Sintered brick prepared from iron ore slag and preparation process thereof
Through the combination of iron ore slag, plastic raw materials, fly ash and polypropylene fiber, combined with crushing, screening, mixing, forming and sintering processes, the problem of sintering difficulty caused by the complexity of iron ore slag is solved, and high strength is achieved. The production of durable sintered bricks reduces production costs and environmental pollution and promotes the recycling of resources.
Patent Information
- Application Number
- CN202411187370.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing technology is difficult to effectively utilize iron ore slag, resulting in waste of resources and environmental pollution. At the same time, when making sintered bricks, it is difficult to sinter because of the complex properties and components of iron ore slag, making it difficult to make bricks that meet building performance and industrialization requirements. material.
Using a combination of 40-80 parts of iron ore slag, 10-30 parts of plastic raw materials, 5-15 parts of fly ash, 10-20 parts of water, 5-15 parts of slag powder, and 5-15 parts of polypropylene fiber, through pulverization, Sintered bricks are prepared by screening, mixing, forming, drying and sintering processes, using iron ore slag powder as raw materials to reduce additional treatment and improve the strength and durability of the bricks.
It realizes the production of high-strength, durability and crack resistance without additional physical or chemical treatment, which reduces production costs, is relatively energy-saving, avoids environmental pollution, and solves the problem of resource recycling.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron ore slag, in particular to a sintered brick made from iron ore slag and a preparation process thereof. Background Art
[0002] There are two types of iron ore slag. One type refers to the glassy byproduct formed when the molten slag from blast furnace ironmaking is rapidly cooled and does not have time to crystallize, and is in the form of fine particles or powder. The other type is the residual slag powder after iron is extracted from iron ore after grinding. This type of iron ore slag is the iron ore waste before blast furnace ironmaking melting. The present invention uses the second type of iron ore slag powder.
[0003] Since the content of components in iron ores from different origins is not the same, the composition of the produced iron ore slag is quite complex. Although some people have used iron ore slag in the prior art, they generally undergo certain physical and chemical treatments to make it meet specific requirements. A lot of manpower and material resources, especially a lot of energy, are consumed in the treatment process, and secondary waste is further generated, which is even more difficult to dispose of or utilize.
[0004] The waste dumping of iron ore slag not only wastes a lot of resources, but also causes serious secondary pollution to the environment. How to clean up and dispose of the waste dumped iron ore slag has become a common concern of all sectors of society. How to effectively and recycle iron ore slag according to local conditions is of great significance to the recycling of resources and the construction of a conservation-oriented society.
[0005] At present, some brick and tile factories are facing the development dilemma of raw material shortage. Using iron ore slag to replace clay to produce sintered bricks can not only avoid secondary pollution to the environment, help deal with iron ore slag waste generated by iron ore production, but also achieve sustainable development of brick and tile factories. However, due to the extremely complex properties and components of iron ore slag, it is easy to break or burst when making sintered bricks, so sintering is difficult. It is difficult to make sintered bricks that meet the requirements of building performance and industrialization in the existing technology. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention provides a sintered brick made from iron ore slag and a preparation process thereof, which solves the problem that it is difficult to make a brick that meets the requirements of building performance and industrialization.
[0007] To achieve the above objectives, the present invention is implemented through the following technical scheme: a sintered brick made of iron ore slag, comprising the following components in parts by weight: 40-80 parts of iron ore slag, 10-30 parts of plastic raw materials, 5-15 parts of fly ash, 10-20 parts of water, 5-15 parts of slag powder, and 5-15 parts of polypropylene fiber.
[0008] Preferably, the iron ore slag is iron tailings with a SiO2 content higher than 45% and a CaO content lower than 12%, and is crushed.
[0009] Preferably, the plastic raw material may be one or a mixture of two or more of clay, coal gangue, kaolin, bentonite, illite, diatomaceous earth and chlorite.
[0010] Preferably, a process for preparing sintered bricks made from iron ore slag comprises the following steps:
[0011] S1: Raw material preparation
[0012] The iron ore slag is crushed and screened to obtain a suitable particle size. The collected iron ore slag is screened to remove larger particles of impurities and foreign matter. For iron ore slag with larger particle size, it is necessary to crush it;
[0013] S2: Mixed
[0014] Mix the iron ore slag with other raw materials, such as clay and fly ash, in a certain proportion;
[0015] S3: Forming
[0016] The mixed raw materials are placed in a molding machine and pressed into the desired shape and size;
[0017] S4: Drying
[0018] Dry the formed bricks to remove moisture;
[0019] S5: Sintering
[0020] The dried bricks are placed in a sintering kiln and sintered at high temperatures to cause the minerals in the bricks to react chemically and form a solid structure.
[0021] S6: Cooling
[0022] The fired bricks are cooled to increase their strength and durability.
[0023] Preferably, in step S2, dry mixing is performed first, the solid raw materials are poured into a mixer for dry mixing, and then an appropriate amount of water is slowly added to the dry mixed raw materials, and polypropylene fibers are added at the same time. Finally, after adding water and fibers, stirring is continued for 10-15 minutes to fully mix the various raw materials with water and evenly distribute the polypropylene fibers in the mixture.
[0024] Preferably, in step S3, a suitable mold is selected to ensure that the size and shape of the mold meet the design requirements of the brick, and then the mixed raw materials are evenly spread in the mold, the mold containing the raw materials is placed in a press, and a certain pressure is applied to compress the raw materials into a brick blank. After the pressing is completed, the mold is removed from the press, and finally the brick blank is removed from the mold.
[0025] Preferably, in step S4, the temperature of the drying chamber should be controlled between 100-150°C, the relative humidity should be controlled between 30%-50%, the air flow rate should be controlled between 1-3m / s, and the moisture content of the dried bricks should be tested using a moisture meter to ensure that the moisture content of the bricks is below 5%.
[0026] Preferably, in step S5, the bricks are preheated first, and the temperature in the preheating zone is generally controlled between 300-600°C. When the bricks enter the sintering zone, the temperature rises to 950-1150°C, and the time in the sintering zone is generally controlled between 30-45 hours.
[0027] The present invention provides a sintered brick made from iron ore slag and a preparation process thereof.
[0028] Beneficial effects:
[0029] The present invention uses iron ore slag powder as raw material, and does not require additional physical or chemical treatment. It can make full use of industrial waste slag and reduce production costs. At the same time, it can produce high-quality sintered bricks with high strength, durability and crack resistance. A certain amount of energy is consumed during the sintering process, but compared with traditional clay brick production, the production process of iron ore slag sintered bricks is relatively energy-saving. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Embodiment 1:
[0032] The embodiment of the present invention provides a sintered brick made of iron ore slag, comprising the following components in parts by weight: 40 parts of iron ore slag, 30 parts of plastic raw materials, 15 parts of fly ash, 20 parts of water, 15 parts of slag powder, and 15 parts of polypropylene fiber;
[0033] Finer fly ash particles can be filled between iron ore slag and clay particles to increase the density of bricks, while coarser particles can act as a skeleton to enhance the strength of bricks.
[0034] The iron ore slag is: iron tailings with SiO2 content higher than 45% and CaO content lower than 12%, and is crushed.
[0035] The plastic raw material can be one or a mixture of two or more of clay, coal gangue, kaolin, bentonite, illite, diatomaceous earth and chlorite;
[0036] In iron ore slag sintered bricks, clay can play a bonding and reinforcing role.
[0037] A process for preparing sintered bricks made from iron ore slag comprises the following steps:
[0038] S1: Raw material preparation
[0039] The iron ore slag is crushed and screened to obtain a suitable particle size. The collected iron ore slag is screened to remove larger particles of impurities and foreign matter. For iron ore slag with larger particle size, it is necessary to crush it;
[0040] S2: Mixed
[0041] Mix the iron ore slag with other raw materials, such as clay and fly ash, in a certain proportion;
[0042] S3: Forming
[0043] The mixed raw materials are placed in a molding machine and pressed into the desired shape and size;
[0044] S4: Drying
[0045] Dry the formed bricks to remove moisture;
[0046] S5: Sintering
[0047] The dried bricks are placed in a sintering kiln and sintered at high temperatures to cause the minerals in the bricks to react chemically and form a solid structure.
[0048] S6: Cooling
[0049] The fired bricks are cooled to increase their strength and durability.
[0050] In step S2, dry mixing is first performed by pouring the solid raw materials into a mixer for dry mixing, then slowly adding an appropriate amount of water to the dry mixed raw materials, and adding polypropylene fibers at the same time, and finally adding water and fibers, and continuing to stir for 10 minutes to fully mix the various raw materials with water and evenly distribute the polypropylene fibers in the mixture;
[0051] The various raw materials such as iron ore slag, fly ash, polypropylene fiber, etc. are fully and evenly mixed to ensure that the performance of the bricks is stable and consistent during the subsequent molding and sintering processes. The uniform mixing can make the different raw materials fully contact with each other, promote the chemical reaction during the sintering process, and improve the strength, durability and other properties of the bricks.
[0052] In step S3, a suitable mold is selected to ensure that the size and shape of the mold meet the design requirements of the brick, and then the mixed raw materials are evenly spread in the mold, and the mold containing the raw materials is placed in a press, and a certain pressure is applied to compress the raw materials into a brick. After the pressing is completed, the mold is taken out of the press, and finally the brick is removed from the mold;
[0053] The mixed raw materials are processed into bricks with a certain shape and size to prepare for subsequent drying and sintering. The formed bricks should have sufficient strength and density to ensure that they will not break or deform during transportation and subsequent processing.
[0054] In step S4, the temperature of the drying chamber should be controlled at 100°C, the relative humidity should be controlled at 30%, the air flow rate should be controlled at 1m / s, and the moisture content of the dried bricks is tested using a moisture meter to ensure that the moisture content of the bricks is below 5%;
[0055] Remove moisture from the bricks to make them dry to a certain degree so that they can be sintered smoothly in the subsequent process, while avoiding cracking, deformation and other problems during sintering caused by excessive moisture.
[0056] In step S5, the bricks are preheated first, and the temperature of the preheating zone is generally controlled at 300°C. When the bricks enter the sintering zone, the temperature rises to 950°C, and the sintering time is generally controlled at 30 hours.
[0057] Through high-temperature heating, the various raw materials in the bricks undergo a series of physical and chemical changes, forming a stable mineral structure, thereby improving the strength, durability and other properties of the bricks.
[0058] Embodiment 2:
[0059] An embodiment of the present invention provides a sintered brick made of iron ore slag, comprising the following components in parts by weight: 80 parts of iron ore slag, 10 parts of plastic raw materials, 5 parts of fly ash, 10 parts of water, 5 parts of slag powder, and 5 parts of polypropylene fiber.
[0060] The iron ore slag is: iron tailings with SiO2 content higher than 45% and CaO content lower than 12%, and is crushed.
[0061] The plastic raw material can be one or a mixture of two or more of clay, coal gangue, kaolin, bentonite, illite, diatomaceous earth and chlorite.
[0062] A process for preparing sintered bricks made from iron ore slag, characterized in that it comprises the following steps:
[0063] S1: Raw material preparation
[0064] The iron ore slag is crushed and screened to obtain a suitable particle size. The collected iron ore slag is screened to remove larger particles of impurities and foreign matter. For iron ore slag with larger particle size, it is necessary to crush it;
[0065] S2: Mixed
[0066] Mix the iron ore slag with other raw materials, such as clay and fly ash, in a certain proportion;
[0067] S3: Forming
[0068] The mixed raw materials are placed in a molding machine and pressed into the desired shape and size;
[0069] S4: Drying
[0070] Dry the formed bricks to remove moisture;
[0071] S5: Sintering
[0072] The dried bricks are placed in a sintering kiln and sintered at high temperatures to cause the minerals in the bricks to react chemically and form a solid structure.
[0073] S6: Cooling
[0074] The fired bricks are cooled to increase their strength and durability.
[0075] In step S2, dry mixing is first performed by pouring the solid raw materials into a mixer for dry mixing, and then slowly adding an appropriate amount of water to the dry mixed raw materials, and adding polypropylene fibers at the same time. Finally, after adding water and fibers, stirring is continued for 15 minutes to fully mix the various raw materials with water and evenly distribute the polypropylene fibers in the mixture.
[0076] In step S3, a suitable mold is selected to ensure that the size and shape of the mold meet the design requirements of the brick, and then the mixed raw materials are evenly spread in the mold, the mold containing the raw materials is placed in a press, and a certain pressure is applied to compress the raw materials into a brick. After the pressing is completed, the mold is removed from the press, and finally the brick is removed from the mold.
[0077] In step S4, the temperature of the drying chamber should be controlled at 150°C, the relative humidity should be controlled at 50%, the air flow rate should be controlled at 3m / s, and the moisture content of the dried bricks is tested using a moisture meter to ensure that the moisture content of the bricks is below 5%.
[0078] In step S5, the bricks are preheated first, and the temperature in the preheating zone is generally controlled at 600°C. When the bricks enter the sintering zone, the temperature rises to 1150°C, and the sintering time is generally controlled at 45 hours.
[0079] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A sintered brick made from iron ore slag, characterized in that: The invention comprises the following components in parts by weight: 40-80 parts of iron ore slag, 10-30 parts of plastic raw materials, 5-15 parts of fly ash, 10-20 parts of water, 5-15 parts of slag powder and 5-15 parts of polypropylene fiber.
2. The sintered brick made of iron ore slag according to claim 1, characterized in that: The iron ore slag is: iron tailings with SiO2 content higher than 45% and CaO content lower than 12%, and is crushed.
3. The sintered brick made of iron ore slag according to claim 1, characterized in that: The plastic raw material can be one or a mixture of two or more of clay, coal gangue, kaolin, bentonite, illite, diatomaceous earth and chlorite.
4. A process for preparing sintered bricks made from iron ore slag, characterized in that: The following steps are involved: S1: Raw material preparation The iron ore slag is crushed and screened to obtain a suitable particle size. The collected iron ore slag is screened to remove larger particles of impurities and foreign matter. For iron ore slag with larger particle size, it is necessary to crush it; S2: Mixed Mix the iron ore slag with other raw materials, such as clay and fly ash, in a certain proportion; S3: Forming The mixed raw materials are placed in a molding machine and pressed into the desired shape and size; S4: Drying Dry the formed bricks to remove moisture; S5: Sintering The dried bricks are placed in a sintering kiln and sintered at high temperatures to cause the minerals in the bricks to react chemically and form a solid structure. S6: Cooling The fired bricks are cooled to increase their strength and durability.
5. The process for preparing sintered bricks made from iron ore slag according to claim 4, characterized in that: In step S2, dry mixing is first performed by pouring the solid raw materials into a mixer for dry mixing, then slowly adding an appropriate amount of water to the dry mixed raw materials, and adding polypropylene fibers at the same time, and finally adding water and fibers, and continuing to stir for 10-15 minutes to fully mix the various raw materials with water and evenly distribute the polypropylene fibers in the mixture.
6. The process for preparing sintered bricks made from iron ore slag according to claim 4, characterized in that: In step S3, a suitable mold is selected to ensure that the size and shape of the mold meet the design requirements of the brick, and then the mixed raw materials are evenly spread in the mold, the mold containing the raw materials is placed in a press, and a certain pressure is applied to compress the raw materials into a brick. After the pressing is completed, the mold is removed from the press, and finally the brick is removed from the mold.
7. The process for preparing sintered bricks made from iron ore slag according to claim 4, characterized in that: In step S4, the temperature of the drying chamber should be controlled between 100-150°C, the relative humidity should be controlled between 30%-50%, the air flow rate should be controlled between 1-3m / s, and the moisture content of the dried bricks is tested using a moisture meter to ensure that the moisture content of the bricks is below 5%.
8. The process for preparing sintered bricks made from iron ore slag according to claim 4, characterized in that: In step S5, the bricks are preheated first, and the temperature in the preheating zone is generally controlled between 300-600°C. When the bricks enter the sintering zone, the temperature rises to 950-1150°C, and the time in the sintering zone is generally controlled between 30-45 hours.