decrease along a preset direction;

[0072] Wherein, the temperature of the first high temperature zone is higher than the temperature of the first medium temperature zone, and the temperature of the first low temperature zone is less than or equal to the temperature of the first medium temperature zone;

[0073] The drying system also has a second preheating zone, a second drying zone, a second drying zone and a second cooling zone in sequence along the preset direction, which are used to perform drying operations during the secondary coating process of the electrode 3, and the frequency of the multiple drying boxes 1 in the second preheating zone, the second drying zone, the second drying zone and the second cooling zone gradually increases along the preset direction.

[0074] The second preheating zone is set as the second medium temperature zone, and the temperature of the drying box 1 therein is set to remain constant or gradually increase along a preset direction;

[0075] The second drying zone is set as the second high temperature zone, and the temperature of the drying box 1 therein is set to gradually increase or first increase and then decrease along a preset direction;

[0076] The second drying zone is set as the second high temperature zone, and the temperature of the drying box 1 therein is set to remain constant or gradually decrease along a preset direction;

[0077] The second temperature reduction zone is set as the second low temperature zone, and the temperature of the drying box 1 therein is set to gradually decrease along a preset direction;

[0078] The temperature of the second high temperature zone is higher than that of the second medium temperature zone, and the temperature of the second low temperature zone is less than or equal to that of the second medium temperature zone.

[0079] Specifically, the production process of graphite negative electrode sheets is used as an example for explanation. The specific setting method of the circulating air frequency and temperature of the drying box 1 can be referred to the table below.

[0080]

[0081]

[0082]

[0083]

[0084] Table 1 Drying box temperature, circulating air frequency parameter table

[0085] The above table shows the temperature and circulating air frequency parameters of the drying box 1 for coating speeds of 70m / min to 100m / min.

[0086] Among them, the first layer of drying box in the above table is used for drying in the first coating process, the second layer of drying box is used for drying in the second coating process, A is the drying box 1 in the first heating zone, B is the drying box 1 in the second heating zone, A1 and A2 are the drying boxes 1 in the first preheating zone, A3-A8 are the drying boxes 1 in the first drying zone, A9 and A10 are the drying boxes 1 in the first drying zone, A11 and A12 are the drying boxes 1 in the first cooling zone; B1 and B2 are the drying boxes 1 in the second preheating zone, B3-B8 are the drying boxes 1 in the second drying zone, B9 and B10 are the drying boxes 1 in the second drying zone, and B11 and B12 are the drying boxes 1 in the second cooling zone.

[0087] The electrode production method of this embodiment can reduce the defective rate caused by folding problems in the production process of graphite negative electrodes, and significantly improve the yield rate of graphite negative electrode production.

[0088] In a possible implementation manner, before the step of coating production, the method further includes:

[0089] Detect the amount of collapse of the foil used in the production of the electrode 3; if the collapse is greater than the preset collapse, replace the foil until the collapse of the foil is less than or equal to the preset collapse.

[0090] This step can ensure that the foil's sag meets the use requirements. Since a large sag is prone to folding, choosing a foil with a small sag can reduce this. The sag is used to characterize the degree of undulation of the foil's shape, and can be detected using an offline foil shape detector.

[0091] Exemplarily, the preset setback definition standard may be 7 mm, and the preset setback may be specifically set according to actual needs.

[0092] In a possible implementation manner, after the step of replacing the foil material if the settling amount is greater than the preset settling amount until the settling amount of the foil material is less than or equal to the preset settling amount, the method further includes:

[0093] The foil is dried in an empty foil state through a drying system; the number of stripes of the dried foil is obtained; and the lower pulling tension of the coating machine is adjusted according to the number of stripes until the number of stripes of the dried foil is zero.

[0094] This step can intuitively and quantifiably evaluate the stability of the foil's running state, and can avoid folding caused by problems with the foil itself and the coating machine's lower traction tension.

[0095] The number of stripes refers to the number of tension stripes generated during the foil drying process. Tension stripes refer to water ripple-like stripes formed along the moving direction of the foil, and a single wave peak is regarded as one stripe. The number of stripes can be obtained by visual observation.

[0096] In a possible embodiment, before performing the coating production step, it also includes: performing a coating production test; obtaining the surface density of the film surface of the electrode 3 after the coating production test; if the surface density is greater than the preset qualified surface density; increasing the temperature of the drying box 1 and performing the coating production test again; until the surface density is less than or equal to the preset qualified surface density.

[0097] In order to further improve the compatibility of this solution, an additional step is added to confirm whether the surface density exceeds the upper limit. The reason is that if the heating of the drying box 1 cannot ensure effective drying of the film surface during the coating process, the surface density will continue to exceed the upper limit. Therefore, a confirmation step is specially added here. If the surface density exceeds the upper limit, the temperature of the drying box 1 can be increased to ensure the drying effect of the film surface.

[0098] Specifically, if the surface density is greater than the preset qualified surface density, the temperature in the first high temperature zone, the first cooling zone, the second high temperature zone and the second cooling zone is increased by 1°C and the coating production test is performed again, which can be more finely adjusted to a state where the surface density meets the requirements.

[0099] Although the embodiments of the present invention have been described in conjunction with the accompanying drawings, those skilled in the art may make various modifications and variations without departing from the spirit and scope of the present invention, and such modifications and variations are all within the scope defined by the appended claims.

Claims

1. A drying system, applied to the production process of a battery pole piece (3), wherein the moving direction of the pole piece (3) is a preset direction, characterized in that: include: A plurality of drying boxes (1) are arranged at intervals along the preset direction, one end of the drying box (1) close to the pole piece (3) forms an air outlet, and both sides of the air outlet have air outlets (101) arranged toward the pole piece (3); An air guide member (2) is assembled and connected to a position of the air outlet end close to the air outlet (101), the air guide member (2) comprises a blocking section (201) and a guiding section (202), the lower part of the blocking section (201) is connected to a side of the air outlet (101) away from the adjacent drying box (1), the guiding section (202) is connected to the upper part of the blocking section (201), the guiding section (202) extends in a direction close to the adjacent drying box (1), and the air guide member (2) is suitable for guiding the airflow at the air outlet (101) to between two adjacent drying boxes (1).

2. The drying system according to claim 1, characterized in that: The air guide member (2) comprises a shielding section (203), and the shielding section (203) is arranged obliquely downward at one end of the guide section (202) away from the blocking section (201); and / or the length of the air guide member (2) is the same as the length of the air outlet (101).

3. The drying system according to claim 1, characterized in that: The invention comprises at least one heating system, wherein the heating system comprises a plurality of drying boxes (1), and the heating system is used for performing a drying operation during a primary coating process or a secondary coating process of an electrode piece, wherein the drying boxes (1) in the same heating system have a preset circulating air frequency, and the circulating air frequency of the plurality of drying boxes (1) gradually increases along the preset direction.

4. The drying system according to claim 3, characterized in that: The drying system sequentially forms a plurality of first heating zones along the preset direction, and the plurality of first heating zones form one heating system. The first heating zone is used for performing a drying operation during a coating process of the electrode (3). Each of the first heating zones has at least two drying boxes (1). The plurality of first heating zones sequentially form a first preheating zone, a first drying zone, a first drying zone, and a first cooling zone along the preset direction. The first preheating zone and the first drying zone form a first high temperature zone, the first drying zone forms a first medium temperature zone, and the first cooling zone forms a first low temperature zone. The temperature of the first high temperature zone is higher than the temperature of the first medium temperature zone, and the temperature of the first low temperature zone is less than or equal to the temperature of the first medium temperature zone. And / or, the drying system forms a plurality of second heating zones in sequence along the preset direction, and the plurality of second heating zones form one heating system, the second heating zone is used for drying during the secondary coating process of the electrode (3), each second heating zone has at least two drying boxes (1), and the plurality of second heating zones are a second preheating zone, a second drying zone, a second drying zone and a second cooling zone in sequence along the preset direction, the second drying zone and the second drying zone form a second high temperature zone, the second preheating zone forms a second medium temperature zone, the second cooling zone forms a second low temperature zone, the temperature of the second high temperature zone is higher than the temperature of the second medium temperature zone, and the temperature of the second low temperature zone is less than or equal to the temperature of the second medium temperature zone.

5. The drying system according to claim 4, characterized in that: The drying system forms a plurality of first heating zones in sequence along the preset direction, and the plurality of first heating zones form one heating system. The first heating zone is used for performing a drying operation during a coating process of the electrode (3). Each of the first heating zones has at least two drying boxes (1). The plurality of first heating zones are a first preheating zone, a first drying zone, a first drying zone and a first cooling zone in sequence along the preset direction. The first preheating zone and the first drying zone form a first high temperature zone, the first drying zone forms a first medium temperature zone, and the first cooling zone forms a first low temperature zone. The temperature of the first high temperature zone is higher than the temperature of the first medium temperature zone, and the temperature of the first low temperature zone is less than or equal to the temperature of the first medium temperature zone. The temperature of the drying box (1) in the first preheating zone remains consistent or gradually decreases along the preset direction. The temperature of the drying box (1) in the first drying zone gradually decreases or first decreases and then increases along the preset direction. The temperature of the drying box (1) in the first drying zone remains consistent or gradually decreases along the preset direction. The temperature of the drying box (1) in the first cooling zone gradually decreases along the preset direction.

6. The drying system according to claim 4, characterized in that: The drying system forms a plurality of second heating zones in sequence along the preset direction, and the plurality of second heating zones form one heating system. The second heating zone is used for performing drying operations during the secondary coating process of the electrode (3). Each second heating zone has at least two drying boxes (1). The plurality of second heating zones are a second preheating zone, a second drying zone, a second drying zone and a second cooling zone in sequence along the preset direction. The second drying zone and the second drying zone form a second high temperature zone. The second preheating zone forms a second medium temperature zone. The second cooling zone forms a second low temperature zone. The temperature of the second high temperature zone is higher than the temperature of the second medium temperature zone. The temperature of the second low temperature zone is less than or equal to the temperature of the second medium temperature zone. The temperature of the drying box (1) in the second preheating zone remains consistent or gradually increases along the preset direction. The temperature of the drying box (1) in the second drying zone gradually increases or first increases and then decreases along the preset direction. The temperature of the drying box (1) in the second drying zone remains consistent or gradually decreases along the preset direction. The temperature of the drying box (1) in the second cooling zone gradually decreases along the preset direction.

7. A method for producing a pole piece, using the drying system according to any one of claims 1 to 6, and used for producing a pole piece (3), wherein the moving direction of the pole piece (3) is a preset direction, characterized in that: include: The airflow blown out of the drying box (1) is guided to between two adjacent drying boxes (1) through an air guide member (2); Carry out coating production.

8. The pole piece production method according to claim 7, characterized in that: Before the coating production step, it also includes: Detecting the amount of depression of the foil material used in the production of the electrode (3); If the settling amount is greater than a preset settling amount, the foil is replaced until the settling amount of the foil is less than or equal to the preset settling amount.

9. The pole piece production method according to claim 8, characterized in that: If the settling amount is greater than a preset settling amount, the step of replacing the foil until the settling amount of the foil is less than or equal to the preset settling amount further includes: Drying the foil in an empty foil state by the drying system; Obtaining the number of stripes on the foil after drying; The lower pulling tension of the coating machine is adjusted according to the number of stripes until the number of stripes on the foil after drying is zero.

10. The pole piece production method according to claim 7, characterized in that: Before the coating production step, it also includes: Conduct coating production tests; Obtaining the surface density of the film surface of the electrode (3) after the coating production test; If the surface density is greater than the preset qualified surface density; Increasing the temperature of the drying box and performing the coating production test again; Until the surface density is less than or equal to the preset qualified surface density.