Double-element doped calcium fluoride laser transparent ceramic and preparation method thereof

Through the preparation of dual-element doped calcium fluoride laser transparent ceramics, the problem of thermal effects of laser crystals under high power density is solved, high density and excellent optical characteristics are achieved, the preparation process is simplified, and the application range is broadened.

CN119059818AActive Publication Date: 2024-12-03SOUTHERN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310631462.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-03
Estimated Expiration
2043-05-30

AI Technical Summary

Technical Problem

Existing laser crystals have problems that thermal effects affect laser performance under high power density, and their scientific and technological foundations are unclear, and there is a lack of research on ion luminescence characteristics and energy transfer mechanisms, which leads to difficulties in manufacturing laser dielectric matrix materials.

Method used

Using dual-element doped calcium fluoride laser transparent ceramics, doped with manganese and erbium to ensure that Er3+ is completely solid solution into the calcium fluoride lattice. There is no need for sintering aid during the preparation process, and the powder particles are of moderate size, which is convenient. Exclusion of sintered pores to improve the density of ceramics.

Benefits of technology

It realizes the high density and excellent optical characteristics of ceramics, with a light transmittance of more than 90%, and excellent performance, simplifies the preparation process, reduces the complexity of equipment and process control, and broadens the application range of laser dielectric matrix materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004258568930000011
    Figure HDA0004258568930000011
Patent Text Reader

Abstract

The invention provides double-element doped calcium fluoride laser transparent ceramic and a preparation method thereof. The double-element doped calcium fluoride laser transparent ceramic is manganese-erbium doped calcium fluoride laser transparent ceramic, and the light transmittance of the double-element doped calcium fluoride laser transparent ceramic within the range of 200-1700 nm is larger than 90%. The double-element doped calcium fluoride laser transparent ceramic is a pure calcium fluoride phase, no impure phase is formed after erbium ions are doped, and Er < 3 + > completely enters calcium fluoride crystal lattices in a solid solution mode. The double-element doped calcium fluoride laser transparent ceramic is good in ceramic densification degree, the density is larger than 99%, and the optical property of the ceramic can be improved. The light transmittance is greater than 90%, and the performance is excellent. The invention also provides a preparation method of the double-element doped calcium fluoride laser transparent ceramic.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of laser medium materials, and in particular relates to a double-element doped calcium fluoride laser transparent ceramic and a preparation method thereof. Background Art

[0002] Calcium fluoride crystal is an excellent laser medium matrix material. CaF2 has a cubic crystal structure. 2+ Located at the vertices and face centers of the unit cell, occupying the F - Half of the cubic void formed, F - Occupies Ca 2+ The lattice site symmetry diversity allows high concentration doping of rare earth ions, a large bandgap (-12eV), a wide light transmission range (125nm~10μm), a small refractive index (~1.434, Vis~NIR), and a low phonon energy (~390cm -1 ), rare earth-doped calcium fluoride materials have different forms of charge compensation, which can easily form broad and smooth absorption and emission spectra, thus facilitating the generation of ultrashort pulsed lasers.

[0003] Solid-state laser materials include laser glass and laser crystals. Among them, laser glass is a solid laser material with glass as the matrix. It is widely used in various types of solid laser devices and has become the main laser material for high-power and high-energy lasers. Laser glass consists of two parts: matrix glass and activation ions. The various physical and chemical properties of laser glass are mainly determined by the matrix glass, while its spectral properties are mainly determined by the activation ions. As the matrix glass of laser glass, optical glass is currently mostly used. Laser glass must have various suitable spectral properties, good transparency and good physical and chemical properties. It is difficult to manufacture laser glass that meets the above requirements at the same time. There are currently four major development directions for laser crystals: purple, blue, green and visible light laser crystals; mid-infrared laser crystals; (1μm band) high-power, high-energy laser crystals; LD pumped ultrafast laser gain and amplification crystals. Laser crystals also have a series of problems that need to be solved urgently, including (1) the basic problems of laser crystal growth science and technology are unclear; (2) there is a lack of research on the luminescence characteristics of ions in the crystal, energy transfer and the mechanism of their interaction with the lattice; (3) LD pumping under high power density (10 4 W / cm 2 ~10 7 W / cm 2 )The thermal effects of laser crystals and their impact on laser performance, etc.

[0004] Therefore, a new laser medium matrix material still needs to be developed. Summary of the invention

[0005] The present invention aims to solve at least one of the above technical problems existing in the prior art. To this end, the present invention provides a double-element doped calcium fluoride laser transparent ceramic, which has a good degree of densification, is conducive to improving the optical properties of the ceramic, has a light transmittance greater than 90%, and has excellent performance.

[0006] The invention also provides a method for preparing double-element doped calcium fluoride laser transparent ceramics.

[0007] A first aspect of the present invention provides a double-element doped calcium fluoride laser transparent ceramic, wherein the double-element doped calcium fluoride laser transparent ceramic is manganese-erbium doped calcium fluoride laser transparent ceramic, and the light transmittance of the double-element doped calcium fluoride laser transparent ceramic is greater than 90%.

[0008] One of the technical solutions of the present invention regarding the double-element doped calcium fluoride laser transparent ceramics has at least the following beneficial effects:

[0009] The double-element doped calcium fluoride laser transparent ceramic of the present invention is a pure calcium fluoride phase, and no impurity phase is formed after being doped with erbium ions. 3+ Completely dissolved into the calcium fluoride lattice.

[0010] The double-element doped calcium fluoride laser transparent ceramic of the present invention has a good ceramic densification degree, which is beneficial to improving the optical properties of the ceramic, has a light transmittance greater than 90%, and has excellent performance.

[0011] According to some embodiments of the present invention, the density of the double-element doped calcium fluoride laser transparent ceramic is greater than 99%.

[0012] The second aspect of the present invention provides a method for preparing the double-element doped calcium fluoride laser transparent ceramic, comprising the following steps:

[0013] S1: Prepare the mixture containing F - anionic solution and containing Mn 2+ , Er 2+ and Ca 2+ of cationic solution;

[0014] S2: adding the anion solution to the cationic solution, mixing, standing and aging, centrifuging, washing and drying the precipitate to obtain a powder;

[0015] S3: Sintering the powder to obtain the double-element doped calcium fluoride laser transparent ceramic.

[0016] A technical solution in the preparation method of double-element doped calcium fluoride laser transparent ceramics of the present invention has at least the following beneficial effects:

[0017] At present, the preparation methods of fluoride transparent ceramics are mainly single crystal hot forging and hot pressing sintering of chemically synthesized powders. The single crystal hot forging method is restricted by the shortcomings of single crystal growth, and the transparent ceramics obtained by hot pressing sintering of chemically synthesized powders have unsatisfactory laser output effects. 3+ It is completely dissolved into the calcium fluoride lattice, and the powder particle size is moderate, which is convenient for the removal of pores in the later sintering process. The prepared ceramic has a good degree of densification, which is beneficial to improving the optical properties of the ceramic.

[0018] The preparation method of the double-element doped calcium fluoride laser transparent ceramics of the present invention comprises the following steps: 2+ +Er 3+ ): During the chemical reaction of CaF2 powder, Mn 2+ and Er 3+ Entering into the lattice structure of CaF2, and along with Mn 2+ and Er 3+ As the doping concentration increases, the more lattice defects there are in the powder, and the lower the crystallinity. For the sintering process, the defects in the powder crystals are conducive to the improvement of sintering activity and can significantly improve its sintering performance. Therefore, in the preparation method of the dual-element doped calcium fluoride laser transparent ceramic of the present invention, no sintering aid is required, the raw materials are easily available, and the preparation method is simple.

[0019] The preparation method of the double-element doped calcium fluoride laser transparent ceramic of the present invention does not require expensive equipment and complicated process control, has undemanding reaction conditions, is easy to realize industrial production, and broadens the application range of laser medium matrix materials.

[0020] According to some embodiments of the present invention, in the anion solution, F - The concentration is 0.5mol / L~2.5mol / L.

[0021] According to some embodiments of the present invention, in the anion solution, the solvent comprises water.

[0022] According to some embodiments of the present invention, in the anion solution, the fluorine source includes KF·2H2O.

[0023] According to some embodiments of the present invention, in the cationic solution, Mn 2+ , Er 2+ and Ca 2+ The concentrations are all between 0.5 mol / L and 2.5 mol / L.

[0024] According to some embodiments of the present invention, in the cationic solution, the solvent comprises water.

[0025] According to some embodiments of the present invention, in the cationic solution, the manganese source includes Mn(NO3)2·4H2O.

[0026] According to some embodiments of the present invention, in the cationic solution, the erbium source includes Er(NO3)3·5H2O.

[0027] According to some embodiments of the present invention, in the cationic solution, the calcium source includes Ca(NO3)2·4H2O.

[0028] According to some embodiments of the present invention, in the cationic solution, Mn 2+ , Er 3+ and Ca 2+ The molar ratio is (1-5):(3-10):(96-85).

[0029] When Mn 2+ and Er 3+ When the content is too high, some Mn 2+ and Er 3+ Failure to dissolve into the CaF2 lattice structure, existing in the form of fluoride, after sintering, fluoride gathers at the grain boundary, affecting the transmittance of the sintered body. 2+ , Er 3+ and Ca 2+ The molar ratio of (1-5):(3-10):(96-85) is an appropriate ratio range.

[0030] Mn in the powder synthesis process 2+ and Er 3+ Into the lattice structure of CaF2, with the increase of doping concentration, the particle size of the powder becomes smaller and smaller, and the powder tends to be cubic. 2+ , Er 3+ and Ca 2+ The molar ratio of Mn 2+ and Er 3+ It completely dissolves into the CaF2 lattice without affecting the sintering properties of the subsequent ceramics.

[0031] According to some embodiments of the present invention, in the process of adding the anion solution into the cationic solution, the addition rate of the anion solution is 1 mL / min to 2.5 mL / min.

[0032] According to some embodiments of the present invention, in the process of adding the anion solution to the cationic solution, the anion solution is added by titration.

[0033] According to some embodiments of the present invention, the particle size of the powder gradually decreases with the increase of the titration speed. When the titration rate is too fast, the powder particles will nucleate too quickly, the powder growth time will be insufficient, and the powder will agglomerate, affecting the subsequent sintering activity. Therefore, 1mL / min to 2.5mL / min is a suitable titration rate.

[0034] According to some embodiments of the present invention, the process of adding the anion solution to the cationic solution is accompanied by stirring.

[0035] According to some embodiments of the present invention, the stirring speed is 200 rpm to 300 rpm.

[0036] According to some embodiments of the present invention, the anion solution is added to the cationic solution, and after the addition, stirring is continued for 20 min to 40 min and then allowed to stand for aging.

[0037] According to some embodiments of the present invention, the static aging time is 10 hours to 15 hours.

[0038] As the aging time increases, the powder changes from disordered polygons to cubic structure powders. Too long an aging time will cause the powder particles to be too large, which is not conducive to the elimination of pores during the sintering process. Therefore, 10h to 15h is the appropriate static aging time.

[0039] According to some embodiments of the present invention, the centrifugal rotation speed is 3500 rpm to 4000 rpm.

[0040] According to some embodiments of the present invention, the centrifugation time is 2 min to 3 min.

[0041] According to some embodiments of the invention, the precipitate is washed with deionized water and ultrasonically treated.

[0042] According to some embodiments of the present invention, the number of cleanings may be 3 to 5 times.

[0043] According to some embodiments of the present invention, after cleaning, the powder is dried.

[0044] According to some embodiments of the present invention, the cleaned precipitate can be placed in a blast-type constant temperature oven at about 60°C for drying for 20 hours, and after drying, it can be passed through a 100-mesh sieve, and the powder under the sieve can be placed in a 120°C oven for drying for later use.

[0045] According to some embodiments of the present invention, the sintering temperature is 650° C. to 750° C.; and / or the sintering time is 2 h to 3 h; and / or the sintering heating rate is 1° C. / min to 1.5° C. / min.

[0046] The temperature is raised to 650℃~750℃ at a rate of 1℃ / min~1.5℃ / min, and kept at this temperature for 2~3h. At this sintering temperature, the grain size grows rapidly, and the pores are gradually eliminated as the sintering temperature increases, and the ceramic is basically completely dense. At a heating rate of 1℃ / min~1.5℃ / min, the pores have enough time to be eliminated during the low-temperature sintering stage, and there is enough time to keep the temperature inside and outside the sample consistent, so that the densification process is synchronized.

[0047] According to some embodiments of the present invention, the method further comprises, after step S3, performing rough grinding and polishing on the dual-element doped calcium fluoride laser transparent ceramic.

[0048] According to some embodiments of the present invention, the rough grinding may be performed on sandpaper.

[0049] According to some embodiments of the present invention, the polishing process may be performed on a polishing machine. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 This is the X-ray powder diffraction pattern of the double-element doped calcium fluoride laser transparent ceramic prepared in Example 1. DETAILED DESCRIPTION

[0051] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.

[0052] In some embodiments of the present invention, the present invention provides a double-element doped calcium fluoride laser transparent ceramic, which is manganese-erbium doped calcium fluoride laser transparent ceramic. The double-element doped calcium fluoride laser transparent ceramic has a density greater than 99% and a transmittance greater than 90%.

[0053] It should be noted that the double-element doped calcium fluoride laser transparent ceramics of the present invention are all pure calcium fluoride phases, and no impurity phase is formed after being doped with erbium ions. 3+ Completely dissolved into the calcium fluoride lattice.

[0054] It can be understood that the double-element doped calcium fluoride laser transparent ceramic of the present invention has a good degree of ceramic densification, which is beneficial to improving the optical properties of the ceramic. The light transmittance is greater than 90%, and the performance is excellent.

[0055] It can be understood that the double-element doped calcium fluoride laser transparent ceramic of the present invention has a good degree of ceramic densification, with a density greater than 99%.

[0056] In some other embodiments of the present invention, the present invention provides a method for preparing the double-element doped calcium fluoride laser transparent ceramic of the present invention, comprising the following steps:

[0057] S1: Prepare the mixture containing F - anionic solution and containing Mn 2+ , Er 2+ and Ca 2+ of cationic solution;

[0058] S2: adding the anion solution to the cationic solution, mixing well, standing and aging, centrifuging, washing and drying the precipitate to obtain a powder;

[0059] S3: Sinter the powder to obtain double-element doped calcium fluoride laser transparent ceramics.

[0060] It is understandable that the current preparation methods for fluoride transparent ceramics are mainly single crystal hot forging and hot pressing sintering of chemically synthesized powders. The single crystal hot forging method is restricted by the shortcomings of single crystal growth, and the transparent ceramics obtained by hot pressing sintering of chemically synthesized powders have unsatisfactory laser output effects. 3+ It is completely dissolved into the calcium fluoride lattice, and the powder particle size is moderate, which is convenient for the removal of pores in the later sintering process. The prepared ceramic has a good degree of densification, which is beneficial to improving the optical properties of the ceramic.

[0061] It can also be understood that the preparation method of the double-element doped calcium fluoride laser transparent ceramic of the present invention, in the synthesis (Mn 2+ +Er 3+ ): During the chemical reaction of CaF2 powder, Mn 2+ and Er 3+ Entering into the lattice structure of CaF2, and along with Mn 2+ and Er 3+ As the doping concentration increases, the more lattice defects there are in the powder, and the lower the crystallinity. For the sintering process, the defects in the powder crystals are conducive to the improvement of sintering activity and can significantly improve its sintering performance. Therefore, in the preparation method of the dual-element doped calcium fluoride laser transparent ceramic of the present invention, no sintering aid is required, the raw materials are easily available, and the preparation method is simple.

[0062] Furthermore, the preparation method of the dual-element doped calcium fluoride laser transparent ceramic of the present invention does not require expensive equipment and complex process control, the reaction conditions are not harsh, and industrial production is easy to achieve, thereby broadening the application range of laser medium matrix materials.

[0063] In some embodiments of the present invention, in the anionic solution, F - The concentration is 0.5mol / L~2.5mol / L.

[0064] In some embodiments of the present invention, in the anion solution, the solvent includes water.

[0065] In some embodiments of the present invention, in the anion solution, the fluorine source includes KF·2H2O.

[0066] In some embodiments of the present invention, in the cationic solution, Mn 2+ , Er 2+ and Ca 2+ The concentrations are all between 0.5 mol / L and 2.5 mol / L.

[0067] In some embodiments of the present invention, in the cationic solution, the solvent includes water.

[0068] In some embodiments of the present invention, in the cationic solution, the manganese source includes Mn(NO3)2·4H2O.

[0069] In some embodiments of the present invention, in the cationic solution, the erbium source includes Er(NO3)3·5H2O.

[0070] In some embodiments of the present invention, in the cationic solution, the calcium source includes Ca(NO3)2·4H2O.

[0071] In some embodiments of the present invention, in the cationic solution, Mn 2+ , Er 3+ and Ca 2+ The molar ratio is (1-5):(3-10):(96-85).

[0072] When Mn 2+ and Er 3+ When the content is too high, some Mn 2+ and Er 3+ Failure to dissolve into the CaF2 lattice structure, existing in the form of fluoride, after sintering, fluoride gathers at the grain boundary, affecting the transmittance of the sintered body. 2+ , Er 3+ and Ca 2+ The molar ratio of (1-5):(3-10):(96-85) is an appropriate ratio range.

[0073] Mn in the powder synthesis process 2+ and Er 3+ Into the lattice structure of CaF2, with the increase of doping concentration, the particle size of the powder becomes smaller and smaller, and the powder tends to be cubic. 2+ , Er 3+ and Ca 2+ The molar ratio of Mn 2+ and Er 3+ It completely dissolves into the CaF2 lattice without affecting the sintering properties of the subsequent ceramics.

[0074] In some embodiments of the present invention, during the process of adding the anion solution into the cationic solution, the addition rate of the anion solution is 1 mL / min to 2.5 mL / min.

[0075] In some embodiments of the present invention, in the process of adding the anion solution into the cationic solution, the anion solution is added by titration.

[0076] In some embodiments of the present invention, the particle size of the powder gradually decreases with the increase of the titration speed. When the titration rate is too fast, the powder particles will nucleate too quickly, the powder growth time will be insufficient, and the powder will agglomerate, affecting the subsequent sintering activity. Therefore, 1mL / min to 2.5mL / min is a suitable titration rate.

[0077] In some embodiments of the present invention, the process of adding the anion solution to the cationic solution is accompanied by stirring.

[0078] In some embodiments of the present invention, the stirring speed is 200 rpm to 300 rpm.

[0079] In some embodiments of the present invention, the anion solution is added to the cationic solution, and after the addition, stirring is continued for 20 minutes to 40 minutes and then allowed to stand for aging.

[0080] In some embodiments of the present invention, the static aging time is 10 hours to 15 hours.

[0081] As the aging time increases, the powder changes from disordered polygons to cubic structure powders. Too long an aging time will cause the powder particles to be too large, which is not conducive to the elimination of pores during the sintering process. Therefore, 10h to 15h is the appropriate static aging time.

[0082] In some embodiments of the present invention, the centrifugal rotation speed is 3500 rpm to 4000 rpm.

[0083] In some embodiments of the present invention, the centrifugation time is 2 min to 3 min.

[0084] In some embodiments of the present invention, the precipitate is washed with deionized water and sonicated.

[0085] In some embodiments of the present invention, the number of cleanings may be 3 to 5 times.

[0086] In some embodiments of the present invention, after washing, the powder is dried.

[0087] In some embodiments of the present invention, the cleaned precipitate can be placed in a blast-type constant temperature oven at about 60°C for drying for 20 hours, and after drying, it can be passed through a 100-mesh sieve, and the powder under the sieve can be placed in a 120°C oven for drying for later use.

[0088] In some embodiments of the present invention, the sintering temperature is 650° C. to 750° C.; and / or the sintering time is 2 h to 3 h; and / or the sintering heating rate is 1° C. / min to 1.5° C. / min.

[0089] The temperature is raised to 650℃~750℃ at a rate of 1℃ / min~1.5℃ / min, and kept at this temperature for 2~3h. At this sintering temperature, the grain size grows rapidly, and the pores are gradually eliminated as the sintering temperature increases, and the ceramic is basically completely dense. At a heating rate of 1℃ / min~1.5℃ / min, the pores have enough time to be eliminated during the low-temperature sintering stage, and there is enough time to keep the temperature inside and outside the sample consistent, so that the densification process is synchronized.

[0090] In some embodiments of the present invention, the method further comprises, after step S3, performing rough grinding and polishing on the dual-element doped calcium fluoride laser transparent ceramic.

[0091] In some embodiments of the present invention, the rough grinding may be performed on sandpaper.

[0092] In some embodiments of the present invention, the polishing process may be performed on a polishing machine.

[0093] The technical solution of the present invention will be better understood with reference to specific embodiments below.

[0094] Example 1

[0095] This embodiment provides a dual-element doped calcium fluoride laser transparent ceramic, which is manganese and erbium doped calcium fluoride laser transparent ceramic. The specific preparation method is:

[0096] (1) 0.001 mol of Mn(NO3)2·4H2O, 0.003 mol of Er(NO3)3·5H2O and 0.096 mol of Ca(NO3)2·4H2O were dissolved in 100 mL of deionized water to prepare a cationic solution, and 0.3 mol of KF·2H2O was dissolved in 200 mL of deionized water to prepare an anionic solution;

[0097] (2) Add the anion solution to the cationic solution at a rate of 1 mL / min and stir evenly at a stirring rate of 200 rpm. After the titration is completed, continue stirring for 40 min and then let stand for 10 h;

[0098] (3) After aging, the solution was centrifuged at 3500 rpm for 3 min, the lower precipitate was removed, washed with deionized water, and ultrasonically treated. After repeated centrifugation, washing, and ultrasonic treatment three times, the precipitate was placed in a 60°C constant temperature oven and dried for 20 h. After drying, it was passed through a 100-mesh sieve, and the powder under the sieve was placed in a 120°C oven and dried for later use;

[0099] (4) The powder is placed in a graphite mold, and the graphite mold is placed in a vacuum hot press furnace for high-temperature sintering. The temperature is raised to 700°C at a rate of 1°C / min and kept at this temperature for 2 hours to obtain manganese erbium doped calcium fluoride laser transparent ceramics.

[0100] Figure 1 is the X-ray powder diffraction pattern of the double-element doped calcium fluoride laser transparent ceramic prepared in this embodiment, refer to Figure 1 It can be seen that compared with the standard spectrum of calcium fluoride, the approximate position of the XRD peaks of the transparent ceramic obtained in this embodiment has not changed substantially, and all are pure calcium fluoride phases, without other impurity peaks, indicating that no impurity phase is formed after doping with erbium ions.

[0101] The density of the ceramic obtained in this embodiment is greater than 99%. After double-sided polishing by a grinding and polishing machine, the light transmittance in the range of 200 to 1700 nm is greater than 92%.

[0102] Example 2

[0103] This embodiment provides a dual-element doped calcium fluoride laser transparent ceramic, which is manganese and erbium doped calcium fluoride laser transparent ceramic. The specific preparation method is:

[0104] (1) 0.005 mol of Mn(NO3)2·4H2O, 0.01 mol of Er(NO3)3·5H2O and 0.085 mol of Ca(NO3)2·4H2O were dissolved in 100 mL of deionized water to prepare a cationic solution, and 0.4 mol of KF·2H2O was dissolved in 200 mL of deionized water to prepare an anionic solution;

[0105] (2) Add the anion solution to the cationic solution at a rate of 2.5 mL / min and stir evenly at a stirring rate of 250 rpm. After the titration is completed, continue stirring for 30 min and then let it stand for 13 h;

[0106] (3) After aging, the solution was centrifuged at 4000 rpm for 2 min, the lower precipitate was removed, washed with deionized water, and ultrasonically treated. After repeated centrifugation, washing, and ultrasonic treatment three times, the precipitate was placed in a 60°C constant temperature oven and dried for 20 h. After drying, it was passed through a 100-mesh sieve, and the powder under the sieve was placed in a 120°C oven and dried for later use;

[0107] (4) The powder is placed in a graphite mold, and the graphite mold is placed in a vacuum hot press furnace for high-temperature sintering. The temperature is raised to 750°C at a rate of 1.5°C / min and kept at this temperature for 2 hours to obtain manganese erbium doped calcium fluoride laser transparent ceramics.

[0108] The density of the ceramic obtained in this embodiment is greater than 99%. After double-sided polishing by a grinding and polishing machine, the light transmittance in the range of 200 to 1700 nm is greater than 90%.

[0109] Example 3

[0110] This embodiment provides a dual-element doped calcium fluoride laser transparent ceramic, which is manganese and erbium doped calcium fluoride laser transparent ceramic. The specific preparation method is:

[0111] (1) 0.004 mol of Mn(NO3)2·4H2O, 0.006 mol of Er(NO3)3·5H2O and 0.09 mol of Ca(NO3)2·4H2O were dissolved in 100 mL of deionized water to prepare a cationic solution, and 0.5 mol of KF·2H2O was dissolved in 200 mL of deionized water to prepare an anionic solution;

[0112] (2) Add the anion solution to the cationic solution at a rate of 2 mL / min and stir evenly at a stirring rate of 300 rpm. After the titration is completed, continue stirring for 20 min and then let it stand for 15 h;

[0113] (3) After aging, the solution was centrifuged at 4000 rpm for 2.5 min, the lower precipitate was removed, washed with deionized water, and ultrasonically treated. After repeated centrifugation, washing, and ultrasonic treatment three times, the precipitate was placed in a 60°C constant temperature oven and dried for 20 h. After drying, it was passed through a 100-mesh sieve, and the powder under the sieve was placed in a 120°C oven and dried for later use;

[0114] (4) The powder is placed in a graphite mold, and the graphite mold is placed in a vacuum hot press furnace for high-temperature sintering. The temperature is raised to 750°C at a rate of 1.5°C / min and kept at this temperature for 3 hours to obtain manganese erbium doped calcium fluoride laser transparent ceramics.

[0115] The density of the ceramic obtained in this embodiment is greater than 99.5%. After double-sided polishing by a grinding and polishing machine, the light transmittance in the range of 200 to 1700 nm is greater than 93%.

[0116] The present invention has been described in detail above in conjunction with the embodiments, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. A double-element doped calcium fluoride laser transparent ceramic, characterized in that: The double-element doped calcium fluoride laser transparent ceramic is manganese and erbium doped calcium fluoride laser transparent ceramic, and the light transmittance of the double-element doped calcium fluoride laser transparent ceramic is greater than 90%.

2. The double-element doped calcium fluoride laser transparent ceramic according to claim 1, characterized in that: The density of the double-element doped calcium fluoride laser transparent ceramic is greater than 99%.

3. A method for preparing the double-element doped calcium fluoride laser transparent ceramics as claimed in claim 1 or 2, characterized in that: The following steps are involved: S1: Prepare the mixture containing F - anionic solution and containing Mn 2+ , Er 2+ and Ca 2+ of cationic solution; S2: adding the anion solution to the cationic solution, mixing, standing and aging, centrifuging, washing and drying the precipitate to obtain a powder; S3: Sintering the powder to obtain the double-element doped calcium fluoride laser transparent ceramic.

4. The method according to claim 3, characterized in that: In the anion solution, F - The concentration is 0.5mol / L~2.5mol / L.

5. The method according to claim 3, characterized in that: In the cationic solution, Mn 2+ , Er 2+ and Ca 2+ The concentrations are all between 0.5 mol / L and 2.5 mol / L.

6. The method according to claim 5, characterized in that In the cationic solution, Mn 2+ , Er 3+ and Ca 2+ The molar ratio is (1-5):(3-10):(96-85).

7. The method according to claim 3, characterized in that In the process of adding the anion solution to the cation solution, the addition rate of the anion solution is 1 mL / min to 2.5 mL / min.

8. The method according to claim 3, characterized in that The static aging time is 10h to 15h.

9. The method according to claim 3, characterized in that: The sintering temperature is 650° C. to 750° C.; and / or, the sintering time is 2 h to 3 h; and / or, the sintering heating rate is 1° C. / min to 1.5° C. / min.

10. The method according to claim 3, characterized in that The method further comprises, after step S3, performing rough grinding and polishing on the ceramic.

Citation Information

Patent Citations

  • Solarization resistant materials having reduced ultraviolet absorption for use in fabrication of optical elements

    US20030158028A1