Active energy ray-polymerizable resin composition and laminate

By using a specific composition of active energy ray polymerizable resin composition in a liquid crystal display device, the problem of insufficient adhesion of the existing adhesive under high and low temperature conditions is solved, and the heat resistance and moisture resistance are significantly improved. It meets the strict performance requirements of LCD display devices.

CN119060263APending Publication Date: 2024-12-03아티엔스가부시키가이샤 +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410476662.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2024-04-19
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing adhesives are insufficient in high and low temperature conditions, and their heat resistance and humidity resistance cannot meet the strict requirements of liquid crystal display devices, especially for automotive-use liquid crystal display devices, which have higher performance on adhesives. demand.

Method used

An active energy ray polymerizable resin composition is used, which comprises a compound containing an ethylene unsaturated double bond group having a hydroxyl group, a compound containing an ethylene unsaturated double bond group without a hydroxyl group, and a metal salt of an organic acid The amino-containing compound with a number average molecular weight of 500 to 40,000 has excellent adhesiveness and heat resistance through specific compositional ratios and structural design.

Benefits of technology

It has achieved excellent adhesive strength under both high and low temperature conditions, and significantly improved heat resistance and humidity resistance, meeting the strict requirements of the adhesive performance of the liquid crystal display device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004800723570000331
    Figure BDA0004800723570000331
  • Figure BDA0004800723570000341
    Figure BDA0004800723570000341
  • Figure BDA0004800723570000351
    Figure BDA0004800723570000351
Patent Text Reader

Abstract

Provided are: an active energy ray-polymerizable resin composition which is capable of forming a laminate having excellent heat resistance and wet heat resistance, while having excellent adhesive strength in a wide temperature range from high temperature to low temperature; and a laminate. The problem of the present application is solved by an active energy ray-polymerizable resin composition which comprises a compound A having an ethylenically unsaturated double bond group and having a hydroxyl group, a compound B having an ethylenically unsaturated double bond group and not having a hydroxyl group, and a radical polymerization initiator E, and which satisfies any one of the following (1) to (4). (1) The composition further contains a metal salt C of an organic acid and a boric acid compound F. And (2) further containing an amino-containing compound D with a number average molecular weight of 500-40000. And (3) further containing a metal salt C of an organic acid and an amino-containing compound D with a number-average molecular weight of 500-40000. And (4) further containing an amino-containing compound D and a boric acid compound F, the number-average molecular weight of which is 500-40000.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an active energy ray-polymerizable resin composition suitable for an adhesive and a laminate thereof. Background Art

[0002] The active energy ray polymerizable resin composition has excellent properties such as high workability and extremely low energy required for further polymerization due to its fast polymerization speed and the fact that it can usually be used without solvent. Examples of the active energy ray polymerizable resin composition include free radical-based, cationic-based, or free radical-cationic combined-based (mixture-based) active energy ray polymerizable resin compositions, which are used in a wide range of fields such as adhesives and coating agents.

[0003] Polarizing elements used in the field of liquid crystal display are usually made by uniaxially stretching polyvinyl alcohol (PVA) after iodine and dye are adsorbed. The polyvinyl alcohol-based polarizing elements shrink due to heat and moisture, resulting in reduced polarization performance. Therefore, a protective film is attached to the surface of the PVA-based polarizing element and used as a polarizing plate.

[0004] In the bonding of PVA-based polarizing elements and protective films, water-based adhesives and active energy ray-polymerizable resin compositions are used. However, from the perspective of the versatility of the substrate used in the protective film, efficiency in production, and energy saving, the use of active energy ray-polymerizable resin compositions as adhesives is being promoted.

[0005] The active energy ray-polymerizable resin composition is required to have sufficient adhesion for laminating a PVA-based polarizing element and a protective film, and properties such as heat resistance, moisture resistance, and water resistance for suppressing a decrease in polarization performance of the PVA-based polarizing element.

[0006] Patent Document 1 discloses a cation-based active energy ray-polymerizable adhesive mainly composed of an epoxy resin containing no aromatic ring to address issues such as adhesive strength of polarizing plates using a film having a lower moisture permeability than triacetylcellulose such as a norbornene-based resin film as a protective film.

[0007] Patent Document 2 discloses an active energy ray-polymerizable adhesive of a mixture type using 2-hydroxybutyl acrylate and 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane as an adhesive that can firmly bond not only to a norbornene-based resin but also to an acrylic resin or a triacetylcellulose film.

[0008] Patent Document 3 discloses a radical-based active energy ray-polymerizable adhesive using acryloylmorpholine and an alkyl acrylate having 10 to 20 carbon atoms in combination to address issues such as water resistance.

[0009] Compared with LCD devices for indoor and mobile use, LCD devices for vehicle use require stricter heat resistance, moisture and heat resistance, and good adhesion in a wide temperature range from high to low temperatures. However, conventional adhesives have insufficient adhesion at high and low temperatures, and their heat resistance and moisture and heat resistance do not meet the required quality.

[0010] Prior art literature

[0011] Patent Literature

[0012] Patent Document 1: Japanese Patent Application Publication No. 2004-245925

[0013] Patent Document 2: Japanese Patent Application Publication No. 2010-018722

[0014] Patent Document 3: Japanese Patent Application Publication No. 2017-194572 Summary of the invention

[0015] Problems to be solved by the invention

[0016] An object of the present invention is to provide an active energy ray-polymerizable resin composition and a laminate that can form a laminate having excellent adhesive strength even at high and low temperatures and excellent heat resistance and moist heat resistance.

[0017] Methods for solving problems

[0018] The present inventors have conducted intensive studies to solve the above problems and, as a result, have found that the above objects can be achieved by using the active energy ray-polymerizable resin composition described below, thereby completing the present invention.

[0019] The present invention relates to an active energy ray-polymerizable resin composition, comprising: a compound (A) containing an ethylenically unsaturated double bond group having a hydroxyl group (excluding (D)), a compound (B) containing an ethylenically unsaturated double bond group not having a hydroxyl group (excluding (D)), and a free radical polymerization initiator (E).

[0020] And satisfy any one of the following (1) to (4).

[0021] (1) It further contains a metal salt of an organic acid (C) and a boric acid compound (F).

[0022] (2) It further contains an amino group-containing compound (D) having a number average molecular weight of 500 to 40,000.

[0023] (3) It further contains a metal salt of an organic acid (C) and an amino group-containing compound (D) having a number average molecular weight of 500 to 40,000.

[0024] (4) It further contains an amino group-containing compound (D) having a number average molecular weight of 500 to 40,000 and a boric acid compound (F).

[0025] In addition, the present invention is an active energy ray polymerizable resin composition, which comprises: a compound containing an ethylenically unsaturated double bond group having a hydroxyl group (A), a compound containing an ethylenically unsaturated double bond group without a hydroxyl group (B), a metal salt of an organic acid (C), an amino compound (D) having a number average molecular weight of 500 to 40,000, a free radical polymerization initiator (E) and a boric acid compound (F).

[0026] In addition, the present invention relates to the above-mentioned active energy ray-polymerizable resin composition, which contains 10 to 60 mass% of the compound (A), 30 to 89 mass% of the compound (B), 0.01 to 5 mass% of the compound (C), 0.1 to 20 mass% of the compound (D), 0.1 to 10 mass% of the compound (E), and 0.1 to 7 mass% of the compound (F) in 100 mass% of the active energy ray-polymerizable resin composition.

[0027] In addition, the present invention relates to the above-mentioned active energy ray-polymerizable resin composition, wherein the compound (B) containing an ethylenically unsaturated double bond group and having no hydroxyl group comprises: a compound (b1) having a weight average molecular weight of 1,000 to 60,000 and having a carbamate structure and two ethylenically unsaturated double bond groups but having no hydroxyl group, and at least one of a compound (b2) having two or more ethylenically unsaturated double bond groups but having no hydroxyl group (excluding (b1)).

[0028] The present invention also relates to the active energy ray-polymerizable resin composition, which contains 1 to 20% by mass of the compound (b1) and 9 to 69% by mass of the compound (b2) based on 100% by mass of the active energy ray-polymerizable resin composition.

[0029] The present invention also relates to a laminate comprising: a first substrate (G1); a resin composition layer composed of the active energy ray-polymerizable resin composition; and a second substrate (G2) in this order.

[0030] In addition, the present invention relates to the above-mentioned laminate, wherein the substrate (G1) and the substrate (G2) are any one selected from the group consisting of polyacetyl cellulose film, polynorbornene film, polypropylene film, polyacrylic acid film, polycarbonate film, polyester film, polyvinyl alcohol film, polyimide film and glass film.

[0031] Effects of the Invention

[0032] According to the present invention, an active energy ray-polymerizable resin composition and a laminated body can be provided, which can form a laminated body having excellent adhesive strength even at high and low temperatures and excellent heat resistance and moist heat resistance. DETAILED DESCRIPTION

[0033] The preferred embodiment of the present invention is described below. In this specification, when expressed as "(meth)acrylic acid", unless otherwise specified, it means "acrylic acid or methacrylic acid" respectively. In addition, the active energy ray polymerizable resin composition is sometimes referred to as the resin composition, the compound (A) containing an ethylenically unsaturated double bond group having a hydroxyl group is referred to as the compound (A), the compound (B) containing an ethylenically unsaturated double bond group without a hydroxyl group is referred to as the compound (B), the metal salt of an organic acid (C) is referred to as the compound (C), the amino-containing compound (D) having a number average molecular weight of 500 to 40,000 is referred to as the compound (D), and the boric acid compound (F) is referred to as the compound (F).

[0034] In addition, the weight average molecular weight (Mw) and the number average molecular weight (Mn) in this specification are the weight average molecular weight and the number average molecular weight calculated|required by gel permeation chromatography (GPC) measurement in terms of polystyrene.

[0035] In the present specification, unless otherwise specified, a numerical range defined using “to” includes the numerical values ​​described before and after “to” as the lower limit and the upper limit of the range.

[0036] In addition, unless otherwise specified, "parts" and "%" respectively mean "parts by mass" and "mass %".

[0037] In addition, various components mentioned in this specification may be used individually by 1 type, or may use 2 or more types together, unless otherwise specified.

[0038] <Ethylenically unsaturated double bond group-containing compound (A) having a hydroxyl group>

[0039] Compound (A) is a compound having a hydroxyl group and an ethylenically unsaturated double bond group. By including compound (A) in the resin composition, hydrogen bonds are formed with the hydrophilic functional groups of the substrate, and the adhesion is improved. Compound (A) preferably has a weight average molecular weight of less than 1,000. If the weight average molecular weight of compound (A) is less than 1,000, the viscosity of the resin composition will not become too high, and the film thickness control during coating becomes easy. In addition, from the viewpoint of adhesion, compound (A) preferably has an ethylenically unsaturated double bond group.

[0040] In addition, in this application, when the number average molecular weight of the ethylenically unsaturated double bond group-containing compound having an amino group is 500 to 40,000, it is handled as an amino group-containing compound (D) described later even if it has a hydroxyl group.

[0041] The content of the compound (A) is preferably 10 to 60% by mass, more preferably 20 to 50% by mass in 100% by mass of the active energy ray-polymerizable resin composition. When the content is 10 to 60% by mass, the balance between low-temperature adhesive strength and high-temperature adhesive strength becomes good.

[0042] The compound (A) is not particularly limited as long as it is a compound having a hydroxyl group and an ethylenically unsaturated double bond group, and the following compounds can be used.

[0043] Examples thereof include 2-hydroxyethyl (meth)acrylate, 1-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 1-hydroxybutyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, cyclohexanedimethanol mono(meth)acrylate, 1-hydroxybutyl (meth)acrylate, Hydroxyl-containing aliphatic (meth)acrylates such as 0-hydroxydecyl acrylate, 12-hydroxylauryl (meth)acrylate, ethyl-α-(hydroxymethyl) (meth)acrylate, or (meth)acrylates having a hydroxyl group at the terminal by ring-opening addition of ε-caprolactone to the above-mentioned hydroxyl-containing compounds having an ethylenically unsaturated double bond group, and alkylene oxide-added (meth)acrylates obtained by repeatedly adding an alkylene oxide such as ethylene oxide, propylene oxide, or butylene oxide to the above-mentioned hydroxyl-containing compounds having an ethylenically unsaturated double bond group;

[0044] For example, hydroxyl-containing aliphatic vinyl ethers such as hydroxyethyl vinyl ether, hydroxypropyl vinyl ether, hydroxybutyl vinyl ether, hydroxyhexyl vinyl ether, hydroxyoctyl vinyl ether, hydroxydecyl vinyl ether, hydroxydodecyl vinyl ether, hydroxyoctadecyl vinyl ether, glycidyl vinyl ether, or alkylene oxide addition vinyl ethers having a hydroxyl group at the terminal obtained by repeatedly adding an alkylene oxide such as ethylene oxide or propylene oxide;

[0045] For example, hydroxyl-containing aliphatic (meth)allyl alcohols or (meth)allyl ethers such as (meth)allyl alcohol, isopropenyl alcohol, dimethyl (meth)allyl alcohol, hydroxyethyl (meth)allyl ether, hydroxypropyl (meth)allyl ether, hydroxybutyl (meth)allyl ether, hydroxyhexyl (meth)allyl ether, hydroxyoctyl (meth)allyl ether, hydroxydecyl (meth)allyl ether, hydroxydodecyl (meth)allyl ether, hydroxyoctadecyl (meth)allyl ether, glycidyl (meth)allyl ether, or alkylene oxide addition (meth)allyl ethers having a hydroxyl group at the terminal obtained by repeatedly adding an alkylene oxide such as ethylene oxide or propylene oxide;

[0046] For example, compounds having ethylenically unsaturated double bonds having multiple hydroxyl groups, such as propylene glycol, butylene glycol, heptene glycol, octenylene glycol, and glyceryl di(meth)acrylate;

[0047] For example, hydroxyl-containing (meth)acrylamides such as N-hydroxyethyl (meth)acrylamide [N-hydroxyethyl acrylamide and N-hydroxyethyl methacrylamide are collectively expressed as "N-hydroxyethyl (meth)acrylamide". The same applies below. ], N-hydroxypropyl (meth)acrylamide, N-hydroxybutyl (meth)acrylamide, N-hydroxyhexyl (meth)acrylamide, and N-hydroxyoctyl (meth)acrylamide;

[0048] For example, monomers having a hydroxyl group and a vinyl group such as vinyl alcohol are used, but the present invention is not particularly limited to these compounds. These monomers may be used alone or in combination of two or more.

[0049] The compound (A) is preferably an acrylic acid ester of a diol having 1 to 6 carbon atoms, and particularly preferably 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate.

[0050] <Ethylenically unsaturated double bond group-containing compound having no hydroxyl group (B)>

[0051] Compound (B) is a compound containing an ethylenically unsaturated double bond group without a hydroxyl group. By including compound (B) in the resin composition, the wet heat resistance is improved. It should be noted that in the present application, when the number average molecular weight of the compound containing an ethylenically unsaturated double bond group having an amino group is 500 to 40,000, it is treated as an amino-containing compound (D) described later.

[0052] The content of the compound (B) is preferably 30 to 89% by mass, more preferably 40 to 71% by mass in 100% by mass of the active energy ray-polymerizable resin composition. If it is 30% by mass or more, the moisture and heat resistance is further improved, and if it is 89% by mass or less, the adhesive force is further improved.

[0053] Compound (B) can be classified into a compound (b1) having a weight average molecular weight of 1,000 to 60,000 and having a carbamate structure and two ethylenically unsaturated double bond groups without a hydroxyl group, a compound (b2) having two or more ethylenically unsaturated double bond groups without a hydroxyl group (excluding (b1)), and a compound (b3) having one ethylenically unsaturated double bond group without a hydroxyl group. Compound (B) preferably includes at least one of compound (b1) and compound (b2), and more preferably includes both compound (b1) and compound (b2). By including compound (b1), the adhesive force at low and high temperatures is improved, and by including compound (b2), the moisture and heat resistance is improved.

[0054] [Compound (b1)]

[0055] Compound (b1) is a compound generally called urethane acrylate, and is a compound having no hydroxyl group. Since compound (b1) has a highly polar urethane bond and a weight average molecular weight of 1,000 to 60,000, the coating has excellent toughness, and thus has excellent adhesion to substrates at low and high temperatures, and improves adhesion. From the perspective of compatibility, viscosity, and adhesion of the polymerized coating, the weight average molecular weight of compound (b1) is particularly preferably in the range of 5,000 to 50,000.

[0056] The content of the compound (b1) is preferably 1 to 20% by mass, more preferably 2 to 10% by mass, in 100% by mass of the active energy ray-polymerizable resin composition. If it is 1% by mass or more, the adhesive force is further improved, and if it is 20% by mass or less, the viscosity does not become too high, and the film thickness control during coating becomes easy.

[0057] Examples of compound (b1) include compounds obtained by reacting a compound having two or more isocyanate groups with compound (A); or compounds obtained by reacting a compound having two or more isocyanate groups with a polyol to obtain a carbamate prepolymer having terminal isocyanate groups, and then reacting the carbamate prepolymer with compound (A).

[0058] The compound (b1) is preferably a compound obtained by reacting a compound having two or more isocyanate groups, a polyol, and the compound (A) at a molar ratio of 2:1:2. By reacting at the above ratio, theoretically a structure having acrylate groups at both ends of one molecule is formed, so that the balance between flexibility and crosslinking density is good, the substrate adhesion and toughness are excellent, and the adhesive force becomes good in a wide temperature range.

[0059] Examples of the compound having two or more isocyanate groups include aromatic polyisocyanates, aliphatic polyisocyanates, aromatic aliphatic polyisocyanates, and alicyclic polyisocyanates.

[0060] More specifically, examples of the aromatic polyisocyanate include 1,3-phenylene diisocyanate, 4,4′-diphenyl diisocyanate, 1,4-phenylene diisocyanate, 4,4′-diphenylmethane diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4′-toluidine diisocyanate, 2,4,6-triisocyanatotoluene, 1,3,5-triisocyanatobenzene, dianisidine diisocyanate, 4,4′-diphenyl ether diisocyanate, and 4,4′,4″-triphenylmethane triisocyanate.

[0061] Examples of the aliphatic polyisocyanate include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (also known as HDI), pentamethylene diisocyanate, 1,2-propylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, dodecamethylene diisocyanate, and 2,4,4-trimethylhexamethylene diisocyanate.

[0062] Examples of the aromatic aliphatic polyisocyanate include ω,ω′-diisocyanate-1,3-dimethylbenzene, ω,ω′-diisocyanate-1,4-dimethylbenzene, ω,ω′-diisocyanate-1,4-diethylbenzene, 1,4-tetramethylxylylene diisocyanate, and 1,3-tetramethylxylylene diisocyanate.

[0063] Examples of the alicyclic polyisocyanate include 3-isocyanate methyl-3,5,5-trimethylcyclohexyl isocyanate (also known as IPDI), 1,3-cyclopentane diisocyanate, 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, 4,4′-methylenebis(cyclohexyl isocyanate), and 1,4-bis(isocyanate methyl)cyclohexane.

[0064] In addition, a part of the above-mentioned polyisocyanate 2-methylpentane-2,4-diol adduct, a trimer having an isocyanurate ring, etc. can also be used. Polyphenylmethane polyisocyanate (another name: PAPI), naphthalene diisocyanate, and their polyisocyanate modified products can also be used. It should be noted that as a polyisocyanate modified product, a modified product having a carbodiimide group, a uretdione group, a ureaimine group, a biuret group that reacts with water, or any group in an isocyanurate group, or two or more of these groups can be used. The reactant of a polyol and a diisocyanate can also be used as a compound having at least two isocyanate groups.

[0065] From the viewpoint of adhesive strength, the compound having an isocyanate group is preferably an aliphatic diisocyanate or an alicyclic diisocyanate compound.

[0066] Examples of the polyol include low molecular weight polyols having a number average molecular weight (Mn) of about 50 to 500 and high molecular weight polyols having a number average molecular weight (Mn) of 500 to 30,000, and any of them can be used without particular limitation.

[0067] More specifically, examples of the low molecular weight polyols include ethylene glycol, propylene glycol, dipropylene glycol, diethylene glycol, triethylene glycol, butanediol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 2-methyl-1,8-octanediol, 3,3'-dihydroxymethylheptane, 2-butyl-2-ethyl-1,3-propanediol, polyoxyethylene glycol (addition mole number is less than or equal to 10 ), polyoxypropylene glycol (addition mole number is less than or equal to 10), propylene glycol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, neopentyl glycol, octanediol, butyl ethyl pentanediol, 2-ethyl-1,3-hexanediol, cyclohexanediol, cyclohexanedimethanol, tricyclodecane dimethanol, cyclopentadienyl dimethanol, dimer glycol and other aliphatic or alicyclic diols;

[0068] Aromatic diols such as 1,3-bis(2-hydroxyethoxy)benzene, 1,2-bis(2-hydroxyethoxy)benzene, 1,4-bis(2-hydroxyethoxy)benzene, 4,4'-methylenediphenol, 4,4'-(2-norbornyl)diphenol, 4,4'-dihydroxybiphenol, o-dihydroxybenzene, m-dihydroxybenzene and p-dihydroxybenzene, 4,4'-isopropylidenephenol, and addition-type bisphenols obtained by adding alkylene oxide to bisphenol.

[0069] Examples of the raw material bisphenol of the addition type bisphenol include bisphenol A and bisphenol F, and examples of the raw material alkylene oxide include ethylene oxide and propylene oxide.

[0070] More specifically, high molecular weight polyols include polyether polyols, polyester polyols, polyamide polyols, polycarbonate polyols, and polyurethane polyols. Polycarbonate polyols are obtained by reacting the above-mentioned low molecular weight diols with carbonate or phosgene.

[0071] Examples of commercially available products of the polyester polyol include Vylon series manufactured by Toyobo Co., Ltd., KURARAY POLYOL P series manufactured by Kuraray Co., Ltd., and Kyowa Paul series manufactured by Kyowa Hakko Chemical Co., Ltd.

[0072] As a commercially available product of the polyamide polyol, TPAE617 manufactured by Fuji Chemical Industries, Ltd. and the like can be used.

[0073] Examples of commercially available products of the polycarbonate polyol include Oxymer N112 manufactured by Perstorp, PCDL series manufactured by Asahi Kasei Chemicals Corporation, and KURARAY POLYOL PMHC series and KURARAY POLYOL C series manufactured by Kuraray Corporation.

[0074] Examples of commercially available polyurethane polyols include Vylon UR series manufactured by Toyobo Co., Ltd., Takelac E158 (hydroxyl value = 20, acid value <3), Takelac E551T (hydroxyl value = 30, acid value <3), and Takelac Y2789 (hydroxyl value = 10, acid value <2) manufactured by Mitsui Chemicals Polyurethanes Co., Ltd.

[0075] In addition, the high molecular weight polyol also includes polyester polyols obtained by ring-opening polymerization of lactones such as polycaprolactone diol, poly(β-methyl-γ-valerolactone) diol, and polyvalerolactone diol.

[0076] From the viewpoint of adhesion, the polyol is preferably a high molecular weight polyether diol or a high molecular weight polyester diol.

[0077] [Compound (b2)]

[0078] Compound (b2) is a compound having two or more ethylenically unsaturated double bond groups but not having a hydroxyl group, excluding (b1). By including compound (b2) in the resin composition, the crosslinking density of the cured composition coating becomes higher and the moisture and heat resistance is improved. Compound (b2) preferably has a weight average molecular weight of less than 1,000. If the weight average molecular weight is less than 1,000, the viscosity of the resin composition will not become too high, and the film thickness control during coating becomes easy. In addition, the ethylenically unsaturated double bond group possessed by (b2) preferably includes one or more (meth) acryloyl groups.

[0079] The content of the compound (b2) is preferably 9 to 69% by mass, more preferably 20 to 60% by mass, in 100% by mass of the active energy ray-polymerizable resin composition. When it is 9 to 69% by mass, the balance between moisture heat resistance and low-temperature adhesive strength and high-temperature adhesive strength becomes good.

[0080] As compound (b2), any compound having two or more ethylenically unsaturated double bonds but not having a hydroxyl group can be used without particular limitation. Examples of compounds having two ethylenically unsaturated double bonds but not having a hydroxyl group include di(meth)acrylates of alkyl glycols such as pentanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 2,2-dimethylpropane-1,3-diol di(meth)acrylate, hexanediol di(meth)acrylate, heptanediol di(meth)acrylate, and nonanediol di(meth)acrylate;

[0081] Alkylene glycol-modified di(meth)acrylates of alkylene glycols such as ethylene oxide-modified pentylene glycol di(meth)acrylate, propylene oxide-modified pentylene glycol di(meth)acrylate, tetramethylene oxide-modified pentylene glycol di(meth)acrylate, ethylene oxide-modified 2,2-dimethylpropane-1,3-diol di(meth)acrylate, propylene oxide-modified 2,2-dimethylpropane-1,3-diol di(meth)acrylate, tetramethylene oxide-modified 2,2-dimethylpropane-1,3-diol di(meth)acrylate, ethylene oxide-modified hexanediol di(meth)acrylate, propylene oxide-modified hexanediol di(meth)acrylate, tetramethylene oxide-modified hexanediol di(meth)acrylate, ethylene oxide-modified heptanediol di(meth)acrylate, propylene oxide-modified heptanediol di(meth)acrylate, and tetramethylene oxide-modified heptanediol di(meth)acrylate;

[0082] Di(meth)acrylates having an alkylene glycol such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, tetramethylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, and neopentyl glycol di(meth)acrylate;

[0083] Di(meth)acrylates having two alkylene glycols such as ethylene glycol-propylene glycol di(meth)acrylate, diethylene glycol-propylene glycol di(meth)acrylate, diethylene glycol-dipropylene glycol di(meth)acrylate, and poly(ethylene glycol-tetramethylene glycol) di(meth)acrylate;

[0084] Di(meth)acrylates having a benzene ring, such as bisphenol A di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, ethoxylated propoxylated bisphenol A di(meth)acrylate, bisphenol F di(meth)acrylate, ethoxylated bisphenol F di(meth)acrylate, ethoxylated propoxylated bisphenol F di(meth)acrylate, and 4,4'-bis(meth)acryloyloxymethylbiphenyl;

[0085] Di(meth)acrylates having an alicyclic structure, such as hydrogenated bisphenol A di(meth)acrylate, EO-modified hydrogenated bisphenol A (meth)acrylate, dimethyloldicyclopentane di(meth)acrylate, 1,3-adamantyl diol di(meth)acrylate, and 3-hydroxy-1,5-adamantyl di(meth)acrylate;

[0086] Vinyl ether compounds such as 2-(2-vinyloxyethoxy)ethyl (meth)acrylate, 1,4-butanediol divinyl ether, diethylene glycol divinyl ether, cyclohexanedimethanol divinyl ether, and triethylene glycol divinyl ether.

[0087] Examples of the compound having three or more ethylenically unsaturated double bond groups but no hydroxyl group include ethylene oxide-modified tri(meth)acrylate, propylene oxide-modified tri(meth)acrylate, and butylene oxide-modified tri(meth)acrylate.

[0088] Trimethylolpropane tri(meth)acrylate, ethylene oxide-modified trimethylolpropane tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, tetramethylene oxide-modified trimethylolpropane tri(meth)acrylate;

[0089] Ditrimethylolpropane tetra(meth)acrylate, ethylene oxide-modified ditrimethylolpropane tetra(meth)acrylate, propylene oxide-modified ditrimethylolpropane tetra(meth)acrylate, tetramethylene oxide-modified ditrimethylolpropane tetra(meth)acrylate;

[0090] Glyceryl tri(meth)acrylate, ethylene oxide modified glyceryl tri(meth)acrylate, propylene oxide modified glyceryl tri(meth)acrylate, tetramethylene oxide modified glyceryl tri(meth)acrylate;

[0091] Pentaerythritol tetra(meth)acrylate, ethylene oxide-modified pentaerythritol tetra(meth)acrylate, propylene oxide-modified pentaerythritol tetra(meth)acrylate, tetramethylene oxide-modified pentaerythritol tetra(meth)acrylate, and the like.

[0092] Among the above-mentioned compounds (b2), from the perspective of both moisture and heat resistance and adhesion, among the compounds having two ethylenically unsaturated double bonds but not having a hydroxyl group, preferred are triethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, hexanediol di(meth)acrylate, nonanediol di(meth)acrylate, and tricyclodecane dimethanol di(meth)acrylate; and as the compounds having three or more ethylenically unsaturated double bonds but not having a hydroxyl group, preferred are glycerol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate and isocyanuric acid ethylene oxide-modified tri(meth)acrylate.

[0093] In addition, compound (b2) preferably comprises a compound having two ethylenically unsaturated double bond groups but no hydroxyl group and a compound having three or more ethylenically unsaturated double bond groups but no hydroxyl group, and the mixing ratio of the compound having two ethylenically unsaturated double bond groups but no hydroxyl group to the compound having three or more ethylenically unsaturated double bond groups but no hydroxyl group (compound having two ethylenically unsaturated double bond groups but no hydroxyl group / compound having three or more ethylenically unsaturated double bond groups but no hydroxyl group) is more preferably 4 / 1 to 1 / 2 (mass ratio).

[0094] The resin composition of the present application may contain a compound (b3) having an ethylenically unsaturated double bond group but not having a hydroxyl group. By including compound (b3), the resin composition can be made low-viscosity and has excellent low-temperature adhesion. The compound (b3) preferably has a weight-average molecular weight of less than 1,000. If the weight-average molecular weight of compound (b3) is less than 1,000, the viscosity of the resin composition will not become too high, and the film thickness control during coating becomes easy.

[0095] The content of the compound (b3) is preferably 0 to 30% by mass in 100% by mass of the active energy ray-polymerizable resin composition. When the content is 0 to 30% by mass, the low-temperature adhesive force becomes good.

[0096] Examples of the compound (b3) having one ethylenically unsaturated double bond group but not having a hydroxyl group include alkyl (meth)acrylates such as n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, and isostearyl (meth)acrylate;

[0097] (meth)acrylates having a terminal alkyl (poly)glycol and an acryloyl group, such as 2-methoxyethyl (meth)acrylate, ethyl carbitol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, and methoxypolyethylene glycol (meth)acrylate;

[0098] (Meth)acrylates having an aromatic ring and one acryloyl group, such as benzyl (meth)acrylate, phenyl (meth)acrylate, phenol ethylene oxide-modified (meth)acrylate, nonylphenol ethylene oxide-modified (meth)acrylate, nonylphenol propylene oxide-modified (meth)acrylate, and monohydroxyethyl (meth)acrylate phthalate;

[0099] For example, (meth)acrylates having an alicyclic structure and one acryloyl group, such as cyclohexyl (meth)acrylate, 1-methyl-1-cyclopentyl (meth)acrylate, 2-(meth)acryloyloxyethyl hexahydrophthalate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, isobornyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, 2-ethyl-2-adamantyl (meth)acrylate, and 2-propyl-2-adamantyl (meth)acrylate;

[0100] (Meth)acrylates having a heterocyclic ring and one acryloyl group, such as tetrahydrofurfuryl (meth)acrylate, tetrahydrofurfuryl alcohol acrylate polymer, 3-ethyl-3-oxetanyl methyl (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl acrylate, and cyclic trimethylolpropane formal (meth)acrylate.

[0101] From the viewpoint of improving low-temperature adhesion, the compound (b3) is preferably dicyclopentenyl (meth)acrylate, dicyclopentyl (meth)acrylate, and isobornyl (meth)acrylate.

[0102] <Metal salt of organic acid (C)>

[0103] Compound (C) is a salt formed by an organic acid and a metal ion. By including compound (C) in the resin composition, heat resistance is improved. In a polarizing plate using a resin composition, it is believed that the acid component contained in the resin composition oozes into the PVA polarizing element under heating conditions and becomes the cause of color change. It is believed that the heat resistance is improved by neutralizing the acid component derived from the monomer, the impurities of the monomer, and the acid component contained as a decomposition product by compound (C).

[0104] The content of the compound (C) is preferably 0.01 to 5 mass %, more preferably 0.01 to 3 mass %, in 100 mass % of the active energy ray-polymerizable resin composition. When it is 0.01 to 5 mass %, excellent heat resistance is achieved.

[0105] Compound (C) can be classified into (c1) formed from an organic acid and a metal ion without an active energy ray polymerizable functional group and (c2) formed from an organic acid and a metal ion having an active energy ray polymerizable functional group. (c2) is preferred because it has excellent curability and can easily achieve both heat resistance and moisture heat resistance.

[0106] Examples of organic acids that do not have an active energy ray-polymerizable functional group include monoacids such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, heptanoic acid, octanoic acid, nonanoic acid, decanoic acid, and stearic acid; diacids such as oxalic acid, succinic acid, adipic acid, phthalic acid, oxaloacetic acid, and glutaric acid; hydroxycarboxylic acids such as lactic acid, glycolic acid, tartaric acid, malic acid, citric acid, gluconic acid, and glyceric acid; acidic amino acids such as 2-oxoglutamic acid and aspartic acid; keto acids such as pyruvic acid, acetoacetic acid, and levulinic acid; aromatic carboxylic acids such as benzoic acid and salicylic acid; polycarboxylic acids such as ethylenediaminetetraacetic acid; and other acids such as isocitric acid, malonic acid, glutaric acid, and glucuronic acid.

[0107] Examples of the organic acid having an active energy ray polymerizable functional group include (meth)acrylic acid, 2-carboxyethyl (meth)acrylate, 2-carboxypropyl (meth)acrylate, 3-carboxypropyl (meth)acrylate, 4-carboxybutyl (meth)acrylate, (meth)acrylic acid dimer, maleic acid, fumaric acid, monomethylmaleic acid, monomethylfumaric acid, aconitic acid, sorbic acid, cinnamic acid, glutaconic acid, citraconic acid, mesaconic acid, itaconic acid, tiglic acid, angelic acid, senecioic acid, crotonic acid, isocrotonic acid, sorbic acid, muconic acid, penicillic acid, geranic acid, citronellal acid, 4-acrylamidobutyric acid, 6- Polylactone (meth)acrylates having a carboxyl group at the terminal by ring-opening addition of a lactone ring, such as acrylamidohexanoic acid, 2-(meth)acryloyloxyethylsuccinic acid, mono(meth)acryloyloxyethyl phthalate, mono(meth)acryloyloxyethyl hexahydrophthalate, mono(meth)acryloyloxypropyl phthalate, and mono(meth)acryloyloxybutyl phthalate; carboxyl group-containing unsaturated double bond-containing carboxylic acids and their anhydrides, such as mono(meth)acrylate ω-carboxypolycaprolactone; 2-vinylbenzoic acid, 3-vinylbenzoic acid, 4-vinylbenzoic acid, and 4-isopropenylbenzenecarboxylic acid.

[0108] Examples of the metal ions include ions of Li, Na, K, Be, Mg, Ca, Sr, Ba, Ti, Zr, Cu, Ag, Zn, Cd, Al, Ga, In, and Sn.

[0109] In particular, (c2) is preferably sodium (meth)acrylate, potassium (meth)acrylate, magnesium di(meth)acrylate, and zinc di(meth)acrylate, from the viewpoint of excellent heat resistance and moist heat resistance.

[0110] <Amino group-containing compound (D) having a number average molecular weight of 500 to 40,000>

[0111] Compound (D) is a compound having a number average molecular weight of 500 to 40,000 and containing an amino group. By including compound (D) in the resin composition, heat resistance is improved. In a polarizing plate using a resin composition, it is believed that the acid component contained in the resin composition oozes into the PVA polarizing element under heating conditions and becomes the cause of color change. It is believed that heat resistance is improved by neutralizing the acid component derived from the monomer, the impurities of the monomer, and the acid component contained as a decomposition product by compound (D).

[0112] The number average molecular weight of the compound (D) is preferably 1000 to 5000. When it is 1000 to 5000, excellent heat resistance and moist heat resistance are achieved.

[0113] The content of the compound (D) is preferably 0.1 to 20% by mass, more preferably 0.5 to 10% by mass, in 100% by mass of the active energy ray-polymerizable resin composition. When it is 0.1 to 20% by mass, excellent heat resistance is achieved.

[0114] The compound (D) can be classified into a compound (d1) not containing an ethylenically unsaturated double bond group and a compound (d2) containing an ethylenically unsaturated double bond group.

[0115] Examples of the compound (d1) include polyethyleneimine, polyallylamine, polyetheramine, melamine resin, guanamine resin, amino group-containing acrylic resin, amino group-containing acrylamide resin, amino group-containing polyester, and amino group-containing vinyl resin.

[0116] The compound (d2) is a compound called an amine-modified oligomer and is also called an amine-modified acrylate, an acrylate-modified amine, a reactive amine co-initiator, a reactive amine catalyst, an acrylate-modified amine catalyst, and the like.

[0117] Compound (d2) can be used without structural limitation as long as it is a compound having a number average molecular weight of 500 to 40,000 and containing an amino group and an ethylenically unsaturated double bond group. As a production method, for example, a dicarboxylic acid containing an amino group can be obtained by a Michael addition reaction of a primary amine with acrylic acid, and then a polyester having a terminal hydroxyl group or a terminal carboxylic acid can be synthesized using the dicarboxylic acid containing an amino group and a diol, and the terminal of the obtained polyester is further modified with acrylic acid to produce the polyester. At this time, when the terminal of the polyester is a hydroxyl group, a compound having an isocyanate group and a (meth)acryloyl group can be reacted to perform (meth)acrylic acid modification. When the terminal of the polyester is a carboxylic acid, a compound having a glycidyl group and a (meth)acryloyl group can be reacted to perform (meth)acrylic acid modification.

[0118] There are many commercial products of compound (d2), for example, CN371NS, CN373, and CN550 manufactured by Sartorius;

[0119] PHOTOCRYL A104, Miramer AS1000, Miramer AS2010, and Miramer SC9610 manufactured by MIWON;

[0120] Ebecryl80, Ebecryl81, Ebecryl83, and Ebecryl7100 manufactured by Daicel-Allnex;

[0121] Etercure 6410, Etercure 6412, Etercure 6417, and Etercure 6410-TF manufactured by Changxing Materials Industry Co., Ltd.

[0122] GU8100W manufactured by Guojing Chemical, etc.

[0123] From the viewpoint of heat resistance, low-temperature adhesive strength and high-temperature adhesive strength, the compound (D) is preferably the compound (d2).

[0124] <Radical polymerization initiator (E)>

[0125] The radical polymerization initiator (E) is a compound that generates radicals by active energy rays. By using the radical polymerization initiator (E), the radical polymerization reaction can be accelerated.

[0126] The radical polymerization initiator (E) can be arbitrarily selected from known radical polymerization initiators and can be used. Specific examples thereof include 2,2-dimethoxy-2-phenylacetophenone, acetophenone, benzophenone, xanthofluorenone, benzaldehyde, anthraquinone, 3-methylacetophenone, 4-chlorobenzophenone, 4,4'-diaminobenzophenone, benzoin propyl ether, benzoin ethyl ether, benzyl dimethyl ketal, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropane-1-one, 2-hydroxy-2-methyl-1-phenylpropane-1-one, camphorquinone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide. Examples of commercially available products include Irgacure-184, 907, 651, 1700, 1800, 819, 369, 261, Darocur-TPO (2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide manufactured by BASF), Omnirad 819 (bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide manufactured by IGM Resins B.V.), Darocur-1173 (manufactured by Merck), Esacure-KIP150, TZT (manufactured by Nippon Siber Hegner Co., Ltd.), Kayacure BMS, and Kayacure DMBI (manufactured by Nippon Kayaku Co., Ltd.).

[0127] From the viewpoint of photobleaching property, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide or bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide is preferred.

[0128] The content of the radical polymerization initiator (E) is preferably 0.1 to 10% by mass in 100% by mass of the active energy ray-polymerizable resin composition.

[0129] <Boric acid compound (F)>

[0130] Compound (F) is a boric acid or a compound having one or more BOH bonds in one molecule, or a boron-containing compound that can be hydrolyzed in the presence of water to form one or more BOH bonds. As a classification, the boric acid derivatives described below are also included in the boric acid compounds. Compound (F) interacts with the hydroxyl group derived from compound (A) and the surface functional group of the substrate, thereby improving adhesion or tightness.

[0131] Boric acid derivatives include: boric acid oxides (e.g., B 2 O 3 );

[0132] Derivatives obtained by the reaction of boric acid with alcohols or phenols, for example boric acid esters such as trimethyl borate, triethyl borate, tri-n-propyl borate, tri-n-butyl borate, triphenyl borate, triisopropyl borate, tri-tert-amyl borate, triphenyl borate, trimethoxyboroxine, tri-2-cyclohexylcyclohexyl borate, triethanolamine borate, triisopropylamine borate, mannitol borate, glycerol borate, and triisopropanolamine borate.

[0133] Boric acid derivatives include derivatives of boric acid, for example, alkyl or alkenyl boronic acids such as methyl boronic acid, ethyl boronic acid, butyl boronic acid and cyclohexyl boronic acid;

[0134] Arylboronic acid such as phenylboronic acid, naphthaleneboronic acid and anthraceneboronic acid, or substituted arylboronic acid having an arbitrary substituent on the aryl group thereof.

[0135] Furthermore, other amino group-containing borate salts and tertiary amine salts of boric acid are also preferred. For example, 2-(β-dimethylaminoisopropoxy)-4,5-dimethyl-1,3,2-dioxaborolane, 2-(β-diethylaminoethoxy)-4,4,6-trimethyl-1,3,2-dioxaborolane, 2-(β-dimethylaminoethoxy)-4,4,6-trimethyl-1,3,2-dioxaborolane, 2-(β-diisopropylaminoethoxy)-1,3,2-dioxaborolane, 2-(β-diisopropylaminoethoxy)-4-methyl-1,3,2-dioxaborolane, 2-(γ-dimethylaminopropoxy)-1,3,6,9-tetraoxo-2-boracycloundecane, and 2-(β-dimethylaminoethoxy)-4,4-(4-hydroxybutyl)-1,3,2-dioxaborolane can be mentioned.

[0136] In addition, the boric acid derivative may also be an organic oligomer or polymer compound containing a boron-containing site, for example, a polymer having a borate group obtained by reacting a polymer borate ester (for example, an active hydrogen-containing polymer (for example, an acrylic polymer or a polysiloxane polymer containing a hydroxyl functional group)) with boric acid or a borate ester.

[0137] As the polymer used as the raw material of the polymer borate ester, a known active hydrogen-containing polymer can be used, and examples thereof include acrylic polymers, polyester polymers, polyurethane polymers, and polyether polymers.

[0138] The boric acid compound (F) described above is preferably boric acid, boric acid ester, or tertiary amine salt of boric acid because they are excellent in solubility in the resin composition. Boric acid is more preferred from the viewpoint of improving adhesion.

[0139] In addition, the boric acid derivative preferably has three or more hydroxyl groups. Examples of the boric acid derivative having three or more hydroxyl groups include 1,4-phenylenediboronic acid (4 hydroxyl groups), tetrahydroxydiborane (4 hydroxyl groups), and triethanolamine borate (3 hydroxyl groups). It should be noted that boric acid and the boric acid derivative can be used alone or in combination.

[0140] The content of the boric acid compound (F) is preferably 0.1 to 7% by mass, and more preferably 0.3 to 3% by mass in 100% by mass of the active energy ray polymerizable resin composition. If 0.1 to 7% by mass of the boric acid compound (F) is used, the adhesiveness and solution stability of the active energy ray polymerizable resin composition are further improved. It should be noted that in the present invention, the active energy ray polymerizable resin composition is also referred to as a solution when it does not contain a solvent.

[0141] <Other ingredients>

[0142] (Active Energy Ray Sensitizer (G))

[0143] In order to improve the reactivity of the radical polymerization initiator (E), an active energy ray sensitizer (G) may be used in combination. Examples of the sensitizer (G) include thioxanthone compounds, anthracene compounds, naphthalene compounds, aminobenzoate compounds, carbazole compounds, perylene, phenothiazine, and Rose Bengal.

[0144] Examples of the sensitizer (G) include thioxanthone compounds such as 2-isopropylthioxanthone, 4-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-hydroxythioxanthone, 2-acetoxythioxanthone, and 2-propoxythioxanthone;

[0145] Anthracene compounds such as 9,10-dimethoxyanthracene, 9,10-ethoxyanthracene, 9,10-dipropoxyanthracene, and 9,10-dibutoxyanthracene; and naphthalene compounds such as 1,4-dimethoxynaphthalene, 1,4-diethoxynaphthalene, 1,4-dipropoxynaphthalene, and 1,4-dibutoxynaphthalene.

[0146] (Cationically polymerizable compound (H))

[0147] The resin composition of the present invention may further contain a cationically polymerizable compound (H) (hereinafter also referred to as compound (H)).

[0148] Compound (H) is a compound having an epoxy group as a three-membered cyclic ether, a compound having an oxetane group as a four-membered cyclic ether, and a compound having a cyclic carbonate group as a cationically polymerizable functional group. Compounds having an ethylenically unsaturated double bond group and a cationically polymerizable functional group are included in compound (H).

[0149] Examples of the compound having an epoxy group (epoxy compound) include aromatic epoxy compounds, aliphatic epoxy compounds, alicyclic epoxy compounds, and epoxy group-containing silane coupling agents.

[0150] Examples of the aromatic epoxy compound include bisphenol A diglycidyl ether, bisphenol F diglycidyl ether, bisphenol S diglycidyl ether, diglycidyl ether of bisphenol A propylene oxide adduct, phenol novolac epoxy resin, cresol novolac epoxy resin, biphenyl type epoxy resin, resorcinol diglycidyl ether, phenyl glycidyl ether, phenol ethylene oxide glycidyl ether, and tert-butylphenyl glycidyl ether.

[0151] The aliphatic epoxy compound is preferably aliphatic monoalcohols, aliphatic polyols, and glycidyl ethers of alkylene oxide adducts thereof.

[0152] Examples of the aliphatic epoxy compound include 2-ethyl-hexyl glycidyl ether, diglycidyl ether of 1,4-butanediol, diglycidyl ether of neopentyl glycol, diglycidyl ether of 1,6-hexanediol, triglycidyl ether of glycerol, triglycidyl ether of trimethylolpropane, diglycidyl ether of polyethylene glycol, diglycidyl ether of polypropylene glycol, and polyglycidyl ethers of polyether polyols obtained by adding one or two or more alkylene oxides (ethylene oxide, polypropylene oxide) to an aliphatic polyol such as ethylene glycol, polypropylene glycol, and glycerol.

[0153] Examples of the compound having an ethylenically unsaturated double bond group and a cationically polymerizable functional group include glycidyl (meth)acrylate, glycidyl vinyl ether, and glycidyl allyl ether.

[0154] Examples of the alicyclic epoxy compound include 1,2-epoxy-4-vinylcyclohexane, 1,2:8,9-diepoxylimonene, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, 2-(3,4-epoxycyclohexyl-5,5-spiro-3,4-epoxy)cyclohexane-m-diol bis(3,4-epoxycyclohexylmethyl)adipate, bis(3,4-epoxy-6-methylcyclohexylmethyl)adipate, etc.

[0155] Examples of the epoxy group-containing silane coupling agent include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 5,6-epoxyhexyltrimethoxysilane, and 5,6-epoxyhexyltriethoxysilane.

[0156] Examples of the compound having an oxetane group include 3-ethyl-3-hydroxymethyloxetane, 1,4-bis[(3-ethyl-3-oxetane)methoxymethyl]benzene, di(1-ethyl-3-oxetane)methyl ether, 3-ethyl-3-(phenoxymethyl)oxetane, 3-ethyl-3-(2-ethyl-hexyloxymethyl)oxetane, phenol novolac oxetane, and 3-ethyl-{(3-triethoxysilylpropoxy)methyl}oxetane.

[0157] Examples of the cyclic carbonate compound include ethylene carbonate and propylene carbonate.

[0158] <Photoacid generator (I)>

[0159] When the resin composition of the present invention contains a cationically polymerizable compound (H), it also contains a photoacid generator (I).

[0160] The acid generator (I) is a substance that generates an acid by irradiation with active energy rays such as visible light, ultraviolet light, X-rays or electron beams, and catalytically initiates the polymerization reaction of the silane compound or the cationic polymerizable compound. Examples of the acid generator include sulfonium salt-based acid generators, iodine-based acid generators, Salt-based acid generator, diazo Salt-based acid generators, ammonium salt-based acid generators, phosphonium salt-based acid generators, etc. Salt-based acid generators, etc.

[0161] Among these, sulfonium salt-based acid generators, iodine-based acid generators, and iodine-based acid generators are preferred from the viewpoint of being able to form an active energy ray-polymerizable resin composition having excellent photodecomposition efficiency and further excellent curing properties. Salt-based acid generator.

[0162] [Sulfonium salt acid generator]

[0163] Examples of the sulfonium salt acid generator include triarylsulfonium hexafluorophosphate, triarylsulfonium hexafluoroantimonate, and triarylsulfonium tetrakis(pentafluorophenyl)borate.

[0164] Examples of commercially available sulfonium salt acid generators include triarylsulfonium hexafluorophosphate (CPI-110P, manufactured by San-Apro) and UVACURE 1590 (manufactured by Daicel Cytec).

[0165] [iodine Salt-based acid generator]

[0166] As iodine Salt-based acid generators include bis(4-tert-butylphenyl)iodide Hexafluorophosphate, (4-methylphenyl)[4(2-methylpropyl)phenyl]iodide Hexafluorophosphate, (4-methylphenyl)(4-isopropylphenyl)iodide Hexafluorophosphate, diphenyl iodide Hexafluoroantimonate, diphenyl iodide Tetrakis(pentafluoro)borate, etc.

[0167] As iodine Commercially available products of salt-based acid generators include, for example, bis(4-tert-butylphenyl)iodide Hexafluorophosphate (WPI-170, manufactured by Wako Pure Chemical Industries, Ltd.), WPI-113 (manufactured by Wako Pure Chemical Industries, Ltd.), IK-1 (manufactured by San-Apro), (4-methylphenyl)[4(2-methylpropyl)phenyl]iodide Hexafluorophosphate (Omnicat 250, IGM resins), etc.

[0168] In the active energy ray polymerizable resin composition of the present invention, as long as it is within the range that does not impair the effect of the present invention, in addition to the above-mentioned components, additives can be appropriately formulated. For example, from the perspectives of reducing the polymerization curing shrinkage, reducing the thermal expansion coefficient, improving dimensional stability, improving the elastic modulus, adjusting viscosity, improving thermal conductivity, improving strength, improving toughness, and improving coloring, an organic or inorganic filler can be formulated. As such a filler, polymers, ceramics, metals, metal oxides, metal salts, dyes and pigments, etc. can be used, and the shape is not particularly limited to particles, fibers, etc. It should be noted that when the above-mentioned polymer is formulated, it is also possible not to use fillers such as flexibility imparting agents, plasticizers, flame retardants, storage stabilizers, antioxidants, ultraviolet absorbers, thixotropy imparting agents, dispersion stabilizers, fluidity imparting agents, defoaming agents, etc., but to dissolve, semi-dissolve or micro-disperse them in the active energy ray polymerizable resin composition in the form of polymer blends or polymer alloys.

[0169] From the perspective of drying equipment and drying energy, the active energy ray polymerizable resin composition of the present invention is preferably substantially free of water and organic solvents. However, in the case where the free radical polymerization initiator (E), the active energy ray sensitizer (G), and the acid generator (I) are poorly soluble or have high viscosity relative to the compound (A) and the compound (B), a small amount of organic solvent may also be included in order to dissolve the free radical polymerization initiator (E). The content of organic solvent in the active energy ray polymerizable resin composition in this case is within 5% by mass. There is no particular limitation on the organic solvent that can be used. Specifically, organic solvents such as methanol, ethanol, isopropanol, acetone, methyl ethyl ketone, methyl isobutyl ketone, methyl acetate, ethyl acetate, butyl acetate, cyclohexane, toluene, xylene and other hydrocarbon solvents and water can be further added to adjust the viscosity of the active energy ray polymerizable resin composition, and the active energy ray polymerizable resin composition can also be heated to reduce the viscosity.

[0170] <Active Energy Ray-Polymerizable Resin Composition>

[0171] The active energy ray-polymerizable resin composition of the present invention is any one of the following (1) to (4).

[0172] (1) comprising compound (A), compound (B), compound (C), free radical polymerization initiator (E) and compound (F)

[0173] (2) comprising compound (A), compound (B), compound (D) and free radical polymerization initiator (E)

[0174] (3) comprising compound (A), compound (B), compound (C), compound (D) and a radical polymerization initiator (E)

[0175] (4) comprising compound (A), compound (B), compound (D), free radical polymerization initiator (E) and compound (F)

[0176] By using the resin composition having such a composition, it is possible to form a laminate having excellent adhesive strength in a wide temperature range from high to low temperatures and having excellent heat resistance and moist heat resistance.

[0177] The resin composition of the present invention is more preferably a composition containing the compound (A), the compound (B), the compound (C), the compound (D), the radical polymerization initiator (E) and the compound (F).

[0178] By including these six components (A) to (F), a laminate having particularly excellent adhesive strength in a wide temperature range from high to low temperatures and having particularly excellent heat resistance and moist heat resistance can be formed.

[0179] <Laminate>

[0180] The laminate of the present invention is a laminate comprising a first substrate (G1), a resin composition layer composed of an active energy ray-polymerizable resin composition, and a second substrate (G2) in this order. It may also be a laminate in which a plurality of substrates are stacked such as substrate (G1) / resin composition layer / substrate (G2) / resin composition layer / substrate (G3). The substrates (G1), (G2), and (G3) may be of the same type or of different types.

[0181] The laminated body can be obtained, for example, as follows.

[0182] The active energy ray polymerizable resin composition can be applied to one side of a transparent film as a film-like substrate to form a film, another transparent film is attached to the film, and the active energy ray polymerizable resin composition is further applied to one side or both sides of the laminate, and the laminate is further laminated on another transparent film, glass, or a transparent molded body to obtain a laminate. It should be noted that the laminate of the present invention is of course not limited to the above-mentioned laminated structure.

[0183] The film thickness of the resin composition layer formed by the active energy ray polymerizable resin composition in the present invention is not particularly limited and can be appropriately adjusted according to the intended use. The viscosity adjustment and coating of the resin composition in these embodiments can be easily implemented by adding a solvent to the active energy ray polymerizable resin composition as needed.

[0184] When the film thickness of the resin composition layer is 0.1 to 6 μm, the viscosity is preferably 1 to 1500 mPa·s, more preferably 10 to 1300 mPa·s, and further preferably 20 to 1000 mPa·s. If the viscosity is less than or equal to 1500 mPa·s, a thin film coating of 0.1 to 6 μm can be achieved when applied to a substrate, and optical properties such as transmittance are also excellent. On the other hand, if the viscosity is greater than or equal to 1 mPa·s, the film thickness control of the resin composition layer becomes easy, so it is preferred.

[0185] When the film thickness of the resin composition layer is 6 to 300 μm, the viscosity is preferably 1,500 to 100,000 mPa·s, and more preferably 3,000 to 50,000 mPa·s.

[0186] <Coating method>

[0187] The active energy ray-polymerizable resin composition of the present invention can be coated by a known coating method such as a Mayer bar, an applicator, a brush, a spray, a roller, a gravure coater, a die coater, a micro gravure coater, a die lip coater, a notch wheel coater, a curtain coater, a knife coater, a reverse coater, or a spin coater.

[0188] <Base material>

[0189] The substrate is a film substrate, a glass plate, a paper processed product, etc., without particular limitation. On the other hand, when the active energy ray polymerizable resin composition of the present invention is used as an adhesive for bonding two or more substrates, in order to irradiate the active energy ray to polymerize it, it is necessary to use a substrate that is easy to transmit the active energy ray. In this case, a transparent film or a transparent glass plate is preferably used. It should be noted that a substrate that is difficult to transmit active energy rays, such as wood, a metal plate, a plastic plate, a paper processed product, etc., can also be used for one of the bonded substrates, and a transparent film or a transparent glass plate can be used for the other, and irradiated from the transparent film or the transparent glass plate side to perform polymerization curing.

[0190] In the laminate of the present invention, a film-like substrate is preferably used as the substrate. As the film-like substrate, there can be mentioned film-like substrates such as glass paper, various plastic films, and synthetic paper, but various transparent plastic films are preferably used. In addition, as the film-like substrate, as long as it is transparent, it can be a single-layer substrate, and it can also be a substrate in a multi-layer state formed by laminating a plurality of substrates.

[0191] In order to make the resin composition adhere to the substrate in the laminate, it is necessary to perform a polymerization reaction of the resin composition by irradiation with active energy rays. The active energy ray polymerization reaction is performed when the resin composition is applied or laminated, and further by irradiation with active energy rays after lamination, but it is preferred to perform the polymerization reaction by irradiation with active energy rays after lamination.

[0192] <Active energy rays>

[0193] The active energy ray polymerizable resin composition of the present invention is applied to a substrate, and the formed film is irradiated with active energy rays, thereby polymerizing and curing. As the irradiation light source of the active energy ray, a light source mainly composed of light in the wavelength range of 150 to 550 nm can be listed, and low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, gallium lamps, chemical lamps, black light lamps, microwave-excited mercury lamps, LED lamps, xenon lamps, etc. In addition, semiconductor lasers, electron beams, etc. can also be used as active energy rays.

[0194] The irradiation intensity of ultraviolet rays is preferably 10 to 3000 mW / cm2 If the irradiation intensity satisfies the above range, rapid curing is easy and degradation of the substrate can be suppressed to a minimum. The cumulative irradiation amount expressed as the product of the irradiation intensity and the irradiation time is preferably 50 to 20,000 mJ / cm 2 If the cumulative exposure amount satisfies the above cumulative exposure amount, curing is easy to achieve in a short time and productivity is further improved.

[0195] <Laminate for optical element>

[0196] The laminate of the present invention is preferably used as an optical laminate, and more preferably as an optical element laminate. The laminated structure of the optical laminate is preferably a sheet-like laminate having multiple layers of transparent film / adhesive layer / transparent film, transparent film / adhesive layer / transparent film / adhesive layer / transparent film, etc. In addition, a part of the transparent film may be replaced by an optical component such as glass or an optical molded body.

[0197] When the laminate of the present invention is used as a laminate for an optical element, it is necessary to use an optical film as a substrate.

[0198] The transparent film that can be used as an optical film is preferably a thermoplastic resin that is excellent in transparency, mechanical strength, thermal stability, moisture barrier properties, and isotropy. The transparent film also refers to a plastic film or a plastic sheet, and examples thereof include polyolefin films such as polyvinyl alcohol film, polytriacetyl cellulose film, polypropylene, polyethylene, polycycloolefin, and ethylene-vinyl acetate copolymer; polyester films such as polyethylene terephthalate and polybutylene terephthalate; polycarbonate films, polynorbornene films, polyarylate films, polyacrylic films, polyphenylene sulfide films, polystyrene films, polyethylene films, polyamide films, polyimide films, polyethylene oxide films, and glass films.

[0199] In particular, for excellent transparency, any one selected from the group consisting of polyacetylcellulose films, polynorbornene films, polypropylene films, polyacrylic acid films, polycarbonate films, polyester films, polyvinyl alcohol films, polyimide films and glass films is preferred.

[0200] When a transparent film is used as a laminate, each film may be used alone or two or more films may be used in combination. For example, a polycycloolefin film may be used on one side and a polyacrylic acid film may be used on the other side.

[0201] The thickness of the transparent film can be appropriately determined, but is generally about 1 to 500 μm, preferably 1 to 300 μm, more preferably 5 to 200 μm, and even more preferably 5 to 150 μm from the viewpoints of strength, workability such as handleability, and thin film properties.

[0202] When transparent films are provided on both sides of a polarizing element as a polarizing film serving as an optical film, transparent films made of the same polymer material may be used on the front and back sides, or transparent films made of different polymer materials may be used.

[0203] When the laminate of the present invention is used for optical element purposes, it is preferred that the substrate uses an optical film. An optical film is a film formed by applying a coating liquid having an optical function to the above-mentioned transparent film. Optical function refers to light transmission, light diffusion, light focusing, refraction, scattering, haze (HAZE), etc. Optical films can be listed, for example, hard coatings, antistatic coatings, anti-glare coatings, polarizing films, phase difference films, elliptically polarizing films, anti-reflective films, light diffusion films, brightness enhancement films, prism films (also referred to as prism sheets), and light guide films (also referred to as light guide plates). They can be used alone or in combination of two or more according to the purpose.

[0204] The polarizing film is also called a polarizing plate, and is a sheet-like optical film having a multilayer structure in which two polytriacetyl cellulose protective films (hereinafter referred to as "TAC films") as polyacetyl cellulose films are laminated on both sides of a polyvinyl alcohol-based polarizing element via an adhesive, and a polycycloolefin film, polyacrylic acid film, polycarbonate film, polyester film, etc. as a polynorbornene film are laminated on one or both sides of a polyvinyl alcohol-based polarizing element. As the adhesive, the active energy ray polymerizable resin composition of the present invention can be suitably used.

[0205] The optical film laminated using the active energy ray polymerizable resin composition of the present invention is preferably further laminated and attached to a transparent film such as a glass plate of a liquid crystal display device, a touch panel module, an organic EL module, or the above-mentioned various plastic films to form a laminate for optical elements.

[0206] More specifically, a polarizing plate (polarizing film) using the active energy ray-polymerizable resin composition as an adhesive can be obtained as follows.

[0207] The polarizing plate (polarizing film) using the active energy ray-polymerizable adhesive is preferably produced by any of the following methods (I) to (III), including the following methods, but is not particularly limited.

[0208] (I) A method of manufacturing by applying an active energy ray-polymerizable adhesive to one side of a protective film as a first transparent film to form a first polymerizable adhesive layer,

[0209] An active energy ray-polymerizable adhesive is applied to one side of the second protective film as a transparent film to form a second active energy ray-polymerizable adhesive layer.

[0210] Next, after simultaneously or sequentially overlapping the first active energy ray-polymerizable adhesive layer and the second active energy ray-polymerizable adhesive layer on each surface of the polyvinyl alcohol-based polarizing element, irradiating the active energy ray to polymerize and cure the first active energy ray-polymerizable adhesive layer and the second active energy ray-polymerizable adhesive layer;

[0211] (II) A method of manufacturing by coating an active energy ray-polymerizable adhesive on one side of a polyvinyl alcohol-based polarizing element to form a first active energy ray-polymerizable adhesive layer, covering the surface of the formed first active energy ray-polymerizable adhesive layer with a first protective film as a transparent film, then coating an active energy ray-polymerizable adhesive on the other side of the polyvinyl alcohol-based polarizing element to form a second active energy ray-polymerizable adhesive layer, covering the surface of the formed second active energy ray-polymerizable adhesive layer with a second protective film, irradiating with active energy rays, and polymerizing and curing the first active energy ray-polymerizable adhesive layer and the second active energy ray-polymerizable adhesive layer; and

[0212] (III) A method of manufacturing by dropping an active energy ray-polymerizable adhesive on the end of the protective film as the first transparent film overlapping the polyvinyl alcohol-based polarizing element and the end of the second protective film overlapping the surface of the polyvinyl alcohol-based polarizing element without the first protective film, and then passing the adhesive between rollers to spread the adhesive between the layers. Then, irradiating the adhesive with active energy rays to polymerize and cure the active energy ray-polymerizable adhesive; etc.

[0213] Example

[0214] Hereinafter, specific examples of the present invention will be described together with comparative examples, but the present invention is not limited to the following examples. In addition, in the following examples and comparative examples, "parts" and "%" represent "parts by mass" and "mass %", respectively, and "RH" refers to relative humidity.

[0215] The amounts in the tables are parts by mass and are converted to non-volatile components excluding the solvent. A blank column in the table indicates that no component is added.

[0216] <Method for measuring weight average molecular weight and number average molecular weight>

[0217] The "weight average molecular weight" is a value measured using a gel permeation chromatograph "HLC-8220GPC" manufactured by Tosoh Corporation, and is a weight average molecular weight and number average molecular weight in terms of polystyrene obtained by connecting four separation chromatographic columns: "TSK-GELSUPER H5000", "TSK-GELSUPER H4000", "TSK-GEL SUPER H3000", and "TSK-GEL SUPER H2000" manufactured by Tosoh Corporation in series, using tetrahydrofuran at a temperature of 40°C as the mobile phase, and measuring at a flow rate of 0.6 ml / min.

[0218] <Method for measuring hydroxyl value>

[0219] The hydroxyl value is determined as follows. Accurately measure about 1 g of the sample in a stoppered Erlenmeyer flask, add 100 ml of a mixed solution of toluene / ethanol (volume ratio: toluene / ethanol = 2 / 1) to dissolve it, then accurately add 5 ml of an acetylating agent (a solution in which 25 g of acetic anhydride is dissolved in pyridine and the volume is set to 100 ml), and stir for about 1 hour. Add phenolphthalein reagent as an indicator and continue stirring for 30 seconds. Then, titrate with 0.1N alcoholic potassium hydroxide solution until the solution turns light red, and use the following formula to calculate the hydroxyl value. The hydroxyl value is set to the value of the resin in the dry state (unit: mgKOH / g).

[0220] Hydroxyl value (mgKOH / g) = [{(ba)×F×28.25} / S] / (non-volatile content concentration / 100)+D

[0221] Where, S: the amount of sample collected (g)

[0222] a: Consumption of 0.1N alcoholic potassium hydroxide solution (ml)

[0223] b: Consumption of 0.1N alcoholic potassium hydroxide solution in blank experiment (ml)

[0224] F: Titer of 0.1N alcoholic potassium hydroxide solution

[0225] D: Acid value (mgKOH / g)

[0226] The materials used in Examples and Comparative Examples are as follows.

[0227] <Compound having an ethylenically unsaturated double bond group and having a hydroxyl group (A)>

[0228] 4HBA: 4-Hydroxybutyl acrylate

[0229] CHDMMA: Cyclohexanedimethanol monoacrylate

[0230] <Ethylenically unsaturated double bond group-containing compound having no hydroxyl group (B)>

[0231] [Compound (b1) having a weight average molecular weight of 1,000 to 60,000, having a urethane structure and two ethylenically unsaturated double bond groups but not having a hydroxyl group]

[0232] b1-1: Urethane acrylate 1 produced by the following method was used.

[0233] b1-2: Urethane acrylate 2 produced by the following method was used.

[0234] <Production of urethane acrylate 1>

[0235] 81.6 parts of polytetramethylene glycol (PTG850 manufactured by Hodogaya Chemical Co., Ltd., hydroxyl value 127.1 mgKOH / g) and 41.4 parts of isophorone diisocyanate were added to a 5-necked separable flask equipped with a stirrer, a reflux cooling tube, a gas introduction tube, a thermometer, and a dropping funnel, and the temperature was raised to 60°C while introducing dry air. 0.05 parts of dibutyltin dilaurate were added thereto, and the reaction was carried out for 1 hour. In addition, 27.0 parts of 4-hydroxybutyl acrylate and 0.15 parts of hydroquinone monomethyl ether were added to the dropping funnel and dropped into the separable flask over 1 hour. After the addition was completed, stirring was continued at 80°C for 3 hours, and the reaction was terminated when the absorption peak of the isocyanate group was confirmed to be absent in the infrared absorption spectrum, and urethane acrylate 1 was obtained. Its weight average molecular weight was 4,000.

[0236] <Production of urethane acrylate 2>

[0237] In a 5-mouth separable flask equipped with a stirrer, a reflux cooling tube, a gas introduction tube, a thermometer, and a dropping funnel, 113.4 parts of a compound obtained by adding 2 mol of ε-caprolactone to 1 mol of 2-hydroxyethyl acrylate (Placcel FA2D manufactured by Daicel Chemical, hydroxyl value 163.0 mgKOH / g), 36.6 parts of isophorone diisocyanate, and 0.15 parts of hydroquinone monomethyl ether were added, and the temperature was raised to 60°C while introducing dry air. 0.04 parts of dibutyltin dilaurate were added thereto, the temperature was raised, and the reaction was carried out at about 80°C for 3 hours. The reaction was terminated when the absorption peak of the isocyanate group was confirmed to be absent in the infrared absorption spectrum, and urethane acrylate 2 was obtained. Its weight average molecular weight was 1,300.

[0238] [Compound (b2) having two or more ethylenically unsaturated double bond groups but no hydroxyl group]

[0239] TPGDA: Tripropylene glycol diacrylate

[0240] INATA: Isocyanuric acid ethylene oxide (EO) modified triacrylate

[0241] [Compound (b3) having one ethylenically unsaturated double bond group but no hydroxyl group]

[0242] IBXA: Isobornyl acrylate

[0243] <Metal salt of organic acid (C)>

[0244] [Metal salt of organic acid formed from an organic acid having no active energy ray-polymerizable functional group and a metal ion (c1)]

[0245] Potassium stearate

[0246] [Metal salt of organic acid formed from an organic acid having an active energy ray-polymerizable functional group and a metal ion (c2)]

[0247] Potassium Acrylate

[0248] Zinc diacrylate

[0249] <Compound (D) having an amino group and having a number average molecular weight of 500 to 40,000>

[0250] [Compound (d1) having an amino group but not having an ethylenically unsaturated double bond group]

[0251] <Production of polyesters (d1-1) to (d1-4) having amino groups without ethylenically unsaturated double bond groups>

[0252] (Production of Polyester (d1-1) Having Amino Group)

[0253] In a 5-necked separable flask equipped with a stirrer, a reflux cooling tube, a distillation device, a gas inlet tube, a thermometer, and a dropping funnel, 61.1 parts of hexylamine and 144.1 parts of acrylic acid were added, and the mixture was reacted at 80°C for 4 hours while introducing dry air. The absence of an absorption peak of the acrylic acid group was confirmed in the infrared absorption spectrum. Then, 236.3 parts of 1,6-hexanediol and 0.34 parts of a solution of tetra-n-butoxytitanium diluted to a concentration of 1w% in 1,6-hexanediol were added while introducing nitrogen, and the temperature was raised to 150°C while stirring. At the beginning of the dehydration stage, the temperature was raised by 20°C every hour, and when it reached 220°C, the temperature was maintained constant and reacted. The reaction was terminated when it was confirmed that the acid value was less than or equal to 3 mgKOH / g, and a polyester (d1-1) with an amino group was obtained. Its number average molecular weight is 440. (Dicarboxylic acid / diol = 1 / 2)

[0254] (Production of Polyester (d1-2) Having Amino Group)

[0255] In a 5-necked separable flask equipped with a stirrer, a reflux cooling tube, a distillation device, a gas inlet tube, a thermometer, and a dropping funnel, 61.1 parts of hexylamine and 144.1 parts of acrylic acid were added, and the mixture was reacted at 80°C for 4 hours while introducing dry air. The absence of an absorption peak of the acrylic acid group was confirmed in the infrared absorption spectrum. Then, 177.3 parts of 1,6-hexanediol and 0.34 parts of a solution of tetra-n-butoxytitanium diluted to a concentration of 1w% in 1,6-hexanediol were added while introducing nitrogen, and the temperature was raised to 150°C while stirring. At the beginning of the dehydration stage, the temperature was raised by 20°C every hour, and when it reached 220°C, the temperature was maintained constant and reacted. The reaction was terminated when it was confirmed that the acid value was less than or equal to 3 mgKOH / g, and a polyester (d1-2) with an amino group was obtained. Its number average molecular weight is 770. (Dicarboxylic acid / diol = 2 / 3)

[0256] (Production of Polyester (d1-3) Having Amino Group)

[0257] In a 5-necked separable flask equipped with a stirrer, a reflux cooling tube, a distillation device, a gas inlet tube, a thermometer, and a dropping funnel, 61.1 parts of hexylamine and 144.1 parts of acrylic acid were added, and the mixture was reacted at 80°C for 4 hours while introducing dry air. The absence of an absorption peak of the acrylic acid group was confirmed in the infrared absorption spectrum. Then, 147.7 parts of 1,6-hexanediol and 0.34 parts of a solution of tetra-n-butoxytitanium diluted to a concentration of 1w% in 1,6-hexanediol were added while introducing nitrogen, and the temperature was raised to 150°C while stirring. At the beginning of the dehydration stage, the temperature was raised by 20°C every hour, and when it reached 220°C, the temperature was maintained constant and reacted. The reaction was terminated when it was confirmed that the acid value was less than or equal to 3 mgKOH / g, and a polyester (d1-3) with an amino group was obtained. Its number average molecular weight is 1400. (Dicarboxylic acid / diol = 4 / 5)

[0258] (Production of Polyester (d1-4) Having Amino Group)

[0259] In a 5-necked separable flask equipped with a stirrer, a reflux cooling tube, a distillation device, a gas inlet tube, a thermometer, and a dropping funnel, 61.1 parts of hexylamine and 144.1 parts of acrylic acid were added, and the mixture was reacted at 80°C for 4 hours while introducing dry air. The absence of an absorption peak of the acrylic acid group was confirmed in the infrared absorption spectrum. Then, 132.9 parts of 1,6-hexanediol and 0.34 parts of a solution of tetra-n-butoxytitanium diluted to a concentration of 1w% in 1,6-hexanediol were added while introducing nitrogen, and the temperature was raised to 150°C while stirring. At the beginning of the dehydration stage, the temperature was raised by 20°C every hour, and when it reached 220°C, the temperature was maintained constant and reacted. The reaction was terminated when it was confirmed that the acid value was less than or equal to 3 mgKOH / g, and an amino-containing polyester (d1-4) was obtained. Its number average molecular weight is 2700. (Dicarboxylic acid / diol = 8 / 9)

[0260] <Acrylic resins having amino groups (d1-5) to (d1-6)>

[0261] The following poly[2-(dimethylamino)ethyl methacrylate] manufactured by Tokyo Chemical Industry Co., Ltd. was used.

[0262] d1-5: poly[2-(dimethylamino)ethyl methacrylate], number average molecular weight 25000

[0263] d1-6: poly[2-(dimethylamino)ethyl methacrylate], number average molecular weight 50,000

[0264] [Compound having an ethylenically unsaturated double bond group and an amino group (d2)]

[0265] The following amine-modified acrylate manufactured by Daicel-Allnex was used.

[0266] Ebecryl7100: amine-modified acrylate, number average molecular weight: 1180, number of acrylic acid groups: 2

[0267] Ebecryl80: amine-modified acrylate, number average molecular weight: 1300, acrylic acid base number: 4

[0268] <Production of a compound (d2-1) having an ethylenically unsaturated double bond group and an amino group>

[0269] Into a 5-necked separable flask equipped with a stirrer, a reflux cooling tube, a gas introduction tube, a thermometer, and a dropping funnel, 360.5 parts of TETRAD-X (N,N,N',N',-tetraglycidyl-m-xylene diamine manufactured by Mitsubishi Gas Chemical Co., Ltd.) and 288.2 parts of acrylic acid were added, and reacted at 80°C for 4 hours while introducing dry air. The absence of an absorption peak of an epoxy group was confirmed in the infrared absorption spectrum, and a compound (d2-1) having four acryloyl groups, four hydroxyl groups, and two amino groups was obtained. The number average molecular weight was 640.

[0270] <Production of acrylic resin (d2-2) having ethylenically unsaturated double bond groups and amino groups>

[0271] 50.6 parts of ethyl acetate, 180 parts by mass of N,N-diethylaminoethyl methacrylate, and 20 parts by mass of 2-hydroxyethyl methacrylate were placed in a reaction tank equipped with a gas introduction tube, a condenser, a stirring blade, and a thermometer. After the temperature was raised to 50°C while nitrogen substitution was performed, 2.3 parts of 1-thioglycerol were added and the temperature was raised to 70°C. 16.8 parts by mass of ethyl acetate and 0.6 parts by mass of 2,2'-azobis(2,4-dimethylvaleronitrile) were placed in a dripping tank, stirred until uniform, and then dripped into the reaction tank over 7 hours. The reaction was continued at the same temperature for 1 hour, and it was confirmed by solid content measurement that 95% or more of the reaction had occurred. Next, the air in the flask was replaced, 32.8 parts by mass of 2-acryloyloxyethyl isocyanate (AOI) and 0.1 parts by mass of hydroquinone were added, and the reaction was carried out at 70°C for 4 hours. FTIR confirmed that 2270 cm based on the isocyanate group -1 After the peak of disappeared, the reaction solution was cooled to obtain a solution of acrylic resin (d2-2) having ethylenically unsaturated double bond groups and amino groups. The number average molecular weight was 22000. The components were dried by heating at 180°C for 20 minutes before use.

[0272] <Radical polymerization initiator (E)>

[0273] TPO: 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (Omnirad TPO manufactured by IGM resins BV)

[0274] <Boric acid compound (F)>

[0275] Boric acid

[0276] 1,4-phenylenediboronic acid

[0277] <Active energy ray sensitizer (G)>

[0278] 2-ITX: 2-isopropylthioxanthone

[0279] [Example 1]

[0280] Into a light-shielded 300 ml glass bottle were placed 40 parts of 4HBA as a compound (A), 5 parts of b1-1 (urethane acrylate 1) as a compound (B), 36 parts of TPGDA, 15 parts of INATA, 1 part of potassium stearate as a compound (C), 2 parts of TPO as a free radical polymerization initiator (E), and 1 part of boric acid as a compound (F), and the mixture was sufficiently stirred using a disperser and then sufficiently degassed to obtain an active energy ray-polymerizable resin composition.

[0281] [Examples 2 to 64, Comparative Examples 1 to 8]

[0282] An active energy ray-polymerizable resin composition was obtained in the same manner as in Example 1 except that the composition and the blending amount (parts by mass) were changed as shown in Tables 1 to 5.

[0283] <Evaluation of laminated body>

[0284] The obtained active energy ray-polymerizable resin composition was used to prepare the following laminate X1, and the laminate was evaluated by the following method. The results are shown in Tables 1 to 5.

[0285] <Manufacturing of Laminated Body X1 (Polarizing Plate)>

[0286] As the transparent film (1), a polytriacetyl cellulose (hereinafter referred to as TAC) film containing an ultraviolet absorber having a thickness of 40 μm was used, and as the transparent film (2), a TAC film containing no ultraviolet absorber having a thickness of 20 μm was used. The surfaces of one side of the transparent films (1) and (2) were heated at 300 W·min / m 2 The films were subjected to corona treatment with a discharge amount of , and then within 1 hour, the active energy ray polymerizable adhesives shown in Tables 1 to 3 were coated on the corona treated surface of each film using a wire bar coater in a thickness of 2 μm to form a coating. A polyvinyl alcohol-based (hereinafter referred to as PVA) polarizing element was sandwiched between the active energy ray polymerizable adhesive layers formed on the transparent films (1) and (2) to obtain a laminate comprising transparent film (1) / adhesive layer / PVA polarizing element / adhesive layer / transparent film (2). The laminate was fixed to the tinplate by cellophane tape on all sides in such a way that the transparent film (1) was in contact with the tinplate.

[0287] The active energy ray irradiation device (manufactured by Toshiba Corporation, high pressure mercury lamp) was used to irradiate the transparent film (2) at a maximum illuminance of 300 mW / cm 2 、Cumulative light intensity 300mJ / cm 2 The ultraviolet rays are used to produce a laminate X1 (polarizing plate).

[0288] <Low temperature adhesion>

[0289] The obtained laminate X1 (polarizing plate) was cut into a size of 25 mm × 150 mm using a cutter as a sample for measurement. A double-sided adhesive tape (DF8712S manufactured by Toyo Chemical Co., Ltd.) was affixed to the surface of the transparent film (2) of the sample, and a laminator was used to bond it to a metal plate to obtain a laminate of the polarizing plate and the metal plate. The obtained laminate was used as a laminate for adhesion measurement. On the polarizing plate, a peeling start was pre-set between the transparent film (2) and the polarizing element, and the laminate for measurement was peeled off at a speed of 300 mm / min and at an angle of 90° at 0°C as the peeling force. At this time, the peeling force between the PVA polarizing element and the transparent film (2) was measured. The peeling force was used as the adhesion and evaluated in 4 levels.

[0290] [Evaluation criteria]

[0291] ◎: No peeling or polarizing plate damage, very good

[0292] ○: Can be peeled off without damaging the polarizing plate, peeling force is greater than or equal to 2.0 (N / 25mm), excellent

[0293] △: Peel force is greater than or equal to 1.0 (N / 25mm) and less than 2.0 (N / 25mm), which is practical

[0294] ×: Peel force is less than 1.0 (N / 25mm), not practical

[0295] <Normal temperature adhesive strength>

[0296] The obtained laminate X1 (polarizing plate) was cut into a size of 25 mm × 150 mm using a cutter as a sample for measurement. A double-sided adhesive tape (DF8712S manufactured by Toyo Chemical Co., Ltd.) was affixed to the surface of the transparent film (2) of the sample, and a laminator was used to bond it to a metal plate to obtain a laminate of the polarizing plate and the metal plate. The obtained laminate was used as a laminate for adhesion measurement. On the polarizing plate, a peeling start was pre-set between the transparent film (2) and the polarizing element, and the laminate for measurement was peeled off at a speed of 300 mm / min and at an angle of 90° at 25°C as the peeling force. At this time, the peeling force between the PVA polarizing element and the transparent film (2) was measured. The peeling force was used as the adhesion and evaluated in 4 levels.

[0297] [Evaluation criteria]

[0298] ◎: No peeling or polarizing plate damage, very good

[0299] ○: Can be peeled off without damaging the polarizing plate, peeling force is greater than or equal to 2.0 (N / 25mm), excellent

[0300] △: Peel force is greater than or equal to 1.0 (N / 25mm) and less than 2.0 (N / 25mm), which is practical

[0301] ×: Peel force is less than 1.0 (N / 25mm), not practical

[0302] <High temperature bonding strength>

[0303] The obtained laminate X1 (polarizing plate) was cut into a size of 25 mm × 150 mm using a cutter as a sample for measurement. A double-sided adhesive tape (DF8712S manufactured by Toyo Chemical Co., Ltd.) was affixed to the surface of the transparent film (2) of the sample, and a laminator was used to bond it to a metal plate to obtain a laminate of the polarizing plate and the metal plate. The obtained laminate was used as a laminate for adhesion measurement. On the polarizing plate, a peeling start was pre-set between the transparent film (2) and the polarizing element, and the laminate for measurement was peeled off at a speed of 300 mm / min and at an angle of 90° at 80°C as the peeling force. At this time, the peeling force between the PVA polarizing element and the transparent film (2) was measured. The peeling force was used as the adhesion and evaluated in 4 levels.

[0304] [Evaluation criteria]

[0305] ◎: No peeling or polarizing plate damage, very good

[0306] ○: Can be peeled off without damaging the polarizing plate, peeling force is greater than or equal to 2.0 (N / 25mm), excellent

[0307] △: Peel force is greater than or equal to 1.0 (N / 25mm) and less than 2.0 (N / 25mm), which is practical

[0308] ×: Peel force is less than 1.0 (N / 25mm), not practical

[0309] <Polarizing plate heat resistance test and humidity and heat resistance test (optical property evaluation)>

[0310] The obtained laminate X1 (polarizing plate) was cut into a size of 40 mm × 40 mm and used as a test sample for the heat resistance test and the moisture and heat resistance test. The optical properties were evaluated before and after the test, and the difference was used as the evaluation result. The optical properties were evaluated by setting the optional accessories for polarizing plate measurement on the UV-visible spectrophotometer V-730 manufactured by JASCO Corporation. The polarization degree and the b value of the monomer hue were used in the optical properties evaluation.

[0311] <Heat resistance test>

[0312] The test sample was tested at 110°C for 500 hours, and the difference in b value before and after the test was evaluated.

[0313] The difference in b value (Δb) = (b value after the test) - (b value before the test)

[0314] [Evaluation criteria]

[0315] ◎: Δb is greater than or equal to 0.00 and less than 2.00, very excellent

[0316] ○: Δb is greater than or equal to 2.00 and less than 4.00, excellent

[0317] △: Δb is greater than or equal to 4.00 and less than or equal to 6.00, which is practical

[0318] ×: Δb is greater than 6.00, not practical

[0319] <Moisture and heat resistance test>

[0320] The test sample was tested at 65° C. and 95% RH for 500 hours, and the difference in polarization degree before and after the test was evaluated.

[0321] Polarization difference (ΔP) = (polarization after the test P) - (polarization before the test P)

[0322] [Evaluation criteria]

[0323] ◎: ΔP greater than or equal to -0.50 and less than or equal to 0.00, very excellent

[0324] ○: ΔP greater than or equal to -1.00 and less than -0.50, excellent

[0325] △: ΔP is greater than or equal to -2.00 and less than -1.00, which is practical

[0326] ×: ΔP is less than -2.00, not practical [Table 1]

[0327]

[0328] [Table 2]

[0329]

[0330] [Table 3]

[0331]

[0332] [Table 4]

[0333]

[0334] [Table 5]

[0335]

Claims

1. An active energy ray polymerizable resin composition comprising: a compound A having a hydroxyl group and containing an ethylenically unsaturated double bond group, a compound B having no hydroxyl group and containing an ethylenically unsaturated double bond group, and a free radical polymerization initiator E, wherein: Compound A does not include compound D, and compound B does not include compound D. The active energy ray-polymerizable resin composition satisfies any one of the following (1) to (4), (1) further comprising a metal salt C of an organic acid and a boric acid compound F, (2) further comprising an amino group-containing compound D having a number average molecular weight of 500 to 40,000, (3) further comprising a metal salt C of an organic acid and an amino group-containing compound D having a number average molecular weight of 500 to 40,000, (4) It further contains an amino group-containing compound D and a boric acid compound F having a number average molecular weight of 500 to 40,000.

2. An active energy ray polymerizable resin composition, comprising: a compound A containing an ethylenically unsaturated double bond group having a hydroxyl group, a compound B containing an ethylenically unsaturated double bond group without a hydroxyl group, a metal salt of an organic acid C, an amino-containing compound D having a number average molecular weight of 500 to 40,000, a free radical polymerization initiator E, and a boric acid compound F.

3. The active energy ray-polymerizable resin composition according to claim 2, which contains 10 to 60 mass % of compound A, 30 to 89 mass % of compound B, 0.01 to 5 mass % of compound C, 0.1 to 20 mass % of compound D, 0.1 to 10 mass % of compound E, and 0.1 to 7 mass % of compound F in 100 mass % of the active energy ray-polymerizable resin composition.

4. The active energy ray-polymerizable resin composition according to any one of claims 1 to 3, wherein the compound B having an ethylenically unsaturated double bond group and having no hydroxyl group comprises: at least one of a compound b1 having a weight average molecular weight of 1,000 to 60,000 and having a urethane structure and two ethylenically unsaturated double bond groups but having no hydroxyl group, and a compound b2 having two or more ethylenically unsaturated double bond groups but having no hydroxyl group, wherein: Compound b2 does not include compound b1. 5 . The active energy ray-polymerizable resin composition according to claim 4 , comprising 1 to 20% by mass of the compound b1 and 9 to 69% by mass of the compound b2 in 100% by mass of the active energy ray-polymerizable resin composition. 6 . A laminate comprising a first substrate G1 , a resin composition layer comprising the active energy ray-polymerizable resin composition according to claim 1 , and a second substrate G2 in this order.

7. The laminate according to claim 6, wherein the substrate G1 and the substrate G2 are each independently any one selected from the group consisting of polyacetylcellulose films, polynorbornene films, polypropylene films, polyacrylic acid films, polycarbonate films, polyester films, polyvinyl alcohol films, polyimide films and glass films.

Citation Information

Patent Citations

  • Polarizing plate, its manufacturing method, optical member, and liquid crystal display device

    JP2004245925A

  • Photocurable adhesive composition and polarizing plate using the same

    JP2010018722A

  • Polarizing film and production method of the same, optical film and image display device

    JP2017194572A