Halogen-free phosphorus-free flame-retardant modified benzoxazine resin as well as preparation method and application thereof

By blending benzoxazine monomers with aldehyde compounds, the method simplifies the preparation of halogen-free and phosphorus-free flame-retardant benzoxazine resin, enhancing its flame retardancy and heat resistance for various applications.

CN119060332AActive Publication Date: 2024-12-03SICHUAN UNIV

Patent Information

Application Number
CN202411312614.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-12-03
Estimated Expiration
2044-09-20

AI Technical Summary

Technical Problem

Existing benzoxazine resins face challenges in achieving high-level flame retardancy while being halogen-free and phosphorus-free, with complex preparation methods and high raw material costs hindering their development.

Method used

A method involving the blending and curing of benzoxazine monomers with aldehyde compounds, optimizing the flame retardant properties and heat resistance by using specific mass ratios and blending techniques.

Benefits of technology

The resulting halogen-free and phosphorus-free flame-retardant modified benzoxazine resin achieves UL94 V-0 flame retardancy and excellent heat resistance, suitable for applications in fiber-reinforced composite materials, rail transit interior parts, printed circuit boards, and coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060332A_ABST
    Figure CN119060332A_ABST
Patent Text Reader

Abstract

The invention discloses halogen-free phosphorus-free flame-retardant modified benzoxazine resin and a preparation method thereof, and the halogen-free phosphorus-free flame-retardant modified benzoxazine resin is obtained by taking more than one benzoxazine monomer and more than one aldehyde compound as raw materials through blending and heating curing, the mass ratio of the benzoxazine monomer to the aldehyde group compound is 100: (1-40); the benzoxazine monomer is a diphenol type benzoxazine monomer, a diamine type benzoxazine monomer, a triphenol type benzoxazine monomer or a triamine type benzoxazine monomer. The invention also provides application of the halogen-free phosphorus-free flame-retardant modified benzoxazine resin in preparation of fiber reinforced composite materials, rail transit interior trim parts, printed circuit boards, coatings, adhesives and the like. The halogen-free phosphorus-free flame-retardant modified benzoxazine resin prepared by the preparation method disclosed by the invention has excellent flame retardance and heat resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials and relates to a benzoxazine resin, in particular to a halogen-free and phosphorus-free flame-retardant modified benzoxazine resin and a preparation method and application thereof. Background Art

[0002] Since the advent of polymers and their application in human daily life, they have increased the fire danger and harm caused by combustion, so the preparation of flame-retardant polymer materials is urgent. Introducing halogen elements or phosphorus elements into polymer materials can achieve flame retardancy of polymer materials, but polymer materials prepared by this method produce toxic gases or environmental problems when burned, causing flame-retardant polymer materials to develop in the direction of halogen-free and phosphorus-free. In addition, introducing flame-retardant elements into resin structures through synthesis has the risk of difficult synthesis, as well as the problem of difficult availability and high price of raw materials.

[0003] Benzoxazine monomers are benzo heterocyclic compounds synthesized from primary amine compounds, phenolic compounds and formaldehyde. Under the action of heating or catalysts, ring-opening polymerization can be carried out to obtain cross-linked cured products. During the curing process, benzoxazine does not release small molecules, has a low curing shrinkage rate, and has high heat resistance, high strength, low water absorption and other properties. It has received extensive attention and has developed rapidly. It has been applied in aerospace, electronics and electrical fields. However, most benzoxazine resins cannot meet high-level flame retardant requirements, which greatly limits the further development of this resin.

[0004] The development of halogen-free and phosphorus-free flame-retardant benzoxazine has aroused widespread interest. Patent CN202010183622.8 discloses a halogen-free and phosphorus-free intrinsic flame-retardant benzoxazine, and introduces an intrinsic flame-retardant benzoxazine prepared based on deoxybenzoin bisphenol, which has excellent heat resistance and high carbon residue rate while having V-0 flame retardant performance, but the phenol source used is costly and difficult to prepare; Patent CN202111203283.6 discloses a high heat-resistant, low dielectric, flame-retardant benzoxazine resin, and introduces alkynyl-containing benzoxazine monomers and alkynyl imide-containing benzoxazine monomers. The two monomers can synergistically improve the flame retardancy of the resin, but the preparation method is complicated and the price of the alkynyl compound is too high. Summary of the invention

[0005] The present invention aims to provide a halogen-free and phosphorus-free flame-retardant modified benzoxazine resin and a preparation method thereof in view of the shortcomings of high raw material cost and complicated preparation method in the preparation of halogen-free and phosphorus-free flame-retardant benzoxazine resin. Benzoxazine is blended and modified by using aldehyde compounds, thereby reducing the difficulty of preparing the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin and optimizing the flame retardant properties and heat resistance of the resin.

[0006] Another object of the present invention is to provide a use of the above-mentioned halogen-free and phosphorus-free flame-retardant modified benzoxazine resin.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions to achieve it.

[0008] The invention provides a method for preparing a halogen-free and phosphorus-free flame-retardant modified benzoxazine resin. The benzoxazine resin is prepared by using one or more benzoxazine monomers and one or more aldehyde compounds as raw materials, blending, heating and curing. The mass ratio of the benzoxazine monomer to the aldehyde compound is 100:(1-40). The benzoxazine monomer is a diphenol-type benzoxazine monomer, a diamine-type benzoxazine monomer, a triphenol-type benzoxazine monomer or a triamine-type benzoxazine monomer.

[0009] The benzoxazine monomer is selected from one of the following structural formulas:

[0010]

[0011] Wherein, the R1 substituent in ac may be H, 1 to 2 -CH3 (when there is one -CH3, it may be at the 2, 3, 4, or 5 position; when there are two -CH3, the two -CH3 are located at the 2 and 3 positions, 2 and 4 positions, 2 and 5 positions, 3 and 4 positions, or 3 and 5 positions, respectively), or -C(CH3)3;

[0012] Wherein, the R2 substituent in dh can be one of the following structural formulas:

[0013]

[0014] The aldehyde compound is an aldehyde having a benzene ring or a heterocyclic structure, or a benzoxazine monomer containing an aldehyde group.

[0015] The aldehyde with a benzene ring or a heterocyclic structure is selected from one of the following structural formulas:

[0016]

[0017] The aldehyde-containing benzoxazine monomer is selected from one of the following structural formulas:

[0018]

[0019] Wherein, the R substituent can be one of the following structures:

[0020]

[0021] In the method for preparing the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin, the mass ratio of the benzoxazine monomer to the aldehyde compound is preferably 100:(3-25), and more preferably 100:(5-20).

[0022] The preparation method of the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin comprises the following steps: melt blending or solution blending of the benzoxazine monomer and the aldehyde compound to obtain a modified benzoxazine blend.

[0023] In one possible implementation, the melt blending temperature is 50-160°C, and the blending time is 0.5-3 hours. In a preferred implementation, the melt blending temperature is 90-140°C, more preferably 100-130°C.

[0024] In one possible implementation, the organic solvent used for solution blending is at least one of acetone, butanone, toluene, xylene, chloroform, 1,4-dioxane, tetrahydrofuran, N,N-dimethylformamide, N-methylpyrrolidone, dimethyl sulfoxide, diethyl ether, etc., the blending temperature is 25-90° C., and the blending time is 0.5-3 hours. In a preferred implementation, the solution blending time is 1-2 hours.

[0025] In one achievable manner, in the blending step, a curing catalyst is also added, and the catalyst is melt-blended or solution-blended with the benzoxazine monomer and the aldehyde compound. The catalyst is at least one of imidazole, benzimidazole, resorcinol, m-aminophenylacetylene, phenolic resin, acetic acid, oxalic acid, aluminum chloride, ferric chloride, etc. The mass ratio of the catalyst to the benzoxazine monomer is (0.5-10):100; in a preferred embodiment, the mass ratio of the catalyst to the benzoxazine monomer is (0.5-3):100.

[0026] The preparation method of the above-mentioned halogen-free and phosphorus-free flame-retardant modified benzoxazine resin, the heating curing step is: the obtained modified benzoxazine blend is subjected to gradient thermal curing at 100-220° C., and the curing time is 8-16 hours. In a preferred implementation, the obtained modified benzoxazine blend is subjected to thermal insulation reaction at 100-220° C. in 4-6 temperature sections to achieve gradient thermal curing.

[0027] The above-mentioned heating and curing step is preferably: the obtained modified benzoxazine blend is subjected to gradient thermal curing at 120-200°C for 8-12 hours. In a preferred implementation, the obtained modified benzoxazine blend is subjected to thermal insulation reaction at 120-200°C in 4-6 temperature sections to achieve gradient thermal curing.

[0028] The present invention also provides a halogen-free and phosphorus-free flame-retardant modified benzoxazine resin prepared by the above method, which has a flame retardant property that can reach UL94 V-0 level and has excellent flame retardant property; at the same time, the glass temperature of the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin can reach 265° C. and has good heat resistance.

[0029] The present invention also provides the use of the above-mentioned halogen-free and phosphorus-free flame-retardant modified benzoxazine resin in the preparation of fiber-reinforced composite materials, rail transit interior parts, printed circuit boards, coatings, adhesives, etc.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] (1) The present invention uses benzoxazine and aldehyde compounds as raw materials, and can prepare halogen-free and phosphorus-free flame-retardant modified benzoxazine resin by blending and heating and curing, which greatly simplifies the preparation method of flame-retardant resin;

[0032] (2) The present invention utilizes aldehyde compounds to perform blending modification on benzoxazine monomers. The copolymerization of aldehydes and benzoxazine can increase the crosslinking density of the system and improve the heat resistance of benzoxazine resins.

[0033] (3) The present invention utilizes aldehyde compounds to carry out blending modification of benzoxazine. When the solidified material is ignited, the aldehyde groups can be oxidized to carboxyl groups and decarboxylated, thereby increasing the release of CO2 and water molecules, thus achieving the purpose of gas phase flame retardancy. At the same time, the co-crosslinking reaction between the aldehyde groups and the benzoxazine monomers at high temperatures can also promote the carbonization of benzoxazine, thus achieving the purpose of solid phase flame retardancy.

[0034] (4) The halogen-free and phosphorus-free flame-retardant modified benzoxazine resin prepared by the present invention has excellent flame retardancy and heat resistance, and can be used to prepare flame-retardant fiber-reinforced composite materials, rail transit interior parts, printed circuit boards, coatings, adhesives and other application fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a standard vertical combustion test picture of the unmodified benzoxazine resin prepared in the comparative example;

[0036] Figure 2 This is a standard vertical combustion test picture of the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin prepared in Example 1;

[0037] Figure 3 The heat resistance test results of the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin prepared in Example 1;

[0038] Figure 4 The heat resistance test results of the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin prepared in Example 2;

[0039] Figure 5 The heat resistance test results of the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin prepared in Example 3;

[0040] Figure 6 The heat resistance test results of the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin prepared in Example 4;

[0041] Figure 7 The heat resistance test results of the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin prepared in Example 5;

[0042] Figure 8 The heat resistance test results of the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin prepared in Example 6;

[0043] Fig. 9 These are the heat resistance test results of the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin prepared in Example 7. DETAILED DESCRIPTION

[0044] The following will clearly and completely describe the technical solutions of the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the present invention.

[0045] In the following examples, unless otherwise specified, the solvents and raw materials used were purchased from outside.

[0046] Example 1

[0047] The preparation steps of the phenol / diaminodiphenylmethane type benzoxazine of structural formula (1) are as follows: phenol, polyformaldehyde and 4,4-diaminodiphenylmethane are added into a reaction kettle at a molar ratio of 2:4:1, toluene is added as a solvent so that the solid content of the reaction system is maintained at 60%, the reaction is carried out at 80° C. for 6 hours, and after the reaction is completed, the layers are washed with water and the solvent is removed to obtain the phenol / diaminodiphenylmethane type benzoxazine.

[0048] The preparation steps of the trimerized p-hydroxybenzaldehyde azine of structural formula (2) are as follows: p-hydroxybenzaldehyde and cyanuric chloride are added into a reaction kettle at a molar ratio of 3:1, a 1M sodium hydroxide aqueous solution prepared by adding sodium hydroxide in an amount equal to that of p-hydroxybenzaldehyde is added into the reaction system, tetrahydrofuran is used as a solvent, and its mass is half of that of the sodium hydroxide aqueous solution, and the reaction is carried out at 50° C. for 6 hours. After the reaction is completed, the trimerized p-hydroxybenzaldehyde azine is filtered, washed with methanol, and then dried to obtain the trimerized p-hydroxybenzaldehyde azine.

[0049]

[0050] Preparation of halogen-free and phosphorus-free flame-retardant modified benzoxazine resin: Take 200 g of phenol / diaminodiphenylmethane type benzoxazine of structural formula (1), add 10 g of trimerized p-hydroxybenzaldehyde azine of structural formula (2) and 1 g of imidazole, melt blend at 120°C for 60 minutes, and then adopt staged heating curing. The specific conditions are heating at 120°C for 2 hours, heating at 140°C for 2 hours, heating at 160°C for 2 hours, heating at 180°C for 2 hours, and heating at 200°C for 2 hours.

[0051] Example 2

[0052] Structural formula (3) was purchased from Adamas with product number 75458D.

[0053] The preparation steps of the trimerized salicylaldehyde azine of structural formula (4) are as follows: salicylaldehyde and cyanuric chloride are added into a reaction kettle at a molar ratio of 3:1, a 1M sodium hydroxide aqueous solution prepared with sodium hydroxide in an amount equal to that of salicylaldehyde is added into the reaction system, tetrahydrofuran is used as a solvent, and its mass is 1 / 4 of the sodium hydroxide aqueous solution, and the reaction is carried out at 55°C for 6h. After the reaction is completed, the trimerized salicylaldehyde azine is filtered and dried to obtain the trimerized salicylaldehyde azine.

[0054] The preparation steps of the vanillin / furfurylamine type benzoxazine of structural formula (5) are as follows: vanillin, polyformaldehyde and furfurylamine are added into a reaction kettle at a molar ratio of 1:2:1, toluene is added as a solvent so that the solid content of the reaction system is maintained at 60%, and the reaction is carried out at 70°C for 12 hours. After the reaction is completed, the reaction system is washed with a 1M sodium hydroxide aqueous solution with a mass% of 1wt% of the reaction system, and then washed with water to separate the layers, and the solvent is removed to obtain the vanillin / furfurylamine type benzoxazine.

[0055]

[0056] Preparation of halogen-free and phosphorus-free flame-retardant modified benzoxazine resin: Take 150 g of phenol / diaminodiphenylmethane type benzoxazine of structural formula (1) (see Example 1 for the preparation steps), add 8 g of biphenyldicarboxaldehyde of structural formula (3), 5 g of trimerized salicylaldehyde of structural formula (4), 3 g of vanillin / furfurylamine type benzoxazine of structural formula (5), and 1 g of resorcinol, melt blend at 130°C for 40 minutes, and then adopt staged heating curing, heating at 140°C for 2 hours, heating at 160°C for 2 hours, heating at 180°C for 2 hours, heating at 200°C for 2 hours, and heating at 220°C for 2 hours.

[0057] Example 3

[0058] The preparation steps of the phenol / diaminodiphenyl ether type benzoxazine of structural formula (6) are as follows: phenol, polyformaldehyde and 4,4-diaminodiphenyl ether are put into a reactor at a molar ratio of 2:4:1, toluene is added as a solvent so that the solid content of the reaction system is maintained at 50%, and the reaction is carried out at 90° C. for 5 hours. After the reaction is completed, the reaction system is washed with a 1M sodium hydroxide aqueous solution with a mass% of 1wt% of the reaction system, and then washed with water to separate the layers, and the solvent is removed to obtain the phenol / diaminodiphenyl ether type benzoxazine.

[0059] Structural formula (7) was purchased from Adamas with product number 85006D.

[0060] The preparation steps of the trimerized vanillin oxadiazine of structural formula (8) are as follows: vanillin and cyanuric chloride are added into a reaction kettle at a molar ratio of 3:1, a 1M sodium hydroxide aqueous solution prepared with sodium hydroxide in an amount equal to that of vanillin is added to the reaction system, tetrahydrofuran is used as a solvent, and its mass is 1 / 2 of the sodium hydroxide aqueous solution, and the reaction is carried out at 40°C for 6 hours. After the reaction is completed, it is filtered and dried to obtain the trimerized vanillin oxadiazine.

[0061]

[0062] Preparation of halogen-free and phosphorus-free flame-retardant modified benzoxazine resin: Take 200 g of phenol / diaminodiphenyl ether type benzoxazine of structural formula (6), add 10 g of 2,5-furandicarboxaldehyde of structural formula (7), 10 g of trimervanillin of structural formula (8), and 2 g of acetic acid, melt blend at 120°C for 40 minutes, and then use staged heating to cure, heating at 120°C for 2 hours, heating at 130°C for 2 hours, heating at 150°C for 2 hours, heating at 170°C for 2 hours, and heating at 180°C for 5 hours.

[0063] Example 4

[0064] The preparation steps of the m-cresol / p-phenylenediamine type benzoxazine of structural formula (9) are as follows: m-cresol, polyformaldehyde and p-phenylenediamine are added into a reaction kettle at a molar ratio of 2:4:1, toluene is added as a solvent to make the solid content of the reaction system 50%, and the reaction is carried out at 90°C for 8 hours. After the reaction is completed, the reaction system is washed with a 1M sodium hydroxide aqueous solution with a mass% of 1wt% of the reaction system, and then washed with water to separate the layers, and the solvent is removed to obtain the m-cresol / p-phenylenediamine type benzoxazine.

[0065]

[0066] Structural formula (10) was purchased from Adamas with product number 122528I.

[0067] Preparation of halogen-free and phosphorus-free flame-retardant modified benzoxazine resin: Take 100 g of m-cresol / p-phenylenediamine type benzoxazine of structural formula (9), add 5 g of trimerized salicylaldehyde of structural formula (4) (for preparation steps, see Example 2), 5 g of trimerized vanilloid aldehyde of structural formula (8) (for preparation steps, see Example 3), 1 g of trimesic acid of structural formula (10), and 0.5 g of oxalic acid, melt blend at 140°C for 30 minutes, and then adopt staged heating curing, heating at 140°C for 2 hours, heating at 150°C for 2 hours, heating at 170°C for 2 hours, heating at 190°C for 2 hours, and heating at 200°C for 2 hours.

[0068] Example 5

[0069] The preparation steps of the m-tert-butylphenol / diaminodiphenyl ether type benzoxazine of structural formula (11) are as follows: m-tert-butylphenol, polyformaldehyde, and 4,4-diaminodiphenyl ether are added into a reactor at a molar ratio of 2:4:1, toluene is added as a solvent so that the solid content of the reaction system reaches 50%, and the reaction is carried out at 90° C. for 7 hours. After the reaction is completed, the reaction system is washed with a 1M sodium hydroxide aqueous solution of 1wt% by mass, and then washed with water to separate the layers, and the solvent is removed to obtain the m-tert-butylphenol / diaminodiphenyl ether type benzoxazine.

[0070] The preparation steps of salicylaldehyde / furfurylamine type benzoxazine of structural formula (12) are as follows: salicylaldehyde, polyformaldehyde and furfurylamine are added into a reaction kettle at a molar ratio of 1:2:1, toluene is added as a solvent so that the solid content of the reaction system reaches 50%, and the reaction is carried out at 85°C for 6 hours. After the reaction is completed, the reaction system is washed with a 1M sodium hydroxide aqueous solution with a mass% of 1wt% of the reaction system, and then washed with water to separate the layers, and the solvent is removed to obtain salicylaldehyde / furfurylamine type benzoxazine.

[0071]

[0072] Preparation of halogen-free and phosphorus-free flame-retardant modified benzoxazine resin: Take 150 g of m-tert-butylphenol / diaminodiphenyl ether type benzoxazine of structural formula (11), add 10 g of salicylaldehyde / furfurylamine type benzoxazine of structural formula (12), 3 g of biphenyl dicarboxaldehyde of structural formula (3) (preparation steps see Example 2), 2 g of trimerized salicylaldehyde of structural formula (4) (preparation steps see Example 2), and 1 g of imidazole, melt blend at 120°C for 60 minutes, and then adopt staged heating curing, heating at 140°C for 2 hours, heating at 160°C for 2 hours, heating at 180°C for 2 hours, and heating at 200°C for 2 hours.

[0073] Example 6

[0074] The preparation steps of the vanillin / m-aminophenylacetylene type benzoxazine of structural formula (13) are as follows: vanillin, polyformaldehyde and m-aminophenylacetylene are added into a reaction kettle at a molar ratio of 1:2:1, toluene is added as a solvent so that the solid content of the system is 60%, and the reaction is carried out at 90°C for 6 hours. After the reaction is completed, the reaction system is washed with a 1M sodium hydroxide aqueous solution with a mass% of 1wt% of the reaction system, and then washed with water to separate the layers, and the solvent is removed to obtain the vanillin / m-aminophenylacetylene type benzoxazine.

[0075] The preparation steps of salicylaldehyde / m-aminophenylacetylene type benzoxazine of structural formula (14) are as follows: salicylaldehyde, polyformaldehyde and m-aminophenylacetylene are added into a reaction kettle at a molar ratio of 1:2:1, toluene is added as a solvent so that the solid content of the system is 60%, and the reaction is carried out at 85°C for 7 hours. After the reaction is completed, the reaction system is washed with a 1M sodium hydroxide aqueous solution of 1wt% by mass of the reaction system, and then washed with water to separate the layers, and the solvent is removed to obtain salicylaldehyde / m-aminophenylacetylene type benzoxazine.

[0076]

[0077] Preparation of halogen-free and phosphorus-free flame-retardant modified benzoxazine resin: Take 100 g of phenol / diaminodiphenylmethane type benzoxazine of structural formula (1) (see Example 1 for the preparation steps), add 10 g of vanillin / m-aminophenylacetylene type benzoxazine of structural formula (13), 5 g of salicylaldehyde / m-aminophenylacetylene type benzoxazine of structural formula (14), 2 g of trimer vanillin oxaline of structural formula (8) (see Example 3 for the preparation steps), and 1 g of oxalic acid, melt blend at 90°C for 60 minutes, and then adopt staged heating curing, heating at 120°C for 2 hours, heating at 140°C for 2 hours, heating at 160°C for 2 hours, heating at 180°C for 2 hours, heating at 200°C for 2 hours, and heating at 220°C for 2 hours.

[0078] Example 7

[0079] The preparation steps of the m-cresol / diaminodiphenylmethane type benzoxazine of structural formula (15) are as follows: m-cresol, paraformaldehyde, and 4,4-diaminodiphenylmethane are added into a reactor at a molar ratio of 2:4:1, toluene is added as a solvent so that the solid content of the reaction system is 50%, and the reaction is carried out at 90° C. for 8 hours. After the reaction is completed, the reaction system is washed with a 1M sodium hydroxide aqueous solution with a mass% of 1wt% of the reaction system, and then washed with water to separate the layers, and the solvent is removed to obtain the m-cresol / diaminodiphenylmethane type benzoxazine.

[0080]

[0081] Preparation of halogen-free and phosphorus-free flame-retardant modified benzoxazine resin: Take 150 g of m-cresol / diaminodiphenylmethane type benzoxazine of structural formula (15), add 5 g of vanillin / m-aminophenylacetylene type benzoxazine of structural formula (13), 5 g of 2,5-furandicarboxaldehyde, 5 g of biphenyldicarboxaldehyde, and 2 g of benzimidazole, melt blend at 120°C for 30 minutes, and then use staged heating to cure, heating at 120°C for 2 hours, heating at 140°C for 2 hours, heating at 160°C for 2 hours, heating at 180°C for 2 hours, and heating at 200°C for 2 hours.

[0082] Example 8

[0083] The preparation steps of the bisphenol F / furfurylamine type benzoxazine of structural formula (16) are as follows: bisphenol F, polyformaldehyde and furfurylamine are added into a reaction kettle at a molar ratio of 1:4:2, toluene is added as a solvent so that the solid content of the reaction system is 55%, and the reaction is carried out at 70°C for 12 hours. After the reaction is completed, the reaction system is washed with a 1M sodium hydroxide aqueous solution with a mass% of 1wt% of the reaction system, and then washed with water to separate the layers, and the solvent is removed to obtain the bisphenol F / furfurylamine type benzoxazine.

[0084]

[0085] Preparation of halogen-free and phosphorus-free flame-retardant modified benzoxazine resin: Take 100 g of bisphenol F / furfurylamine type benzoxazine of structural formula (16), add 10 g of biphenyl dicarboxaldehyde of structural formula (3), 15 g of vanillin / furfurylamine type benzoxazine of structural formula (5), and 2 g of imidazole, melt blend at 120°C for 40 minutes, and then use staged heating to cure, heating at 120°C for 2 hours, heating at 140°C for 2 hours, heating at 160°C for 2 hours, heating at 180°C for 2 hours, and heating at 200°C for 2 hours.

[0086] Example 9

[0087] The preparation steps of the bisphenol F / aniline type benzoxazine of structural formula (17) are as follows: bisphenol F, polyformaldehyde and aniline are added into a reaction kettle at a molar ratio of 1:4:2, toluene is added as a solvent so that the solid content of the reaction system is 50%, and the reaction is carried out at 75°C for 10 hours. After the reaction is completed, the reaction system is washed with a 1M sodium hydroxide aqueous solution with a mass% of 1wt% of the reaction system, and then washed with water to separate the layers, and the solvent is removed to obtain the bisphenol F / aniline type benzoxazine.

[0088]

[0089] Preparation of halogen-free and phosphorus-free flame-retardant modified benzoxazine resin: Take 150 g of bisphenol F / aniline type benzoxazine of structural formula (17), add 20 g of trimerized p-hydroxybenzaldehyde azine of structural formula (2), and 10 g of vanillin / m-aminophenylacetylene type benzoxazine of structural formula (13), melt blend at 110°C for 60 minutes, and then use staged heating to cure, heating at 140°C for 2 hours, heating at 160°C for 2 hours, heating at 180°C for 2 hours, and heating at 200°C for 2 hours.

[0090] Example 10

[0091] Preparation of halogen-free and phosphorus-free flame-retardant modified benzoxazine resin: Take 200 g of phenol / diaminodiphenylmethane type benzoxazine of structural formula (1), add 1 g of trimesaldehyde of structural formula (10), 1 g of trimerized p-hydroxybenzaldehyde azine of structural formula (2), and 6 g of imidazole, melt blend at 120°C for 60 minutes, and then adopt staged heating curing, the specific conditions are heating at 120°C for 2 hours, heating at 140°C for 2 hours, heating at 160°C for 2 hours, heating at 180°C for 2 hours, and heating at 200°C for 2 hours.

[0092] Embodiment 11

[0093] Preparation of halogen-free and phosphorus-free flame-retardant modified benzoxazine resin: Take 100 g of m-tert-butylphenol / diaminodiphenyl ether type benzoxazine of structural formula (11), add 15 g of vanillin / furfurylamine type benzoxazine of structural formula (5), 10 g of vanillin / m-aminophenylethynyl type benzoxazine of structural formula (13), and 10 g of benzimidazole, melt blend at 100°C for 40 minutes, and then use staged heating to cure, the specific conditions are heating at 120°C for 2 hours, heating at 140°C for 2 hours, heating at 160°C for 2 hours, heating at 180°C for 2 hours, heating at 200°C for 2 hours, and heating at 220°C for 1 hour.

[0094] Example 12

[0095] Preparation of halogen-free and phosphorus-free flame-retardant modified benzoxazine resin: Take 100 g of phenol / diaminodiphenyl ether type benzoxazine of structural formula (6), add 30 g of vanillin / furfurylamine type benzoxazine of structural formula (5), 10 g of vanillin / m-aminophenylethynyl type benzoxazine of structural formula (13), and 0.5 g of acetic acid, melt blend at 90°C for 30 minutes, and then use staged heating to cure. The specific conditions are heating at 140°C for 2 hours, heating at 160°C for 2 hours, heating at 180°C for 2 hours, heating at 200°C for 2 hours, and heating at 220°C for 2 hours.

[0096] Embodiment 13

[0097] Preparation of halogen-free and phosphorus-free flame-retardant modified benzoxazine resin: Take 200 g of phenol / diaminodiphenylmethane type benzoxazine of structural formula (1), add 1 g of 2,5-furandicarboxaldehyde of structural formula (7) and 5 g of trisalicylic aldehyde of structural formula (4), melt blend at 120°C for 60 minutes, and then use staged heating to cure. The specific conditions are heating at 140°C for 2 hours, heating at 160°C for 2 hours, heating at 180°C for 2 hours, and heating at 200°C for 2 hours.

[0098] Embodiment 14

[0099] Preparation of halogen-free and phosphorus-free flame-retardant modified benzoxazine resin: Take 100 g of phenol / diaminodiphenylmethane type benzoxazine of structural formula (1), dissolve it in 200 mL of acetone at 40° C., add 3 g of biphenyldicarboxaldehyde of structural formula (3) and 5 g of trimervanillin of structural formula (8), blend the solution for 60 minutes, then remove the acetone by rotary evaporation at 60° C., and further dry in a vacuum oven at 120° C. for 10 minutes; then adopt staged heating curing, the specific conditions are heating at 120° C. for 2 hours, heating at 140° C. for 2 hours, heating at 160° C. for 2 hours, heating at 180° C. for 2 hours, and heating at 200° C. for 2 hours.

[0100] Comparative Example

[0101] Preparation of unmodified benzoxazine resin: 100 g of phenol / diaminodiphenylmethane type benzoxazine of structural formula (1) was used as raw material and cured by heating in stages. The specific conditions were: heating at 120°C for 2 h, heating at 140°C for 2 h, heating at 160°C for 2 h, heating at 180°C for 2 h, and heating at 200°C for 2 h.

[0102] Performance Testing

[0103] 1. The unmodified benzoxazine resin and the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin prepared in Examples 1-7 were subjected to a standard vertical combustion test (5 specimens were taken for each sample, with a size of 125 mm × 13 mm × 3 mm). The test process was as follows: the sample was clamped vertically on the test instrument with a fixture, and the timing was started from the time when the fire source contacted the bottom of the sample. The fire source was removed after 10 seconds of ignition, and the flame duration t1 at the bottom of the sample was recorded. After the sample was extinguished, the sample was ignited again, and the fire source was removed after 10 seconds, and the flame duration t2 at the bottom of the sample was recorded. When t1 and t2 were both less than 10 seconds, and the total burning time ∑(t1+t2) of the group of 5 specimens after the fire source was removed was less than 50 seconds, the sample was deemed to have V-0 flame retardancy; when t1 and t2 were both less than 30 seconds, and the total burning time ∑(t1+t2) of the group of 5 specimens after the fire source was removed was less than 250 seconds, the sample was deemed to have V-1 flame retardancy. The results are shown in Tables 1-8.

[0104] Table 1 Standard vertical combustion test results of unmodified benzoxazine resin in comparative example

[0105]

[0106] Table 2 Standard vertical burning test results of halogen-free and phosphorus-free flame retardant modified benzoxazine resin in Example 1

[0107]

[0108] Table 3 Standard vertical combustion test results of Example 2

[0109]

[0110] Table 4 Standard vertical combustion test results of Example 3

[0111]

[0112] Table 5 Standard vertical combustion test results of Example 4

[0113]

[0114]

[0115] Table 6 Standard vertical combustion test results of Example 5

[0116]

[0117] Table 7 Standard vertical combustion test results of Example 6

[0118]

[0119] Table 8 Standard vertical combustion test results of Example 7

[0120]

[0121] The results show that the unmodified benzoxazine resin has only UL94 V-1 flame retardancy, while the modified benzoxazine resin has UL94 V-0 flame retardancy.

[0122] also, Figure 1 and Figure 2 The standard vertical combustion test pictures of the unmodified benzoxazine resin prepared in the comparative example and the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin prepared in Example 1 are given; it can be intuitively seen from the figure that for the unmodified benzoxazine resin, the second ignition is still not extinguished 20s away from the fire; while for the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin prepared in Example 1, the second ignition is extinguished 2s away from the fire. Therefore, the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin prepared by the method of the present invention has better flame retardancy.

[0123] 2. The heat resistance test of the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin prepared in Examples 1-7 was carried out. The results are as follows: Figure 3-Figure 9 shown.

[0124] The glass transition temperature of the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin prepared in Examples 1-7 is 230-265° C. It can be seen that the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin prepared in the present invention has good heat resistance.

[0125] Those skilled in the art will appreciate that the embodiments described herein are intended to help readers understand the principles of the present invention, and should be understood that the protection scope of the present invention is not limited to such specific statements and embodiments. Those skilled in the art can make various other specific variations and combinations that do not deviate from the essence of the present invention based on the technical revelations disclosed by the present invention, and these variations and combinations are still within the protection scope of the present invention.

Claims

1. A method for preparing a halogen-free and phosphorus-free flame-retardant modified benzoxazine resin, characterized in that: The benzoxazine monomer is prepared by mixing and curing one or more benzoxazine monomers and one or more aldehyde compounds as raw materials; the mass ratio of the benzoxazine monomer to the aldehyde compound is 100:(1-40); the benzoxazine monomer is a diphenol-type benzoxazine monomer, a diamine-type benzoxazine monomer, a triphenol-type benzoxazine monomer or a triamine-type benzoxazine monomer.

2. The method for preparing the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin according to claim 1, characterized in that: The benzoxazine monomer is selected from one of the following structural formulas: Wherein, the R1 substituent in ac can be -H, 1 to 2 -CH3, or -C(CH3)3; Wherein, the R2 substituent in dh can be one of the following structural formulas:

3. The method for preparing the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin according to claim 1, characterized in that: The aldehyde compound is an aldehyde having a benzene ring or a heterocyclic structure, or a benzoxazine monomer containing an aldehyde group.

4. The method for preparing the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin according to claim 3, characterized in that: The aldehyde with a benzene ring or a heterocyclic structure is selected from one of the following structural formulas: The aldehyde-containing benzoxazine monomer is selected from one of the following structural formulas: Wherein, the R substituent can be one of the following structures:

5. The method for preparing the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin according to claim 1, characterized in that: The mass ratio of the benzoxazine monomer to the aldehyde compound is 100:(3-25).

6. The method for preparing the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin according to any one of claims 1 to 5, characterized in that: The blending step comprises: melt blending or solution blending the benzoxazine monomer and the aldehyde compound to obtain a modified benzoxazine blend.

7. The method for preparing the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin according to claim 6, characterized in that: The melt blending temperature is 50-160°C and the blending time is 0.5-3h; The organic solvent used for solution blending is at least one of acetone, butanone, toluene, xylene, chloroform, 1,4-dioxane, tetrahydrofuran, N,N-dimethylformamide, N-methylpyrrolidone, dimethyl sulfoxide and ether. The blending temperature is 25-90° C. and the blending time is 0.5-3h.

8. The method for preparing the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin according to claim 6, characterized in that: In the blending step, a curing catalyst is also added, and the catalyst is melt-blended or solution-blended with the benzoxazine monomer and the aldehyde compound; the catalyst is at least one of imidazole, benzimidazole, resorcinol, m-aminophenylacetylene, phenolic resin, acetic acid, oxalic acid, aluminum chloride, ferric chloride, etc.; the mass ratio of the catalyst to the benzoxazine monomer is (0.5-10):

100.

9. The method for preparing the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin according to any one of claims 1 to 5, characterized in that: The heating and curing step is as follows: the obtained modified benzoxazine blend is subjected to gradient thermal curing at 100-220° C. in 4-6 temperature sections, and the curing time is 8-16 hours.

10. The halogen-free and phosphorus-free flame-retardant modified benzoxazine resin prepared by the method according to any one of claims 1 to 9.

11. Use of the halogen-free and phosphorus-free flame-retardant modified benzoxazine resin according to claim 10 in the preparation of fiber-reinforced composite materials, rail transit interior parts, printed circuit boards, coatings, and adhesives.

Citation Information

Patent Citations

  • Benzoxazine intrinsic flame-retardant resin and preparation method thereof

    CN111234211A

  • Flame-retardant high-heat-resistance low-dielectric benzoxazine resin and preparation method thereof

    CN113896850A

  • Intrinsic flame-retardant benzoxazine resin and preparation method thereof

    CN111205419A

  • Preparation method of benzoxazine resin containing Schiff base structure based on melamine

    CN115521427A

  • Benzo oxaxine intermediate containing aldehyde group and its preparation method

    CN1865250A

Cited By

  • Amine curing agent containing benzoxazine, epoxy resin composition and application thereof

    CN119955089A

  • Benzoxazine-containing amine curing agent, epoxy resin composition and use thereof

    CN119955089B

  • Halogen-free flame-retardant benzoxazine-epoxy / aramid fiber composite material and preparation method thereof

    CN120098411A