Near-net forming manufacturing method for bearing retainer
Through the methods of upset punching, frame reaming and prototyping ring rolling, the problems of excessive waste and large cutting volume caused by rectangular cross-sectional blanks are solved, and the near-net forming of the bearing cage is achieved, which improves material utilization and Productivity.
Patent Information
- Application Number
- CN202411106302.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-12-03
AI Technical Summary
During the production process of existing bearing cages, rectangular cross-section blanks lead to a lot of waste and a large amount of cutting, resulting in low raw material utilization, high production costs and long processing cycles.
By using upset punching, frame reaming and prototyping ring rolling methods, the near-purity of special-shaped forgings is achieved through heating, blank making, upsetting, length drawing, punching, reaming, pressing flat and prototyping ring rolling. Forming.
The raw material utilization rate is improved by about 50%, reducing production costs, shortening processing cycles, and improving production efficiency.
Smart Images

Figure CN119056988A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of bearing processing, in particular to a near-net-shape manufacturing method for a bearing retainer. Background Art
[0002] The bearing cage, also known as the bearing retainer, is a bearing component used to isolate or guide the rolling element and keep it in the bearing. The bearing cage size of large bearings used in special fields is generally 1.5 meters to 4.5 meters in diameter. The finished product has a thin wall thickness and a complex shape. Most of the existing technologies still use upsetting punching, horse frame expansion, and ring rolling to produce forgings. Because the cross-section of the blank after ring rolling is rectangular, the wall thickness of the finished forging is thin, and more waste is generated during the machining process, resulting in low raw material utilization, high production costs, and long processing cycles. At the same time, the amount of cutting processing is large, resulting in increased cutting stress and processing deformation. Summary of the invention
[0003] In view of the above problems, the present application provides a near-net-form manufacturing method for a bearing retainer, which realizes the near-net-form of special-shaped forgings and solves the problems of large waste and large cutting amount caused by rectangular cross-section blanks.
[0004] The technical solution adopted by the present invention to solve the technical problem is:
[0005] A near-net-shape manufacturing method for a bearing retainer comprises the following steps:
[0006] First, cut the material;
[0007] Second, heating;
[0008] Third, blank making;
[0009] 3.1 The heated raw materials are sequentially subjected to upsetting, drawing and punching to obtain preforms;
[0010] 3.2 The preform obtained in step 3.1 is sleeved on the horse bar and placed on the horse frame for hole expansion;
[0011] 3.3 Place the preform after hole expansion vertically on the press workbench, and press and flatten the preform to make it reach a preset height H;
[0012] Fourth, the preform obtained in the third step is subjected to contour ring rolling by means of a ring rolling device, wherein a core roller of the ring rolling device comprises a central axis portion and a forming portion coaxially arranged on the central axis portion, a forming surface is arranged on the outer side of a main roller of the ring rolling device, and the forming portion is opposite to the forming surface, and a blank forging is obtained by extruding the preform.
[0013] Furthermore, the main roller is provided with limiting portions at the upper and lower ends of the forming surface, respectively, and the forming surface and the two limiting portions together form a forming groove.
[0014] Furthermore, in step 3.3, the flattened height H of the preform is less than or equal to the distance between the two limiting portions.
[0015] Furthermore, the blank forging obtained in the fourth step comprises two bearing retainers, and the two bearing retainers are symmetrically arranged with their large ends facing each other.
[0016] Furthermore, the blank forging obtained in the fourth step is segmented to obtain blank forging monomers, each of which comprises a bearing retainer.
[0017] Furthermore, the blank forging body is subjected to rough machining, NDT inspection and fine machining in sequence.
[0018] Furthermore, the raw material in the first step is a continuous casting round billet made of S355 material with a diameter of φ400 mm and a height-to-diameter ratio of 2.1.
[0019] Furthermore, in the second step, the raw materials are placed in a natural gas heating furnace and heated to 1230°C.
[0020] Furthermore, in the third step, the deformation amount of upsetting is 52%, and the deformation amount of hole expansion is 65%.
[0021] Furthermore, the core roller adopts an integral structure.
[0022] The beneficial effects of the present invention are:
[0023] The near-net-shape manufacturing method of a bearing retainer provided in the embodiment of the present application changes the existing forming method of upsetting punching, horse frame expansion, and rectangular ring rolling to a method of upsetting punching, horse frame expansion, and contoured ring rolling, thereby achieving near-net-shape forming of special-shaped forgings, solving the problems of large amounts of waste and large amounts of cutting caused by rectangular blanks, improving the utilization rate of raw materials, reducing production costs, and improving production efficiency. Compared with the same type of rectangular forgings, the bearing retainer forgings produced by the present application scheme have a material utilization rate of about 50% in terms of raw material consumption. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a schematic diagram of the structure during ring rolling;
[0025] Figure 2 It is a schematic diagram of the forging of the bearing cage blank;
[0026] Figure 3 It is a schematic diagram of the structure of the bearing cage blank forging after cutting;
[0027] Figure 4 This is a schematic diagram of the structure of the bearing retainer blank forging after machining after cutting.
[0028] In the figure: 11, main roller; 111, forming surface; 112, limiting part; 12, core roller; 121, central axis part; 122, forming part; 13, end roller;
[0029] 2. Preform;
[0030] 31. Blank forging; 32. Blank forging monomer;
[0031] 4. Finished product. DETAILED DESCRIPTION
[0032] In order to enable those skilled in the art to better understand the technical solutions in the present application, the technical solutions in the embodiments of the present application will be described in detail below in conjunction with the drawings in the embodiments of the present application, and the described embodiments are only part of the embodiments of the present application, not all of the embodiments. All other embodiments obtained by those skilled in the art without creative work on the basis of the embodiments of the present application shall belong to the protection scope of the present application.
[0033] A near-net-shape manufacturing method for a bearing retainer comprises the following steps:
[0034] First, blanking: As a specific implementation, the raw material in this embodiment is a continuous casting round billet made of S355 material with a diameter of 400 mm and a height-to-diameter ratio of 2.1.
[0035] Second, heating. Put the prepared S355 raw materials into a natural gas heating furnace and heat them to 1230℃. The heating process is carried out according to the heating specifications.
[0036] Third, blank making.
[0037] 3.1 The heated raw material is subjected to upsetting, drawing and punching in sequence to obtain a preform 2. The upsetting deformation is 52%.
[0038] 3.2 The preform 2 obtained in step 3.1 is sleeved on the horse bar and placed on the horse frame for hole expansion. The hole expansion deformation is 65%, and the inner diameter of the preform 2 after hole expansion is larger than the maximum diameter of the core roller 12, so that the preform 2 can be smoothly sleeved on the core roller 12 of the ring rolling machine.
[0039] When punching in step 3.1, the diameter of the punch used should be larger than the diameter of the horse bar, so as to ensure that the horse bar can pass through the preform 2 obtained in step 3.1. As a specific implementation, the diameter of the horse bar in this embodiment is 220mm, and when punching in step 3.1, the diameter of the punch used is 250mm. Since the raw material will shrink to a certain extent after punching, the use of a 250mm punch can ensure that the inner diameter of the preform 2 is larger than the diameter of the horse bar.
[0040] 3.3 Leveling. The manipulator places the preform 2 after hole expansion vertically (ie, the axis of the preform 2 extends in the vertical direction) on the press workbench, and presses and levels the preform 2, so that the preform 2 reaches a preset height H.
[0041] Fourthly, the preform 2 obtained in the third step is subjected to profile ring rolling by a ring rolling device to obtain a blank forging 31 .
[0042] like Figure 1 As shown, the preform 2 obtained in the third step is placed on the workbench of the ring rolling equipment, the core roller 12 of the ring rolling equipment is inserted into the inner hole of the preform 2, and the preform 2 is pushed against the main roller 11 of the ring rolling equipment, and the end of the preform 2 facing away from the main roller 11 is extended between the two end rollers 13, and then the ring rolling equipment is turned on for ring rolling.
[0043] like Figure 1 As shown, the core roller 12 includes a central axis portion 121 and a forming portion 122 coaxially arranged on the central axis portion 121, and a forming surface 111 coaxially arranged with the main roller 11 is provided on the outer cylindrical surface of the main roller 11. The forming portion 122 is opposite to the forming surface 111, and the blank forging 31 is obtained by extruding the preform 2. The inner edge of the cross section of the blank forging 31 coincides with the cross section shape of the forming portion 122, and the outer edge of the cross section of the blank forging 31 coincides with the interface of the forming surface 111.
[0044] By adopting a core roller 12 and a main roller 11 whose shapes match those of the bearing retainer, a blank forging 31 whose shape is close to that of the bearing retainer is directly obtained under the extrusion of the core roller 12 and the main roller 11, thereby achieving near-net forming of the bearing retainer, solving the problems of large waste and large cutting amount caused by rectangular blanks, improving the utilization rate of raw materials, reducing production costs, and improving production efficiency.
[0045] Furthermore, if Figure 1As shown, the main roller 11 is provided with limiting portions 112 at the upper and lower ends of the forming surface 111, and the forming surface 111 and the two limiting portions 112 together form a forming groove coaxially surrounding the outside of the main roller 11. In step 3.3, the flattened height H of the preform 2 is less than or equal to the distance between the two limiting portions 112. This can prevent the blank forging 31 from moving up and down during the ring rolling process, and can reliably limit the overall height of the blank forging 31 through the two limiting portions 112, thereby ensuring the reliability of the processing size.
[0046] Preferably, the core roller 12 adopts an integral structure.
[0047] Furthermore, if Figure 2 As shown, the blank forging 31 obtained in the fourth step includes two bearing retainers, which are symmetrically arranged with their large ends facing each other. Accordingly, in the first step, sawing and cutting are performed according to the weight of the blanking of two pieces in one.
[0048] Furthermore, if Figure 2 and Figure 3 As shown, according to Figure 2 The blank forging 31 obtained in the fourth step is divided according to the dividing line shown in Figure 3 The blank forging units 32 shown, each of which includes a bearing retainer.
[0049] The use of a two-piece near-net-shape forming method not only reduces the production cycle of a single product, but also reduces processing allowances and improves material utilization.
[0050] Furthermore, the blank forging unit 32 is subjected to rough machining, NDT inspection and fine machining in sequence to obtain a finished product 4.
[0051] Other embodiments obtained by those skilled in the art by combining, splitting, reorganizing, etc. the embodiments of the present application on the basis of the embodiments provided in the present application do not exceed the protection scope of the present application.
[0052] The above specific implementation methods have detailed the purpose, technical solutions and beneficial effects of the embodiments of the present application. The above are only specific implementation methods of the embodiments of the present application and are not used to limit the protection scope of the embodiments of the present application. That is, any modifications, equivalent substitutions, improvements, etc. made on the basis of the embodiments of the present application should be included in the protection scope of the embodiments of the present application.
Claims
1. A near-net-shape manufacturing method for a bearing retainer, characterized in that: The following steps are included: First, cut the material; Second, heating; Third, blank making; 3.1 The heated raw material is subjected to upsetting, drawing and punching in sequence to obtain a preform (2); 3.2 The preform (2) obtained in step 3.1 is sleeved on the horse bar and placed on the horse frame for hole expansion; 3.3 vertically placing the preform (2) after hole expansion on the press workbench, and pressing and flattening the preform (2) to make the preform (2) reach a preset height H; Fourth, the preform (2) obtained in the third step is subjected to profile ring rolling by means of a ring rolling device, wherein the core roller (12) of the ring rolling device comprises a central axis portion (121) and a forming portion (122) coaxially arranged on the central axis portion (121), and a forming surface (111) is arranged on the outer side of the main roller (11) of the ring rolling device, and the forming portion (122) is opposite to the forming surface (111), and a blank forging (31) is obtained by extruding the preform (2).
2. A near-net-shape manufacturing method for a bearing retainer according to claim 1, characterized in that: The main roller (11) is provided with limiting portions (112) at the upper and lower ends of the molding surface (111), respectively, and the molding surface (111) and the two limiting portions (112) together form a molding groove.
3. A near-net-shape manufacturing method for a bearing retainer according to claim 2, characterized in that: In step 3.3, the flattened height H of the preform (2) is less than or equal to the distance between the two limiting portions (112).
4. A near-net-shape manufacturing method for a bearing retainer according to claim 1, characterized in that: The blank forging (31) obtained in the fourth step comprises two bearing retainers, which are symmetrically arranged with their large ends facing each other.
5. A near-net-shape manufacturing method for a bearing retainer according to claim 4, characterized in that: The blank forging (31) obtained in the fourth step is divided to obtain blank forging monomers (32), each of which comprises a bearing retainer.
6. A near-net-shape manufacturing method for a bearing retainer according to claim 5, characterized in that: The blank forging single body (32) is subjected to rough machining, NDT inspection and fine machining in sequence.
7. A near-net-shape manufacturing method for a bearing retainer according to claim 1, characterized in that: The raw material in the first step is a continuous casting round billet made of S355 material with a diameter of φ400mm and a height-to-diameter ratio of 2.
1.
8. The near-net-shape manufacturing method of a bearing retainer according to claim 1, characterized in that: In the second step, the raw materials are placed in a natural gas heating furnace and heated to 1230°C.
9. The near-net-shape manufacturing method of a bearing retainer according to claim 1, characterized in that: In the third step, the deformation amount of upsetting is 52% and the deformation amount of hole expansion is 65%.
10. The near-net-shape manufacturing method of a bearing retainer according to claim 1, characterized in that: The core roller (12) adopts an integral structure.
Citation Information
Patent Citations
Method for simultaneously rolling and expanding two trapezoid-cross-section flange ring forge pieces
CN102615223A
Low-alloy high-strength high-impact-energy extra-large special-shaped ring forging and forging method thereof
CN108914015A
Near net forming method of extra-large bearing iron retainer
CN110625056A
Profiling ring rolling forming technology for arc inner table ring-shaped forge piece
CN110773690A
Near-net forming method for high-temperature alloy special-shaped ring forged piece
CN114309398A