Coal-based hard carbon with gradient structure as well as preparation method and application of coal-based hard carbon
The gradient structure coal-based hard carbon prepared by oxidative crosslinking and gradient reduction treatment solves the problem of insufficient performance of coal-based hard carbon materials under low temperature conditions, and achieves high sodium storage capacity and cycle stability of the negative electrode material of sodium ion battery, satisfying the The commercial demand for sodium ion batteries at low temperatures.
Patent Information
- Application Number
- CN202411194391.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-28
AI Technical Summary
The existing coal-based hard carbon materials lack sufficient performance under low temperature conditions, are prone to surface side reactions, and lack ion storage sites, which limits the energy density and cycling stability of sodium ion batteries.
Coal-based hard carbon with gradient structure is prepared by oxidative crosslinking and gradient reduction treatment, and its microstructure is controlled to form a disordered carbon sheet layer with curved internal surroundings and a microcrystalline structure with a high surface order, reducing surface side reactions and Increase ion storage sites.
The low-temperature performance of sodium ion battery negative electrode materials is significantly improved, including high sodium storage capacity, long platform capacity and high cycling stability, meeting the needs of high energy density and power density.
Smart Images

Figure CN119059512A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion battery electrode materials, and in particular to a coal-based hard carbon with a gradient structure and a preparation method and application thereof. Background Art
[0002] With the growing global demand for clean energy and the increasing need for reliable energy storage solutions in extreme environments, the research and development of low-temperature batteries is particularly important. Sodium-ion batteries show unique advantages in large-scale energy storage applications due to their abundant resources and low cost. However, the insufficient performance of sodium-ion batteries under low temperature conditions limits their widespread use in cold areas such as electric vehicles and outdoor energy storage facilities. By improving electrolyte materials, positive and negative electrode materials and their structural design, scientists are working to improve the energy density, cycle stability and safety of these batteries to overcome this challenge and broaden the application range of sodium-ion batteries. Among them, the negative electrode material is of great significance to the energy density of sodium-ion batteries, especially the platform capacity at low potential, which directly affects the energy density of the whole battery.
[0003] Carbon materials are widely used as negative electrode materials for sodium ion batteries because of their high stability, good conductivity, and adjustable microstructure. Among them, hard carbon materials have a low degree of graphitization and are mainly composed of a large number of disordered carbon microcrystals stacked in an interlaced manner, with a large interlayer spacing and a large number of nanopores, which provide ideal active sites for the storage of sodium ions. At the same time, hard carbon materials have low sodium storage potential, high reversible capacity, and excellent cycle stability in sodium ion batteries, and are considered to be the most promising high-quality negative electrode materials for sodium ion batteries.
[0004] my country is rich in coal resources, and its composition structure contains a large number of graphite-like microcrystals and polycyclic aromatic clusters, with a high carbonization yield, making it an excellent carbonaceous raw material. Although coal-based carbon materials with high carbon content and strong conductivity can be obtained from coal through coal selection and carbonization. However, the coal-based carbon materials prepared by direct coal carbonization have a high degree of order, are easy to form a graphite-like structure, and lack closed-pore sodium storage sites. Researchers have improved the disorder of materials through pre-oxidation, template method and other means, but the highly disordered surface is prone to cause side reactions and is not conducive to charge transfer on the electrode surface at low temperatures. Under low temperature conditions, the viscosity of the electrolyte increases, the liquid phase diffusion is delayed, the solid phase diffusion in the electrode material is slow, and the charge transfer at the interface between the electrolyte and the electrode material is slow. Surface coating can reduce the occurrence of surface side reactions and improve the surface conductivity of the material, but due to the existence of the surface coating layer and the internal two-phase interface, the resistance of solid phase diffusion is increased, and there are also problems such as reducing the volume energy density of the negative electrode material and difficult to control the coating uniformity, which cannot meet the needs of high-performance low-temperature sodium ion battery negative electrode materials.
[0005] Therefore, there is an urgent need to develop a method for preparing a gradient-structured coal-based hard carbon that can provide abundant ion storage sites, reduce the occurrence of surface side reactions and phase interface problems, and improve the low-temperature sodium storage capacity and ion diffusion rate. Summary of the invention
[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a gradient-structured coal-based hard carbon and its preparation method and application, which solves the technical problems of the prior art such as the complicated preparation method of coal-based hard carbon, few ion storage sites, easy surface side reactions, and phase interface and uniformity in the coating treatment.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The present invention provides a method for preparing coal-based hard carbon with a gradient structure, comprising the following steps:
[0009] (1) oxidatively crosslinking the deashed coal-based precursor in a solvent to obtain an over-oxidized coal-based precursor;
[0010] (2) subjecting the over-oxidized coal-based precursor to a gradient reduction treatment in a reducing atmosphere to obtain a gradient-reduced precursor;
[0011] (3) Finally, the gradient-reduced precursor is sequentially carbonized to obtain a coal-based hard carbon material with a gradient structure.
[0012] Further, the coal-based precursor includes one or more of lignite, bituminous coal, anthracite, coal tar, petroleum tar, coal coke and petroleum coke;
[0013] The particle size of the coal-based precursor is 100 to 800 meshes.
[0014] Furthermore, the solvent includes one or more of water, ethanol, propanol and ether.
[0015] Furthermore, the oxidant used in the oxidative crosslinking process includes one or more of peroxides, persulfides, oxidizing acids and acid anhydrides.
[0016] Furthermore, the temperature of the oxidative crosslinking is 80 to 200° C., the pressure of the oxidative crosslinking is 0.1 to 2.3 MPa, and the time of the oxidative crosslinking is 3 to 10 hours;
[0017] The mass volume ratio of the coal-based precursor, the oxidant and the solvent is 8-12 g: 2 g: 10-70 mL.
[0018] Furthermore, the gas of the reducing atmosphere includes one or more of hydrogen, carbon monoxide and methane;
[0019] The temperature of the gradient reduction treatment is 100-500° C., and the time of the gradient reduction treatment is 1-5 hours.
[0020] Furthermore, the temperature of the carbonization treatment is 1000-2000°C, the heating rate is 0.5-20°C / min, and the carbonization treatment time is 0.5-10h;
[0021] The carbonization treatment is performed in a protective gas, and the protective gas includes an inert gas or a vacuum environment.
[0022] The present invention provides a coal-based hard carbon with a gradient structure prepared by the method for preparing the coal-based hard carbon with a gradient structure.
[0023] The present invention also provides an application of a gradient-structured coal-based hard carbon in the preparation of a negative electrode material for a sodium ion battery.
[0024] Beneficial effects of the present invention:
[0025] (1) The present invention prepares a coal-based hard carbon material with a gradient increasing degree of amorphism from the surface to the inside by gradient reduction after over-oxidation, and prepares a controllable gradient microstructure of coal-based hard carbon by controlling the temperature, pressure, and solution concentration of the oxidative cross-linking reaction in a solvent wet environment, the temperature, time, and gas atmosphere of the gradient reduction treatment, and the carbonization temperature, time, and heating rate.
[0026] (2) The negative electrode material of the coal-based hard carbon sodium ion battery prepared in the present invention has a gradient functional distribution. The interior is a disordered carbon layer that is curved and surrounded, stacked to form closed pores, creating abundant sites for the filling of sodium ions at low potentials; and the near-surface is a microcrystalline carbon structure with a high degree of order, which reduces surface side reactions and thus exhibits excellent electrochemical performance.
[0027] (3) The negative electrode material of the coal-based hard carbon sodium ion battery prepared in the present invention has abundant sodium-philic sodium storage sites inside and a sodium-phobic inert structure on the surface. The carbon structure has a gradient transition from the surface to the inside without producing an obvious phase separation interface, thereby enhancing the internal solid phase diffusion and reducing the surface charge transfer resistance, thereby exhibiting excellent low-temperature performance.
[0028] (4) The coal-based hard carbon prepared by this method has excellent electrochemical properties as anode materials for sodium ion batteries, including high sodium storage capacity (303.3 mAh g -1 ), long low-potential platform sodium storage capacity (platform capacity below 0.1V is 222mAh / g), high first coulombic efficiency (84.6%) and high cycle stability, which can meet the commercialization needs of sodium-ion batteries with high energy density and power density. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a process flow chart for preparing a gradient structure coal-based hard carbon negative electrode material in Example 1 of the present invention.
[0030] Figure 2 This is the XRD pattern of the gradient-structured coal-based hard carbon sodium-ion battery negative electrode material prepared in Example 1.
[0031] Figure 3 This is a scanning electron microscope image of the gradient structure coal-based hard carbon sodium ion battery negative electrode material prepared in Example 1 of the present invention.
[0032] Figure 4 This is a transmission electron microscope image and carbon structure model of the gradient structure coal-based hard carbon sodium ion battery negative electrode material prepared in Example 1 of the present invention.
[0033] Figure 5 This is a charge-discharge curve diagram of the first three cycles of the gradient structure coal-based hard carbon negative electrode material prepared in Example 1 of the present invention.
[0034] Figure 6 This is a low temperature performance diagram of the gradient structure coal-based hard carbon negative electrode material prepared in Example 1 of the present invention.
[0035] Figure 7 It is a transmission electron microscope image of the coal-based hard carbon negative electrode material obtained in Comparative Examples 1, 2, and 3 of the present invention.
[0036] Figure 8 The cyclic voltammetry curves of the sodium ion batteries prepared in Example 1 and Comparative Examples 1 to 3, wherein (a) is the cyclic voltammetry curve of the sodium ion battery prepared in Example 1, (b) is the cyclic voltammetry curve of the sodium ion battery prepared in Comparative Example 1, (c) is the cyclic voltammetry curve of the sodium ion battery prepared in Comparative Example 2, and (d) is the cyclic voltammetry curve of the sodium ion battery prepared in Comparative Example 3; DETAILED DESCRIPTION
[0037] The present invention provides a method for preparing coal-based hard carbon with a gradient structure, comprising the following steps:
[0038] (1) oxidatively crosslinking the deashed coal-based precursor in a solvent to obtain an over-oxidized coal-based precursor;
[0039] (2) subjecting the over-oxidized coal-based precursor to a gradient reduction treatment in a reducing atmosphere to obtain a gradient-reduced precursor;
[0040] (3) Finally, the gradient-reduced precursor is sequentially carbonized to obtain a coal-based hard carbon material with a gradient structure.
[0041] In the present invention, the coal-based precursor is obtained by heating and mixing a carbon precursor and a mixed acid solution and then allowing the mixture to stand;
[0042] The coal-based precursor includes one or more of lignite, bituminous coal, anthracite, coal tar, petroleum tar, coal coke and petroleum coke, preferably one or more of lignite, bituminous coal, anthracite, coal tar and petroleum tar, more preferably one or more of lignite, bituminous coal, anthracite and coal tar;
[0043] In the present invention, the particle size of the coal-based precursor is 100 to 800 meshes, preferably 200 to 500 meshes.
[0044] In the present invention, the solvent includes one or more of water, ethanol, propanol and diethyl ether, preferably one or more of water, ethanol and diethyl ether.
[0045] In the present invention, the oxidant used in the oxidative crosslinking process includes one or more of peroxides, persulfides, oxidizing acids and acid anhydrides, preferably one or more of peroxides, oxidizing acids and acid anhydrides, and more preferably peroxides and / or acid anhydrides.
[0046] In the present invention, the temperature of the oxidative crosslinking is 80 to 200°C, preferably 100 to 180°C, and more preferably 140 to 160°C; the pressure of the oxidative crosslinking is 0.1 to 2.3 MPa, preferably 0.11 to 2.0 MPa, and more preferably 0.12 to 1.5 MPa; the time of the oxidative crosslinking is 3 to 10 h, preferably 3 to 8 h, and more preferably 3 to 5 h.
[0047] In the present invention, the mass volume ratio of the coal-based precursor, oxidant and solvent is 8-12g:2g:10-70mL, preferably 9-11g:2g:15-60mL, and more preferably 10g:2g:20-50mL.
[0048] In the present invention, the temperature of the gradient reduction treatment is 100-500°C, preferably 150-450°C, and more preferably 200-400°C; the time of the gradient reduction treatment is 1-5h, preferably 1-4.5h, and more preferably 1-4h.
[0049] In the present invention, the gas of the reducing atmosphere includes one or more of hydrogen, carbon monoxide and methane, preferably hydrogen and / or methane, and more preferably hydrogen.
[0050] In the present invention, the temperature of the carbonization treatment is 1000-2000° C., the heating rate is 0.5-20° C. / min, and the time of the carbonization treatment is 0.5-10 h.
[0051] Preferably, the temperature of the carbonization treatment is 1100-1800° C., the heating rate is 1-15° C. / min, and the time of the carbonization treatment is 1-9 h.
[0052] Further preferably, the temperature of the carbonization treatment is 1200-1600° C., the heating rate is independently 2-10° C. / min, and the carbonization treatment time is 2-8 h.
[0053] In the present invention, the carbonization treatment is carried out in a protective gas, and the protective gas includes an inert gas or a vacuum environment, preferably an inert gas.
[0054] In the present invention, the carbonization treatment further includes pickling.
[0055] In the present invention, by controlling the temperature, pressure, solution concentration of the oxidative cross-linking reaction under high temperature and high pressure in a solvent wet environment, the temperature, time, gas atmosphere of the gradient reduction treatment, as well as the carbonization temperature, time and heating rate, the oxygen content and oxygen configuration of the coal-based precursor can be controlled, and the size, distribution state and degree of crystallization of the graphite-like microcrystalline region of the coal-based hard carbon material can be regulated, thereby obtaining a coal-based hard carbon negative electrode material with an adjustable micro-gradient structure.
[0056] In the present invention, the wetting environment for oxidative crosslinking is to use 10 to 70 mL of solvent for wetting per 10 g of precursor, and oxidation and crosslinking are promoted by solvent wetting and high temperature and high pressure environment.
[0057] The present invention provides a coal-based hard carbon with a gradient structure prepared by the method for preparing the coal-based hard carbon with a gradient structure.
[0058] In the present invention, coal-based hard carbon has a gradient carbon structure, with the interior being curved and disordered carbon sheets stacked to form closed pores, forming abundant sodium-philic sodium storage sites; while the near-surface is a microcrystalline carbon structure with a higher degree of order, forming a sodium-phobic inert structure, reducing surface side reactions, thereby enhancing internal solid phase diffusion and reducing surface charge transfer resistance.
[0059] The present invention also provides an application of a gradient-structured coal-based hard carbon in the preparation of a negative electrode material for a sodium ion battery.
[0060] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0061] Example 1
[0062] This embodiment provides a method for preparing a gradient structure coal-based hard carbon negative electrode material, and its process flow chart is as follows: Figure 1 As shown, the following steps are included:
[0063] 10 g of deashed lignite was weighed, crushed and passed through a 200-mesh sieve, then mixed with 2 g of maleic anhydride and added to a reactor, and then 40 mL of deionized water was added, and the mixture was reacted at 160° C. and 0.12 MPa for 3 h. After washing, the mixture was filtered and dried to obtain over-oxidized cross-linked lignite.
[0064] The over-oxidized lignite was subjected to gradient reduction treatment in an argon-hydrogen mixed gas atmosphere, and the temperature was raised to 300°C at a rate of 5°C / min. The gradient reduction treatment time was 1 h, wherein the volume ratio of the hydrogen and argon flow rates in the argon-hydrogen mixed gas was V H2 / V Ar =10 / 90mL min -1 ;
[0065] In an argon atmosphere, the temperature was raised to 1500°C at a rate of 5°C / min for carbonization treatment for 3 hours. Finally, after acid washing, a gradient-structured coal-based hard carbon was obtained.
[0066] The gradient-structured coal-based hard carbon prepared in Example 1 is in powder morphology. Transmission electron microscopy images show abundant sp2 graphite-like region crystallites and sp3 defect structures. The amorphous degree increases from the surface to the inside, and the ID / IG value is 1.18.
[0067] The gradient structure coal-based hard carbon prepared in Example 1 is used as the negative electrode material to prepare a sodium ion battery. The preparation method of the sodium ion battery comprises the following steps:
[0068] Gradient structure coal-based dense negative electrode material, acetylene black and sodium carboxymethyl cellulose were weighed in a mass ratio of 92:3:5 and then evenly coated on copper foil. After drying at 60°C for 12 hours, a battery electrode was obtained. The active material loading of the negative electrode was greater than 1 mg cm -2 The obtained battery pole piece was used as the working electrode, the sodium sheet was used as the counter electrode, the diaphragm was made of GF / D glass fiber, the electrolyte was 1M NaPF6 (the solvent included dimethyl ether), and all assembly processes were carried out in a glove box.
[0069] The sodium ion battery prepared in Example 1 was tested.
[0070] Figure 2 This is the XRD pattern of the gradient-structured coal-based hard carbon sodium-ion battery negative electrode material prepared in Example 1. It can be seen from the figure that the XRD pattern of the gradient-structured coal-based hard carbon shows two broad diffraction peaks at 22° and 43°, which are typical diffraction peaks of the (002) and (100) crystal planes in disordered carbon.
[0071] Figure 3This is a scanning electron microscope image of the gradient-structured coal-based hard carbon sodium-ion battery negative electrode material prepared in Example 1. It can be seen from the electron microscope image that the coal-based hard carbon negative electrode material presents an irregular particle shape.
[0072] Figure 4 This is a transmission electron micrograph of the gradient-structured coal-based hard carbon sodium-ion battery negative electrode material prepared in Example 1. As can be seen from the figure, the interior of the coal-based hard carbon with a gradient structure is a curved and disordered carbon layer stacked to form closed pores, while the near-surface is a microcrystalline carbon structure with a higher degree of order.
[0073] Figure 5 The charge-discharge curve of the gradient structure coal-based hard carbon negative electrode material prepared in Example 1 in the first three weeks is shown in the figure. It can be seen from the figure that the discharge curve of the coal-based hard carbon negative electrode material shows a typical slope area and platform area. The reversible capacity of the negative electrode material is 303.3 mAh g -1 The first efficiency is 84.6%, and the 0.1V platform capacity is 222mAh·g -1 .
[0074] Figure 6 The sodium storage capacity of the gradient structure coal-based hard carbon anode material prepared in Example 1 at different low temperatures. It can be seen from the figure that at 25, 0, -10, -20, -30, and -40 °C, the reversible capacities of the gradient structure coal-based hard carbon anode material are 300, 271, 254, 232, 214, and 195 mAh g -1 , showing excellent performance at low temperatures.
[0075] Example 2
[0076] Weigh 10g of deashed lignite, crush it and pass it through a 200-mesh sieve, then mix it with 2g of maleic anhydride and add it to a reactor, then add 40mL of deionized water, react at 100℃ and 0.1MPa for 3h, wash it, filter it and dry it to obtain the oxidized lignite;
[0077] The over-oxidized lignite was subjected to gradient reduction treatment in an argon-hydrogen mixed gas atmosphere, and the temperature was raised to 300°C at a rate of 5°C / min. The gradient reduction treatment time was 1 h, wherein the volume ratio of the hydrogen and argon flow rates in the argon-hydrogen mixed gas was V H2 / V Ar =10 / 90mL min -1 ;
[0078] In an argon atmosphere, the temperature was raised to 1600°C at a rate of 5°C / min for carbonization treatment for 3 hours. Finally, after acid washing, a gradient-structured coal-based hard carbon was obtained.
[0079] The gradient structure coal-based hard carbon prepared in Example 2 has a powder morphology. The transmission electron microscope image shows abundant sp2 graphite-like region crystallites and sp3 defect structures. The amorphous degree increases from the surface to the inside, and the ID / IG value is 1.15.
[0080] The sodium ion battery was prepared according to the method of Example 1, and the sodium ion battery prepared in Example 2 was subjected to electrochemical testing. The test results showed that the sodium ion battery had a high first coulombic efficiency (85.4%), a high reversible capacity (294.5 mAh·g -1 ), 0.1V platform capacity is 226mAh·g -1 The reversible capacity of sodium ion battery at 0°C is 268 mAh g -1 , the reversible capacity is 216 mAh g at -30 °C -1 .
[0081] Example 3
[0082] 10 g of deashed lignite was weighed, crushed and passed through a 200-mesh sieve, then mixed with 2 g of maleic anhydride and added to a reactor, and then 40 mL of deionized water was added, and the mixture was reacted at 200°C and 1.5 MPa for 3 h. After washing, the mixture was filtered and dried to obtain over-oxidized lignite.
[0083] The over-oxidized lignite was subjected to gradient reduction treatment in an argon-hydrogen mixed gas atmosphere, and the temperature was raised to 300°C at a rate of 5°C / min. The gradient reduction treatment time was 1 h, wherein the volume ratio of the hydrogen and argon flow rates in the argon-hydrogen mixed gas was V H2 / V Ar =10 / 90mL min -1 ;
[0084] In an argon atmosphere, the temperature was raised to 1400°C at a rate of 5°C / min for carbonization treatment for 3 hours. Finally, after acid washing, a gradient-structured coal-based hard carbon was obtained.
[0085] The gradient structure coal-based hard carbon prepared in Example 3 has a powder morphology. The transmission electron microscope image shows abundant sp2 graphite-like region microcrystals and sp3 defect structures. The amorphous degree increases from the surface to the inside, and the ID / IG value is 1.23.
[0086] The sodium ion battery was prepared according to the method of Example 1, and the sodium ion battery prepared in Example 3 was electrochemically tested. The test results showed that the sodium ion battery had a high first coulomb efficiency (82.4%), a high reversible capacity (291.3 mAh·g -1 ), the platform capacity below 0.1V is 193mAh·g -1 The reversible capacity of sodium ion batteries at 0°C is 264 mAh g -1, the reversible capacity is 208 mAh g at -30 °C -1 .
[0087] Example 4
[0088] 10 g of deashed lignite was weighed, crushed and passed through a 200-mesh sieve, then mixed with 2 g of maleic anhydride and added to a reactor, and then 40 mL of ethanol was added, reacted at 160°C and 0.12 MPa for 3 h, washed, filtered and dried to obtain over-oxidized lignite;
[0089] The over-oxidized lignite was subjected to low-temperature heat treatment in an argon-hydrogen mixed gas atmosphere, and the temperature was raised to 300°C at a rate of 5°C / min. The low-temperature heat treatment time was 1 h, wherein the volume ratio of the hydrogen and argon flow rates in the argon-hydrogen mixed gas was V H2 / V Ar =10 / 90mLmin -1 ;
[0090] In an argon atmosphere, the temperature was raised to 1500°C at a rate of 5°C / min for carbonization treatment for 3 hours. Finally, after acid washing, a gradient-structured coal-based hard carbon was obtained.
[0091] The gradient structure coal-based hard carbon prepared in Example 4 has a powder morphology. The transmission electron microscope image shows abundant sp2 graphite-like region crystallites and sp3 defect structures. The amorphous degree increases from the surface to the inside, and the ID / IG value is 1.20.
[0092] The sodium ion battery was prepared according to the method of Example 1, and the sodium ion battery prepared in Example 4 was subjected to electrochemical testing. The test results showed that the sodium ion battery had a high first coulombic efficiency (85.2%), a high reversible capacity (298.4 mAh·g -1 ), the platform capacity below 0.1V is 214mAh·g -1 The reversible capacity of sodium ion batteries at 0°C is 256 mAh g -1 , the reversible capacity is 205 mAh g at -30 °C -1 .
[0093] Example 5
[0094] The difference between this embodiment and embodiment 1 is that the temperature of the gradient reduction treatment is 200°C.
[0095] The rest of the preparation methods and parameters were the same as those in Example 1.
[0096] Example 6
[0097] The difference between this embodiment and embodiment 1 is that the temperature of the gradient reduction treatment is 400°C.
[0098] The rest of the preparation methods and parameters were the same as those in Example 1.
[0099] Example 7
[0100] The difference between this embodiment and embodiment 1 is that the reducing gas introduced in the gradient reduction treatment is methane.
[0101] The rest of the preparation methods and parameters were the same as those in Example 1.
[0102] Example 8
[0103] The difference between this embodiment and embodiment 1 is that the coal precursor used is anthracite.
[0104] The rest of the preparation methods and parameters were the same as those in Example 1.
[0105] Comparative Example 1
[0106] The difference between this comparative example and Example 1 is that the liquid phase oxidation and gradient reduction operations are not performed.
[0107] The rest of the preparation methods and parameters were the same as those in Example 1.
[0108] Comparative Example 2
[0109] The difference between this comparative example and Example 1 is that liquid phase oxidation is not performed.
[0110] The rest of the preparation methods and parameters were the same as those in Example 1.
[0111] Comparative Example 3
[0112] The difference between this comparative example and Example 1 is that no gradient reduction treatment is performed.
[0113] The rest of the preparation methods and parameters were the same as those in Example 1.
[0114] Electrochemical performance tests were performed on the sodium ion batteries prepared in Examples 1 to 8 and Comparative Examples 1 to 3, including:
[0115] Cyclic voltammetry: voltage range 0-2.5 V, scan rate 0.1 mV s -1 , scan 3 times.
[0116] Charge and discharge test: The voltage range is 0-2.5V, and the charge and discharge test is carried out at a current density of 20mA / g to obtain the charge and discharge specific capacity and the first efficiency.
[0117] Low temperature performance test: The test temperature is 0, -10, -20, -30, -40℃, the voltage range is 0-2.5V, and the charge and discharge test is carried out at a current density of 20mA / g.
[0118] The test results are shown in Table 1.
[0119] Table 1 Performance test results of sodium ion batteries prepared in Examples 1 to 8 and Comparative Examples 1 to 3
[0120]
[0121]
[0122] It can be seen from Examples 1 and 2, 3, and 4 that if the oxidative cross-linking reaction temperature is increased, or ethanol is used for solvent thermal treatment, that is, the oxidative cross-linking strength is increased, the molecular structure of the polycyclic aromatic hydrocarbons in the coal will be modified too much, resulting in a large number of polycyclic aromatic hydrocarbon molecules and cross-linking. In the later carbonization process, oxygen-containing functional groups will escape seriously, forming hard carbon with many defects. If the oxidation temperature is too low, it will not have a sufficient oxidative cross-linking effect, resulting in the inability of the carbon sheets inside the carbon particles to bend and stack to form closed-cell sites, which will cause the reversible capacity of the hard carbon to decrease, the first effect to decrease, and the cycle performance to deteriorate.
[0123] It can be seen from Example 1 and Examples 5, 6, and 7 that if the temperature of the gradient reduction process increases, that is, the reduction intensity increases, there will be fewer oxygen-containing groups in the coal, and most of the molecular structures of condensed aromatic hydrocarbons will still tend to be ordered in the later carbonization, resulting in a lower reversible capacity of the coal-based hard carbon and worse cycle performance; if the gradient reduction reaction temperature is lowered or methane is used as a reducing gas, the gradient reduction effect will not be obvious, which is not conducive to near-surface ordering and the reduction of side reactions, resulting in a reduction in the first effect.
[0124] It can be seen from Example 1 and Example 8 that if the process method described in the present invention is not limited to lignite as raw material, it also has excellent modification effects on other coal precursors such as anthracite, that is, the general principle of the present invention is universal for different coal precursors.
[0125] It can be seen from Example 1 and Comparative Example 1 that if lignite is directly carbonized without any pretreatment, the polycyclic aromatic hydrocarbon molecules in the coal will tend to be ordered, easily forming a graphite-like structure, forming a hard carbon with a high degree of order, and lacking closed-cell sodium storage sites.
[0126] It can be seen from Example 1 and Comparative Example 2 that if gradient reduction treatment is not carried out after liquid-phase oxidation, due to the serious escape of oxygen atoms caused by excessive cross-linking between condensed aromatic hydrocarbon molecules during the carbonization process, more defects will be formed in the hard carbon, which will lead to excessive near-surface disorder and failure to form a long-range ordered structure, resulting in an increase in specific surface area and a decrease in the first effect.
[0127] It can be seen from Example 1 and Comparative Example 3 that if only hydrogen reduction treatment is performed before carbonization, it will lead to excessive deoxidation of the precursor, excessive development of carbon sheets during the carbonization process, and the formation of a highly ordered graphite-like structure.
[0128] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a gradient structure coal-based hard carbon, characterized in that: The following steps are involved: (1) oxidatively crosslinking the deashed coal-based precursor in a solvent to obtain an over-oxidized coal-based precursor; (2) subjecting the over-oxidized coal-based precursor to a gradient reduction treatment in a reducing atmosphere to obtain a gradient-reduced precursor; (3) Finally, the gradient-reduced precursor is sequentially carbonized to obtain a coal-based hard carbon material with a gradient structure.
2. The method for preparing the gradient structured coal-based hard carbon according to claim 1, characterized in that: The coal-based precursor includes one or more of lignite, bituminous coal, anthracite, coal tar, petroleum tar, coal coke and petroleum coke; The particle size of the coal-based precursor is 100 to 800 meshes.
3. The method for preparing the gradient structured coal-based hard carbon according to claim 1 or 2, characterized in that: The solvent includes one or more of water, ethanol, propanol and ether.
4. The method for preparing the gradient structure coal-based hard carbon according to claim 3, characterized in that: The oxidant used in the liquid phase oxidation process includes one or more of peroxides, persulfides, oxidizing acids and acid anhydrides.
5. The method for preparing the gradient structured coal-based hard carbon according to claim 1, 2 or 4, characterized in that: The temperature of the oxidative crosslinking is 80 to 200° C., the pressure of the oxidative crosslinking is 0.1 to 2.3 MPa, and the time of the oxidative crosslinking is 3 to 10 hours; The mass volume ratio of the coal-based precursor, the oxidant and the solvent is 8-12 g: 2 g: 10-70 mL.
6. The method for preparing the gradient structure coal-based hard carbon according to claim 5, characterized in that: The gas of the reducing atmosphere includes one or more of hydrogen, carbon monoxide and methane; The temperature of the gradient reduction treatment is 100-500° C., and the time of the gradient reduction treatment is 1-5 hours.
7. The method for preparing the gradient structure coal-based hard carbon according to claim 6, characterized in that: The temperature of the carbonization treatment is 1000-2000°C, the heating rate is 0.5-20°C / min, and the carbonization treatment time is 0.5-10h; The carbonization treatment is performed in a protective gas, and the protective gas includes an inert gas or a vacuum environment.
8. Coal-based hard carbon with a gradient structure prepared by the method for preparing coal-based hard carbon with a gradient structure according to any one of claims 1 to 7.
9. Use of the gradient structured coal-based hard carbon according to claim 8 in preparing negative electrode materials for sodium ion batteries.
Citation Information
Patent Citations
Coal-based hard carbon negative electrode material of sodium ion battery, preparation method and application thereof
CN113381013A
Preparation method and application of coal pitch-based hard carbon material
CN117550585A
Sodium-ion battery negative electrode material based on resin and asphalt as well as preparation method and application of sodium-ion battery negative electrode material
CN117902565A
Lithium battery negative electrode material carbonization system and carbonization method
CN118129455A
Asphalt-based sodium ion battery negative electrode material and preparation method thereof