Rapid road repairing material as well as preparation method and application thereof

By using components such as ultrafine silicate cement, sulfur aluminate cement with specific ratios in road repair materials, the problems of complex construction and poor durability in the existing technology are solved, and early strength, crack resistance and resistance are achieved The impact repair effect ensures rapid traffic recovery and high durability.

CN119059785AActive Publication Date: 2024-12-03SHANDONG DONGHUA TECH CO LTD

Patent Information

Application Number
CN202411580414.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-07
Publication Date
2024-12-03
Estimated Expiration
2044-11-07

AI Technical Summary

Technical Problem

The existing road repair materials are complex and time-consuming, with slow strength growth and poor durability, making it difficult to quickly achieve traffic recovery, and there are problems of insufficient penetration and adhesion of the base layer.

Method used

A type of ultrafine silicate cement, sulfur aluminate cement, coarse sand, fine sand, ultrafine powder, cellulose ether, expansion agent, water reducing agent, retarder, defoaming agent and redispersible latex are used. The powdered road rapid repair material is formed through specific stirring and preparation methods to form premature, crack-resistant and impact-resistant repair material. The compressive strength reaches more than 30MPa in 4 hours and the compressive strength reaches more than 60MPa in 28 days.

Benefits of technology

It realizes the early strength, crack resistance and impact resistance of road repair materials, and has good adhesion to the original concrete quickly, shortens the repair time, improves the durability and compressive resistance after repair, and ensures the convenience of traffic recovery. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059785A_ABST
    Figure CN119059785A_ABST
Patent Text Reader

Abstract

The invention discloses a rapid road repairing material and a preparation method and application thereof, and belongs to the technical field of road repairing materials. The rapid road repairing material is prepared from the following components in parts by weight: 28 to 34.5 parts of superfine Portland cement, 6.0 to 11.6 parts of superfine micro powder, 10.5 to 14.5 parts of sulphoaluminate cement, 27.0 to 29.3 parts of coarse sand, 16.5 to 18.9 parts of fine sand, 0.01 to 0.05 part of cellulose ether, 0.07 to 0.15 part of an expanding agent, 0.20 to 0.25 part of a water reducing agent, 0.08 to 0.12 part of a retarder, 0.02 to 0.06 part of lithium carbonate, 0.10 to 0.15 part of a de-foaming agent and 0.49 to 0.92 part of redispersible latex powder. The rapid road repairing material has the characteristics of early strength, crack resistance, impact resistance, self-leveling, rapid curing at normal temperature and good cohesiveness with original concrete, the compressive strength reaches 30 MPa or above within 4 hours, and traffic can be opened after the road surface is repaired for 4 hours; and the 28-day compressive strength reaches 60 MPa or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of road repair materials, and in particular relates to a rapid road repair material and a preparation method and application thereof. Background Art

[0002] The construction process of ordinary cement-based repair materials is complicated, time-consuming, and requires long traffic closures. In addition, the durability of new and old concrete is not optimistic. The main reasons that affect the service life of traditional repair materials are the poor permeability and adhesion of the base layer, with a bonding strength of only 0.5MPa; the base layer is prone to cracking due to temperature and alternating stress, and has poor toughness and durability. Affected by the above reasons, it causes overall cracking and falling off.

[0003] The existing road repair materials on the market have the following shortcomings: first, the repair time is relatively long, and the strength increases slowly. Usually, it is difficult to reach 15MPa in 4 hours, which makes it difficult to open to traffic quickly, and some even cannot be opened to traffic for several days. Second, road repair materials have a common problem of poor penetration and bonding with the base layer. It is difficult to achieve a tight penetration and bonding with the base layer, and they often have poor durability. After a year of alternating hot and cold weather, they often crack and fall off as a whole, seriously affecting the quality of the repair. Third, the maintenance time after repair is short, and there are problems with old cracks and temperature cracks that cannot be repaired, which seriously affects traffic roads and economic and social development. Summary of the invention

[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a road rapid repair material and a preparation method and application thereof; the road rapid repair material of the present invention has the characteristics of early strength, crack resistance, impact resistance, self-leveling, rapid curing at room temperature and good adhesion with original concrete, and the 4-hour compressive strength reaches more than 30MPa, and the road surface can be opened to traffic within 4 hours of repair; the 28-day compressive strength reaches more than 60MPa.

[0005] In order to achieve the above-mentioned purpose, the road rapid repair material comprises the following components, measured by weight: 28 to 34.5 parts of ultrafine silicate cement, 6.0 to 11.6 parts of ultrafine powder, 10.5 to 14.5 parts of sulphoaluminate cement, 27.0 to 29.3 parts of coarse sand, 16.5 to 18.9 parts of fine sand, 0.01 to 0.05 parts of cellulose ether, 0.07 to 0.15 parts of expansion agent, 0.20 to 0.25 parts of water reducer, 0.08 to 0.12 parts of retarder, 0.02 to 0.06 parts of lithium carbonate, 0.10 to 0.15 parts of defoamer and 0.49 to 0.92 parts of redispersible latex powder.

[0006] The ultrafine silicate cement is 31-33 parts, the ultrafine powder is 7.0-9.0 parts, the sulphoaluminate cement is 11.5-13.0 parts, the coarse sand is 28.0-29.1 parts, the fine sand is 17.9-18.5 parts, the cellulose ether is 0.02-0.04 parts, the expansion agent is 0.08-0.10 parts, the water reducer is 0.21-0.23 parts, the retarder is 0.9-0.11 parts, the lithium carbonate is 0.03-0.05 parts, the defoamer is 0.11-0.13 parts, and the redispersible latex powder is 0.6-0.8 parts. The water-cement ratio is 0.17:1. If the water-cement ratio is too small, the hydration heat will be large, the concrete will be easy to crack, and it will be unfavorable for on-site construction operation; if the water-cement ratio is too large, the strength of the concrete will be reduced. Lithium carbonate has the effect of increasing strength; the cellulose ether in the mortar dissolves in water, and the surface activity ensures that the cementitious material is effectively and evenly distributed in the system. Cellulose ether, as a protective colloid, "wraps" the solid particles and forms a lubricating film on their outer surface, making the mortar system more stable and preventing cracks in the road surface; the sulphoaluminate cement is 300 mesh.

[0007] The ultrafine powder is composed of 19-21% by mass of slag powder, 9-11% by mass of primary fly ash, 0.5-1.5% by mass of DC-C13 reinforcing agent, 6-8% by mass of PII52.5R cement and 61-63% by mass of compound gypsum; the compound gypsum is composed of 80% by mass of calcium sulfate and 20% by mass of hydrogen fluoride. The ultrafine powder has the characteristics of good filling, corrosion resistance and good fluidity, and can adjust the setting time of the material; the ultrafine powder is 700-900 mesh, preferably, the ultrafine powder is 800 mesh, and the preferred ultrafine powder can solidify quickly, with an initial setting time of 15min and a final setting time of 50min.

[0008] The average particle size of the ultrafine silicate cement is D50=4µm, D95=10µm; the specific surface area is 1150~1250m 2 / kg; the particle size distribution is 0.2~0.3µm>3.5%, 0.3~1.0µm>20%, 1.0~5.0µm>70% and 5.0~10.0µm<2.8%. Ultrafine silicate cement has good permeability, and the prepared slurry has good fluidity and diffusivity. The ultrafine silicate cement is 1000-1500 mesh, preferably, the ultrafine silicate cement is 1250 mesh; the preferred ultrafine silicate cement particles are evenly distributed, have anti-bending and anti-compression properties, and can greatly improve adhesion and strength.

[0009] The coarse sand particle size is 0.125-0.25 mm, and the fine sand particle size is 0.075 mm-0.1 mm. Different coarse sands and fine sands are added to adjust the material particle size distribution, increase the density, and obtain higher strength.

[0010] The strength grade of the ultrafine silicate cement is ≥75MPa, and the strength grade of the sulphoaluminate cement is ≥42.5MPa; the sulphoaluminate cement can control the setting time and can increase the early strength to within 4 to 24 hours.

[0011] The expansion agent is UEA expansion agent, the water reducer is polycarboxylic acid water reducer, the retarder is sodium citrate, the defoamer is polyether defoamer, and the redispersible latex powder is a copolymer of ethylene and vinyl acetate. UEA expansion agent effectively compensates for the early shrinkage of the quick repair material and reduces the risk of cracking after use. Polycarboxylic acid water reducer has great dispersibility and extremely high water reduction rate. Sodium citrate can improve the setting time, improve the tensile, compressive and antifreeze properties, and facilitate construction. Polyether defoamers can eliminate the generation of bubbles in the slurry, avoiding the generation of bubbles that affect the later strength. The redispersible latex powder is a copolymer of ethylene and vinyl acetate with the characteristics of thermoplastic materials, and forms an ideal bonding system with inorganic materials. Each component brings its own properties and complements each other, which can improve bonding, cohesion and wear resistance; the rebound depth is small and has good impact resistance; enhances flexural strength and durability, and reduces water absorption.

[0012] Cellulose ether is dissolved in water. Its surface activity ensures that the cementitious material is effectively and evenly distributed in the system. Cellulose ether, as a protective colloid, "wraps" the solid particles and forms a lubricating film on their outer surface, making the mortar system more stable and preventing the occurrence of road cracks.

[0013] The present invention also provides a method for preparing a road rapid repair material, comprising the following steps: (1) Stir ultrafine silicate cement, sulphoaluminate cement, coarse sand, fine sand and ultrafine powder at a rate of 90 to 110 r / min for 3 to 5 minutes to mix evenly to obtain component A; (2) Mix cellulose ether, swelling agent, polycarboxylic acid water reducer, retarder, polyether defoamer, redispersible latex powder and lithium carbonate by stirring at a rate of 110 to 130 r / min for 3 to 5 minutes to obtain component B; (3) Component A and component B are stirred at a rate of 90 to 110 r / min for 30 to 35 min to mix evenly, and then packaged and sealed in a three-layer laminated ziplock bag to obtain the road rapid repair material.

[0014] The stirring equipment required for the stirring in step (1) includes a stirring box, a stirring shaft, an aeration box and a fan. The stirring shaft is arranged in the stirring box. The air outlet of the aeration box is connected to the lower part of the stirring box. The air inlet of the aeration box is connected to the fan. The fan is turned on to suspend the material in the stirring box and fully homogenize it.

[0015] The diameter of the twin-shaft mixer is 700 mm, and the length of the tank is 3000-4000 mm. The twin-shaft mixer has the advantages of high efficiency, small footprint, compact structure, good sealing, stable operation, long service life, and safe and easy operation. The blower is a Roots blower.

[0016] The packaging machine is a rotary packaging machine, which has the advantages of high automation, fast packaging speed, suitability for packaging of various types of products, high safety factor, high bag making precision and easy operation. The three-layer laminated valve bag can prevent the material from getting damp and solidifying.

[0017] The quick repair material is used for road repair. The construction steps of the road quick repair material are as follows: (1) cleaning, (2) moistening, (3) adding diamond steel mesh, quick repair material preparation: the amount of water added accounts for 15% to 16% of the total mass of the repair material, (4) repairing, and (5) maintenance.

[0018] (1) Cleaning: First, remove the loose parts of the bulging, peeling, cracked and damaged parts. If they are not removed cleanly, it will affect the bonding strength of the ground in the later stage. The parts below 3mm, the parts that are too flat and the parts with oil pollution should be roughened. The roughening method is to use a professional roughening machine or manual electric pickaxe to roughen; clean the loose soil and debris on the bottom, and flush it with a high-pressure water gun. When flushing, the mud should be flushed out of the working surface and prevented from flowing back.

[0019] (2) Moisturizing: After flushing with water, the water should be kept on the working surface for 3 to 5 minutes to fully moisten the working surface until water seepage stops (no bubbles are observed). The working surface must be kept moist during construction, but no water should be accumulated.

[0020] (3) Add diamond steel mesh and prepare the rapid repair material: add diamond steel mesh when the working surface is wet. The size of the diamond steel mesh is 20*20*2mm. The diamond steel mesh can increase the overall strength and protect the steel bars. It can be used on wet bases and in wet environments and can be used as emergency repair materials. Prepare the rapid repair material: first pour water into a container and then add the road rapid repair material. Mix the road rapid repair material and water. The amount of water added should account for 15% to 16% of the total mass of the repair material. It is strictly forbidden to add more water. Stir thoroughly and evenly until there are no dry powder bubbles.

[0021] (4) Repair: Pour the road quick repair material evenly mixed with water onto the treated work surface and spread it flat with a scraper or trowel; the construction should be completed within 30 minutes from the time of adding water.

[0022] (5) Maintenance: The road surface needs to be sprayed with clean water within 1 to 2 hours of construction to keep it moist. Covering it with moist linen or plant fiber canvas can keep it moist, which can reduce the increase in surface temperature and prevent it from drying out prematurely.

[0023] Packaging, transportation and storage: Packed in three-layer laminated ziplock bags, 25kg / bag, with a shelf life of 6 months.

[0024] It must be stored in a dry and ventilated room with the packaging bag sealed to prevent moisture and freezing.

[0025] Compared with the prior art, the present invention has the following beneficial effects: (1) The road rapid repair material described in the present invention has the characteristics of early strength, crack resistance, impact resistance, self-leveling, rapid curing at room temperature and good adhesion with the original concrete. The 4-hour compressive strength reaches more than 30MPa, and the road surface can be opened to traffic within 4 hours after repair; the 28-day compressive strength reaches more than 60MPa.

[0026] (2) The road rapid repair material described in the present invention has strong adhesion, anti-stripping, excellent durability and a thermal expansion coefficient close to that of concrete; it can restore the original performance of the concrete pavement and at the same time have good impermeability.

[0027] (3) The road rapid repair material described in the present invention is an alkaline system, has good compatibility with cement and does not cause corrosion to steel bars; the diamond steel mesh can increase the overall strength and has protective properties for the steel bars, and can be used on a wet base and in a wet environment.

[0028] (4) The road rapid repair material of the present invention is non-toxic to the human body and has the characteristics of being non-flammable, safe, environmentally friendly, and easy to store and transport. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 A top view of a twin-shaft mixer.

[0030] Figure 2 A side view of a twin-shaft mixer.

[0031] Among them: 1. stirring box 2. stirring shaft 3. air inlet of charging box 4. air outlet of charging box 5. charging box 6. fan. DETAILED DESCRIPTION

[0032] The present invention will be further described below in conjunction with the embodiments, and Embodiment 4 is the best embodiment of the present invention.

[0033] The chemical additives used in the examples and comparative examples of the present invention are all commercially available, and their specific information is as follows: Ultrafine silicate cement: industrial grade, purchased from Shandong Donghua Technology Co., Ltd.; slag powder: industrial grade, purchased from Lingshou Zhaochen Mineral Products Co., Ltd.; primary fly ash: industrial grade, purchased from Lingshou Laipeng Mineral Products Business Department; calcium sulfate: industrial grade, Jinan Deqiao Chemical Technology Co., Ltd.; hydrogen fluoride: industrial grade, Shandong Weijin Chemical Technology Co., Ltd.; DC-C13 enhancer, industrial grade, purchased from Beijing Dechang Weiye Construction Engineering Technology Co., Ltd.; PII52.5R cement: industrial grade, purchased from Taizhou Jingmei Building Materials Co., Ltd.; sulphoaluminate cement: industrial grade, purchased from Qiyin Cement Plant Co., Ltd.; coarse sand: industrial grade, purchased from Tianjin Senda Weiye Building Materials Co., Ltd.; fine sand: industrial grade, purchased from Tianjin Senda Weiye Building Materials Co., Ltd.; cellulose ether: industrial grade, purchased from Jinan Ruilin Chemical Co., Ltd.; UEA expander: industrial grade, purchased from Shandong Ruiyuan Biotechnology Co., Ltd.; polycarboxylic acid water reducer: industrial grade, purchased from Shandong Bofei Cement Technology Service Co., Ltd.; sodium citrate: industrial grade, purchased from Shandong Kunteng Chemical Co., Ltd.; lithium carbonate: industrial grade, purchased from Shandong Suihua Biotechnology Co., Ltd.; polyether defoamer: industrial grade, purchased from Shandong Yuquan New Materials Technology Co., Ltd.; redispersible latex powder: industrial grade, purchased from Shandong Kaimaoxing Chemical Co., Ltd.; diamond steel mesh: industrial grade, purchased from Anping County Yuefeng Stainless Steel Trading Co., Ltd.; twin-shaft mixer: model ZJ700, purchased from Zhengkuang Machinery; water: ordinary tap water.

[0034] Example 1 A method for preparing a road rapid repair material comprises the following steps: (1) 28 parts of ultrafine silicate cement (1250 mesh), 14.5 parts of sulphoaluminate cement (300 mesh), 28.5 parts of coarse sand, 18.8 parts of fine sand and 9.0 parts of ultrafine powder (800 mesh), wherein the ultrafine powder consists of 20% by weight of slag powder, 10% by weight of primary fly ash, 1% by weight of DC-C13 reinforcing agent, 7% by weight of PII52.5R cement and 62% by weight of compound gypsum, are measured by a spiral metering scale and mixed in a twin-shaft mixer, and stirred at a rate of 100 r / min for 4 min to obtain component A.

[0035] See also Figure 1~2 The double-shaft stirring in this embodiment includes a stirring box 1, a stirring shaft 2, an aeration box 5 and a fan 6. The stirring shaft 2 is arranged in the stirring box, the air outlet 4 of the aeration box 5 is connected to the lower part of the stirring box 1, and the air inlet 3 of the aeration box is connected to the fan 6. Turn on the fan 6 to suspend the material in the stirring box 1 and fully homogenize it. This equipment is used in the embodiments of the present invention.

[0036] (2) 0.04 parts of cellulose ether, 0.08 parts of UEA expander, 0.24 parts of polycarboxylic acid water reducer, 0.12 parts of sodium citrate, 0.12 parts of polyether defoamer, 0.55 parts of redispersible latex powder and 0.05 parts of lithium carbonate were weighed using an electronic scale and stirred at a rate of 120 r / min for 4 min to obtain component B.

[0037] (3) Stir component A and component B at a rate of 100 r / min for 33 min. After mixing evenly, the road rapid repair material is obtained.

[0038] The construction steps of road rapid repair materials are as follows: (1) Cleaning: First, remove the loose parts of the bulging, peeling, cracked and damaged parts; clean the loose soil and debris on the bottom surface, and flush it with a high-pressure water gun. When flushing, the mud should be flushed out of the working surface and prevented from flowing back; (2) Moisturizing: After flushing with water, the water should be kept on the working surface for 4 minutes to fully moisten the working surface until water no longer seeps in (no bubbles are observed). The working surface must be kept moist during construction, but no water should accumulate; (3) Adding diamond steel mesh: Add diamond steel mesh when the working surface is wet. The size of the diamond steel mesh is 20*20*2mm. To prepare the rapid repair material, first pour water into the container and then add the road rapid repair material. Mix the road rapid repair material with 15.5 parts of water. Stir thoroughly and evenly until there are no dry powder bubbles. (4) Repair: Pour the road quick repair material mixed evenly with water onto the treated working surface and flatten it with a scraper; (5) Maintenance: The road surface needs to be sprayed with clean water within 1.5 hours of construction to keep it moist, and the moist effect can be achieved by covering it with moist burlap.

[0039] Example 2 A method for preparing a road rapid repair material comprises the following steps: (1) 29.5 parts of ultrafine silicate cement (1250 mesh), 13 parts of sulphoaluminate cement (300 mesh), 28 parts of coarse sand, 17.9 parts of fine sand and 10.5 parts of ultrafine powder (800 mesh), wherein the ultrafine powder consists of 20% by weight of slag powder, 10% by weight of primary fly ash, 1% by weight of DC-C13 reinforcing agent, 7% by weight of PII52.5R cement and 62% by weight of compound gypsum, are weighed using a spiral metering scale and mixed in a twin-shaft mixer, and stirred at a rate of 100 r / min for 4 min to obtain component A; (2) 0.03 parts of cellulose ether, 0.09 parts of UEA expander, 0.22 parts of polycarboxylic acid water reducer, 0.11 parts of sodium citrate, 0.12 parts of polyether defoamer, 0.49 parts of redispersible latex powder and 0.04 parts of lithium carbonate were weighed using an electronic scale and stirred at a rate of 120 r / min for 4 min to obtain component B; (3) Stir component A and component B at a rate of 100 r / min for 33 min. After mixing evenly, the road rapid repair material is obtained.

[0040] The construction steps of road rapid repair materials are as follows: (1) Cleaning: First, remove the loose parts of the bulging, peeling, cracked and damaged parts; clean the loose soil and debris on the bottom surface, and flush it with a high-pressure water gun. When flushing, the mud should be flushed out of the working surface and prevented from flowing back; (2) Moisturizing: After flushing with water, the water should be kept on the working surface for 4 minutes to fully moisten the working surface until water no longer seeps in (no bubbles are observed). The working surface must be kept moist during construction, but no water should accumulate; (3) Adding diamond steel mesh: Add diamond steel mesh when the working surface is wet. The size of the diamond steel mesh is 20*20*2mm. To prepare the rapid repair material, first pour water into the container and then add the road rapid repair material. Mix the road rapid repair material with 15.5 parts of water. Stir thoroughly and evenly until there are no dry powder bubbles. (4) Repair: Pour the road quick repair material mixed evenly with water onto the treated working surface and flatten it with a scraper; (5) Maintenance: The road surface needs to be sprayed with clean water within 1.5 hours of construction to keep it moist, and the moist effect can be achieved by covering it with moist burlap.

[0041] Example 3 A method for preparing a road rapid repair material comprises the following steps: (1) 28 parts of ultrafine silicate cement (1250 mesh), 14.5 parts of sulphoaluminate cement (300 mesh), 28.5 parts of coarse sand, 18.9 parts of fine sand and 9.0 parts of ultrafine powder (800 mesh), the ultrafine powder consisting of 20% by weight of slag powder, 10% by weight of primary fly ash, 1% by weight of DC-C13 reinforcing agent, 7% by weight of PII52.5R cement and 62% by weight of compound gypsum, were weighed using a spiral metering scale and mixed in a twin-shaft mixer, and stirred at a rate of 100 r / min for 4 min to obtain component A; (2) 0.04 parts of cellulose ether, 0.15 parts of UEA expander, 0 parts of polycarboxylic acid water reducer, 0.12 parts of sodium citrate, 0.13 parts of polyether defoamer, 0.60 parts of redispersible latex powder and 0.06 parts of lithium carbonate were weighed using an electronic scale and stirred at a rate of 120 r / min for 4 min to obtain component B; (3) Stir component A and component B at a rate of 100 r / min for 33 min. After mixing evenly, the road rapid repair material is obtained.

[0042] The construction steps of road rapid repair materials are as follows: (1) Cleaning: First, remove the loose parts of the bulging, peeling, cracked and damaged parts; clean the loose soil and debris on the bottom surface, and flush it with a high-pressure water gun. When flushing, the mud should be flushed out of the working surface and prevented from flowing back; (2) Moisturizing: After flushing with water, the water should be kept on the working surface for 4 minutes to fully moisten the working surface until water no longer seeps in (no bubbles are observed). The working surface must be kept moist during construction, but no water should accumulate; (3) Adding diamond steel mesh: Add diamond steel mesh when the working surface is wet. The size of the diamond steel mesh is 20*20*2mm. To prepare the rapid repair material, first pour water into the container and then add the road rapid repair material. Mix the road rapid repair material with 15.5 parts of water. Stir thoroughly and evenly until there are no dry powder bubbles. (4) Repair: Pour the road quick repair material mixed evenly with water onto the treated working surface and flatten it with a scraper; (5) Maintenance: The road surface needs to be sprayed with clean water within 1.5 hours of construction to keep it moist, and the moist effect can be achieved by covering it with moist burlap.

[0043] Example 4 A method for preparing a road rapid repair material comprises the following steps: (1) 32 parts of ultrafine silicate cement (1250 mesh), 12.2 parts of sulphoaluminate cement (300 mesh), 28.5 parts of coarse sand, 18 parts of fine sand and 8 parts of ultrafine powder (800 mesh), the ultrafine powder consisting of 20% by weight of slag powder, 10% by weight of primary fly ash, 1% by weight of DC-C13 reinforcing agent, 7% by weight of PII52.5R cement and 62% by weight of compound gypsum, were weighed using a spiral metering scale and mixed in a twin-shaft mixer, and stirred at a rate of 100 r / min for 4 min to obtain component A; (2) 0.03 parts of cellulose ether, 0.09 parts of UEA expander, 0.22 parts of polycarboxylic acid water reducer, 0.1 parts of sodium citrate, 0.12 parts of polyether defoamer, 0.70 parts of redispersible latex powder and 0.04 parts of lithium carbonate were weighed using an electronic scale, and stirred at a rate of 120 r / min for 3 min to obtain component B; (3) Stir component A and component B at a rate of 100 r / min for 33 min. After mixing evenly, the road rapid repair material is obtained.

[0044] The construction steps of road rapid repair materials are as follows: (1) Cleaning: First, remove the loose parts of the bulging, peeling, cracked and damaged parts; clean the loose soil and debris on the bottom surface, and flush it with a high-pressure water gun. When flushing, the mud should be flushed out of the working surface and prevented from flowing back; (2) Moisturizing: After flushing with water, the water should be kept on the working surface for 4 minutes to fully moisten the working surface until water no longer seeps in (no bubbles are observed). The working surface must be kept moist during construction, but no water should accumulate; (3) Adding diamond steel mesh: Add diamond steel mesh when the working surface is wet. The size of the diamond steel mesh is 20*20*2mm. To prepare the rapid repair material, first pour water into the container and then add the road rapid repair material. Mix the road rapid repair material with 15.5 parts of water. Stir thoroughly and evenly until there are no dry powder bubbles. (4) Repair: Pour the road quick repair material mixed evenly with water onto the treated working surface and flatten it with a scraper; (5) Maintenance: The road surface needs to be sprayed with clean water within 1.5 hours of construction to keep it moist, and the moist effect can be achieved by covering it with moist burlap.

[0045] Example 5 A method for preparing a road rapid repair material comprises the following steps: (1) 29.5 parts of ultrafine silicate cement (1250 mesh), 13 parts of sulphoaluminate cement (300 mesh), 28 parts of coarse sand, 17.9 parts of fine sand and 10.5 parts of ultrafine powder (800 mesh), the ultrafine powder consisting of 20% by weight of slag powder, 10% by weight of primary fly ash, 1% by weight of DC-C13 reinforcing agent, 7% by weight of PII52.5R cement and 62% by weight of compound gypsum, were weighed using a spiral metering scale and mixed in a twin-shaft mixer, and stirred at a rate of 100 r / min for 4 min to obtain component A; (2) 0.04 parts of cellulose ether, 0 parts of UEA expander, 0.25 parts of polycarboxylic acid water reducer, 0.12 parts of sodium citrate, 0.13 parts of polyether defoamer, 0.50 parts of redispersible latex powder and 0.06 parts of lithium carbonate were weighed using an electronic scale and stirred at a rate of 120 r / min for 4 min to obtain component B; (3) Stir component A and component B at a rate of 100 r / min for 33 min. After mixing evenly, the road rapid repair material is obtained.

[0046] The construction steps of road rapid repair materials are as follows: (1) Cleaning: First, remove the loose parts of the bulging, peeling, cracked and damaged parts; clean the loose soil and debris on the bottom surface, and flush it with a high-pressure water gun. When flushing, the mud should be flushed out of the working surface and prevented from flowing back; (2) Moisturizing: After flushing with water, the water should be kept on the working surface for 4 minutes to fully moisten the working surface until water no longer seeps in (no bubbles are observed). The working surface must be kept moist during construction, but no water should accumulate; (3) Adding diamond steel mesh: Add diamond steel mesh when the working surface is wet. The size of the diamond steel mesh is 20*20*2mm. To prepare the rapid repair material, first pour water into the container and then add the road rapid repair material. Mix the road rapid repair material with 15.5 parts of water. Stir thoroughly and evenly until there are no dry powder bubbles. (4) Repair: Pour the road quick repair material mixed evenly with water onto the treated working surface and flatten it with a scraper; (5) Maintenance: The road surface needs to be sprayed with clean water within 1.5 hours of construction to keep it moist, and the moist effect can be achieved by covering it with moist burlap.

[0047] Example 6 A method for preparing a road rapid repair material comprises the following steps: (1) 34.5 parts of ultrafine silicate cement (1250 mesh), 11.3 parts of sulphoaluminate cement (300 mesh), 29.3 parts of coarse sand, 16.5 parts of fine sand and 7 parts of ultrafine powder (800 mesh), the ultrafine powder consisting of 20% by weight of slag powder, 10% by weight of primary fly ash, 1% by weight of DC-C13 reinforcing agent, 7% by weight of PII52.5R cement and 62% by weight of compound gypsum, were weighed using a spiral metering scale and mixed in a twin-shaft mixer, and stirred at a rate of 100 r / min for 4 min to obtain component A; (2) 0.02 parts of cellulose ether, 0.12 parts of UEA expander, 0.2 parts of polycarboxylic acid water reducer, 0.08 parts of sodium citrate, 0.11 parts of polyether defoamer, 0.84 parts of redispersible latex powder and 0.03 parts of lithium carbonate were weighed using an electronic scale and stirred at a rate of 120 r / min for 4 min to obtain component B; (3) Stir component A and component B at a rate of 100 r / min for 33 min. After mixing evenly, the road rapid repair material is obtained.

[0048] The construction steps of road rapid repair materials are as follows: (1) Cleaning: First, remove the loose parts of the bulging, peeling, cracked and damaged parts; clean the loose soil and debris on the bottom surface, and flush it with a high-pressure water gun. When flushing, the mud should be flushed out of the working surface and prevented from flowing back; (2) Moisturizing: After flushing with water, the water should be kept on the working surface for 4 minutes to fully moisten the working surface until water no longer seeps in (no bubbles are observed). The working surface must be kept moist during construction, but no water should accumulate; (3) Adding diamond steel mesh: Add diamond steel mesh when the working surface is wet. The size of the diamond steel mesh is 20*20*2mm. To prepare the rapid repair material, first pour water into the container and then add the road rapid repair material. Mix the road rapid repair material with 15.5 parts of water. Stir thoroughly and evenly until there are no dry powder bubbles. (4) Repair: Pour the road quick repair material mixed evenly with water onto the treated working surface and flatten it with a scraper; (5) Maintenance: The road surface needs to be sprayed with clean water within 1.5 hours of construction to keep it moist, and the moist effect can be achieved by covering it with moist burlap.

[0049] Example 7 A method for preparing a road rapid repair material comprises the following steps: (1) 31 parts of ultrafine silicate cement (1250 mesh), 10.50 parts of sulphoaluminate cement (300 mesh), 27 parts of coarse sand, 18.5 parts of fine sand and 11.6 parts of ultrafine powder (800 mesh), the ultrafine powder consisting of 20% by weight of slag powder, 10% by weight of primary fly ash, 1% by weight of DC-C13 reinforcing agent, 7% by weight of PII52.5R cement and 62% by weight of compound gypsum, were weighed using a spiral metering scale and mixed in a twin-shaft mixer, and stirred at a rate of 100 r / min for 4 min to obtain component A; (2) 0.05 parts of cellulose ether, 0.07 parts of UEA expander, 0.23 parts of polycarboxylic acid water reducer, 0.10 parts of sodium citrate, 0.10 parts of polyether defoamer, 0.80 parts of redispersible latex powder and 0.05 parts of lithium carbonate were weighed using an electronic scale and stirred at a rate of 120 r / min for 4 min to obtain component B; (3) Stir component A and component B at a rate of 100 r / min for 33 min. After mixing evenly, the road rapid repair material is obtained.

[0050] The construction steps of road rapid repair materials are as follows: (1) Cleaning: First, remove the loose parts of the bulging, peeling, cracked and damaged parts; clean the loose soil and debris on the bottom surface, and flush it with a high-pressure water gun. When flushing, the mud should be flushed out of the working surface and prevented from flowing back; (2) Moisturizing: After flushing with water, the water should be kept on the working surface for 4 minutes to fully moisten the working surface until water no longer seeps in (no bubbles are observed). The working surface must be kept moist during construction, but no water should accumulate; (3) Adding diamond steel mesh: Add diamond steel mesh when the working surface is wet. The size of the diamond steel mesh is 20*20*2mm. To prepare the rapid repair material, first pour water into the container and then add the road rapid repair material. Mix the road rapid repair material with 15.5 parts of water. Stir thoroughly and evenly until there are no dry powder bubbles. (4) Repair: Pour the road quick repair material mixed evenly with water onto the treated working surface and flatten it with a scraper; (5) Maintenance: The road surface needs to be sprayed with clean water within 1.5 hours of construction to keep it moist, and the moist effect can be achieved by covering it with moist burlap.

[0051] Example 8 A method for preparing a road rapid repair material comprises the following steps: (1) 33 parts of ultrafine silicate cement (1250 mesh), 11.5 parts of sulphoaluminate cement (300 mesh), 29.1 parts of coarse sand, 18.9 parts of fine sand and 6.0 parts of ultrafine powder (800 mesh), the ultrafine powder consisting of 20% by weight of slag powder, 10% by weight of primary fly ash, 1% by weight of DC-C13 reinforcing agent, 7% by weight of PII52.5R cement and 62% by weight of compound gypsum, were weighed using a spiral metering scale and mixed in a twin-shaft mixer, and stirred at a rate of 100 r / min for 4 min to obtain component A; (2) 0.01 part of cellulose ether, 0.10 part of UEA expander, 0.21 part of polycarboxylic acid water reducer, 0.09 part of sodium citrate, 0.15 part of polyether defoamer, 0.92 part of redispersible latex powder and 0.02 part of lithium carbonate were weighed using an electronic scale and stirred at a rate of 120 r / min for 4 min to obtain component B; (3) Stir component A and component B at a rate of 100 r / min for 33 min. After mixing evenly, the road rapid repair material is obtained.

[0052] The construction steps of road rapid repair materials are as follows: (1) Cleaning: First, remove the loose parts of the bulging, peeling, cracked and damaged parts; clean the loose soil and debris on the bottom surface, and flush it with a high-pressure water gun. When flushing, the mud should be flushed out of the working surface and prevented from flowing back; (2) Moisturizing: After flushing with water, the water should be kept on the working surface for 4 minutes to fully moisten the working surface until water no longer seeps in (no bubbles are observed). The working surface must be kept moist during construction, but no water should accumulate; (3) Adding diamond steel mesh: Add diamond steel mesh when the working surface is wet. The size of the diamond steel mesh is 20*20*2mm. To prepare the rapid repair material, first pour water into the container and then add the road rapid repair material. Mix the road rapid repair material with 15.5 parts of water. Stir thoroughly and evenly until there are no dry powder bubbles. (4) Repair: Pour the road quick repair material mixed evenly with water onto the treated working surface and flatten it with a scraper; (5) Maintenance: The road surface needs to be sprayed with clean water within 1.5 hours of construction to keep it moist, and the moist effect can be achieved by covering it with moist burlap.

[0053] Example 9 A method for preparing a road rapid repair material comprises the following steps: (1) 32 parts of ultrafine silicate cement (1000 mesh), 12.2 parts of sulphoaluminate cement (300 mesh), 28.5 parts of coarse sand, 18 parts of fine sand and 8 parts of ultrafine powder (700 mesh), the ultrafine powder consisting of 19% by weight of slag powder, 9% by weight of primary fly ash, 0.5% by weight of DC-C13 reinforcing agent, 6% by weight of PII52.5R cement and 61% by weight of compound gypsum, were weighed using a spiral metering scale and mixed in a twin-shaft mixer, and stirred at a rate of 90 r / min for 3 min to obtain component A; (2) 0.03 parts of cellulose ether, 0.09 parts of UEA expander, 0.22 parts of polycarboxylic acid water reducer, 0.1 parts of sodium citrate, 0.12 parts of polyether defoamer, 0.70 parts of redispersible latex powder and 0.04 parts of lithium carbonate were weighed using an electronic scale, and stirred at a rate of 110 r / min for 3 min to obtain component B; (3) Stir component A and component B at a rate of 90 r / min for 30 min. After mixing evenly, the road rapid repair material is obtained.

[0054] The construction steps of road rapid repair materials are as follows: (1) Cleaning: First, remove the loose parts of the bulging, peeling, cracked and damaged parts; clean the loose soil and debris on the bottom surface, and flush it with a high-pressure water gun. When flushing, the mud should be flushed out of the working surface and prevented from flowing back; (2) Moisturizing: After flushing with water, the water should be kept on the working surface for 3 minutes to fully moisten the working surface until water no longer seeps (no bubbles are observed). The working surface must be kept moist during construction, but no water should be accumulated; (3) Adding diamond steel mesh: Add diamond steel mesh when the working surface is wet. The size of the diamond steel mesh is 20*20*2mm. To prepare the rapid repair material, first pour water into the container and then put in the road rapid repair material. Mix the road rapid repair material with 15 parts of water. Stir thoroughly and evenly until there are no dry powder bubbles. (4) Repair: Pour the road quick repair material evenly mixed with water onto the treated work surface and spread it flat with a trowel; (5) Maintenance: The road surface needs to be sprayed with clean water within 1 hour of construction to keep it moist, and the moist effect can be achieved by covering it with moist plant fiber canvas.

[0055] Example 10 A method for preparing a road rapid repair material comprises the following steps: (1) 32 parts of ultrafine silicate cement (1500 mesh), 12.2 parts of sulphoaluminate cement (300 mesh), 28.5 parts of coarse sand, 18 parts of fine sand and 8 parts of ultrafine powder (900 mesh), the ultrafine powder consisting of 21% by weight of slag powder, 11% by weight of primary fly ash, 1.5% by weight of DC-C13 reinforcing agent, 7% by weight of PII52.5R cement and 63% by weight of compound gypsum, were weighed using a spiral metering scale and mixed in a twin-shaft mixer, and stirred at a rate of 110 r / min for 5 min to obtain component A; (2) 0.03 parts of cellulose ether, 0.09 parts of UEA expander, 0.22 parts of polycarboxylic acid water reducer, 0.1 parts of sodium citrate, 0.12 parts of polyether defoamer, 0.70 parts of redispersible latex powder and 0.04 parts of lithium carbonate were weighed using an electronic scale and stirred at a rate of 130 r / min for 5 min to obtain component B; (3) Stir component A and component B at a rate of 110 r / min for 35 min. After mixing evenly, the road rapid repair material is obtained.

[0056] The construction steps of road rapid repair materials are as follows: (1) Cleaning: First, remove the loose parts of the bulging, peeling, cracked and damaged parts; clean the loose soil and debris on the bottom surface, and flush it with a high-pressure water gun. When flushing, the mud should be flushed out of the working surface and prevented from flowing back; (2) Moisturizing: After flushing with water, the water should be kept on the working surface for 5 minutes to fully moisten the working surface until water no longer seeps in (observe that no bubbles emerge). The working surface must be kept moist during construction, but no water should accumulate; (3) Adding diamond steel mesh: Add diamond steel mesh when the working surface is wet. The size of the diamond steel mesh is 20*20*2mm. To prepare the rapid repair material, first pour water into the container and then put in the road rapid repair material. Mix the road rapid repair material with 16 parts of water. Stir thoroughly and evenly until there are no dry powder bubbles. (4) Repair: Pour the road quick repair material evenly mixed with water onto the treated work surface and spread it flat with a trowel; (5) Maintenance: The road surface needs to be sprayed with clean water within 2 hours of construction to keep it moist, and the moist effect can be achieved by covering it with moist plant fiber canvas.

[0057] Comparative Example 1 The preparation method of the road rapid repair material described in this comparative example has the same steps as those of Example 4, except that no ultrafine silicate cement is added to the raw materials, and 44.2 parts of sulphoaluminate cement are added.

[0058] Comparative Example 2 The preparation method of the road rapid repair material described in this comparative example has the same steps as those of Example 4, except that sulphoaluminate cement is not added to the raw materials, but 44.2 parts of ultrafine silicate cement are added.

[0059] Comparative Example 3 The preparation method of the road rapid repair material described in this comparative example has the same steps as Example 4, except that no ultrafine powder is added to the raw materials, and 36 parts of ultrafine silicate cement and 16.2 parts of sulphoaluminate cement are added.

[0060] Performance Testing The performance of the road rapid repair materials prepared in the examples and comparative examples was tested, and the specific test results are shown in Table 1.

[0061] The setting time of road rapid repair materials is tested in accordance with GB / T1346-2011 "Test Methods for Water Consumption, Setting Time and Stability of Cement Standard Consistency"; The compressive strength of road rapid repair materials is tested in accordance with GB / T17671-2021 "Test method for strength of cement mortar (ISO method)"; The bonding strength of road rapid repair materials is tested in accordance with JG / J70-2009 "Standard for Test Methods for Basic Properties of Building Mortar"; The crack resistance of road rapid repair materials is tested in accordance with JC / T2234-2014 "Test Method for Early Crack Resistance of Cement"; The impact resistance of road rapid repair materials is tested in accordance with GB / T50475 "Technical Specifications for Concrete Rebound Method Testing"; The self-leveling performance of road rapid repair materials is tested in accordance with JC / T985-2017 "Cement-based self-leveling mortar for ground use".

[0062] Table 1 Performance test results of the road rapid repair materials of the embodiment and the comparative example .

[0063] It can be seen from the results in Table 1 that the road rapid repair material provided by the present invention has the characteristics of early strength, crack resistance, impact resistance, self-leveling, rapid curing at room temperature and good adhesion with the original concrete. The 4-hour compressive strength reaches more than 30MPa, and the road surface can be opened to traffic within 4 hours of repair, laying the foundation for rapid construction and ensuring construction quality. The water-cement ratio is 0.17:1, and it has good physical and mechanical properties and impermeability, improved durability and compressive resistance, and the thermal expansion coefficient is close to that of concrete; the 28-day compressive strength is as high as more than 60MPa, which solves the shortcomings of difficult repair of damaged road surfaces, poor bonding with concrete, and epoxy mortar cracking the base concrete.

[0064] The present invention effectively solves the common problems of base adhesion, unrepairable cracks, and slow strength growth through the research and preparation of various high-performance materials, and realizes rapid repair of the road surface. The maintenance time of the repaired road surface is only 1 to 2 hours, which improves the durability of the repaired road surface and reduces traffic costs.

[0065] It can be seen from the performance test results of Comparative Example 1 that ultrafine silicate cement can improve compression resistance, adhesion and strength; it can be seen from the performance test results of Comparative Example 2 that sulphoaluminate cement can accelerate the coagulation and hardening speed and improve the strength and volume stability of the repair material; it can be seen from the performance test results of Comparative Example 3 that ultrafine powder can adjust the coagulation time of the material and increase the fluidity of the material.

[0066] The road quick repair material of the present invention is an alkaline system, has good compatibility with cement and does not corrode steel bars. It is non-toxic to the human body and has non-flammable properties. It is safe, environmentally friendly, and easy to store and transport. The construction process is simple to operate. It can be used by adding water and stirring on site. The construction is convenient and the impact on traffic is reduced.

[0067] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A road rapid repair material, characterized in that: The invention comprises the following components in parts by weight: 28 to 34.5 parts of ultrafine silicate cement, 6.0 to 11.6 parts of ultrafine powder, 10.5 to 14.5 parts of sulphoaluminate cement, 27.0 to 29.3 parts of coarse sand, 16.5 to 18.9 parts of fine sand, 0.01 to 0.05 parts of cellulose ether, 0.07 to 0.15 parts of expansion agent, 0.20 to 0.25 parts of water reducing agent, 0.08 to 0.12 parts of retarder, 0.02 to 0.06 parts of lithium carbonate, 0.10 to 0.15 parts of defoaming agent and 0.49 to 0.92 parts of redispersible latex powder.

2. A road rapid repair material according to claim 1, characterized in that: The invention relates to 31-33 parts of ultrafine silicate cement, 7.0-9.0 parts of ultrafine powder, 11.5-13.0 parts of sulphoaluminate cement, 28.0-29.1 parts of coarse sand, 17.9-18.5 parts of fine sand, 0.02-0.04 parts of cellulose ether, 0.08-0.10 parts of expansion agent, 0.21-0.23 parts of water reducing agent, 0.9-0.11 parts of retarder, 0.03-0.05 parts of lithium carbonate, 0.11-0.13 parts of defoaming agent and 0.6-0.8 parts of redispersible latex powder, in parts by weight.

3. A road rapid repair material according to claim 1, characterized in that: The ultrafine powder consists of 19-21% by mass of slag powder, 9-11% by mass of primary fly ash, 0.5-1.5% by mass of DC-C13 reinforcing agent, 6-8% by mass of PⅠⅠ52.5R cement and 61-63% by mass of compound gypsum.

4. A road rapid repair material according to claim 1, characterized in that: The average particle size of the ultrafine silicate cement is D50=4µm, D95=10µm; the specific surface area is 1150~1250m 2 / kg.

5. A road rapid repair material according to claim 1, characterized in that: The coarse sand particle size is 0.125-0.25 mm, and the fine sand particle size is 0.075 mm-0.1 mm.

6. A road rapid repair material according to claim 1, characterized in that: The strength grade of the ultrafine silicate cement is ≥75MPa, and the strength grade of the sulphoaluminate cement is ≥42.5MPa.

7. A road rapid repair material according to claim 1, characterized in that: The expansion agent is a UEA expansion agent, the water reducer is a polycarboxylic acid water reducer, the retarder is sodium citrate, the defoamer is a polyether defoamer, and the redispersible latex powder is a copolymer of ethylene and vinyl acetate.

8. A method for preparing the road rapid repair material according to any one of claims 1 to 7, characterized in that: The steps include: (1) Stir ultrafine silicate cement, sulphoaluminate cement, coarse sand, fine sand and ultrafine powder at a rate of 90 to 110 r / min for 3 to 5 minutes to mix evenly to obtain component A; (2) Mix cellulose ether, swelling agent, polycarboxylic acid water reducer, retarder, polyether defoamer, redispersible latex powder and lithium carbonate by stirring at a rate of 110 to 130 r / min for 3 to 5 minutes to obtain component B; (3) Component A and component B are stirred at a rate of 90 to 110 r / min for 30 to 35 min to mix evenly, and then packaged and sealed in a three-layer laminated ziplock bag to obtain the road rapid repair material.

9. The method for preparing a road rapid repair material according to claim 8, characterized in that: The stirring equipment required for the stirring in step (1) comprises a stirring box (1), a stirring shaft (2), an aeration box (5) and a fan (6), wherein the stirring shaft (2) is arranged in the stirring box, the air outlet (4) of the aeration box (5) is connected to the lower part of the stirring box (1), and the air inlet (3) of the aeration box is connected to the fan (6). The fan (6) is turned on to suspend the material in the stirring box (1) and fully homogenize it.

10. Use of a road rapid repair material according to any one of claims 1 to 7, characterized in that: The rapid repair material is used for road repair.

Citation Information

Patent Citations

  • Cement-based rapid pavement repairing material and preparing method thereof

    CN106082891A

  • Quick repair mortar for high-speed railway concrete track slab and preparation method thereof

    CN111533517A

  • Quick-setting, quick-hardening, super-early-strength and high-crack-resistance pavement patching material and preparation method thereof

    CN111574174A

  • Pavement repair material prepared from industrial solid waste and used for winter construction

    WO2024066530A1

Cited By

  • Heavy-duty pavement rapid repair material as well as preparation method and application thereof

    CN121063887A