Porous iron-based pyrophosphate positive electrode material, preparation method and application thereof
The preparation of a porous iron-based phosphoric acid pyrophosphate electrode material with enhanced conductivity addresses the conductivity issues of iron-based phosphate pyrophosphate cathodes, improving sodium-ion battery performance through increased sodium ion transmission and carbon coating uniformity.
Patent Information
- Application Number
- CN202411555576.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-04
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Iron-based phosphate pyrophosphate cathode materials in sodium-ion batteries suffer from low electronic and ionic conductivity due to agglomeration and large particle sizes, limiting their electrochemical performance and battery capacity.
A method to prepare a porous iron-based phosphoric acid pyrophosphate positive electrode material through spray-drying and sintering with a pore-forming agent, resulting in a material with a specific surface area of 15-30 cm²/g, enhancing sodium ion transmission and carbon coating uniformity.
The porous structure improves the electrochemical performance by increasing conductivity and material utilization, achieving discharge capacities of 109.1 to 118.4 mAh/g in sodium-ion batteries.
Smart Images

Figure CN119059509A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to a porous iron-based phosphoric acid pyrophosphate positive electrode material, a preparation method and application thereof in sodium ion batteries. Background Art
[0002] Sodium-ion batteries are expected to be widely used in energy storage due to their similar embedding chemical mechanism to lithium-ion batteries, lower raw material costs and abundant sodium resources. However, the development of sodium-ion batteries is restricted by cathode materials. At present, the cathode materials being studied include layered oxides, polyanions and Prussian blue materials. However, the irreversible phase change problem of layered oxides during the cycle, and the existence of crystal water and defects in Prussian blue materials limit their practical application. In comparison, polyanion cathode materials have stable cycle performance and are the best choice. Among them, iron-based phosphate pyrophosphate has the advantages of good structural stability and environmental friendliness, and has good application prospects. However, iron-based phosphate pyrophosphate still has the problem of low electronic and ionic conductivity, which must be solved by nano-sizing and carbon coating modification. Patent (CN115196610A) uses iron-based phosphate pyrophosphate cathode materials prepared by traditional synthesis methods. The material powder is easy to agglomerate and the particle size is large, resulting in low material specific surface area and electrode material utilization, which affects the battery capacity. In order to improve the electrochemical performance of iron-based phosphoric acid pyrophosphate cathode materials, it is necessary to develop an iron-based phosphoric acid pyrophosphate cathode material with a porous structure. Summary of the invention
[0003] In view of the problems existing in the prior art, the present invention provides a porous iron-based phosphoric acid pyrophosphate positive electrode material, a preparation method and application thereof in a sodium ion battery.
[0004] The present invention is achieved by a method for preparing a porous iron-based phosphoric acid pyrophosphate positive electrode material, comprising the following steps: (1) The sodium source, iron source, phosphorus source, carbon source and pore-forming agent are sand-milled in a certain proportion and then spray-dried to obtain a precursor.
[0005] (2) The precursor is placed in an inert atmosphere for sintering to obtain the porous mixed composite phosphate positive electrode material.
[0006] Furthermore, the sodium source is one or both of sodium oxalate and sodium carbonate.
[0007] Furthermore, the iron source is one or both of ferrous oxalate and ferric phosphate.
[0008] Furthermore, the phosphorus source is one or both of sodium dihydrogen phosphate and disodium hydrogen phosphate.
[0009] Furthermore, the carbon source is one or more of glucose, sucrose and citric acid.
[0010] Furthermore, the pore-forming agent is oxalic acid.
[0011] Furthermore, the sintering uses an inert atmosphere of argon or nitrogen or a mixed atmosphere of argon and hydrogen, and the sintering steps are sintering at 300-400° C. for 3-6 h and sintering at 450-650° C. for 5-15 h.
[0012] The present invention also provides a porous iron-based phosphoric acid pyrophosphate positive electrode material, wherein the porous iron-based phosphoric acid pyrophosphate positive electrode material is Na 3+x Fe 2+x (PO4) 1+x P2O7, where 0≤x≤1.5.
[0013] Furthermore, the specific surface area of the cathode material is 15-30 cm 2 g.
[0014] The present invention also provides an application of a porous iron-based phosphoric acid pyrophosphate positive electrode material in a sodium ion battery.
[0015] In combination with the above technical solutions and the technical problems solved, the advantages and positive effects of the technical solutions to be protected by the present invention are as follows: First, compared with the prior art, the porous iron-based phosphate pyrophosphate positive electrode material prepared by the present invention can not only nanosize the primary particles of the material, and the porous structure can increase the transmission rate of sodium ions, but also make the carbon coating more uniform, improve the conductivity of the material, and effectively improve the electrochemical performance of the material.
[0016] The method used in the present invention has the advantages of simple and controllable process and can realize large-scale industrial production.
[0017] Second, considering the technical solution as a whole or from the perspective of the product, the technical effects and advantages of the technical solution to be protected by the present invention are described in detail as follows: The preparation method of the porous iron-based phosphoric acid pyrophosphate positive electrode material provided by the invention is simple, controllable and low in cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a flow chart of the method for preparing porous iron-based phosphate pyrophosphate positive electrode material provided by an embodiment of the present invention.
[0019] Figure 2 This is the X-ray diffraction pattern of the Na4Fe3(PO4)2P2O7 sample provided in Example 1 of the present invention.
[0020] Figure 3This is a scanning electron microscope image of the Na4Fe3(PO4)2P2O7 sample provided in Example 1 of the present invention.
[0021] Figure 4 It is a charge and discharge curve diagram of the Na4Fe3(PO4)2P2O7 sample provided in Example 1 of the present invention after assembling the battery at a current density of 10 mA / g. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0023] In order to enable those skilled in the art to fully understand how to implement the present invention in detail, this section is an explanatory embodiment that expands and describes the technical solution of the claims.
[0024] like Figure 1 As shown, the method for preparing a porous iron-based phosphate pyrophosphate positive electrode material for a sodium ion battery provided by an embodiment of the present invention comprises the following steps: S01, grinding a sodium source, an iron source, a phosphorus source, a carbon source, and a pore-forming agent in a certain proportion, and then spray drying to obtain a precursor.
[0025] S02, placing the precursor in an inert atmosphere for sintering to obtain the porous iron-based phosphate pyrophosphate positive electrode material.
[0026] The porous iron-based phosphate pyrophosphate positive electrode material is Na 3+x Fe 2+x (PO4) 1+x P2O7, where 0≤x≤1.5.
[0027] The sodium source is one or both of sodium oxalate and sodium carbonate, the iron source is one or both of ferric oxalate and ferric phosphate, the phosphorus source is one or both of sodium dihydrogen phosphate and disodium hydrogen phosphate, the carbon source is one of glucose, sucrose and citric acid, and the pore former is oxalic acid.
[0028] The sintering process uses an inert atmosphere of argon or nitrogen or a mixed atmosphere of argon and hydrogen, and the sintering steps are sintering at 300-400° C. for 3-6 h and sintering at 450-650° C. for 5-15 h.
[0029] The specific surface area of the porous iron-based phosphoric acid pyrophosphate positive electrode material is 15-30 cm 2 g.
[0030] The embodiment of the present invention also provides an application of a method for preparing a porous iron-based phosphate pyrophosphate positive electrode material for a sodium ion battery. The porous iron-based phosphate pyrophosphate positive electrode material is prepared by the method for preparing a porous iron-based phosphate pyrophosphate positive electrode material for a sodium ion battery, which can nanosize the primary particles of the material. The porous structure can increase the transmission rate of sodium ions, and can also make the carbon coating more uniform, thereby increasing the conductivity of the material and effectively improving the electrochemical performance of the material.
[0031] The embodiment of the present invention also provides the use of the porous iron-based phosphate pyrophosphate positive electrode material in a sodium ion battery.
[0032] In order to make the disclosure of the present invention more complete, it is described below through more specific embodiments.
[0033] Example 1 Combine 5.3g Na2CO3, 28.77g FeC2O4, 15.08g FePO4, 35.99g NaH2PO4, 25g C6H 12 O6 and 9.0gH2C2O4 were added into 500ml water for dispersion, and then sand-milled at 2000r / min for 1h, followed by spray drying to obtain a precursor. The precursor was then placed in a tubular furnace and sintered at 300°C for 4h and at 550°C for 10h in an argon atmosphere to finally obtain a porous Na4Fe3(PO4)2P2O7 material. Figure 2 This is the XRD diagram of the porous Na4Fe3(PO4)2P2O7 material. It can be seen that there are no other impurities, indicating that the pure phase Na4Fe3(PO4)2P2O7 material has been successfully synthesized. Figure 3 This is a scanning electron microscope image of a porous Na4Fe3(PO4)2P2O7 material. It can be seen that the material has obvious pores, indicating that the synthesized Na4Fe3(PO4)2P2O7 material is porous. The material in the embodiment of the present invention is used as the positive electrode, metallic sodium is used as the negative electrode, glass fiber is used as the separator, and the electrolyte is 1 mol NaPF6 dissolved in a mixed solvent of propylene carbonate (PC), ethylene carbonate (EC) and ethyl methyl carbonate (EMC). Their volume ratio DMC:EC:EMC=1:1:1, button batteries are assembled, and charge and discharge tests are performed. The current density is 10 mA / g, and the voltage range is 2-4.0 V. Figure 4 The charge-discharge curve of the Na4Fe3(PO4)2P2O7 sample assembled into a battery at a current density of 10 mA / g provided in the embodiment of the present invention is shown in FIG. 1 . The battery can discharge 109.1 mAh g -1 The capacity reflects the good electrochemical performance.
[0034] Example 2 9.38 g Na2C2O4, 36.20 g FePO4, 14.19 g Na2HPO4, 20 g C6H8O7, and 4.5 g H2C2O4 were added to 500 ml water for dispersion, and then sand-milled at 2000 r / min for 1 h, followed by spray drying to obtain a precursor, which was then placed in a tubular furnace and sintered at 350 °C for 5 h and at 575 °C for 12 h in an argon atmosphere to obtain a porous Na 3.4 Fe 2.4 (PO4) 1.4 P2O7 material. The material in the embodiment of the present invention is used as the positive electrode, metallic sodium is used as the negative electrode, glass fiber is used as the separator, and the electrolyte is 1 mol NaPF6 dissolved in a mixed solvent of propylene carbonate (PC), ethylene carbonate (EC) and ethyl methyl carbonate (EMC), and their volume ratio DMC:EC:EMC=1:1:1. A button cell is assembled and a charge and discharge test is performed. The current density is 10 mA / g, the voltage range is 2-4.0 V, and the capacity discharged by the battery is 105.6 mAh g -1 .
[0035] Example 3 Combine 10.72g Na2C2O4, 14.39g FeC2O4, 24.13g FePO4, 23.99g NaH2PO4, 24g C 12 H 22 O 11 4.5 g H2C2O4 was added to 500 ml water for dispersion, and then sand milled at 2000 r / min for 1 h, followed by spray drying to obtain a precursor, which was then placed in a tubular furnace and sintered at 400 °C for 3 h and at 600 °C for 8 h in a nitrogen atmosphere to finally obtain a porous Na 3.6 Fe 2.6 (PO4) 1.6 P2O7 material. The material in the embodiment of the present invention is used as the positive electrode, sodium metal is used as the negative electrode, glass fiber is used as the separator, and the electrolyte is 1 mol NaPF6 dissolved in a mixed solvent of propylene carbonate (PC), ethylene carbonate (EC) and ethyl methyl carbonate (EMC), and their volume ratio DMC:EC:EMC=1:1:1. A button battery is assembled and a charge and discharge test is performed. The current density is 10 mA / g, the voltage range is 2-4.0 V, and the capacity discharged by the battery is 107.3 mAh g -1 .
[0036] Example 4 1.06 g Na2CO3, 28.77 g FeC2O4, 18.10 g FePO4, 28.39 g Na2HPO4, 25 g C6H8O7, and 11.25 g H2C2O4 were added to 500 ml of water for dispersion, and then sand-milled at 2000 r / min for 1 h, followed by spray drying to obtain a precursor, which was then placed in a tubular furnace and sintered at 370 ° C for 4 h and at 560 ° C for 13 h in an argon atmosphere to finally obtain a porous Na 4.2 Fe 3.2 (PO4) 2.2 P2O7 material. The material in the embodiment of the present invention is used as the positive electrode, metallic sodium is used as the negative electrode, glass fiber is used as the separator, and the electrolyte is 1 mol NaPF6 dissolved in a mixed solvent of propylene carbonate (PC), ethylene carbonate (EC) and ethyl methyl carbonate (EMC), and their volume ratio DMC:EC:EMC=1:1:1. A button cell is assembled and a charge and discharge test is performed. The current density is 10 mA / g, the voltage range is 2-4.0 V, and the capacity discharged by the battery is 113.5 mAh g -1 .
[0037] Example 5 6.70 g Na2C2O4, 2.65 g Na2CO3, 14.39 g FeC2O4, 37.70 g FePO4, 14.2 g Na2HPO4, 12.0 g Na2HPO4, 25 g C6H8O7, and 10 g H2C2O4 were added to 500 ml of water for dispersion, and then sand-milled at 2000 r / min for 1 h, followed by spray drying to obtain a precursor, which was then placed in a tubular furnace and sintered at 380 ° C for 4.5 h and at 580 ° C for 12 h in an argon: hydrogen = 95:5 atmosphere to finally obtain a porous Na 4.5 Fe 3.5 (PO4) 2.5 P2O7 material. The material in the embodiment of the present invention is used as the positive electrode, metallic sodium is used as the negative electrode, glass fiber is used as the separator, and the electrolyte is 1 mol NaPF6 dissolved in a mixed solvent of propylene carbonate (PC), ethylene carbonate (EC) and ethyl methyl carbonate (EMC), and their volume ratio DMC:EC:EMC=1:1:1. A button cell is assembled and a charge and discharge test is performed. The current density is 10 mA / g, the voltage range is 2-4.0V, and the capacity discharged by the battery is 118.4 mAh g -1 .
[0038] The present invention also prepared comparative examples 1-5 without adding pore-forming agent according to examples 1-5.
[0039] The embodiments of the present invention have achieved some positive effects during the development or use process, and indeed have great advantages over the prior art. The following content is described in conjunction with data, tables, etc. of the test process.
[0040] The specific surface area results of iron-based phosphoric acid pyrophosphate prepared in Examples 1-5 of the present invention and Comparative Examples 1-5 are shown in Table 1. As can be seen from Table 1, the specific surface area of the material with the addition of the pore-forming agent is significantly improved.
[0041] Table 1 Specific surface areas of porous iron-based phosphate pyrophosphate prepared in Examples 1-5 and iron-based phosphate pyrophosphate prepared in Comparative Examples 1-5
[0042] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a porous iron-based phosphoric acid pyrophosphate positive electrode material, characterized in that: The following steps are involved: (1) grinding a sodium source, an iron source, a phosphorus source, a carbon source, and a pore-forming agent, and then spray drying the mixture to obtain a precursor; (2) The precursor is placed in an inert atmosphere for sintering to obtain the porous iron-based phosphate pyrophosphate positive electrode material.
2. The method for preparing the porous iron-based phosphoric acid pyrophosphate positive electrode material according to claim 1, characterized in that: The sodium source is one or both of sodium oxalate and sodium carbonate.
3. The method for preparing the porous iron-based phosphoric acid pyrophosphate positive electrode material according to claim 1, characterized in that: The iron source is one or both of ferric oxalate and ferric phosphate.
4. The method for preparing the porous iron-based phosphate pyrophosphate positive electrode material according to claim 1, characterized in that: The phosphorus source is one or both of sodium dihydrogen phosphate and disodium hydrogen phosphate.
5. The method for preparing the porous iron-based phosphoric acid pyrophosphate positive electrode material according to claim 1, characterized in that: The carbon source is one or more of glucose, sucrose and citric acid.
6. The method for preparing the porous iron-based phosphoric acid pyrophosphate positive electrode material according to claim 1, characterized in that: The pore-forming agent is oxalic acid.
7. The method for preparing the porous iron-based phosphate pyrophosphate positive electrode material according to claim 1, characterized in that: The sintering uses an inert atmosphere of argon or nitrogen or a mixed atmosphere of argon and hydrogen, and the sintering steps are sintering at 300-400°C for 3-6 h and sintering at 450-650°C for 5-15 h.
8. A porous iron-based phosphoric acid pyrophosphate positive electrode material prepared according to the method according to any one of claims 1 to 7, characterized in that: The porous iron-based phosphate pyrophosphate positive electrode material is Na 3+x Fe 2+x (PO4) 1+x P2O7, where 0≤x≤1.
5.
9. The porous iron-based phosphoric acid pyrophosphate positive electrode material according to claim 8, characterized in that The specific surface area of the positive electrode material is 15-30 cm 2 g.
10. Use of the porous iron-based phosphoric acid pyrophosphate positive electrode material according to claim 8 or 9 in a sodium ion battery.
Citation Information
Patent Citations
Iron-based pyrophosphate material as well as preparation method and application thereof
CN116675207A
Porous ferric sodium pyrophosphate / carbon composite material as well as preparation method and application thereof
CN116799131A
Preparation method of high-performance sodium ion battery positive electrode material Na4Fe3 (PO4) 2P2O7
CN117585658A
Sodium ferric pyrophosphate sodium ion battery positive electrode material and preparation method thereof
CN118047362A
Iron-based polyphosphate material with uniform mesoporous structure as well as preparation and application of iron-based polyphosphate material
CN118561258A
Cited By
Preparation method of porous sodium-ion battery sodium ferric phosphate pyrophosphate positive electrode material
CN120622438A