Method for preparing continuous fiber from Hetian jade abandoned ore and fly ash and continuous fiber

By mixing Hetian jade ore with fly ash and heating and melting wires at high temperature, continuous fibers with high tensile breaking strength were prepared, which solved the problem of insufficient utilization of Hetian jade ore, expanded its application field and improved Fiber properties.

CN119059731APending Publication Date: 2024-12-03HEBEI GEO UNIVERSITY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411147814.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Hetian jade abandoned mineral lacks effective high-value utilization methods in the existing technology, and is mainly used to mix with other materials to make building materials, resulting in limited application scenarios and low value, which is not conducive to environmental protection promotion.

Method used

After mixing the Hetian jade ore with fly ash in a specific proportion, it is heated and melted at high temperature, then cooled and melted again and wired at high linear speed to prepare continuous fibers, using its high tensile fracture strength and resistance to external force damage.

Benefits of technology

It has realized the high-value utilization of Hetian jade abandoned ore, expanded its application field, and produced continuous fibers with high tensile fracture strength and resistance to external force failure, suitable for the fiber field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059731A_ABST
    Figure CN119059731A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing a continuous fiber from Hetian jade waste ore and fly ash and the continuous fiber, and belongs to the technical field of fiber processing.The method specifically comprises the steps that the Hetian jade waste ore and the fly ash are crushed into powder, and the particle size of the powder is not larger than 160 meshes; the Hetian jade abandoned ore is a waste material in the Hetian jade mining and processing process; the fly ash is thermal power plant fire coal solid waste; the preparation method comprises the following steps: uniformly mixing 80%-40% by mass of Hetian jade abandoned ore powder and 20%-60% by mass of fly ash powder according to a mass fraction of the Hetian jade abandoned ore powder; heating and melting the mixed material at 1400-1500 DEG C, and cooling to obtain a solid state; and melting the solid material again in a range of 1300-1500 DEG C, and then drawing at a linear speed of 10-20 m / s to obtain the continuous fiber. By means of the treatment scheme, high-value utilization of the Hetian jade abandoned ore is achieved, and therefore the application field of the Hetian jade abandoned ore is expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fiber processing, and in particular to a method for preparing continuous fibers from Hetian jade waste ore and fly ash, and the continuous fibers. Background Art

[0002] Abandoned Hetian jade ore refers to solid waste generated during the development, processing, and carving of Hetian jade. The main mineral composition is still tremolite and a small amount of diopside, with a fiber interwoven structure, and the internal silicon-oxygen skeleton is mainly chain silicate. It has no industrial application value at present.

[0003] At present, the most common treatment method is to mix it with other materials to make building materials, etc. However, this not only has limited usage scenarios, but the value of the processed products is also limited and far lower than the cost of secondary processing, which is not conducive to the promotion of environmental protection at all.

[0004] Therefore, how to make high-value use of abandoned Hetian jade mines has become a research difficulty. Summary of the invention

[0005] Therefore, in order to overcome the shortcomings of the above-mentioned prior art, the present invention provides a method for preparing continuous fibers from abandoned Hetian jade ore and fly ash and continuous fibers, which can realize high-value utilization of abandoned Hetian jade ore, thereby expanding its application field.

[0006] In order to achieve the above-mentioned object, the present invention provides a method for preparing continuous fibers from Hetian jade abandoned ore and fly ash, comprising: S1, crushing the Hetian jade abandoned ore and fly ash into powder respectively, wherein the powder particle size is not more than 160. The Hetian jade abandoned ore is the waste material in the mining and processing process of Hetian jade, wherein tremolite is the main mineral and diopside is the secondary mineral; the fly ash is the solid waste of coal combustion in thermal power plants, wherein SiO 2 >55%、Al 2 O 3 >30%,Fe 2 O 3 The content is 2-5%, and other oxides are <10%; S2, uniformly mixing the Hetian jade abandoned ore powder and the fly ash powder according to the mass fraction, wherein the mass fraction of the Hetian jade abandoned ore powder is 80%-40%, and the mass fraction of the fly ash powder is 20%-60%; S3, the mixed material is heated and melted at 1400-1500°C, and is solid after cooling; S4, the solid material is melted again in the range of 1300-1500°C, and then spinning at a linear speed of 10-20m / s to obtain continuous fibers.

[0007] In one embodiment, in S3, the mixed material is heated at 1400-1500° C. for 2-6 hours.

[0008] In one embodiment, the chemical composition of the Hetian jade abandoned ore is SiO 2 >55%, MgO+CaO>38%, Fe 2 O 3 +Al 2 O 3 <2%, other oxide components <5%.

[0009] In one embodiment, in S4, the silicate glass is placed in a container with a small hole of 2 to 3 mm at the bottom, melted again in the range of 1300 to 1500°C, and then the melt is quickly pulled by a metal wire to a winding machine to draw at a line speed of 10 to 20 m / s to obtain continuous fibers.

[0010] In one embodiment, S3 heats the mixed material in a platinum container; and / or S4 heats the silicate glass in a platinum container or a platinum-rhodium alloy container having a small hole of 2 to 3 mm at the bottom.

[0011] A continuous fiber is prepared by the above method.

[0012] In one embodiment, the continuous fiber has a diameter of 6 to 25 μm, a tensile strength of 700 to 2000 MPa, and an elastic modulus of 50 to 70 MPa.

[0013] Compared with the prior art, the advantages of the present invention are that the discarded Hetian jade ore and fly ash are mixed to produce continuous fibers, which not only realizes the secondary utilization of the discarded Hetian jade ore, but also the produced continuous fibers have the properties of high tensile strength, resistance to external damage, and not easy to break, and can be applied in the fiber field. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0015] Figure 1 These are the process steps of the method for preparing continuous fibers from Hetian jade waste ore and fly ash in an embodiment of the present invention. DETAILED DESCRIPTION

[0016] The embodiments of the present application are described in detail below with reference to the accompanying drawings.

[0017] The following describes the implementation methods of the present application through specific examples, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The present application can also be implemented or applied through other different specific implementation methods, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present application. It should be noted that, in the absence of conflict, the following embodiments and the features in the embodiments can be combined with each other. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present application.

[0018] It should be noted that various aspects of the embodiments within the scope of protection of the present invention are described below. It should be apparent that the aspects described herein can be embodied in a wide variety of forms, and any specific structure and / or function described herein is merely illustrative. Based on the present application, it should be understood by those skilled in the art that an aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. For example, any number and aspect described herein can be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein can be used to implement this device and / or practice this method.

[0019] It should also be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present application. The drawings only show components related to the present application rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0020] Additionally, in the following description, specific details are provided to facilitate a thorough understanding of the examples. However, it will be understood by those skilled in the art that the aspects described may be practiced without these specific details.

[0021] The present application provides a method for preparing continuous fibers from Hetian jade waste ore and fly ash, comprising the following steps:

[0022] S1, crush the Hetian jade ore and fly ash into powder respectively, and the powder particle size is not more than 160 mesh; Hetian jade ore is the waste material in the mining and processing of Hetian jade, in which tremolite is the main mineral and diopside is the secondary mineral; fly ash is the solid waste of coal burning in thermal power plants, in which SiO 2 >55%、Al 2 O 3 >30%,Fe 2O 3 Content 2-5%, other oxides <10%.

[0023] Abandoned Hetian jade ore refers to the part of Hetian jade that cannot be used as jade material during mining and processing, among which tremolite is the main mineral and diopside is the secondary mineral. Tremolite is a metamorphic rock formed by the mixed deposition of dolomite and quartz, and the crystals are often arranged in radial or columnar shapes. Diopside is a common type of pyroxene, belonging to the monoclinic system. It is a silicate mineral and a silicate of calcium and magnesium. Fly ash is a common coal-fired solid waste. It is fly ash formed by high-temperature calcination of impurities mainly composed of clay minerals associated with coal. Its main chemical component is SiO 2 and Al 2 O 3 , may contain a certain amount of Fe 2 O 3 .

[0024] The purpose of crushing the abandoned Hetian jade ore and fly ash into powder is to facilitate the subsequent melting process, so the powder particle size is not larger than 160 mesh.

[0025] S2, uniformly mixing the Hetian jade waste ore powder and the fly ash powder according to mass fractions, wherein the mass fraction of the Hetian jade waste ore powder is 80% to 40%, and the mass fraction of the fly ash powder is 20% to 60%.

[0026] The mixing method can be grinding mixing, ball milling or air flow crushing, etc. The mass fraction ratio of Hetian jade waste ore powder and fly ash powder in the mixture is 80% to 40%: 20% to 60%.

[0027] S3, the mixed materials are heated to melt at 1400-1500°C and become solid after cooling.

[0028] The mixed materials are heated and melted at 1400-1500°C and solidified after cooling. The molten materials can be cooled at room temperature or by quenching. By cooling the molten materials by quenching, silicate glass can be obtained.

[0029] S4, the solid material is melted again in the range of 1300-1500°C, and then drawn at a linear speed of 10-20 m / s to obtain continuous fibers.

[0030] The solid material is melted again in the range of 1300-1500°C, and then drawn at a linear speed of 10-20m / s to obtain continuous fibers.

[0031] The above steps can be used to produce continuous fibers. In one embodiment, the continuous fibers have a diameter of 6 to 25 μm, a tensile strength of 700 to 2000 MPa, and an elastic modulus of 50 to 70 MPa.

[0032] The above method mixes abandoned Hetian jade ore and fly ash to produce continuous fibers, which not only realizes the secondary utilization of the abandoned Hetian jade ore, but also produces continuous fibers with high tensile strength, resistance to external damage, and not easy to break, and can be used in the fiber field.

[0033] In one embodiment, in S3, the mixed material is heated at 1400-1500° C. for 2-6 hours.

[0034] In one embodiment, the chemical composition of Hetian jade abandoned ore is SiO 2 >55%, MgO+CaO>38%, Fe 2 O 3 +Al 2 O 3 <2%, other oxide components <5%.

[0035] In one embodiment, in S4, silicate glass is placed in a container with a small hole of 2 to 3 mm at the bottom, melted again in the range of 1300 to 1500°C, and then the melt is quickly pulled by a metal wire to a winding machine to draw at a line speed of 10 to 20 m / s to obtain continuous fibers.

[0036] In one embodiment, S3 heats the mixed material in a platinum container; and / or

[0037] S4 Place the silicate glass in a platinum container or a platinum-rhodium alloy container with a small hole of 2 to 3 mm at the bottom and heat it.

[0038] Example

[0039] The following table discloses the specific composition of a type of Hetian jade abandoned ore and fly ash:

[0040] Sample <![CDATA[SiO 2 ]]> <![CDATA[Al 2 THE 3 ]]> <![CDATA[Fe 2 THE 3 ]]> MgO CaO other Hotan Jade Abandoned Mine 56.09 0.79 0.67 24.07 14.85 4.53 Fly ash 56.38 33.10 3.22 0.77 1.51 5.12

[0041] Example 1

[0042] S1, crushing the Hetian jade waste ore and fly ash into powder respectively, and the powder particle size is not more than 160 mesh;

[0043] S2, uniformly mixing the Hetian jade waste ore powder and the fly ash powder according to mass fractions, wherein the mass fraction of the Hetian jade waste ore in the mixture is 80%, and the mass fraction of the fly ash in the mixture is 20%;

[0044] S3, the mixed material is heated to melt at 1500°C and becomes solid after cooling;

[0045] S4, the solid material is melted again in the range of 1500°C, and then drawn at a linear speed of 18m / s to obtain continuous fibers.

[0046] The continuous fiber prepared by the method has a fiber diameter of 14 μm, a tensile breaking strength of 910 MPa, and an elastic modulus of 58 GPa.

[0047] Example 2

[0048] S1, crushing the Hetian jade waste ore and fly ash into powder respectively, and the powder particle size is not more than 160 mesh;

[0049] S2, uniformly mixing the Hetian jade waste ore powder and the fly ash powder according to mass fractions, wherein the mass fraction of the Hetian jade waste ore in the mixture is 70%, and the mass fraction of the fly ash in the mixture is 30%;

[0050] S3, the mixed material is heated to melt at 1480°C and becomes solid after cooling;

[0051] S4, the solid material is melted again in the range of 1480°C, and then drawn at a linear speed of 18m / s to obtain continuous fibers.

[0052] The continuous fiber prepared by the method has a fiber diameter of 13 μm, a tensile breaking strength of 1110 MPa, and an elastic modulus of 56 GPa.

[0053] Example 3

[0054] S1, crushing the Hetian jade waste ore and fly ash into powder respectively, and the powder particle size is not more than 160 mesh;

[0055] S2, uniformly mixing the Hetian jade waste ore powder and the fly ash powder according to mass fractions, wherein the mass fraction of the Hetian jade waste ore in the mixture is 60%, and the mass fraction of the fly ash in the mixture is 40%;

[0056] S3, the mixed material is heated to melt at 1360°C and becomes solid after cooling;

[0057] S4, the solid material is melted again in the range of 1360°C, and then drawn at a linear speed of 18m / s to obtain continuous fibers.

[0058] The continuous fiber prepared by the method has a fiber diameter of 13.5 μm, a tensile breaking strength of 1200 MPa, and an elastic modulus of 61 GPa.

[0059] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed in the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing continuous fibers from Hetian jade waste ore and fly ash, characterized in that: include: S1, crushing the abandoned Hetian jade ore and fly ash into powder respectively, with the particle size of the powder not exceeding 160 mesh; the abandoned Hetian jade ore is the waste material in the mining and processing of Hetian jade, wherein tremolite is the main mineral and diopside is the secondary mineral; fly ash is the solid waste from coal combustion in thermal power plants, wherein SiO2>55%, Al2O3>30%, Fe2O3 content 2-5%, and other oxides <10%; S2, uniformly mixing the Hetian jade waste ore powder and the fly ash powder according to mass fraction, wherein the mass fraction of the Hetian jade waste ore powder is 80% to 40%, and the mass fraction of the fly ash powder is 20% to 60%; S3, the mixed materials are heated to melt at 1400-1500°C and become solid after cooling; S4, melting the solid material again in the range of 1300-1500° C., and then spinning at a linear speed of 10-20 m / s to obtain continuous fibers.

2. The method according to claim 1, characterized in that In S3, the mixed materials are heated at 1400-1500° C. for 2-6 hours.

3. The method according to claim 1, characterized in that The chemical composition of the abandoned Hetian jade ore includes SiO2>55%, MgO+CaO>38%, Fe2O3+Al2O3<2%, and other oxide components<5%.

4. The method according to claim 1, characterized in that: In S4, the silicate glass is placed in a container with a small hole of 2 to 3 mm at the bottom, melted again in the range of 1300 to 1500° C., and then the melt is quickly pulled to a winding machine with a metal wire to draw a wire at a line speed of 10 to 20 m / s to obtain continuous fibers.

5. The method according to claim 1, characterized in that S3 heating the mixed material in a platinum container; and / or S4: placing the silicate glass in a platinum container or a platinum-rhodium alloy container with a small hole of 2 to 3 mm at the bottom and heating it.

6. A continuous fiber, characterized in that: The continuous fiber is prepared by the method according to any one of claims 1 to 5.

7. The continuous fiber according to claim 6, characterized in that The continuous fiber has a diameter of 6 to 25 μm, a tensile breaking strength of 700 to 2000 MPa, and an elastic modulus of 50 to 70 MPa.

Citation Information

Patent Citations

  • Glass fiber capable of being used as advanced reinforced substrate of composite material

    CN101691278A

  • Production method of fly ash insulation boards

    CN102873738A

  • Middle-alkali fly ash continuous fiber and preparation method thereof

    CN105366947A

  • High-thermal-stability solid waste-based continuous fiber and preparation method and application thereof

    CN111747653A

  • High-performance glass fiber composition, glass fiber thereof, and composite material

    US20180118608A1