Preparation method of bulk phase doped metal element titanium niobate negative electrode material

By doping metal elements in bulk phase into titanium niobate materials, the problems of poor conductivity and low Li+ diffusion coefficient are solved, and the electrochemical performance of lithium-ion batteries is improved and suitable for commercial applications.

CN119059561APending Publication Date: 2024-12-03NINGBO UNIVERSITY OF TECHNOLOGY +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310622700.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The poor conductivity and low Li+ diffusion coefficient of the titanium niobate negative electrode material have limited Coulomb efficiency and rate performance in lithium-ion batteries, hindering its commercial application.

Method used

By mixing the titanium source and niobium source with the urea solution, adding the cationic precursor, stirring and precipitating with the oxalic acid solution, and calcining at high temperature, the bulk doping of metal elements in the titanium niobate material can be achieved, the unit cell volume is increased and the lithium ions are widened. Transmission channel to improve electrochemical performance.

Benefits of technology

It has achieved the improvement of the conductive properties of titanium niobate material, enhanced the lithium ion transmission rate, improved the electrochemical performance, and simplified the process, suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059561A_ABST
    Figure CN119059561A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of secondary battery negative electrode materials, and particularly relates to a preparation method of a bulk phase doped metal element titanium niobate negative electrode material. The preparation method of the bulk phase doped metal element titanium niobate negative electrode material comprises the following steps: adding a titanium source and a niobium source into an ethanol solution of urea, then adding a cation precursor to obtain a titanium niobate precursor solution containing doped cations, mixing and stirring the titanium niobate precursor solution with an ethanol solution of oxalic acid to obtain a white precipitate, washing, drying, and carrying out high-temperature calcination. The titanium niobate negative electrode material with good conductivity is obtained by simply heating, stirring and precipitating and combining high-temperature calcination to realize bulk phase doping of cations in the titanium niobate material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of secondary battery negative electrode materials, and in particular relates to a method for preparing a bulk phase doped metal element titanium niobate negative electrode material. Background Art

[0002] With the rapid development of new energy electric vehicles, higher and higher requirements are placed on the performance of power lithium batteries, especially fast charging performance and safety performance. The current development of high specific capacity electrode materials, combined with advanced battery structure design, has continuously improved the energy density of lithium-ion batteries, but the resulting safety hazards have increased significantly. Among the negative electrode materials, titanium niobate has excellent fast charging performance, safety performance and high specific capacity. The use of titanium niobate to replace commercial negative electrode materials can effectively improve the safety and fast charging performance of lithium-ion batteries. However, the current titanium niobate negative electrode materials still have the following two defects: First, the energy band gap of titanium niobate is relatively wide (~2.9eV), of which Ti 4+ and Nb 5+ are all in the highest valence state, with no unpaired electrons, resulting in poor conductivity of the material; second, Li + The low diffusion coefficient leads to a large interface impedance between the titanium niobate negative electrode material and the electrolyte. The above defects make the electronic conductivity and ionic conductivity of the titanium niobate negative electrode material low, which seriously limits the coulombic efficiency and rate performance of the titanium niobate negative electrode material, thus hindering the commercial application of titanium niobate negative electrode materials in lithium-ion batteries.

[0003] At present, the commonly used method of cation doping titanium niobate is mainly to ball mill the metal oxide and titanium niobate, and then to achieve it through high-temperature calcination or gel method. The preparation method of carbon-coated niobate doped modified titanium niobate material in Chinese patent CN112736250A is to mix titanium source, niobium source and water and ball mill, spray dry, high-temperature sinter, and then mix and ball mill with organic carbon source, and sinter again at high temperature to obtain carbon-coated titanium niobate material. The preparation method of tin-carbon co-doped titanium niobate material in Chinese patent CN 111874947A is to add niobium source, titanium source and organic tin source to dispersant, ball mill and dry to obtain precursor, and high-temperature calcination to obtain tin-carbon co-doped titanium niobate material. In the titanium niobate material obtained by the above method, the cations are mainly distributed on the surface of titanium niobate particles, and the bulk doping of metal elements is not achieved, and the improvement of the intrinsic conductivity of titanium niobate material is relatively limited. Summary of the invention

[0004] The purpose of the present invention is to solve the above problems and provide a method for preparing a bulk phase doped metal element titanium niobate negative electrode material, which can efficiently realize the bulk phase doping of metal elements in the titanium niobate negative electrode material and effectively improve the conductive properties of the titanium niobate negative electrode material.

[0005] The preparation method of the bulk phase doped metal element titanium niobate negative electrode material in the technical solution of the present invention comprises adding a titanium source and a niobium source into a urea solution, then adding a cationic precursor to obtain a titanium niobate precursor solution containing doped cations, mixing and stirring with an oxalic acid solution to obtain a white precipitate, washing, drying, and then calcining at a high temperature.

[0006] The nitrogen atom of urea has a lone pair of electrons, which can coordinate with cations to form a complex. After oxalic acid precipitation, titanium niobate containing doped cations is obtained. After high-temperature calcination, part of the titanium or niobium in the titanium niobate material crystal is replaced by cations to obtain a bulk phase titanium niobate negative electrode material doped with metal elements.

[0007] Furthermore, the titanium source is one or more of titanate compounds, titanium isopropoxide, titanium tert-butoxide, titanium n-butoxide, titanyl sulfate, and titanium tetrachloride.

[0008] Furthermore, the niobium source is one or more of niobium pentachloride, niobium ethoxide, niobium n-butoxide, niobium ethoxide, and niobium oxalate.

[0009] Furthermore, the molar ratio of the titanium source to the niobium source is 1.0:0.5-5.0.

[0010] Furthermore, the urea solution is formed by dissolving urea in a solvent, and the solvent is a polar solvent, which is one or more of ethanol, ethylene glycol, glycerol, and propylene glycol.

[0011] Furthermore, the concentration of the urea solution is 0.01 to 0.05 g / ml.

[0012] Furthermore, the cationic precursor is one or more of tin metal salt, magnesium metal salt, lithium metal salt, antimony metal salt, zinc metal salt, nickel metal salt, cobalt metal salt, and manganese metal salt. After the cation is doped into the crystal structure of the titanium niobate material, the unit cell volume can be increased, the lithium ion transmission channel can be widened, and the lithium ion transmission rate can be accelerated, thereby improving the electrochemical performance of the titanium niobate material.

[0013] Furthermore, the molar amount of cations in the cation precursor is 10-40% of the total molar amount of the titanium source and the niobium source. When the amount of cation doping is too much, the crystal structure will be destroyed, the integrity of the titanium niobate crystal will be affected, and the electrochemical performance will be reduced.

[0014] Furthermore, the oxalic acid solution is formed by dissolving oxalic acid in a solvent, and the solvent is a polar solvent, which is one or more of ethanol, ethylene glycol, glycerol, and propylene glycol.

[0015] Furthermore, the concentration of the oxalic acid solution is 0.01 to 0.04 g / ml.

[0016] Furthermore, the mixing and stirring is performed using a peristaltic pump, and the mixing speed is 1.0 to 5.0 mL / min. Furthermore, the temperature during the mixing and stirring is 80 to 120° C., and the time is 0.5 to 2.0 h.

[0017] Furthermore, washing is performed by washing with ethanol and water in sequence 2 to 3 times.

[0018] Furthermore, the drying temperature is 80-100° C. and the drying time is 4-6 hours.

[0019] Furthermore, high temperature calcination is carried out in an oxygen atmosphere, the calcination temperature is 650-1000° C., and the time is 4-6 hours.

[0020] Another object of the present invention is to provide a bulk phase doped metal element titanium niobate negative electrode material prepared by the above preparation method.

[0021] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0022] (1) Through simple heating and stirring precipitation combined with high-temperature calcination, the bulk doping of cations in the titanium niobate material is achieved to obtain a titanium niobate negative electrode material with good conductive properties;

[0023] (2) After cation doping, it enters the crystal structure of titanium niobate material, which can increase the unit cell volume, broaden the lithium ion transmission channel, and accelerate the lithium ion transmission rate, thereby improving the electrochemical performance of titanium niobate material;

[0024] (3) The nitrogen atom of urea has a lone pair of electrons, which can coordinate with cations to form a complex, and then precipitate with oxalic acid to obtain titanium niobate containing doped cations. After high-temperature calcination, part of the titanium or niobium in the titanium niobate material crystal is replaced by cations, and a bulk phase titanium niobate negative electrode material doped with metal elements is obtained in situ.

[0025] (4) The method for preparing titanium niobate negative electrode material of the present invention is simple and environmentally friendly, with a fast process and controllable conditions, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The SEM images of the bulk phase doped metal element titanium niobate negative electrode material obtained in Example 1: (a) high magnification SEM image, (b) low magnification SEM image;

[0027] Figure 2 This is a rate performance diagram of the bulk phase doped metal element titanium niobate negative electrode material obtained in Example 1;

[0028] Figure 3 This is a rate performance diagram of the titanium niobate negative electrode material obtained in Comparative Example 1. DETAILED DESCRIPTION

[0029] The technical scheme of the present invention is further described below by specific examples and accompanying drawings. It should be understood that the specific examples described herein are only used to help understand the present invention and are not used for specific limitations of the present invention. The accompanying drawings used herein are only for better illustrating the disclosure of the present invention and do not have a limiting effect on the scope of protection. Unless otherwise specified, the raw materials used in the embodiments of the present invention are all commonly used raw materials in the art, and the methods used in the embodiments are all conventional methods in the art.

[0030] Example 1

[0031] The method for preparing the bulk phase doped metal element titanium niobate negative electrode material of this embodiment comprises the following steps:

[0032] (1) dissolving 0.84 g of urea in 20 ml of ethanol to obtain a urea solution with a concentration of 0.042 g / ml, adding 0.14 g of titanium isopropoxide and 0.27 g of niobium pentachloride and stirring evenly, adding 0.1 g of tin tetrachloride and stirring to obtain a titanium niobate precursor solution containing tin ions;

[0033] (2) dissolving 0.63 g of oxalic acid in 20 ml of ethanol to obtain an oxalic acid solution with a concentration of 0.032 g / ml, using a peristaltic pump to mix the oxalic acid solution with a titanium niobate precursor solution containing tin ions within 10 min, and reacting at 80° C. for 2 h to obtain a white precipitate;

[0034] (3) The white precipitate obtained in step (2) is washed and dried, and then calcined at 1000° C. for 4 h in an oxygen atmosphere to obtain a bulk-doped titanium niobate negative electrode material, such as Figure 1 shown.

[0035] Example 2

[0036] The method for preparing the bulk phase doped metal element titanium niobate negative electrode material of this embodiment comprises the following steps:

[0037] (1) dissolving 0.8 g of urea in 20 ml of ethanol to obtain a urea solution with a concentration of 0.04 g / ml, adding 0.14 g of titanium tetrachloride and 0.27 g of niobium ethoxide and stirring evenly, adding 0.1 g of tin tetrachloride and stirring to obtain a titanium niobate precursor solution containing tin ions;

[0038] (2) dissolving 0.63 g of oxalic acid in 20 ml of ethanol to obtain an oxalic acid solution with a concentration of 0.032 g / ml, using a peristaltic pump to mix the oxalic acid solution with a titanium niobate precursor solution containing tin ions within 10 min, and reacting at 90° C. for 1.5 h to obtain a white precipitate;

[0039] (3) The white precipitate obtained in step (2) is washed and dried, and then calcined at 1000° C. for 4 h in an oxygen atmosphere to obtain a bulk-doped titanium niobate negative electrode material.

[0040] Example 3

[0041] The method for preparing the bulk phase doped metal element titanium niobate negative electrode material of this embodiment comprises the following steps:

[0042] (1) dissolving 0.84 g of urea in 20 ml of ethanol to obtain a urea solution with a concentration of 0.042 g / ml, adding 0.14 g of titanium isopropoxide and 0.27 g of niobium pentachloride and stirring evenly, adding 0.05 g of magnesium chloride and stirring to obtain a titanium niobate precursor solution containing magnesium ions;

[0043] (2) dissolving 0.6 g of oxalic acid in 20 ml of ethanol to obtain an oxalic acid solution with a concentration of 0.03 g / ml, using a peristaltic pump to mix the oxalic acid solution with a titanium niobate precursor solution containing magnesium ions within 10 minutes, and reacting at 90° C. for 2 hours to obtain a white precipitate;

[0044] (3) The white precipitate obtained in step (2) is washed and dried, and then calcined at 950° C. for 5 h in an oxygen atmosphere to obtain a bulk-doped titanium niobate negative electrode material.

[0045] Example 4

[0046] The only difference between this embodiment and embodiment 1 is that in step (2), 0.63 g of oxalic acid is dissolved in 20 ml of ethanol to obtain an oxalic acid solution with a concentration of 0.032 g / ml, which is mixed evenly with the titanium niobate precursor solution containing tin ions within 35 minutes using a peristaltic pump, and reacted at 80° C. for 2 hours to obtain a white precipitate.

[0047] Example 5

[0048] The only difference between this embodiment and embodiment 1 is that in step (2), 0.63 g of oxalic acid is dissolved in 20 ml of ethanol to obtain an oxalic acid solution with a concentration of 0.032 g / ml, which is mixed evenly with the titanium niobate precursor solution containing tin ions within 5 minutes using a peristaltic pump, and reacted at 80° C. for 2 hours to obtain a white precipitate.

[0049] Comparative Example 1

[0050] The preparation method of the titanium niobate negative electrode material of this comparative example comprises the following steps:

[0051] (1) dissolving 0.84 g of urea in 20 ml of ethanol to obtain a urea solution with a concentration of 0.042 g / ml, adding 0.14 g of titanium isopropoxide and 0.27 g of niobium pentachloride and stirring to obtain a titanium niobate precursor solution;

[0052] (2) dissolving 0.63 g of oxalic acid in 20 ml of ethanol to obtain an oxalic acid solution with a concentration of 0.032 g / ml, using a peristaltic pump to mix the oxalic acid solution with the titanium niobate precursor solution within 10 min, and reacting at 80° C. for 2 h to obtain a white precipitate;

[0053] (3) The white precipitate obtained in step (2) is washed and dried, and then calcined at 1000° C. for 4 h in an oxygen atmosphere to obtain a bulk-doped titanium niobate negative electrode material.

[0054] Comparative Example 2

[0055] The difference between this comparative example and Example 1 is that in step (1), 0.84 g of urea is dissolved in 20 ml of ethanol to obtain a urea solution with a concentration of 0.042 g / ml, 0.14 g of titanium isopropoxide and 0.27 g of niobium pentachloride are added and stirred evenly, and 0.03 g of tin tetrachloride is added and stirred to obtain a titanium niobate precursor solution containing tin ions.

[0056] Comparative Example 3

[0057] The difference between this comparative example and Example 1 is that in step (1), 0.84 g of urea is dissolved in 20 ml of ethanol to obtain a urea solution with a concentration of 0.042 g / ml, 0.14 g of titanium isopropoxide and 0.27 g of niobium pentachloride are added and stirred evenly, and 0.2 g of tin tetrachloride is added and stirred to obtain a titanium niobate precursor solution containing tin ions.

[0058] The titanium niobate negative electrode material obtained in the above embodiments and comparative examples was used as an active material, mixed with acetylene black and a binder (PVDF) in a mass ratio of 70:20:10, and N-methylpyrrolidone was added to prepare a slurry, which was evenly coated on the current collector copper foil and dried at 110°C in vacuum for 12 h. The dried copper foil was cut into discs with a diameter of 14 mm and compacted at 20 MPa for 40 s to obtain the negative electrode sheet of the battery. Finally, the negative electrode sheet, lithium sheet, separator (Celgard2400) and electrolyte were assembled into a CR2032 button battery in a glove box filled with argon atmosphere. The electrochemical performance of the half-cell at different currents was tested using a blue battery test system, 1C=400mAg -1 , the voltage range is 0.8-3.0V (vs.Li + / Li), the test results are shown in Table 1.

[0059] Table 1 Button cell capacity at different currents (mAhg -1 )Data Sheet

[0060]

[0061]

[0062] pass Figure 2 As shown in Table 1, the titanium niobate negative electrode materials obtained in Examples 1-3 have good conductivity and rate performance for lithium ion batteries. In Example 4, the titanium niobate precursor solution containing tin ions and the oxalic acid solution are mixed too slowly, and the titanium niobate nanospheres in the obtained titanium niobate negative electrode material are relatively dense, which reduces the wettability of the electrolyte to the negative electrode material, reduces the lithium ion transmission rate, and deteriorates the conductivity. In Example 5, the titanium niobate precursor solution containing tin ions and the oxalic acid solution are mixed too quickly, and the surface pores of the titanium niobate nanospheres in the obtained titanium niobate negative electrode material increase, which triggers more side reactions and reduces the electrochemical performance. Figure 3 As can be seen from Table 1, the titanium niobate negative electrode material obtained in Comparative Example 1 is not doped with metal elements, and due to its lower electrical conductivity, its high-rate charge and discharge performance is poor; too few metal elements are added during the preparation of the titanium niobate negative electrode material obtained in Comparative Example 2, which has little effect on the unit cell volume and poor high-rate charge and discharge performance; too many metal elements are added during the preparation of the titanium niobate negative electrode material obtained in Comparative Example 3, resulting in serious deformation of the crystal structure of the titanium niobate negative electrode material, causing a decrease in the high-rate charge and discharge performance.

[0063] Finally, it should be noted that the specific embodiments described herein are merely examples of the spirit of the present invention, and are not intended to limit the implementation methods of the present invention. Those skilled in the art of the present invention may make various modifications or supplements to the described embodiments or replace them in similar ways. It is not necessary and impossible to provide all examples of all implementation methods here. However, these obvious changes or modifications derived from the essential spirit of the present invention still fall within the scope of protection of the present invention, and interpreting them as any additional limitation is contrary to the spirit of the present invention.

Claims

1. A method for preparing a bulk phase doped metal element titanium niobate negative electrode material, It is characterized in that The preparation method comprises: adding a titanium source and a niobium source into a urea solution, then adding a cationic precursor to obtain a titanium niobate precursor solution containing doped cations, mixing and stirring with an oxalic acid solution to obtain a white precipitate, washing, drying, and then calcining at a high temperature.

2. The preparation method according to claim 1, It is characterized in that The molar ratio of the titanium source to the niobium source is 1.0:0.5-5.

0.

3. The preparation method according to claim 1, It is characterized in that The concentration of the urea solution is 0.01-0.05 g / ml.

4. The preparation method according to claim 1, It is characterized in that The cationic precursor is one or more of tin metal salt, magnesium metal salt and lithium metal salt.

5. The preparation method according to claim 1, It is characterized in that The molar amount of the cation in the cation precursor is 10 to 40% of the total molar amount of the titanium source and the niobium source.

6. The preparation method according to claim 1, It is characterized in that The concentration of the oxalic acid solution is 0.01-0.04 g / ml.

7. The preparation method according to claim 1, It is characterized in that The mixing and stirring is performed using a peristaltic pump, and the mixing speed is 1.5 to 5.0 mL / min.

8. The preparation method according to claim 1, It is characterized in that The temperature during mixing and stirring is 80-120°C and the time is 0.5-2.0h.

9. The preparation method according to claim 1, It is characterized in that High temperature calcination is carried out in an oxygen atmosphere, the calcination temperature is 650-1000°C, and the time is 4-6 hours.

10. A bulk phase doped metal element titanium niobate negative electrode material, It is characterized in that The method is prepared according to claim 1.

Citation Information

Patent Citations

  • Tin-carbon co-doped titanium niobate material as well as preparation method and application thereof

    CN111874947A

  • Carbon-coated niobium-doped modified titanium niobate material and preparation method thereof

    CN112736250A