Luminescent polycarbonate membrane
Through the three-layer structure design of the luminescent polycarbonate diaphragm, the wear and fall of the polycarbonate anti-counterfeiting coating is solved, and efficient and long-term anti-counterfeiting effect is achieved, simplifying the process flow and reducing costs.
Patent Information
- Application Number
- CN202411307978.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-12-03
AI Technical Summary
The existing polycarbonate anti-counterfeiting coatings are prone to wear and fall off during use, resulting in a reduced anti-counterfeiting effect, and are complex in process and high in cost, which affects information security.
The three-layer structure design of luminescent polycarbonate diaphragm is designed, the intermediate layer is a luminescent agent, and the upper and lower surface layers are light diffusing agents. It is prepared by a twin-screw extruder and a three-layer co-extrusion calendering film forming process to avoid chemical adhesives The use of the anti-counterfeiting coating improves the uniformity and durability of the anti-counterfeiting coating.
It realizes the efficient and long-term effect of the anti-counterfeiting coating, avoids wear and peeling problems, simplifies the process flow, reduces production costs, and improves the light transmittance and haze of the material, and has good application prospects.
Smart Images

Figure CN119058207A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polycarbonate films and relates to a luminous polycarbonate membrane. Background Art
[0002] Polycarbonate is a thermoplastic material with excellent electrical insulation, light stability, transparency, heat resistance, good mechanical properties, etc. With the advancement of science and technology, the application areas of polycarbonate are gradually expanding, such as electronic appliances, new energy, optical materials, automobiles, etc. With the acceleration of the globalization process, the frequency of exchanges between people and materials is increasing, which in turn puts forward higher requirements for information security technology.
[0003] According to traditional technology classification, it can be divided into digital and material categories: the former uses physical signal detection to detect the authenticity of information with the help of chips and antennas; the latter uses special materials to achieve the purpose of information anti-counterfeiting, and applies ink with specific anti-counterfeiting functions on a preset polymer substrate through printing, coating and other means. This type of ink includes: ultraviolet fluorescent anti-counterfeiting ink, thermosensitive anti-counterfeiting ink, photosensitive color-changing anti-counterfeiting ink, magnetic anti-counterfeiting ink, visual color-changing anti-counterfeiting ink, pressure-sensitive anti-counterfeiting ink and anti-alteration anti-counterfeiting ink. However, the ink used contains volatile irritating solvents, which have adverse effects on human health and pollute the natural environment; in addition, the process is cumbersome and the production cost is high. At the same time, during use, the anti-counterfeiting coating will wear and fall off, affecting or even losing the anti-counterfeiting effect. Summary of the invention
[0004] In order to overcome the above-mentioned shortcomings, one of the purposes of the present invention is to provide a luminous polycarbonate film, which can avoid the problems of wear and fall of the anti-counterfeiting coating and improve the timeliness and reliability of anti-counterfeiting. In order to achieve the above objectives, the technical solution adopted by the present invention is: a luminescent polycarbonate film, including an intermediate layer and a surface layer, the surface layer including an upper surface layer and a lower surface layer arranged in the thickness direction of the intermediate layer; the raw materials for preparing the intermediate layer include polycarbonate, a luminescent agent and a dispersant, and the raw materials for preparing the surface layer include polycarbonate, a light diffuser and a dispersant.
[0005] The addition of luminescent agent makes polycarbonate present special fluorescent effect under specific light conditions. Light diffuser increases the haze of the material and improves the uniformity of luminescence. Dispersant helps the luminescent agent and light diffuser to be evenly dispersed in the polycarbonate matrix, improves the compatibility of the luminescent agent and light diffuser with the matrix, improves the physical properties of the material, improves the surface crystal points and convex point defects, and has excellent comprehensive performance, rapid light response, uniform luminescence, few surface crystal points and few convex point defects.
[0006] Furthermore, the melt volume flow rate of the polycarbonate is 8-12 cm³ / 10 min. The melt volume flow rate MVR is measured according to ISO 1133 standard, and the test conditions are as follows: 300° C., 1.2 kg.
[0007] Furthermore, the light diffusing agent is selected from one or more of silicones, acrylates, and silicon powder.
[0008] Furthermore, the light diffuser is selected from one or more of organic silicone resin spherical powder, core-shell acrylate, and spherical silicon powder.
[0009] Furthermore, the dispersant is selected from one or more of stearic acid amide, palmitamide, and ethylene bis-12-hydroxystearic acid amide.
[0010] Furthermore, the luminescent agent is selected from one or more of oxides, nitrides, nitrogen oxides, sulfides, selenides, halides, zinc, cadmium, manganese, aluminum, silicon, and rare earth metals.
[0011] Furthermore, the luminescent agent is selected from one or more of alkaline earth aluminates, sulfides, and alkaline earth silicates.
[0012] Furthermore, the raw materials for preparing the surface layer include 94.5-99.8 parts of polycarbonate, 0.1-5 parts of light diffuser and 0.1-0.5 parts of dispersant by weight. By limiting the parts of polycarbonate, light diffuser and dispersant in the raw materials of the surface layer, the surface layer has good light transmittance and haze.
[0013] Exemplarily, the raw materials for preparing the surface layer include polycarbonate in an amount of 94.5 parts, 95 parts, 96 parts, 97 parts, 98 parts, 99 parts, 99.8 parts or a range consisting of any two of them; The amount of the light diffuser is 0.1 part, 0.5 part, 1 part, 2 parts, 3 parts, 4 parts, 5 parts or any two of them; The amount of the dispersant is 0.1 part, 0.5 part, 1 part, 2 parts, 3 parts, 4 parts, 5 parts or a range consisting of any two of them.
[0014] Furthermore, the raw materials for preparing the intermediate layer include, by weight, 94.5-99.8 parts of polycarbonate, 0.1-5 parts of luminescent agent and 0.1-0.5 parts of dispersant.
[0015] Exemplarily, the amount of the luminescent agent is 0.1 parts, 0.5 parts, 1 parts, 2 parts, 3 parts, 4 parts, 5 parts or a range consisting of any two of them.
[0016] Further, the thickness of the luminescent polycarbonate film is 100-900 μm. Exemplarily, the thickness of the luminescent polycarbonate film is 100 μm, 200 μm, 300 μm, 400 μm, 500 μm, 600 μm, 700 μm, 800 μm, 900 μm or a range consisting of any two thereof.
[0017] Furthermore, the thickness of the upper surface layer and the lower surface layer are equal.
[0018] Further, the thickness of the upper surface layer is 30-270 μm, the thickness of the middle layer is 40-400 μm, and the thickness of the lower surface layer is 30-270 μm. Exemplarily, the thickness of the upper surface layer or the lower surface layer is 30 μm, 50 μm, 100 μm, 150 μm, 200 μm, 250 μm, 270 μm, or any two thereof; the thickness of the middle layer is 40 μm, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm, 400 μm, or any two thereof.
[0019] Further, the thickness ratio of the upper surface layer to the middle layer is 1:0.5 to 8, and the thickness ratio of the lower surface layer to the middle layer is 1:0.5 to 8. Exemplarily, the thickness ratio of the upper surface layer or the lower surface layer to the middle layer is 1:0.5, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8 or a range consisting of any two thereof.
[0020] A method for preparing the luminous polycarbonate film as described above comprises the following steps: S1, 94.5-99.8 parts of polycarbonate, 0.1-5 parts of light diffusing agent, and 0.1-0.5 parts of dispersing agent are mixed, and melt-extruded and granulated by a twin-screw extruder to obtain a surface layer material; S2, 94.5-99.8 parts of polycarbonate, 0.1-5 parts of luminescent agent and 0.1-0.5 parts of dispersant are mixed, and melt-extruded and granulated by a twin-screw extruder to obtain an intermediate layer material; S3, the surface layer material and the middle layer material are added into the ABC three-layer sheet single screw extruder, and after being melted and plasticized by the screw, they pass through the slit of the flat die head of the three-layer structure and enter the three-roller calendering to form a luminous polycarbonate film.
[0021] In the preparation method, the three-layer film is compounded together by adopting the process of three-layer co-extrusion film forming. The process is simple, no chemical adhesive is used in the processing, it is environmentally friendly, and it has high performance characteristics, so it can achieve the purpose of changing the luminous brightness and uniformity, and has good application prospects.
[0022] Further, the polycarbonate is dried at 100-110° C. for 4-5 hours; the light diffusing agent is dried at 60-70° C. for 5-8 hours; and the luminescent agent is dried at 100-110° C. for 4-5 hours.
[0023] Furthermore, the screw speed of the twin-screw extruder in S2 is 400 rpm / min.
[0024] Furthermore, the temperatures of each zone of the twin-screw extruder in S2 are: 90°C in zone 1, 240°C in zone 2, 250°C in zone 3, 260°C in zone 4, 260°C in zone 5, 260°C in zone 6, and the die head temperature is 260°C.
[0025] Furthermore, S3 also includes the following step: drying the surface layer material and the middle layer material at 100-110° C. for 4-5 hours, so that the moisture content of the surface layer material and the middle layer material is less than 0.02%.
[0026] Further, in S3, the process temperature of the ABC three-layer sheet single screw extruder is: screw section temperature 240-270°C, connector temperature 260-270°C, die head temperature 270°C, and calender roller temperature 100-110°C. Furthermore, the A screw in the ABC three-layer sheet single screw extruder corresponds to the middle layer of the film, the B screw corresponds to the upper surface layer of the film, and the C screw corresponds to the lower surface layer of the film.
[0027] The beneficial effects of the present invention are: 1) The luminescent polycarbonate film is a sandwich structure, with the middle layer being the luminescent layer and the upper and lower layers being the light diffusion layers. The luminescent agent is dispersed in the polycarbonate to make the luminescent layer, and the light diffusion agent is dispersed in the polycarbonate to make the light diffusion layer. By adding the luminescent agent and the light diffusion agent, polycarbonate has a special fluorescent effect under certain conditions. This polycarbonate is melt extruded to prepare a film with an anti-counterfeiting fluorescent effect, thereby avoiding the problem of wear and fall-off of the anti-counterfeiting coating, and improving the timeliness and reliability of anti-counterfeiting.
[0028] 2) Dispersants help the luminescent agent and light diffuser to be evenly dispersed in the polycarbonate matrix, improve the compatibility of the luminescent agent and light diffuser with the matrix, improve the material properties, improve the surface crystal points and convex point defects, and have excellent comprehensive performance, rapid light response, uniform luminescence, few surface crystal points, and few convex point defects.
[0029] 3) The three-layer film is compounded together by a three-layer co-extrusion film forming process. The process is simple, no chemical adhesives are used in the processing, it is environmentally friendly, and has high performance characteristics, achieving the purpose of changing the luminous brightness and uniformity, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The illustrative embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0031] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0032] Figure 1 This is a schematic diagram of the luminous polycarbonate film of the present invention; Figure 2 This is a SEM image of the luminescent polycarbonate film of the present invention.
[0033] Among them: 1. middle layer; 2. upper surface layer; 3. lower surface layer; 4. light diffuser particles; 5. luminescent agent particles. DETAILED DESCRIPTION
[0034] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0035] Except as shown in the operating examples or otherwise indicated, all numbers used in the specification and claims to indicate the amount of ingredients, physicochemical properties, etc. are understood to be adjusted by the term "about" in all cases. Therefore, unless otherwise indicated, the numerical parameters listed in the above specification and the attached claims are approximate values, and those skilled in the art can use the teachings disclosed herein to seek to obtain the desired properties and appropriately change these approximate values. The use of numerical ranges expressed as endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4 and 5, etc.
[0036] The luminescent polycarbonate film of the present invention is a sandwich structure, wherein the middle layer is the luminescent layer, and the upper and lower layers are light diffusion layers. The luminescent agent is dispersed in the polycarbonate to make the luminescent layer, and the light diffusion agent is dispersed in the polycarbonate to make the light diffusion layer. The light diffusion principle formula is as shown in Formula 1, wherein I in Formula 1 is P is the scattered light intensity, N is the unit volume element of the scattering particle, r is the radius of the scattering particle, m is the ratio of the dispersed phase to the dispersed medium, φ χis the angle between the incident light beam and the observation direction, d is the distance between the observer and the scattering particles, A is the wavelength of the incident light, and I0 is the intensity of the incident light.
[0037]
[0038] Formula 1 Middle layer: The raw materials for preparing the middle layer include 94.5-99.8 parts of polycarbonate, 0.1-5 parts of luminescent agent and 0.1-0.5 parts of dispersant, wherein: the MVR of the polycarbonate is 8-12 cm³ / 10min.
[0039] The luminescent agent is an oxide, nitride, nitrogen oxide, sulfide, selenide, halide or one or a mixture of zinc, cadmium, manganese, aluminum, silicon and various rare earth metals. When the luminescent agent is irradiated with light of a specific wavelength, it will be excited to produce fluorescence of a specific wavelength, and this fluorescence has a special color.
[0040] Dispersant is one or a mixture of stearic acid amide, palmitamide, ethylene bis-12-hydroxystearic acid amide. Dispersant (Dispersing agent) is a surfactant, and its structure consists of an anchoring segment and a chain segment. The anchoring segment can be adsorbed and or bonded to the surface of the dispersed particles, and the chain segment can be dissolved in the matrix, so that the interface energy between the dispersed particles and the matrix is reduced, so that the dispersed particles can be evenly distributed in the matrix. Due to its large molecular weight, it can stably adsorb on the surface of the dispersed particles, is not easy to fall off, and can prevent the particles from settling or agglomerating, thereby promoting the dispersed particles to be stably dispersed in the matrix.
[0041] surface layer: The surface layer comprises an upper surface layer and a lower surface layer arranged in the thickness direction of the middle layer. The raw materials for preparing the surface layer comprise 94.5-99.8 parts of polycarbonate, 0.1-5 parts of light diffuser and 0.1-0.5 parts of dispersant.
[0042] The polycarbonate in the surface layer and the polycarbonate in the middle layer are made of the same raw material, and the melt volume flow rate MVR is 8-12cm³ / 10min.
[0043] The light diffuser is one or a mixture of organic silicon, acrylate, and silicon micropowder. Due to the different refractive indices of the substrate and the light diffuser, the light will be refracted multiple times after passing through the diffuser, making the light uniform and achieving a soft light effect. At the same time, the light energy loss is small, thus solving the problem of uniform light and light transmission.
[0044] The dispersant is one or a mixture of stearic acid amide, palmitamide, ethylene bis-12-hydroxystearic acid amide. Dispersant (Dispersing agent) is a surfactant, and its structure consists of an anchoring segment and a chain segment. The anchoring segment can be adsorbed and or bonded to the surface of the dispersed particles, and the chain segment can be dissolved in the matrix, so that the interface energy between the dispersed particles and the matrix is reduced, so that the dispersed particles are evenly distributed in the matrix. Due to its large molecular weight, it can stably adsorb on the surface of the dispersed particles, is not easy to fall off, and can prevent the particles from settling or agglomerating, thereby promoting the dispersed particles to be stably dispersed in the matrix.
[0045] Sandwich structure: See attached Figure 1 and attached Figure 2 As shown, the middle layer 1 is a luminescent layer, and the upper surface layer 2 and the lower surface layer 3 are both light diffusion layers. The luminescent agent particles 5 are dispersed in the polycarbonate to form the luminescent layer, and the light diffusion agent particles 4 are dispersed in the polycarbonate to form the light diffusion layer. Under the action of the dispersant, the luminescent agent (particle size: 20-50μm) changes the interface between the luminescent agent and the matrix polycarbonate, avoids the luminescent agent agglomeration, and then shows a certain luminescent uniformity.
[0046] The light diffuser in the surface layer can be evenly dispersed in the polycarbonate matrix under the action of the dispersant, thereby improving the haze of the material. When light hits the light diffuser, it scatters, making the light evenly dispersed, thereby improving the uniformity of the film's luminescence. In addition, the surface layer in the three-layer structure design can also cover the surface defects of the middle layer and improve the appearance.
[0047] An embodiment of the present invention provides a method for preparing a luminescent polycarbonate film, which specifically comprises the following steps: S1: Weigh 94.5-99.8 parts of polycarbonate, 0.1-5 parts of light diffuser and 0.1-0.5 parts of dispersant, dry the polycarbonate at 100-110° C. for 4-5 hours, dry the light diffuser at 60-70° C. for 5-8 hours, mix them evenly, and melt-extrude and granulate them through a twin-screw extruder to obtain a surface material; S2: Weigh 94.5-99.8 parts of polycarbonate, 0.1-5 parts of luminescent agent and 0.1-0.5 parts of dispersant, dry the polycarbonate and luminescent agent at 100-110°C for 4-5 hours, mix them evenly, and melt-extrude and granulate them through a twin-screw extruder to obtain an intermediate layer material. The screw speed of the twin-screw extruder is 400rpm / min, and the temperatures of each zone of the twin-screw extruder are: 90°C for zone 1, 240°C for zone 2, 250°C for zone 3, 260°C for zone 4, 260°C for zone 5, 260°C for zone 6, and 260°C for die head.
[0048] S3: drying the surface layer material prepared in S1 and the intermediate layer material prepared in S2 at 100-110° C. for 4-5 hours to make the moisture content less than 0.02%; The dried surface layer material and the middle layer material are added to the ABC three-layer sheet single screw extruder, melted and plasticized by the screw, and then passed through the three-layer flat die slit to enter the three-roller calendering to form a luminous polycarbonate film. The A screw in the ABC three-layer sheet single screw extruder corresponds to the middle layer of the film, the B screw corresponds to the upper surface layer of the film, and the C screw corresponds to the lower surface layer of the film.
[0049] ABC three-layer sheet single screw extruder process temperature: screw section temperature 240-270℃, connector temperature 260-270℃, die head temperature 270℃, calender roller temperature 100-110℃.
[0050] The three-layer film is compounded together by a three-layer co-extrusion film forming process. The process is simple, no chemical adhesives are used in the processing, it is environmentally friendly, and has high performance characteristics, so it can achieve the purpose of changing the luminous brightness and uniformity, and has good application prospects.
[0051] Example The following examples describe the disclosure of the present invention in more detail, and these examples are intended for illustrative purposes only, as various modifications and variations within the scope of the disclosure of the present invention will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.
[0052] in:
[0053] Example 1 The weight percentages of the surface layer material and the middle layer material of a luminous polycarbonate film are shown in Table 1.
[0054] The preparation method of the luminescent polycarbonate film comprises the following steps: S1: Weigh polycarbonate, silicone resin spherical micropowder light diffuser, and ethylene bis-12-hydroxystearic acid amide according to weight, dry the polycarbonate at 105±5°C for 4 hours, and dry the light diffuser at 65±5°C for 6 hours, mix them evenly, and melt-extrude and granulate them through a twin-screw extruder to obtain a surface material; S2: Weigh polycarbonate, luminescent alkaline earth aluminate, and ethylene bis-12-hydroxystearic acid amide according to their weight proportions, dry the polycarbonate and luminescent alkaline earth aluminate at 105±5°C for 5 hours, mix them evenly, and melt-extrude and granulate them through a twin-screw extruder to obtain an intermediate layer material; wherein the screw speed of the twin-screw extruder is 400rpm / min, and the temperatures of each zone of the twin-screw extruder are: 90°C for zone 1, 240°C for zone 2, 250°C for zone 3, 260°C for zone 4, 260°C for zone 5, 260°C for zone 6, and 260°C for die head.
[0055] S3: drying the surface layer material prepared in S1 and the middle layer material prepared in S2 at 105±5°C for 4 hours, wherein the moisture content of the surface layer material and the middle layer material is less than 0.02%; The dried surface layer material and the middle layer material are added into the ABC three-layer sheet single screw extruder, melted and plasticized by the screw, and then passed through the slit of the three-layer flat die head to enter the three-roller calendering to make a luminous polycarbonate film.
[0056] ABC three-layer sheet single screw extruder process temperature: screw section temperature 255±15℃, connector temperature 265±5℃, die head temperature 270℃, calender roller temperature 105±5℃. See attached Figure 2 As shown, the A screw in the ABC three-layer sheet single screw extruder corresponds to the middle layer 1 of the film, the B screw corresponds to the upper surface layer 2 of the film, and the C screw corresponds to the lower surface layer 3 of the film.
[0057] Example 2-3 The difference between Example 2-3 and Example 1 is that the polycarbonate and light diffuser components of the surface material are different, and the rest are the same as Example 1. The specific components are shown in Table 1.
[0058] Example 4 The difference between Example 4 and Example 1 is that the polycarbonate and luminescent agent components of the intermediate layer material are different, and the rest are the same as Example 1. The specific components are shown in Table 1.
[0059] Embodiment 5-6 The difference between Example 5-6 and Example 4 is that the polycarbonate and light diffuser components of the surface material are different, and the rest are the same as Example 4. The specific components are shown in Table 1.
[0060] Example 7 The difference between Example 7 and Example 1 is that the polycarbonate and luminescent agent components of the intermediate layer material are different, and the rest are the same as Example 1. The specific components are shown in Table 1.
[0061] Embodiment 8-9 The difference between Example 8-9 and Example 7 is that the polycarbonate and light diffuser components of the surface material are different, and the rest are the same as Example 7. The specific components are shown in Table 1.
[0062] Examples 10-13 The difference between Examples 10-13 and Example 1 is that the diaphragm thickness is different, and the other aspects are the same as Example 1. The specific diaphragm thickness is shown in Table 2.
[0063] Examples 14-16 The difference between Examples 14-16 and Example 1 is that the thickness ratios of each layer are different, and the rest are the same as Example 1. The specific layer thicknesses are shown in Table 2.
[0064] Embodiment 17 The difference between Example 17 and Example 1 is that the light diffuser added is a core-shell type acrylate light diffuser, the luminescent agent is a sulfide, and the dispersant is stearic acid amide. The rest is the same as Example 1.
[0065] Embodiment 18 The difference between Example 18 and Example 1 is that the light diffuser added is spherical silicon micropowder light diffuser, the luminescent agent is alkaline earth silicate, and the dispersant is palmitamide. The rest is the same as Example 1.
[0066] Comparative Example 1 The difference between this comparative example and Example 1 is that the surface material does not contain a light diffuser, and the amount of the light diffuser is increased on the polycarbonate. The rest is the same as Example 1. The specific components are shown in Table 1.
[0067] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that the intermediate layer material does not contain a luminescent agent, and the proportion of the luminescent agent is increased on the polycarbonate. The other components are the same as those in Example 1. The specific components are shown in Table 1.
[0068] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that the light diffuser in the surface material is 7 parts, the polycarbonate is 92.9 parts, and the rest is the same as Example 1. The specific components are shown in Table 1.
[0069] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that the number of luminescent agents in the intermediate layer material is 7 parts, and the number of polycarbonate is 92.9 parts. The other parts are the same as those in Example 1. The specific components are shown in Table 1.
[0070] Comparative Example 5 The difference between Comparative Example 5 and Example 1 is that the light diffuser in the surface layer material and the luminescent agent in the middle layer material are both 7 parts, the polycarbonate is 92.9 parts, and the rest are the same as Example 1. The specific components are shown in Table 1.
[0071] Comparative Examples 6-7 The difference between Comparative Examples 6-7 and Example 1 is that the diaphragm thickness is different, and the other aspects are the same as Example 1. The specific diaphragm thickness is shown in Table 2.
[0072] Comparative Example 8 The difference between Comparative Example 8 and Example 1 is that the thickness of the lower surface layer is different and no upper surface layer is provided. The other aspects are the same as Example 1. The specific layer thickness is shown in Table 2.
[0073] Comparative Examples 9-10 The difference between Comparative Examples 9-10 and Example 1 is that the thickness of the surface layer is different, and the rest is the same as Example 1. The specific layer thickness is shown in Table 2.
[0074] Table 1: Comparison of dosage
[0075] Note: PC: polycarbonate; PD: light diffuser; DA: dispersant; LA: luminescent agent.
[0076] Experimental Example 1 The luminescent polycarbonate films prepared in Examples 1-18 and Comparative Examples 1-10 were subjected to thickness tests, specifically measuring the specific thickness and the thickness of the upper surface layer, the thickness of the middle layer and the thickness of the lower surface layer of the prepared luminescent polycarbonate films, wherein the thickness of the luminescent polycarbonate films was tested by a micrometer, and the layer thickness (the thickness of the upper surface layer, the thickness of the middle layer and the thickness of the lower surface layer) was tested by a scanning electron microscope, and the test results are shown in Table 2. .
[0077] Table 2: Thickness comparison table
[0078] Experimental Example 2 The performance test of the luminous polycarbonate films prepared in Examples 1-18 and Comparative Examples 1-10 was carried out. The transmittance and haze were tested by a transmittance / haze tester. The test standards were as follows: The tensile strength test standard is carried out in accordance with ISO 527; The test standard for elongation at break is carried out in accordance with ISO 527; The test standards for light transmittance and haze are based on ASTM D1003.
[0079] The test results are shown in Table 3.
[0080] Table 3: Performance comparison table
[0081] It can be seen from Table 3 that the luminescent polycarbonate films prepared in Examples 1-18 of the present invention have good luminescent intensity and luminescent uniformity based on good mechanical properties. Specifically, the tensile strength is 63-68 MPa, the elongation at break is 106-114%, the light transmittance is 62-84%, and the haze is 70-87%.
[0082] From the performance test data of the luminescent polycarbonate films prepared in Example 1 and Examples 14-16, it can be seen that the upper surface layer thickness: middle layer thickness: lower surface layer thickness is in the range of 1:0.5~8:1, and the prepared polycarbonate films have good tensile strength and transmittance.
[0083] From the performance test data of the luminescent polycarbonate films prepared in Example 1 and Examples 10-13, it can be seen that the luminescent polycarbonate films have a thickness in the range of 100-900 μm and have good mechanical properties, light transmittance and haze.
[0084] From the performance test data of the luminescent polycarbonate films prepared in Comparative Example 1 and Example 1, it can be seen that the surface material of Comparative Example 1 adopts a solution without a light diffusing agent, and the haze is poor, resulting in uneven luminescence.
[0085] From the performance test data of the luminescent polycarbonate films prepared in Comparative Example 2 and Example 1, it can be seen that the intermediate layer material of Comparative Example 2 adopts a solution without a luminescent agent, and the film does not emit light.
[0086] From the performance test data of the luminescent polycarbonate films prepared in Comparative Example 3 and Examples 1 and 3, it can be seen that the surface material of Comparative Example 3 adopts a high content of light diffusing agent, has high haze and poor light transmittance.
[0087] From the performance test data of the luminescent polycarbonate films prepared in Comparative Example 4 and Example 1, it can be seen that the intermediate layer material of Comparative Example 4 adopts a high-content luminescent agent solution, and the luminescent agent is an inorganic powder, which will cause a large loss of the elongation at break of the material and is not conducive to maintaining the mechanical properties.
[0088] From the performance test data of the luminescent polycarbonate films prepared in Comparative Example 5 and Example 1, it can be seen that the surface layer and middle layer materials of Comparative Example 5 use a high content of dispersant and luminescent agent, which has an adverse effect on the light transmittance and mechanical properties of the material.
[0089] From the performance test data of the luminescent polycarbonate films prepared in Comparative Examples 6-7 and Example 1, it can be seen that the film thickness of Comparative Example 6 is thin, 80 μm, the haze is poor, and the luminescence is uneven; the film thickness of Comparative Example 7 is high, 1000 μm, and the film transmittance is poor. The optimal thickness of the luminescent polycarbonate film is 100-900 μm.
[0090] From the performance test data of the luminescent polycarbonate films prepared in Comparative Examples 8-10 and Example 1, it can be seen that: Comparative Example 8 has no upper surface material, resulting in inconsistent haze on the upper and lower surfaces and uneven luminescence; the thickness of the surface layer of Comparative Examples 9-10 is inconsistent, resulting in inconsistent haze on the upper and lower surfaces and uneven luminescence. Therefore, the upper surface layer and the lower surface layer are set in the middle layer, and the thickness of the upper surface layer and the lower surface layer are the same, which has the best effect.
[0091] The present invention illustrates the detailed process equipment and process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process equipment and process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process equipment and process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, change of structural morphology, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0092] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0093] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0094] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A luminous polycarbonate film, characterized in that: It includes an intermediate layer and a surface layer, wherein the surface layer includes an upper surface layer and a lower surface layer arranged in the thickness direction of the intermediate layer; the raw materials for preparing the intermediate layer include polycarbonate, a luminescent agent and a dispersant, and the raw materials for preparing the surface layer include polycarbonate, a light diffuser and a dispersant.
2. The luminous polycarbonate film according to claim 1, characterized in that: The melt volume flow rate of polycarbonate is 8-12 cm³ / 10min.
3. The luminous polycarbonate film according to claim 1, characterized in that: The luminescent agent is selected from one or more of oxides, nitrides, nitrogen oxides, sulfides, selenides, halides, zinc, cadmium, manganese, aluminum, silicon, and rare earth metals.
4. The luminous polycarbonate film according to claim 1, characterized in that: The light diffuser is selected from one or more of silicone, acrylate and silica powder.
5. The luminous polycarbonate film according to claim 1, characterized in that: The dispersant is selected from one or more of stearic acid amide, palmitamide, and ethylene bis-12-hydroxystearic acid amide.
6. The luminous polycarbonate film according to claim 1, characterized in that: By weight, the raw materials for preparing the surface layer include 94.5-99.8 parts of polycarbonate, 0.1-5 parts of light diffuser and 0.1-0.5 parts of dispersant; the raw materials for preparing the middle layer include 94.5-99.8 parts of polycarbonate, 0.1-5 parts of luminescent agent and 0.1-0.5 parts of dispersant.
7. The luminous polycarbonate film according to claim 1, characterized in that: The thickness of the luminous polycarbonate film is 100-900 μm.
8. The luminous polycarbonate film according to claim 1, characterized in that: The thickness of the upper and lower surfaces is equal.
9. The luminous polycarbonate film according to claim 1, characterized in that: The thickness of the upper surface layer is 30~270μm, the thickness of the middle layer is 40~400μm, and the thickness of the lower surface layer is 30~270μm.
10. The luminous polycarbonate film according to claim 1, characterized in that: The thickness ratio of the upper surface layer to the middle layer is 1:0.5~8, and the thickness ratio of the lower surface layer to the middle layer is 1:0.5~8.
Citation Information
Patent Citations
Functional film as well as preparation method and application thereof
CN113502036A
Infrared penetration type polycarbonate composite material as well as preparation method and application thereof
CN115805740A
Phosphorescent sheet and manufacturing method thereof
JP2014079965A