Production method of wide-specification electro-galvanized outer plate for side wall

Through hot continuous rolling, cold continuous rolling, continuous annealing and electrogalvanizing processes, the production process of electrogalvanized outer plates is controlled, and the problem of electroplating and ignition of wide-width boards is solved, the surface quality and stamping performance are improved, and the body is beautiful and environmentally friendly coating is met. Installation requirements.

CN119056903APending Publication Date: 2024-12-03武汉钢铁有限公司
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410971378.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The wide-width board forms a micro-cell discharge and ignition between the contact gap between the roller surface of the wide-width board and the contact gap between the roller surface, resulting in imprint defects and affecting the aesthetics and performance of the car body.

Method used

Using hot continuous rolling, cold continuous rolling, continuous annealing and electrogalvanizing processes, the furnace time, heating temperature, rolled plate convexity, cold rolling total pressure reduction rate, plating solution concentration and electroplating tension are controlled to ensure the surface quality and coating of the sheet. Install performance.

Benefits of technology

It reduces the defects of silk spots and poor plate shape, improves the surface morphology and stamping performance of the electroplated galvanized outer plate, avoids the problem of electroplating and ignition, and meets the user's environmentally friendly and medium-coating-free process requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to a production method of a wide-width-specification electro-galvanized outer plate for a side wall, which comprises the following steps: smelting a base material, casting into a plate blank, and carrying out hot continuous rolling, cold continuous rolling, continuous annealing, finishing and electro-galvanizing to obtain the required electro-galvanized outer plate. The produced electro-galvanized outer plate can meet the surface appearance requirement of a user for an environment-friendly floating-coat-free process; in the hot rolling process, the in-furnace time and the rolling temperature are controlled, the scale is prevented from being too thick, the descaling process and the water nozzle replacement period are standardized, and the situation that the surface quality of a finished product cannot meet the outer plate requirement due to filament spot defects is reduced; small convexity rolling is adopted to reduce the electroplating sparking problem caused by poor wide plate shape, and the waviness and roughness of the plate surface are controlled in the cold rolling process to meet the surface appearance technical requirements of user environment-friendly coating; attenuation is controlled in the electroplating process, tension is improved, and the problem that a wide plate is prone to deviation is solved. The electro-galvanized outer plate produced by the invention has high surface quality and excellent stamping performance and coating performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal plate processing, and in particular to a method for producing a wide-width electro-galvanized outer plate for side panels. Background Art

[0002] As new energy vehicle models become larger and larger, the requirements for the width of steel plates are also getting wider and wider. They are mainly used in the manufacture of large-sized SUVs, MPVs, etc. Wide-width plates have high surface quality, excellent stamping performance and painting performance, and can meet the needs of large-sized car bodies, such as doors and side panels, to be formed in one go, avoiding splicing and welding, and improving the appearance of the car body. However, wide-width plates are prone to plate shape problems, and micro-battery discharge and sparking are formed in the gap between the electroplating process and the roller surface, causing embossing defects. Summary of the invention

[0003] In order to solve the above problems, the present invention provides a method for producing a wide-width electro-galvanized outer plate for side panels, and the produced product has high surface quality, excellent stamping performance and coating performance.

[0004] The technical solution adopted by the present invention is: a method for producing a wide-width electrogalvanized outer plate for side panels, characterized in that the substrate is smelted and cast into a slab, and then hot-rolled, cold-rolled, continuously annealed, skin-passed and electrogalvanized; specifically comprising the following steps:

[0005] S1, hot rolling: based on the furnace time control range, high temperature time ≤ 120min, total time ≤ 220min; control the steel burning temperature, reduce the heating temperature, furnace ≤ 1200℃, RT2 upper and lower surface full length temperature ≤ 1020℃; wide strip steel plate shape control, rolling plate shape convexity target control within 30μm;

[0006] S2, cold rolling: total cold rolling reduction rate 80-83%;

[0007] S3, continuous annealing and leveling: the soaking temperature is 820-860℃, the terminal temperature of rapid cooling is 440-470℃, and the strip speed is 120-150m / min; after continuous annealing, the steel plate is leveled, and the leveling elongation is 0.5-0.6%;

[0008] S4. Electrogalvanizing: The zinc ion concentration in the plating solution is 100-140 g / L, the pH value range is 1.2-1.8, the plating solution temperature is controlled at 50-52°C, the free acid concentration in the plating solution is controlled in the range of 5-7 g / l, and the speed of the strip passing through the electroplating tank is 60-100 m / min; the tension of the strip in the electroplating section is increased to above 52 KN to prevent the strip from running off.

[0009] Preferably, in step S1, high-pressure water descaling is started for all passes of rough rolling, and the replacement cycle of the descaling nozzle is less than 6 months.

[0010] Preferably, in step S2, the 5# rack adopts a roughness of 3.0 μm.

[0011] Preferably, in step S3, the surface roughness Ra of the roller is controlled between 2.0 and 2.3 μm, and the roller surface RPc is controlled above 100.

[0012] Preferably, in step S4, the steel strip after continuous annealing and leveling is cleaned through alkali washing, brushing, electrolytic degreasing and rinsing steps and then enters the electro-galvanizing tank, using a gravity electroplating process.

[0013] Preferably, in step S4, the main salt component of the electro-galvanizing solution is zinc sulfate.

[0014] Preferably, the components and weight percentage of the substrate are: C: ≤0.0012, Si: ≤0.02, Mn: 0.05-0.2, P: ≤0.02, S: ≤0.01, Al: 0.03-0.09, Ti≤0.03%, and the remainder is Fe and other inevitable impurities.

[0015] Preferably, the electro-galvanized outer sheet produced has a yield point RP0.2: 100-150Mpa; a tensile strength Rm: 250-310Mpa; an elongation A80mm: ≥46%; a plastic strain ratio r90 ≥2.5, and a work hardening index n90 ≥0.23.

[0016] As a preference, it is suitable for electro-galvanized outer panels above 1750mm.

[0017] The beneficial effects achieved by the present invention are as follows: the electro-galvanized outer plate produced by the present invention is sensitive to the thread spot defect and can meet the surface morphology requirements of the user's environmentally friendly mid-coating-free process; in the hot rolling process, the furnace time and rolling temperature are controlled to avoid excessive thickness of the oxidized iron scale, the descaling process and the water nozzle replacement cycle are standardized, and the thread spot defect causes the surface quality of the finished product to fail to meet the outer plate requirements; small convexity (the convexity target is controlled at 30μm) rolling is adopted to reduce the electroplating sparking problem caused by poor wide-width plate shape, and the plate surface corrugation and roughness are controlled in the cold rolling process to meet the surface morphology technical requirements of the user's environmentally friendly coating; in the electroplating process, the attenuation is controlled, and the tension is increased (the tension is increased from 38KN to 52KN) to reduce the deviation problem that wide-width plates are prone to. DETAILED DESCRIPTION

[0018] The technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] The invention discloses a method for producing a wide-width electrogalvanized outer plate for side panels, which uses ultra-low carbon smelting components (as shown in Table 1), smelts and casts the slabs, and then performs hot rolling, cold rolling, continuous annealing, skin pass and electrogalvanizing.

[0020] C Yes Mn P S Al You ≤0.0012 ≤0.02 0.05~0.2 ≤0.02 ≤0.01 0.03~0.09 ≤0.03

[0021] Table 1

[0022] In the hot rolling process, in order to control the surface quality and reduce the thread spot defect, the furnace time control range is established (high temperature time ≤ 120min, total time ≤ 220min), the high temperature rolling process is cancelled, the heating temperature is lowered, the furnace out of ≤ 1200℃, the RT2 upper and lower surface full length temperature ≤ 1020℃, and the production organization is standardized to avoid excessive iron thickness caused by excessive furnace time; start the high-pressure water descaling for the whole rough rolling pass, and the replacement cycle of the descaling nozzle is less than 6 months; wide strip shape control, in order to reduce the local sparking caused by poor contact between the strip and the roller surface in the electroplating process and cause the imprinting problem, the rolling plate shape is controlled according to the small convexity (the convexity target control is 30μm).

[0023] In the cold rolling process, in order to improve the coating performance and reduce the corrugation of the plate surface, while achieving the roughness required by the user, the 5# stand adopts 3.0 roughness rolling; the total cold rolling reduction rate is 80-83%.

[0024] The continuous annealing soaking temperature is 840-860°C, the rapid cooling endpoint temperature is 440-470°C, and the annealing strip speed is controlled to be stable at 120-150m / min to promote the initial nucleation and growth of γ-oriented texture grains, thereby obtaining good deep drawing performance. The temperature is required to remain stable during the production process; after annealing, it is flattened and the elongation is controlled at 0.5-0.6%; the surface roughness Ra of the flattened roller after annealing needs to be controlled between 2.0 and 2.3μm, and the roller surface RPc is controlled above 100.

[0025] After continuous annealing, the strip steel is cleaned by alkali washing, brushing, electrolytic degreasing, rinsing and other processes before entering the electrogalvanizing tank. The gravity electroplating process is adopted. The main component of the electrogalvanizing bath is zinc sulfate, which provides zinc ions in the bath. The zinc ion concentration in the bath is 100-140g / L. The concentration affects the electrodeposition speed. The pH value range is 1.2-1.8. In order to reduce the roughness attenuation, the bath temperature is strictly controlled at 50-52°C, the free acid concentration in the bath is controlled in the range of 5-7g / l, and the speed of the strip steel passing through the electroplating tank is 60-100m / min. At the same time, the tension of the electroplating process is increased to prevent the strip steel from running off.

[0026] The properties of the electro-galvanized outer sheet produced by the present invention are shown in Table 2:

[0027]

[0028] Table 2

[0029] Embodiment 1:

[0030] Substrate: Ultra-low carbon component design containing Ti is selected;

[0031] Hot rolling and coiling: 110 minutes in furnace high temperature, 220 minutes in total; control the steel burning temperature, lower the heating temperature, furnace out of 1200℃, RT2 upper and lower surface full length temperature 980℃, cancel the high temperature rolling process, lower the heating high temperature section temperature; wide strip shape control, rolling shape according to small convexity control, convexity 25μm;

[0032] Cold rolling: total cold rolling reduction rate is 80%; 5# stand adopts 3.0μm roughness;

[0033] Continuous annealing and leveling: The cold-rolled thin plate is continuously annealed, the soaking temperature is 820℃, the terminal temperature of rapid cooling is 440℃, the strip speed is 120m / min, and the steel plate is leveled after continuous annealing, and the leveling elongation is 0.5%; the surface roughness of the roller is Ra2.0μm, and the roller surface RPc is controlled at 100;

[0034] Galvanizing: The zinc ion concentration in the plating solution is 100g / L, the pH value is 1.2, the plating solution temperature is 50℃, the free acid concentration in the plating solution is 5g / l, and the speed of the strip passing through the plating tank is 60m / min; at the same time, the tension of the electroplating process is increased to 52KN.

[0035] Performance test results of Example 1

[0036]

[0037] Example 2

[0038] Substrate: Ultra-low carbon component design containing Ti is selected;

[0039] Hot rolling and coiling: 90 minutes in furnace high temperature, 180 minutes in total; control the steel burning temperature, lower the heating temperature, furnace out of 1000℃, RT2 upper and lower surface full length temperature 900℃, cancel the high temperature rolling process, lower the heating high temperature section temperature; wide strip shape control, rolling shape according to small convexity control, convexity 30μm;

[0040] Cold rolling: total cold rolling reduction rate is 83%; 5# stand adopts 3.0μm roughness;

[0041] Continuous annealing and leveling: The cold-rolled thin plate is continuously annealed, the soaking temperature is 860℃, the rapid cooling end temperature is 470℃, the strip speed is 150m / min, and the steel plate is leveled after continuous annealing, and the leveling elongation is 0.6%; the surface roughness of the roller is Ra2.3μm, and the roller surface RPc120;

[0042] Galvanizing: The zinc ion concentration in the plating solution is 140g / L, the pH value is 1.8, the plating solution temperature is 52°C, the free acid concentration in the plating solution is 7g / l, and the speed of the strip passing through the plating tank is 100m / min; at the same time, the tension of the electroplating process is increased to 55KN.

[0043] Performance test results of Example 2

[0044]

[0045] Example 3

[0046] Substrate: Ultra-low carbon component design containing Ti is selected;

[0047] Hot rolling and coiling: 100 minutes at high temperature in the furnace, 205 minutes in total; control the steel burning temperature, lower the heating temperature, 1100°C out of the furnace, 1000°C for the entire length of the upper and lower surfaces of RT2, cancel the high-temperature rolling process, and lower the temperature of the high-temperature heating section; wide strip steel plate shape control, rolling plate shape is controlled according to small convexity, 27μm convexity;

[0048] Cold rolling: total cold rolling reduction rate is 82%; 5# stand adopts 3.0μm roughness;

[0049] Continuous annealing and leveling: The cold-rolled thin plate is continuously annealed, the soaking temperature is 830℃, the rapid cooling end temperature is 450℃, the strip speed is 130m / min, and the steel plate is leveled after continuous annealing, and the leveling elongation is 0.6%; the surface roughness of the roller is Ra2.2μm, and the roller surface RPc105;

[0050] Galvanizing: The zinc ion concentration in the plating solution is 120g / L, the pH value is 1.5, the plating solution temperature is 51°C, the free acid concentration in the plating solution is 6g / l, and the speed of the strip passing through the electroplating tank is 80m / min; at the same time, the tension of the electroplating process is increased to 53KN.

[0051] Performance test results of Example 3

[0052]

[0053] Example 4

[0054] Substrate: Ultra-low carbon component design containing Ti is selected;

[0055] Hot rolling and coiling: 115min in furnace high temperature time, 210min in total; control the steel burning temperature, lower the heating temperature, furnace out of 1100℃, RT2 upper and lower surface full length temperature 980℃, cancel the high temperature rolling process, lower the heating high temperature section temperature; wide strip steel plate shape control, rolling plate shape according to small convexity control, convexity 29μm;

[0056] Cold rolling: total cold rolling reduction rate is 81%; 5# stand adopts 3.0μm roughness;

[0057] Continuous annealing and leveling: The cold-rolled thin plate is continuously annealed, the soaking temperature is 850℃, the rapid cooling end temperature is 460℃, the strip speed is 140m / min, and the steel plate is leveled after continuous annealing, and the leveling elongation is 0.55%; the surface roughness of the roller is Ra2.1μm, and the roller surface RPc110;

[0058] Galvanizing: The zinc ion concentration in the plating solution is 130g / L, the pH value is 1.6, the plating solution temperature is 51°C, the free acid concentration in the plating solution is 6g / l, and the speed of the strip passing through the plating tank is 90m / min; at the same time, the tension of the electroplating process is increased to 54KN.

[0059] Performance test results of Example 4

[0060]

[0061] Example 5

[0062] Substrate: Ultra-low carbon component design containing Ti is selected;

[0063] Hot rolling and coiling: 110 minutes in furnace high temperature, 200 minutes in total; control the steel burning temperature, lower the heating temperature, furnace out of 1200℃, RT2 upper and lower surface full length temperature 1000℃, cancel the high temperature rolling process, lower the heating high temperature section temperature; wide strip steel plate shape control, rolling plate shape according to small convexity control, convexity 30μm;

[0064] Cold rolling: total cold rolling reduction rate is 80%; 5# stand adopts 2.5μm roughness;

[0065] Continuous annealing and leveling: The cold-rolled thin plate is continuously annealed, the soaking temperature is 830℃, the terminal temperature of rapid cooling is 470℃, the strip speed is 130m / min, and the steel plate is leveled after continuous annealing, and the leveling elongation is 0.4%; the surface roughness of the roller is Ra1.8μm, and the roller surface RPc90;

[0066] Galvanizing: The zinc ion concentration in the plating solution is 160g / L, the pH value is 1.5, the plating solution temperature is 54°C, the free acid concentration in the plating solution is 11g / l, the speed of the strip passing through the plating tank is 80m / min; the tension of the electroplating process is 36KN.

[0067] Performance test results of Example 5

[0068]

[0069] The product produced in Example 5 has serious surface silk spots, the steel coil deviates seriously and causes edge damage, and the roughness Ra is low, which does not meet the performance and surface requirements of automobile outer panels.

[0070] Example 6

[0071] Substrate: Ultra-low carbon component design containing Ti is selected;

[0072] Hot rolling and coiling: 130min in furnace high temperature time, 230min in total; control the steel burning temperature, lower the heating temperature, furnace exit ≤1200℃, RT2 upper and lower surface full length temperature ≤1020℃, cancel the high temperature rolling process, lower the heating high temperature section temperature; wide strip steel plate shape control, rolling plate shape according to small convexity control, convexity 50μm;

[0073] Cold rolling: total cold rolling reduction rate is 82%; 5# stand adopts 2.5μm roughness;

[0074] Continuous annealing and leveling: The cold-rolled thin plate is continuously annealed, the soaking temperature is 830℃, the terminal temperature of rapid cooling is 470℃, the strip speed is 130m / min, and the steel plate is leveled after continuous annealing, and the leveling elongation is 0.4%; the surface roughness of the roller is Ra1.8μm, and the roller surface RPc90;

[0075] Galvanizing: The zinc ion concentration in the plating solution is 160g / L, the pH value is 1.5, the plating solution temperature is 54°C, the free acid concentration in the plating solution is 11g / l, the speed of the strip passing through the plating tank is 80m / min; the tension of the electroplating process is 53KN.

[0076] Performance test results of Example 6

[0077]

[0078] The product produced in Example 6 has serious surface silk spots, and the steel coil deviates seriously, resulting in edge damage, which does not meet the performance and surface requirements of automobile outer panels.

[0079] It should be noted that the description of the above technical solutions is exemplary, and this specification can be embodied in different forms and should not be interpreted as being limited to the technical solutions set forth herein. On the contrary, providing these descriptions will make the disclosure of the present invention thorough and complete, and will fully convey the scope disclosed in this specification to those skilled in the art. In addition, the technical solutions of the present invention are limited only by the scope of the claims.

[0080] Finally, it should be pointed out that the above embodiments are only representative examples of the present invention. Obviously, the present invention is not limited to the above embodiments, and there are many variations. Any simple modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention should be considered to belong to the protection scope of the present invention.

Claims

1. A method for producing wide-width electro-galvanized outer plates for side panels. Features: The base material is melted and cast into slabs, and then hot-rolled, cold-rolled, continuously annealed, skin-passed and electro-galvanized; The specific steps include: S1, hot rolling: based on the furnace time control range, high temperature time ≤ 120min, total time ≤ 220min; control the steel burning temperature, reduce the heating temperature, furnace ≤ 1200℃, RT2 upper and lower surface full length temperature ≤ 1020℃; wide strip steel plate shape control, rolling plate shape convexity target control within 30μm; S2, cold rolling; S3, continuous annealing and leveling: the soaking temperature is 820-860℃, the terminal temperature of rapid cooling is 440-470℃, and the strip speed is 120-150m / min; after continuous annealing, the steel plate is leveled, and the leveling elongation is 0.5-0.6%; S4. Electrogalvanizing: The zinc ion concentration in the plating solution is 100-140 g / L, the pH value range is 1.2-1.8, the plating solution temperature is controlled at 50-52°C, the free acid concentration in the plating solution is controlled in the range of 5-7 g / l, the speed of the strip passing through the electroplating tank is 60-100 m / min; the tension of the strip in the electroplating section is increased to above 52 KN.

2. The method for producing the wide-width electrogalvanized outer sheet for side panels according to claim 1, Features: In step S1, high-pressure water descaling is started for all rough rolling passes, and the replacement cycle of the descaling nozzle is less than 6 months.

3. The method for producing the wide-width electro-galvanized outer sheet for side panels according to claim 1, Features: In step S2, the 5# rack adopts a roughness of 3.0 μm.

4. The method for producing a wide-width electrogalvanized outer sheet for side panels according to claim 1, Features: In step S3, the surface roughness Ra of the rolling mill roll is controlled between 2.0 and 2.3 μm, and the surface roughness RPc of the rolling mill roll is controlled above 100.

5. The method for producing a wide-width electro-galvanized outer sheet for side panels according to claim 1, Features: In step S4, the strip steel after continuous annealing and leveling is cleaned by alkali washing, brushing, electrolytic degreasing and rinsing and then enters the electro-galvanizing tank, using a gravity electroplating process.

6. The method for producing a wide-width electrogalvanized outer sheet for side panels according to claim 1, Features: In step S4, the main salt component of the electro-galvanizing solution is zinc sulfate.

7. The method for producing a wide-width electro-galvanized outer sheet for side panels according to claim 1, Features: In step S2, the total cold rolling reduction ratio is 80 to 83%.

8. The method for producing a wide-width electro-galvanized outer sheet for side panels according to claim 1, Features: The components and weight percentage of the substrate are: C: ≤0.0012, Si: ≤0.02, Mn: 0.05-0.2, P: ≤0.02, S: ≤0.01, Al: 0.03-0.09, Ti≤0.03%, and the balance is Fe and other inevitable impurities.

9. The method for producing a wide-width electro-galvanized outer sheet for side panels according to claim 1, Features: The electro-galvanized outer plate produced has a yield point RP0.2: 100~150Mpa; tensile strength Rm: 250~310Mpa; elongation A80mm: ≥46%; plastic strain ratio r90≥2.5, and work hardening index n90≥0.

23.

10. The method for producing a wide-width electro-galvanized outer sheet for side panels according to claim 1, Features: Applicable to electro-galvanized outer panels above 1750mm.

Citation Information

Patent Citations

  • Method for producing cold-rolled sheet for surface coating and plating base plate

    CN102716905A

  • Hot galvanizing steel plate for car and production method thereof

    CN102839322A

  • Hot-rolled pickled steel plate for electrogalvanizing and production method thereof

    CN111455259A

  • Method for reducing color difference defect on surface of electro-galvanized plate

    CN115558760A

  • Method for producing alloyed galvanized plate with plate width larger than or equal to 1800 mm

    CN115647047A