Wide-temperature low-power-consumption magnetic core and preparation method thereof

By adding specific auxiliary materials and process processing to magnetic materials, a wide temperature and low power consumption manganese zinc ferrite core is prepared, which solves the temperature and power consumption limitations of existing magnetic materials, and achieves high inductance and low inductance The effect of power loss is suitable for the rapid development of electronic products.

CN119059806AActive Publication Date: 2024-12-03广东尚朋电磁科技有限公司
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411050846.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-12-03
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

Existing magnetic materials have limitations in terms of use temperature, magnetic permeability and power consumption, and cannot meet the rapid development and energy-saving needs of electronic products.

Method used

Fe2O3, ZnO and MnO are used as main components, combined with CaCO3, ZrO2, Nb2O, Co2O3, nano SiO2, nano TiO2, Ta2O5, V2O5, Bi2O3 and HfO2, and wide temperature and low work are prepared through ball milling, spray granulation and sintering processes. The consumed manganese zinc ferrite core regulates the physical properties and losses of the material.

Benefits of technology

It realizes the low power consumption performance of the magnetic core in a wide temperature range, meets the requirements of high inductance, high energy conversion rate and low power loss, and expands the application range of the magnetic core.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004974870830000081
    Figure BDA0004974870830000081
Patent Text Reader

Abstract

The invention relates to the technical field of magnetic core processing, in particular to a wide-temperature low-power-consumption magnetic core and a preparation method thereof. A wide-temperature low-power-consumption magnetic core comprises a main component, a first auxiliary material and a second auxiliary material, and the main component is composed of Fe2O3, ZnO and MnO; the first auxiliary material is prepared from CaCO3, ZrO2, Nb2O, Co2O3, nano SiO2, and nano TiO2; the second auxiliary material is prepared from Ta2O5, V2O5, Bi2O3 and HfO2; the wide-temperature and low-power-consumption performance of the manganese-zinc ferrite is basically realized by controlling the adding range of the main body component and the first auxiliary material, and the loss is modified by adding the second auxiliary material, so that relatively low power loss is realized at each temperature, the application range of the wide-temperature and low-power-consumption magnetic core under extreme conditions can be solved to a great extent, and the application range of the wide-temperature and low-power-consumption magnetic core is expanded. And the requirements of high energy conversion rate, low power loss and wide-temperature use of the wide-temperature low-power-consumption magnetic core are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of magnetic core processing technology, and in particular to a wide-temperature and low-power consumption magnetic core and a preparation method thereof. Background Art

[0002] Magnetic core refers to a sintered magnetic metal oxide composed of a mixture of various iron oxides. Currently, most of the magnetic cores with superior functions are made of soft ferrite. Since the soft ferrite material was successfully developed by the Philips Laboratory in the Netherlands in 1935, it has a history of more than 80 years. Since the magnetism of ferrite comes from ferrimagnetism, its saturation magnetization intensity is lower than that of metal magnetism, but its resistivity ρ is much higher than that of metal magnetism, so it has good high-frequency characteristics. In the field of weak current and high-frequency technology, soft ferrite has unique advantages. Magnetic cores made of this type of material are the core components of various inductors, electronic transformers, choke coils, suppressors, filters, etc.

[0003] Due to the rapid development of the electronic information industry, the speed of electronic product replacement has accelerated, and the products have developed towards environmental protection, energy saving and miniaturization. This has led to unprecedented development of magnetic materials, the basic materials of electronic products. A large number of applications in the communications industry, IT industry, automotive industry, etc. have promoted the rapid development of high-performance ferrite products.

[0004] At present, the size of household electronic products is gradually reduced, and energy saving and consumption reduction are required, which leads to the development of power transformer structure towards miniaturization and flatness, which greatly reduces product weight and reduces costs. Existing magnetic materials cannot meet the needs of industry development due to limitations such as operating temperature, magnetic permeability, and power consumption. Summary of the invention

[0005] The purpose of this application is to provide a wide-temperature, low-power consumption magnetic core and a preparation method thereof in view of the deficiencies in current technology.

[0006] In a first aspect, the present application provides a wide temperature and low power consumption magnetic core, which adopts the following technical solution: A wide temperature and low power consumption magnetic core, comprising a main component, a first auxiliary material and a second auxiliary material, wherein the main component, in terms of molar fraction, is composed of Fe2O3, ZnO and MnO, with a content of Fe2O3 52.3-52.9mol%, ZnO 7.58.2mol%, and the rest being MnO; the first auxiliary material comprises CaCO3, ZrO2, Nb2O, Co2O3, nano-SiO2, and nano-TiO2; the first auxiliary material, in terms of the total weight of the main component, comprises the following components: CaCO3 0.03-0.05wt%, ZrO2 0.002-0.005wt%, Nb2O 0.02-0.03wt%, Co2O3 0.20-0.26wt%, nano-SiO2 0.004-0.007wt%, nano-TiO2 0.006-0.009wt%; the second auxiliary material includes Ta2O5, V2O5, Bi2O3, and HfO2; the second auxiliary material is calculated based on the total weight of the main components, and the content of each auxiliary material component is Ta2O50.03-0.05wt%, V2O50.06-0.09wt%, Bi2O30.05-0.08wt%, HfO20.01-0.04wt%, the particle size of the nano-SiO2 is 20-40 nanometers, and the particle size of the nano-TiO2 is 40-80 nanometers.

[0007] By adopting the above technical scheme, in the present application, the main components Fe2O3, ZnO and MnO serve as the basis for forming manganese-zinc ferrite, Fe2O3 provides magnetism, ZnO can improve the material's ability to resist saturation magnetic fields, and MnO can increase the material's resistivity and specific permeability. The role of the first auxiliary material is mainly to change the material's physical properties by regulating the content of different elements. The addition of CaCO3 can promote the growth of grains and the reduction of the hysteresis loop, ZrO2 and Nb2O5 can improve the material's ability to resist saturation magnetic fields, the addition of Co2O3 can increase the material's thermal stability against magnetic fields, and the addition of nano-SiO2 and nano-TiO2 can reduce the loss of the hysteresis loop and permeability of the magnetic core. The role of the second auxiliary material is to further improve the material's performance. The addition of Ta2O5 and V2O5 can significantly reduce the material's loss, the addition of Bi2O3 can increase the material's saturation magnetic induction intensity and residual induction intensity, and the addition of HfO2 can improve the material's stability against magnetic fields. The synergistic effect of each component in this application is to make the manganese-zinc ferrite core have the performance of wide temperature and low power consumption by comprehensively regulating the types and contents of the main components and auxiliary materials. The main components provide the basic performance of manganese-zinc ferrite, and the first auxiliary material further improves the performance of the material by regulating grain growth, reducing the loss of hysteresis loop and magnetic permeability, and the addition of the second auxiliary material can modify the loss and enhance the stability of the material. Through the synergistic effect, the core can have low power consumption in a wide temperature range, meeting the requirements of high inductance, high energy conversion rate and wide temperature use.

[0008] In a second aspect, the present application provides a method for preparing a wide temperature and low power consumption magnetic core, using the following technical solution: A method for preparing a wide temperature and low power consumption magnetic core, using the raw materials of the wide temperature and low power consumption magnetic core described above, comprising the following steps: S21, batching and ball milling: mixing the main components Fe2O3, ZnO and MnO according to the formula, then adding water in a ball mill for mixing and ball milling, cyclic ball milling for 30-60 minutes, drying, and then pre-calcining at a temperature of 850-900° C. for 1.5-2.5 hours in an air atmosphere to obtain a pre-calcined material; S22, secondary ball milling: mixing the first auxiliary material, the second auxiliary material and the pre-burned material obtained in step S31, performing secondary ball milling and drying to obtain ball milled powder; S23, spray granulation and molding: the powder after stirring is sequentially passed through a 100-mesh sieve, and then transferred into a spray tower, and spray granulated into particles of 50-200 μm; the particles are molded into magnetic core blanks; S24, sintering: including the following sintering steps: heating the magnetic core blank to a first temperature of 1250-1350°C, introducing a certain amount of oxygen during the first heat preservation, cooling to a second temperature of 300-350°C at a first cooling rate under a balanced oxygen partial pressure atmosphere, second heat preservation, and finally cooling to a third temperature of 60-70°C at a second cooling rate, and then naturally cooling to room temperature to obtain a wide temperature and low power consumption magnetic core.

[0009] By adopting the above technical scheme, the preparation method in the present application mainly includes the following steps: S21, batching and ball milling: the purpose of this step is to mix and ball mill the main components Fe2O3, ZnO and MnO, and make the powders uniformly mixed by ball milling, and make the grains finer. Deionized water added during the ball milling process helps the mixing and ball milling of the powders. S22, secondary ball milling: in this step, the first auxiliary material, the second auxiliary material and the pre-sintered material are mixed for secondary ball milling to further enhance the mixing uniformity of each component, thereby obtaining a more stable particle size. S23, spray granulation and molding: the ball milled powder is spray granulated, and spray granulation can form the powder into particles, making it easier to mold. During the molding process, the particles are pressed or injection molded to form a blank of the magnetic core. S24, sintering: this step is to densify the magnetic core blank and form a solid structure by high temperature treatment. Through the process of heating, heat preservation and cooling, the grains in the material are fused and formed into a continuous structure. Sintering plays a vital role in improving the performance of the magnetic core. Through the synergistic effect of the above steps, a magnetic core with wide temperature and low power consumption performance can be prepared. During the batching and ball milling process of the main component and the first auxiliary material, the ball milling makes the powder mixed evenly and the grains fine, thereby improving the physical properties of the material. The addition of the second auxiliary material further modifies the loss of the material and improves the stability of the material. During the spray granulation and molding process, particles suitable for molding are formed and a magnetic core blank is obtained, which provides a good prerequisite for subsequent sintering. Sintering causes the grains of the magnetic core to fuse and form a dense structure, so that the magnetic core has the performance of wide temperature and low power consumption. Through the synergistic effect of each step, the preparation method in the present application can achieve the performance of manganese-zinc ferrite with wide temperature and low power consumption, and meet the requirements of high inductance, high energy conversion rate, low power loss and wide temperature use.

[0010] Preferably, in step S21, the mass ratio of raw material: grinding medium: water put into the ball mill is 1:6-8:1.2-1.6, and the grinding medium is a zirconium ball of Φ0.4-0.55 mm.

[0011] Preferably, in step S22, the secondary sand milling time is 2-3 hours; and the particle size D50 of the ball-milled powder is 0.8-1.0 μm.

[0012] Preferably, in step S23, a binder is added during the spray granulation process, and the binder is a composition of polyvinyl alcohol and zinc stearate in a mass ratio of 5:1-3.

[0013] Preferably, the concentration of the binder solution is 6-8wt%, and the binder accounts for 8-10% of the sieved ball-milled powder.

[0014] By adopting the above technical scheme, in step S23, the role of adding a binder during the spray granulation process is to agglomerate the powder into particles and help form a magnetic core blank. The composition of the binder is polyvinyl alcohol and zinc stearate, which can provide sufficient bonding force and plasticity, so that the powder forms particles during the spray granulation process and maintains the shape during the subsequent molding process. The solution concentration of the binder is 6-8wt%. By controlling the concentration, it can be ensured that the solution has appropriate viscosity and fluidity, which is convenient for the spray granulation process. The amount of binder added is 8-10% of the powder after the ball mill powder is sieved. By controlling the amount of binder added, the powder can obtain sufficient bonding force, thereby forming a relatively stable particle structure. The addition of the binder in step S23 can make the powder easier to form particles and maintain the stability of the particle shape, thereby providing good conditions for the subsequent molding process. The addition of the binder can also help improve the density and strength of the particles during the spray granulation process, thereby improving the physical properties of the final magnetic core.

[0015] Preferably, in step S23, the molding pressure is 80-150 MPa and the molding time is 30-100 s.

[0016] Preferably, in step S24, the heating rate of the heating is 2-3°C / min, and the insulation time at the first temperature is 3-6h.

[0017] Preferably, in step S24, the first cooling rate is 1.5-2°C / min, the second temperature holding time is 5-8h, and the second cooling rate is 0.2-0.4°C / min.

[0018] Preferably, in step S24, the oxygen content in the balanced oxygen partial pressure atmosphere is 1.8-2.3 vol%.

[0019] By adopting the above technical scheme, in step S24, when the magnetic core blank is sintered, a certain amount of oxygen is introduced under the atmosphere of balanced oxygen partial pressure, wherein the oxygen content is 1.8-2.3vol%. The existence and control of the balanced oxygen partial pressure in this step are very important, and cooperate with other steps to jointly realize the preparation of a wide temperature and low power consumption magnetic core. During the sintering process, the existence of the balanced oxygen partial pressure can affect the magnetic properties and electrical properties of the magnetic core. The appropriate oxygen content can control the crystal structure and magnetic properties of the magnetic core, thereby affecting the low power loss and wide temperature characteristics of the magnetic core. Specifically, the appropriate oxygen content helps to form an ideal magnetic grain structure, improve the saturation magnetization and coercive force of the magnetic core, thereby improving the inductance and energy conversion rate of the magnetic core. In addition, controlling the oxygen content can also effectively regulate the hysteresis loss of the magnetic core, so that the magnetic core can maintain a low power loss in all temperature ranges. By controlling the oxygen content in the balanced oxygen partial pressure atmosphere, the regulation of the magnetic core grain structure and magnetic properties can be achieved during the sintering process, thereby achieving the requirements of a wide temperature and low power consumption magnetic core.

[0020] In summary, the beneficial technical effects of this application are: 1. Control the addition range of the main component and the first auxiliary material to achieve the performance of manganese-zinc ferrite with wide temperature and low power consumption. By mixing the main components such as Fe2O3, ZnO and MnO, a magnetic core material with good wide temperature characteristics can be obtained.

[0021] 2. Add the second auxiliary material to modify the loss, so that there is a lower power loss at each temperature. By mixing the first auxiliary material, the second auxiliary material and the pre-burned material, the loss of the magnetic core can be adjusted to achieve the effect of low power consumption.

[0022] 3. Solve the application scope under extreme conditions. This preparation method can maintain the wide temperature and low power consumption performance of the magnetic core under extreme temperature conditions, so that the magnetic core can still work normally in high or low temperature environments, expanding the application scope of the magnetic core.

[0023] 4. Meet the requirements for high inductance, high energy conversion rate, low power loss and wide temperature use of wide temperature and low power consumption magnetic core. The magnetic core obtained by this preparation method has high inductance and energy conversion rate, low power loss, and can work stably in a wide temperature range. DETAILED DESCRIPTION

[0024] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0025] Example 1 A wide temperature and low power consumption magnetic core, comprising a main component, a first auxiliary material and a second auxiliary material, wherein the main component, in terms of molar fraction, is composed of Fe2O3, ZnO and MnO, with a content of Fe2O3 52.3mol%, ZnO 7.5mol%, and the rest being MnO; the first auxiliary material comprises CaCO3, ZrO2, Nb2O, Co2O3, nano-SiO2, and nano-TiO2; the first auxiliary material, in terms of the total weight of the main component, comprises the following components: CaCO3 0.03wt%, ZrO2 0.002wt%, Nb2O 0.02wt%, Co2O3 0.20wt%, nano-SiO2 0.004wt%, nano-TiO2 0.006wt%; the second auxiliary material includes Ta2O5, V2O5, Bi2O3, and HfO2; the second auxiliary material is calculated based on the total weight of the main components, and the content of each auxiliary material component is Ta2O50.03wt%, V2O50.06wt%, Bi2O30.05wt%, HfO20.01wt%, the particle size of the nano-SiO2 is 20-40 nanometers, and the particle size of the nano-TiO2 is 40-80 nanometers.

[0026] A method for preparing a wide temperature range and low power consumption magnetic core, using the raw materials of the wide temperature range and low power consumption magnetic core, comprises the following steps: S21, ingredients and ball milling: main components Fe2O3, ZnO and MnO are mixed according to the formula amount, and then water is added to the ball mill for mixing and ball milling. The mass ratio of the raw material put into the ball mill: grinding medium: water is 1:6:1.2, and the grinding medium is a zirconium ball of Φ0.4-0.55 mm. The cyclic ball milling is carried out for 30 minutes, drying, and then pre-calcining at a temperature of 850° C. for 2.5 hours in an air atmosphere to obtain a pre-calcined material; S22, secondary ball milling: mixing the first auxiliary material, the second auxiliary material and the pre-sintered material obtained in step S31, performing secondary ball milling and drying to obtain ball milled powder, wherein the secondary sand milling time is 2 hours, and the particle size D50 of the ball milled powder is 0.8-1.0 μm; S23, spray granulation and molding: the powder after stirring is sequentially passed through a 100 mesh sieve, and then transferred into a spray tower, and spray granulated into particles of 50-200 μm; a binder is added during the spray granulation process, wherein the binder is a composition of polyvinyl alcohol and zinc stearate in a mass ratio of 5:1, the concentration of the binder solution is 6wt%, and the binder is 8% of the powder after the ball-milled powder is sieved; the particles are molded into a magnetic core blank, and the molding pressure is 80MPa, and the time is 1 00s; S24, sintering: including the following sintering steps: heating the magnetic core blank to a first temperature of 1250°C at a heating rate of 2°C / min, introducing a certain amount of oxygen during the first insulation period of 6 hours, cooling to a second temperature of 300°C at a first cooling rate of 1.5°C / min under an oxygen content of 1.8vol% in a balanced oxygen partial pressure atmosphere, and insulation for 8 hours, and finally cooling to a third temperature of 60°C at a second cooling rate of 0.2°C / min, and then naturally cooling to room temperature to obtain a wide temperature and low power consumption magnetic core.

[0027] Example 2 A wide temperature and low power consumption magnetic core, comprising a main component, a first auxiliary material and a second auxiliary material, wherein the main component, in terms of molar fraction, is composed of Fe2O3, ZnO and MnO, with a content of Fe2O3 52.9mol%, ZnO 8.2mol%, and the rest being MnO; the first auxiliary material comprises CaCO3, ZrO2, Nb2O, Co2O3, nano-SiO2, and nano-TiO2; the first auxiliary material, in terms of the total weight of the main component, comprises the following components: CaCO3 0.05wt%, ZrO2 0.005wt%, Nb2O 0.03wt%, Co2O3 0.26wt%, nano-SiO2 0.007wt%, nano-TiO2 0.009wt%; the second auxiliary material includes Ta2O5, V2O5, Bi2O3, and HfO2; the second auxiliary material is calculated based on the total weight of the main components, and the content of each auxiliary material component is Ta2O50.05wt%, V2O50.09wt%, Bi2O30.08wt%, and HfO20.04wt%, the particle size of the nano-SiO2 is 20-40 nanometers, and the particle size of the nano-TiO2 is 40-80 nanometers.

[0028] A method for preparing a wide temperature range and low power consumption magnetic core, using the raw materials of the wide temperature range and low power consumption magnetic core, comprises the following steps: S21, batching and ball milling: main components Fe2O3, ZnO and MnO are mixed according to the formula amount, and then water is added to the ball mill for mixing and ball milling, the mass ratio of the raw material put into the ball mill: grinding medium: water is 1:8:1.6, the grinding medium is a zirconium ball of Φ0.4-0.55mm, the ball milling is circulated for 60min, and the drying is carried out, and then the pre-burned material is obtained after being pre-burned at a temperature of 900°C for 1.5h in an air atmosphere; S22, secondary ball milling: mixing the first auxiliary material, the second auxiliary material and the pre-sintered material obtained in step S31, performing secondary ball milling and drying to obtain ball milled powder, wherein the secondary sand milling time is 3 hours, and the particle size D50 of the ball milled powder is 0.8-1.0 μm; S23, spray granulation and molding: the powder after stirring is sequentially passed through a 100-mesh sieve, and then transferred into a spray tower, and spray granulated into particles of 50-200 μm; a binder is added during the spray granulation process, wherein the binder is a composition of polyvinyl alcohol and zinc stearate in a mass ratio of 5:3, the concentration of the binder solution is 8wt%, and the binder is 10% of the powder after the ball-milled powder is sieved, and the particles are molded into magnetic core blanks, and the molding pressure is 150MPa, and the time is S24, sintering: including the following sintering steps: heating the magnetic core blank to a first temperature of 1350°C at a heating rate of 3°C / min, introducing a certain amount of oxygen during the first insulation period of 3h, cooling to a second temperature of 350°C at a first cooling rate of 2°C / min under an oxygen content of 2.3vol% in a balanced oxygen partial pressure atmosphere, and insulation for 3h, and finally cooling to a third temperature of 70°C at a second cooling rate of 0.4°C / min, and then naturally cooling to room temperature to obtain a wide temperature and low power consumption magnetic core.

[0029] Example 3 A wide temperature and low power consumption magnetic core, comprising a main component, a first auxiliary material and a second auxiliary material, wherein the main component, in terms of molar fraction, is composed of Fe2O3, ZnO and MnO, with a content of Fe2O3 52.6mol%, ZnO 7.9mol%, and the rest being MnO; the first auxiliary material comprises CaCO3, ZrO2, Nb2O, Co2O3, nano-SiO2, and nano-TiO2; the first auxiliary material, in terms of the total weight of the main component, comprises the following components: CaCO3 0.04wt%, ZrO2 0.004wt%, Nb2O 0.025wt%, Co2O3 0.23wt%, nano-SiO2 0.006wt%, nano-TiO2 0.007wt%; the second auxiliary material includes Ta2O5, V2O5, Bi2O3, and HfO2; the second auxiliary material is calculated based on the total weight of the main components, and the content of each auxiliary material component is Ta2O50.04wt%, V2O50.07wt%, Bi2O30.07wt%, HfO20.03wt%, the particle size of the nano-SiO2 is 20-40 nanometers, and the particle size of the nano-TiO2 is 40-80 nanometers.

[0030] A method for preparing a wide temperature range and low power consumption magnetic core, using the raw materials of the wide temperature range and low power consumption magnetic core, comprises the following steps: S21, batching and ball milling: the main components Fe2O3, ZnO and MnO are mixed according to the formula amount, and then water is added to the ball mill for mixing and ball milling. The mass ratio of the raw material: grinding medium: water in the ball mill is 1:7:1.4, and the grinding medium is a zirconium ball of Φ0.4-0.55mm. The ball milling is circulated for 45min, dried, and then pre-fired at 880°C for 2h in an air atmosphere to obtain a pre-fired material; S22, secondary ball milling: the first auxiliary material, the second auxiliary material and the pre-fired material obtained in step S31 are mixed, and the ball milled powder is obtained after secondary ball milling and drying. The time of the secondary sand milling is 2.5h, and the particle size D50 of the ball milled powder is 0.8-1.0μm; S23, spray granulation and molding: the powder after stirring is sequentially sieved through a 100-mesh sieve, and then transferred into a spray tower, and spray granulated into 50-200 μm particles; a binder is added during the spray granulation process, the binder is a composition of polyvinyl alcohol and zinc stearate in a mass ratio of 5:2, the binder solution concentration is 7wt%, the binder is 9% of the powder after the ball-milled powder is sieved, the particles are formed into a magnetic core blank, the forming pressure is 120MPa, and the time is 70s; S24, sintering: comprising the following sintering steps: heating the magnetic core blank to a first temperature of 1300°C at a heating rate of 2.5°C / min, introducing a certain amount of oxygen during the first insulation for 4h, cooling to a second temperature of 330°C at a first cooling rate of 1.8°C / min under an oxygen content of 2vol% in a balanced oxygen partial pressure atmosphere, heating for 7h, and finally cooling to a third temperature of 65°C at a second cooling rate of 0.3°C / min, and then naturally cooling to room temperature to obtain a wide temperature and low power consumption magnetic core.

[0031] Comparative Example 1 The same as Example 3, except that the content of ZnO is changed to ZnO 7.0 mol%.

[0032] Comparative Example 2 The same as Example 3, except that the content of nano-TiO2 is changed to 0, that is, no TiO2 is added.

[0033] Comparative Example 3 The same as Example 3, except that the content of the nano-TiO2 is changed to 0.015wt%.

[0034] Comparative Example 4 The same as Example 3, except that the content of Ta2O5 is changed to 0, that is, no Ta2O5 is added.

[0035] Comparative Example 5 The same as Example 3, except that the content of Ta2O5 is changed to 0.08wt%.

[0036] Comparative Example 6 The same as Example 3, except that the content of V2O5 is changed to 0, that is, no V2O5 is added.

[0037] Comparative Example 7 The same as Example 3, except that the content of V2O5 is changed to 0.13wt%.

[0038] Comparative Example 8 The same as Example 3, except that the oxygen content in the equilibrium oxygen partial pressure atmosphere is changed to 1.4 vol%.

[0039] Comparative Example 9 The same as Example 3, except that the binder is replaced by a composition of polyvinyl alcohol and zinc stearate in a mass ratio of 5:2 using an equal amount of polyvinyl alcohol of equal concentration.

[0040] Comparative Example 10 The same as Example 3, except that the binder is a composition of polyvinyl alcohol and zinc stearate in a mass ratio of 5:2, with an equal amount and concentration of zinc stearate being used instead.

[0041] Performance Testing The performance of the wide temperature and low power consumption magnetic cores prepared by Example 1, Example 3 and Comparative Examples 1 to Comparative Examples 10 were tested. The specific testing method was: in accordance with the standard SJ20966-2006 soft ferrite material measurement method, using an IWATSUB-H analyzer (SY-8219), and the results are shown in Table 1.

[0042] Table 1 As can be seen from Table 1, the wide temperature and low power consumption magnetic cores prepared in Examples 1-3, by controlling the contents of ZnO, TiO2, Ta2O5, V2O5 and the type and amount of binder, optimize the oxygen content of the sintering process, effectively reduce the loss of the wide temperature and low power consumption magnetic cores at -40-150°C, and have the advantages of wide operating temperature range and low power consumption. The wide temperature and low power consumption magnetic cores applied for basically achieve the performance of manganese zinc ferrite with wide temperature and low power consumption by controlling the addition range of the main components and the first auxiliary material, and add the second auxiliary material to modify the loss, so that there is a lower power loss at each temperature, which can largely solve the application range of the wide temperature and low power consumption magnetic cores under extreme conditions, meet the requirements of high inductance, high energy conversion rate, low power loss and wide temperature use of the wide temperature and low power consumption magnetic cores, and have great application potential.

[0043] As can be seen from Table 1, from the comparative analysis of the performance of the wide temperature and low power consumption magnetic cores obtained in Example 3 and Comparative Example 1, the ZnO content is too low and the loss is relatively high.

[0044] As can be seen from Table 1, from the comparative analysis of the performance of the wide temperature and low power consumption magnetic cores obtained in Example 3 and Comparative Examples 2-3, when the TiO2 content is too low or too high, the loss trend is not smooth and the loss is also high.

[0045] As can be seen from Table 1, from the comparative analysis of the performance of the wide temperature and low power consumption magnetic cores obtained in Example 3 and Comparative Examples 4-5, it can be seen that too low or too high a Ta2O5 content significantly affects the loss.

[0046] As can be seen from Table 1, from the comparative analysis of the performance of the wide temperature and low power consumption magnetic cores obtained in Example 3 and Comparative Examples 6-7, it can be seen that too low or too high a V2O5 content significantly affects the loss.

[0047] As can be seen from Table 1, from the comparative analysis of the performance of the wide temperature and low power consumption magnetic cores obtained in Example 3 and Comparative Example 8, the oxygen content is relatively low, resulting in relatively high losses.

[0048] As can be seen from Table 1, from the comparative analysis of the performance of the wide temperature and low power consumption magnetic cores obtained in Example 3 and Comparative Examples 9-10, the performance of the wide temperature and low power consumption magnetic cores finally obtained by using the binder as a composition of polyvinyl alcohol and zinc stearate in a mass ratio of 5:2 is better.

[0049] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation methods of the present application can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the protection scope of the present application.

Claims

1. A wide temperature and low power consumption magnetic core, characterized in that: The invention comprises a main component, a first auxiliary material and a second auxiliary material. The main component is composed of Fe2O3, ZnO and MnO in molar fraction, with a content of Fe2O3 52.352.9mol%, ZnO 7.58.2mol%, and the rest being MnO. The first auxiliary material comprises CaCO3, ZrO2, Nb2O, Co2O3, nano-SiO2 and nano-TiO2. The first auxiliary material comprises, based on the total weight of the main component, the content of each auxiliary material component is: CaCO3 0.03-0.05wt%, ZrO2 0.0020.005wt%, Nb2O 0.020.03wt%, Co2O3 0.200.26wt%, nano-SiO2 0.004-0.007wt%, nano-TiO2 0.006-0.009wt%; the second auxiliary material includes Ta2O5, V2O5, Bi2O3, and HfO2; the second auxiliary material is calculated based on the total weight of the main components, and the content of each auxiliary material component is Ta2O50.03-0.05wt%, V2O50.06-0.09wt%, Bi2O30.05-0.08wt%, HfO20.01-0.04wt%, the particle size of the nano-SiO2 is 20-40 nanometers, and the particle size of the nano-TiO2 is 40-80 nanometers.

2. A method for preparing a wide temperature and low power consumption magnetic core, characterized in that: Using the raw material of the wide temperature and low power consumption magnetic core according to claim 1, the method comprises the following steps: S21, batching and ball milling: mixing the main components Fe2O3, ZnO and MnO according to the formula, then adding water in a ball mill for mixing and ball milling, cyclic ball milling for 30-60 minutes, drying, and then pre-calcining at a temperature of 850-900° C. for 1.5-2.5 hours in an air atmosphere to obtain a pre-calcined material; S22, secondary ball milling: mixing the first auxiliary material, the second auxiliary material and the pre-burned material obtained in step S31, performing secondary ball milling and drying to obtain ball milled powder; S23, spray granulation and molding: the powder after stirring is sequentially passed through a 100-mesh sieve, and then transferred into a spray tower, and spray granulated into particles of 50-200 μm; the particles are molded into magnetic core blanks; S24, sintering: including the following sintering steps: heating the magnetic core blank to a first temperature of 1250-1350°C, introducing a certain amount of oxygen during the first heat preservation, cooling to a second temperature of 300-350°C at a first cooling rate under a balanced oxygen partial pressure atmosphere, second heat preservation, and finally cooling to a third temperature of 60-70°C at a second cooling rate, and then naturally cooling to room temperature to obtain a wide temperature and low power consumption magnetic core.

3. The method for preparing a wide temperature and low power consumption magnetic core according to claim 2, characterized in that: In step S21, the mass ratio of raw material: grinding medium: water put into the ball mill is 1:6-8:1.2-1.6, and the grinding medium is a zirconium ball of Φ0.4-0.55 mm.

4. The method for preparing a wide temperature and low power consumption magnetic core according to claim 2, characterized in that: In step S22, the secondary sand milling time is 2-3 hours; the particle size D50 of the ball-milled powder is 0.8-1.0 μm.

5. The method for preparing a magnetic core with a wide temperature range and low power consumption according to claim 2, characterized in that: In step S23, a binder is added during the spray granulation process, wherein the binder is a composition of polyvinyl alcohol and zinc stearate in a mass ratio of 5:1-3.

6. The method for preparing a magnetic core with a wide temperature range and low power consumption according to claim 5, characterized in that: The concentration of the binder solution is 6-8wt%, and the binder accounts for 8-10% of the powder after the ball-milled powder is sieved.

7. The method for preparing a wide temperature and low power consumption magnetic core according to claim 2, characterized in that: In step S23, the molding pressure is 80-150 MPa and the molding time is 30-100 s.

8. The method for preparing a wide temperature and low power consumption magnetic core according to claim 2, characterized in that: In step S24, the heating rate of the heating is 2-3°C / min, and the insulation time at the first temperature is 3-6h.

9. The method for preparing a wide temperature and low power consumption magnetic core according to claim 2, characterized in that: In step S24, the first cooling rate is 1.5-2°C / min, the second temperature holding time is 5-8h, and the second cooling rate is 0.2-0.4°C / min.

10. The method for preparing a magnetic core with a wide temperature range and low power consumption according to claim 2, characterized in that: In step S24, the oxygen content in the equilibrium oxygen partial pressure atmosphere is 1.82.3 vol%.

Citation Information

Patent Citations

  • Wide-temperature ultralow-loss manganese zinc power ferrite magnetic core

    CN102795850A

  • Broadband wide temperature range high-power density low-loss manganese-zinc soft magnetic ferrite material and preparation method thereof

    CN107473727A

  • Manganese-zinc ferrite material with wide temperature range and low power consumption and preparation method thereof

    CN112408969A

  • Wide-temperature-range ultralow-power-consumption manganese-zinc ferrite material and preparation method thereof

    CN112707723A

  • Variable-frequency wide-temperature-range low-loss high-magnetic-flux-density MnZn power ferrite and preparation method thereof

    CN113024235A