Early strength type concrete for road as well as preparation method and application of early strength type concrete
By using silicate cement, sulfoaluminate cement and gypsum in concrete for early-strength roads, combined with steel fibers and composite admixtures, the problems of on-site mixing pollution and long road closure in the existing technology are solved. , realizes ready-mix transportation and efficient repair of concrete for early-strength roads, and improves the durability and construction performance of concrete.
Patent Information
- Application Number
- CN202411182345.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
AI Technical Summary
The existing early strength repair materials are mixed on site, which are seriously polluted and have a long time to block the road, which cannot meet the long-term collapse performance requirements, affecting traffic safety.
Silicate cement, sulfoaluminate cement and gypsum are used as gel materials, combined with admixture, steel fibers and composite admixtures to prepare early-strength road concrete, which can be premixed at the mixing station and transported to site pouring , reduce on-site mixing and improve slump preservation performance.
It has realized the premixed transportation and pouring of concrete for early-strength roads, shortened the road closure time, improved the crack resistance, flexural resistance and corrosion resistance of concrete, reduced the frequency of road repair, and met the opening standards.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of concrete, and in particular relates to an early-strength concrete for roads and a preparation method thereof. Background Art
[0002] With the rapid increase in traffic volume in my country and the approaching service life of roads, concrete pavements will suffer varying degrees of damage. If they are not repaired in time, the road damage will become more and more serious, endangering traffic safety and causing traffic pressure.
[0003] At present, the early-strength repair materials on the market are all mixed on-site, with no requirements for collapse resistance, only requirements for early strength.
[0004] Therefore, there is an urgent need for a road repair material that can strengthen early and has long-term collapse-preserving properties. It can be mixed at a mixing station and transported to the site for pouring, solving the pollution problem of on-site mixing and achieving the purpose of reducing repair time. Summary of the invention
[0005] The technical problem actually solved by the present invention is to provide a premixed early-strength road concrete with early-strength performance and long collapse-retaining performance in view of the deficiencies in the prior art.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] The invention discloses an early-strength concrete for roads. The raw materials of the early-strength concrete for roads include, by weight, 10 to 20 parts of silicate cement, 5 to 15 parts of sulphoaluminate cement, 0 to 5 parts of gypsum, 0.5 to 5 parts of admixture, 50 to 100 parts of aggregate, 0.5 to 3 parts of admixture, 0 to 5 parts of steel fiber and 5 to 10 parts of water. The added amount of gypsum is not zero, and the added amount of steel fiber is not zero.
[0008] In some specific embodiments, the raw materials of the early-strength road concrete include 10-20 parts of silicate cement, 6-10 parts of sulphoaluminate cement, 0.5-3 parts of gypsum, 0.5-3 parts of admixture, 70-95 parts of aggregate, 0.5-2 parts of admixture, 0.5-5 parts of steel fiber and 6-8 parts of water.
[0009] According to some embodiments of the present invention, the aggregate is composed of fine aggregate and coarse aggregate in a mass ratio of 30-40:40-55, the particle size of the fine aggregate is less than 4.75 mm, and the particle size of the coarse aggregate is 5-25 mm.
[0010] In some specific embodiments, the fine aggregate is continuously graded sand with a particle size of less than 4.75 mm, and the coarse aggregate is continuously graded crushed stone with a particle size of 5 to 25 mm.
[0011] In some specific embodiments, the silicate cement is a silicate cement with a 28-day standard mortar compressive strength of 52.5 MPa. The sulphoaluminate cement can be selected without limitation, and specifically can be strength grades SAC52.5, SAC42.5, and the like.
[0012] In some specific embodiments, the admixture is a composite admixture, which includes a water reducer, a sulphoaluminate retarder, tartaric acid, lithium carbonate and water-retaining gel powder.
[0013] In some specific embodiments, the composite admixture includes, by weight, 30 to 50 parts of a water reducing agent, 30 to 45 parts of a sulphoaluminate retarder, 4 to 15 parts of tartaric acid, 5 to 15 parts of lithium carbonate and 0.5 to 5 parts of a water retaining gel powder.
[0014] The sulphoaluminate retarder is an admixture mainly composed of organic and inorganic phases and sodium citrate, which can delay the setting time of sulphoaluminate cement. The water-retaining gel powder is one or a combination of rubber powder and cellulose ether.
[0015] In some specific embodiments, the admixture is one or a combination of fly ash, modified fly ash vitrified microspheres, and mineral powder.
[0016] In some specific embodiments, the gypsum is anhydrous gypsum, hemihydrate gypsum or a combination of them.
[0017] The second technical solution adopted by the present invention is: a method for preparing the above-mentioned early-strength road concrete, comprising the step of stirring and mixing the raw materials of the early-strength road concrete.
[0018] The third technical solution adopted by the present invention: application of the above-mentioned early-strength road concrete in road repair.
[0019] A road repair method comprises the following steps:
[0020] (1) mixing the raw materials of the early-strength road concrete described above in a mixer to obtain a premix;
[0021] (2) placing the premix in a tank truck and transporting it to the construction site;
[0022] (3) pouring the premix to the desired construction location, vibrating, and finishing at one time;
[0023] (4) Before initial setting, perform secondary finishing;
[0024] (5) After final setting, watering and film covering are carried out for maintenance.
[0025] In step (2), during the transportation process, the tank body of the tank truck needs to rotate slowly and continuously.
[0026] In step (3), if the ambient temperature is lower than 25° C., the premix is subjected to heat preservation after pouring. The heat preservation may be performed by using an electric blanket.
[0027] In step (3), the vibration is performed by a vibrating rod to increase the working performance of the concrete; and watering and curing cannot be performed after the first finishing.
[0028] In step (4), the secondary finishing is performed when the raw materials are stirred for about 4±0.5h, and the concrete becomes slightly heated.
[0029] In step (5), after the final setting, the surface of the concrete turns white and has a preliminary hardness.
[0030] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:
[0031] The present invention adopts silicate cement, sulphoaluminate cement and gypsum as gel materials, and combines admixtures, aggregates, steel fibers and composite admixtures to prepare concrete with excellent collapse resistance, can be transported by tank trucks, does not require on-site mixing, and has excellent green environmental protection properties. The concrete can reach a strength of more than 30MPa within 6 to 8 hours, meeting traffic standards, reducing road closure time, and reducing urban management pressure and operating costs.
[0032] The concrete of the present invention also has the properties of crack resistance, bending resistance and corrosion resistance, thereby ensuring the durability of the concrete and reducing the frequency of road repairs. DETAILED DESCRIPTION
[0033] Existing concrete for road repair usually needs to be mixed on site, and has no requirements for collapse resistance, but only early strength. The present invention uses three components, silicate cement, sulphoaluminate cement and gypsum, as gel materials, combined with admixtures, aggregates, steel fibers and composite admixtures to prepare concrete, which can maintain collapse for about 2 hours, can be in a premixed form, does not require on-site mixing, greatly shortens the road closure period, and finally sets before 6 to 8 hours and reaches a strength of more than 30MPa, which meets the traffic standards, further shortening the road closure period.
[0034] The technical solution of the present invention is described in detail below in conjunction with specific embodiments so that those skilled in the art can better understand and implement the technical solution of the present invention, but the present invention is not limited to the scope of the examples.
[0035] In the following examples and comparative examples, the raw materials used are specifically selected as follows:
[0036] The silicate cement is PO 52.5 silicate cement; the sulphoaluminate cement is SAC52.5 sulphoaluminate cement;
[0037] The gypsum is anhydrite;
[0038] The admixture is fly ash;
[0039] The sand is continuously graded river sand with a particle size of less than 4.75 mm;
[0040] The crushed stone is a continuously graded crushed stone with a particle size of 5 to 25 mm;
[0041] The steel fibers are 4 cm long thick steel fibers.
[0042] Example 1
[0043] The raw material formula of the early-strength road concrete provided in this embodiment is shown in Table 1. In this embodiment, the admixture consists of 40 parts of polycarboxylate water reducer, 35 parts of sulphoaluminate retarder, 13 parts of tartaric acid, 10 parts of industrial lithium carbonate and 2 parts of cellulose ether.
[0044] Prepared by the following method:
[0045] Add sand and gravel into a mixing pot, then add Portland cement, sulphoaluminate cement, gypsum, fly ash, admixtures and steel fiber and mix for 60 seconds;
[0046] Add water into the mixing pot and mix, and then stir for 120 seconds until it is fully mixed to obtain an early-strength concrete mixture for roads.
[0047] Example 2
[0048] The raw material formula of the early-strength road concrete provided in this embodiment is shown in Table 1, and the admixture consists of 42 parts of polycarboxylate water reducer, 38 parts of sulphoaluminate retarder, 10 parts of tartaric acid, 8 parts of industrial lithium carbonate and 2 parts of rubber powder.
[0049] The preparation method is the same as Example 1.
[0050] Comparative Examples 1-2
[0051] The raw material formula of the concrete provided in Comparative Examples 1-2 is shown in Table 1, and the rest is the same as in Example 1.
[0052] Comparative Example 3
[0053] The concrete provided in this comparative example is different from that in Example 2 in that no steel fiber is added.
[0054] Comparative Example 4
[0055] The concrete provided in this comparative example is different from that in Example 2 in that no gypsum is added.
[0056] Comparative Example 5
[0057] The concrete provided in this comparative example is different from that in Example 2 in that about 30% more sulphoaluminate retarder is added, specifically, the amount of sulphoaluminate retarder is 49 parts.
[0058] Comparative Example 6
[0059] The concrete provided in this comparative example is different from that in Example 2 in that the amount of sulphoaluminate retarder added is about 30% less, specifically, the amount of sulphoaluminate retarder used is 26 parts.
[0060] Table 1 shows the raw material formula of concrete of Examples 1 to 2 and Comparative Examples 1 to 6 (in parts by weight)
[0061] raw material Example 1 Example 2 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Portland cement 13 15 14.6 21.4 15 15 15 15 Sulphoaluminate cement 7 9 0 0 9 9 9 9 plaster 1 2 0 0 2 0 2 2 Fly ash 1.5 1 9.7 1.7 1 1 1 1 sand 27 24 23.9 24.5 24 24 24 24 gravel 42 41 44.4 45.3 41 41 41 41 Admixtures 1 1.5 0.1 0.1 1.5 1.5 1.5 1.5 Steel Fiber 2 1 0 0 0 1 1 1 water 5.5 5.5 7.3 7 5.5 5.5 5.5 5.5
[0062] The concrete of Examples 1 to 2 and Comparative Examples 1 to 6 were tested for performance, and the results are shown in Table 2, where:
[0063] The test method for concrete slump is the method specified in GB / T 50080-2016 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures".
[0064] The test method for compressive strength is the method specified in GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete".
[0065] The concrete sample preparation method is as follows: pour the above-mentioned mixture into a mold, and after molding, cure it under standard curing conditions (20±2°C, relative humidity>95%) for 28 days to obtain a concrete sample.
[0066] Table 2 shows the performance test results of the concrete of Examples 1 to 2 and Comparative Examples 1 to 6
[0067]
[0068]
[0069] In Table 2, “—” indicates no strength.
[0070] As can be seen from Table 2, the initial slump of the concrete of the representative embodiment of the present application is larger, and it has excellent fluidity. The slump of the ordinary concrete of Comparative Examples 1 and 2 is small, and it can be seen that the working performance of the early-strength road concrete is more excellent. The early strength of 6h early strength Examples 1 and 2 is greater than 30MPa, which meets the requirements for traffic, while the ordinary concrete of Comparative Examples 1 and 2 has no strength. The strength of the early-strength road concrete of 1d strength Examples 1 and 2 is higher than that of the ordinary concrete of Comparative Examples 1 and 2, and the 28d strength, the ordinary concrete is slightly higher, but the strength of the early-strength road concrete of Examples 1 and 2 also reaches the required 60MPa. The 6h early strength of the early-strength road concrete lacking steel fiber in Comparative Example 3 does not decrease too much, and the 1d and 28d strengths have a certain degree of decrease. Comparative Example 4 does not add gypsum, gypsum has the effect of adjusting the setting time and increasing the strength in the early stage, and has the effect of micro-expansion reinforcement in the later stage. The early strength and late strength of concrete caused by not adding gypsum have both decreased significantly, which does not meet the requirements. In Example 5, after the sulphoaluminate retarder of the admixture was added by 30%, the concrete had serious early bleeding and the setting time was delayed, resulting in the failure to measure the 6h strength and a decrease in one-day strength. Due to bleeding, the pores in the concrete increased and the final strength also decreased, barely meeting the requirements. In Example 6, after the sulphoaluminate retarder of the admixture was added by 30%, the early collapse protection effect of the concrete was poor, and the concrete hardened in 1.5h, which could not achieve the expected collapse protection effect. It would condense in the mixing tank during production and transportation, causing losses. Due to the small amount of retarder in Example 6, the 6h strength was slightly higher. This is because after the early hydration peak of the sulphoaluminate cement, the strength growth slowed down, and the 1-day strength and 28-day strength were not much different from those of Example 2.
[0071] The composite admixture used in the present invention cooperates with other components of concrete to effectively maintain the early working performance of concrete, and can maintain the working performance for 2 hours, and the slump reduction value of 2 hours does not exceed 30mm, thereby ensuring construction, and final setting before 6 to 8 hours, and the compressive strength of concrete reaches more than 30MPa, thereby meeting the requirements for traffic. Due to the addition of steel fiber, the anti-bending and anti-cracking properties of early-strength road concrete are well enhanced, and sulphoaluminate cement has an anti-corrosion effect. The addition of these materials not only enables concrete to achieve an early strength effect, but also enables early-strength road concrete to have excellent anti-cracking, anti-bending and anti-corrosion properties, thereby ensuring the durability of concrete. In short, the concrete of the present invention has excellent anti-crack, anti-bending and anti-corrosion properties while maintaining high slump and early strength, thereby ensuring the durability of concrete.
[0072] When the concrete of the representative embodiment of the present application is used for road repair, the method is as follows:
[0073] (1) mixing the raw materials of the above concrete in a mixer to obtain a premix;
[0074] (2) The premix is placed in a tank truck and transported to the construction site. During the transportation process, the tank truck body rotates slowly and continuously;
[0075] (3) Pour the premix to the required construction location, vibrate with a vibrator to increase the concrete working performance, and perform a surface finishing at the same time. Do not spray water for curing;
[0076] (4) After the raw materials have been mixed for about 4 hours and before the initial setting, the concrete will heat up slightly and the secondary finishing will be carried out;
[0077] (5) After final setting, the surface turns white and has initial hardness, and watering and film covering are carried out for maintenance.
[0078] When used for road repair, it can be in premixed form, eliminating the need for mixing at the construction site, greatly shortening the road closure time.
[0079] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
[0080] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. An early-strength road concrete, characterized in that: The raw materials of the early-strength road concrete include 10-20 parts of silicate cement, 5-15 parts of sulphoaluminate cement, 0-5 parts of gypsum, 0.5-5 parts of admixture, 50-100 parts of aggregate, 0.5-3 parts of admixture, 0-5 parts of steel fiber and 5-10 parts of water by weight, and the added amount of gypsum is not zero, the added amount of steel fiber is not zero, and the admixture is a composite admixture, which includes a water reducer, a sulphoaluminate retarder, tartaric acid, lithium carbonate and water-retaining gel powder.
2. The early-strength road concrete according to claim 1, characterized in that: The raw materials of the early strength road concrete include 10-20 parts of silicate cement, 6-10 parts of sulphoaluminate cement, 0.5-3 parts of gypsum, 0.5-3 parts of admixture, 70-95 parts of aggregate, 0.5-2 parts of admixture, 0.5-5 parts of steel fiber and 6-8 parts of water.
3. The early-strength road concrete according to claim 1 or 2, characterized in that: The aggregate is composed of fine aggregate and coarse aggregate in a mass ratio of 30-40:40-55. The particle size of the fine aggregate is less than 4.75 mm, and the particle size of the coarse aggregate is 5-25 mm.
4. The early-strength road concrete according to claim 3, characterized in that: The fine aggregate is continuously graded sand with a particle size of less than 4.75 mm, and the coarse aggregate is continuously graded crushed stone with a particle size of 5 to 25 mm.
5. The early-strength road concrete according to claim 1 or 2, characterized in that: The silicate cement is silicate cement with a 28-day standard mortar compressive strength of 52.5 MPa.
6. The early-strength road concrete according to claim 1 or 2, characterized in that: In parts by weight, the composite admixture includes 30-50 parts of water reducing agent, 30-45 parts of sulphoaluminate retarder, 4-15 parts of tartaric acid, 5-15 parts of lithium carbonate and 0.5-5 parts of water-retaining gel powder.
7. The early-strength road concrete according to claim 1, characterized in that: The admixture is one or a combination of fly ash, modified fly ash vitrified microbeads, and mineral powder.
8. The early-strength road concrete according to claim 1, characterized in that: The gypsum is one or a combination of anhydrous gypsum and hemihydrate gypsum.
9. A method for preparing the early-strength road concrete according to any one of claims 1 to 8, characterized in that: The method comprises the steps of stirring and mixing the raw materials of the early-strength road concrete.
10. Use of the early-strength road concrete according to any one of claims 1 to 8 in road repair.