Metal oxide / metal ion cross-linked polyvinyl alcohol porous composite material and preparation method thereof
By using surface functionalized Fe3O4@-COOH powder and Na+ as crosslinking agents, replacing the interaction of aldehydes with PVA macromolecules to form a crosslinked network structure, the problems of aldehyde residue and acid contamination in PVA porous materials are solved, and the problem of aldehyde residue and acid contamination in PVA porous materials is achieved Preparation of high-performance polyvinyl alcohol porous composite materials without aldehydes and acids.
Patent Information
- Application Number
- CN202411215560.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-02
AI Technical Summary
In the existing methods for preparing PVA porous materials by acetalization, the residual large amount of aldehyde compounds are harmful to personal health, and high acidity catalysts are required to lead to environmental pollution.
Surface functionalized Fe3O4@-COOH powder and Na+ are used as green composite crosslinking agents to replace aldehydes and PVA macromolecules to form a crosslinked network structure, avoiding the residue of aldehydes and the use of acid catalysts.
The problems of aldehyde residue and acid contamination in PVA porous materials were solved, and a polyvinyl alcohol porous composite material without aldehyde and acid was prepared, which had excellent mechanical properties and water absorption properties, and was simple to wash without pollution.
Smart Images

Figure CN119060404A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of PVA porous materials, and in particular to a metal oxide / metal ion cross-linked polyvinyl alcohol porous composite material and a preparation method thereof. Background Art
[0002] Polyvinyl alcohol (PVA) is a water-soluble linear high molecular polymer. Each repeating unit side chain contains a hydrophilic hydroxyl group, which has good film-forming properties, adhesion and biocompatibility. It can be prepared into products with various forms through different cross-linking processes, and can be used to prepare a variety of polymers through condensation reactions with aldehydes (formaldehyde, acetaldehyde, butyraldehyde). It is widely used. Among them, PVA porous material (sponge) is widely used in medical polymer materials and cleaning industries because it is soft and elastic after absorbing water and has good biocompatibility.
[0003] The widely used polyvinyl alcohol porous material is prepared by acetalization of PVA and aldehyde monomers under acidic catalyst. Under acidic conditions, the carbonyl group of formaldehyde is converted to H + It is protonated and then forms a hemiacetal structure with the hydroxyl oxygen. The -OH of the hemiacetal is unstable and dehydrates and condenses with the hydroxyl hydrogen on the PVA to form a 1,3-dioxane ring. In addition, the carbonyl group of the aldehyde may also react with one hydroxyl group in each of the two polyvinyl alcohol macromolecules to form a cross-linked network structure between the macromolecules, thereby obtaining a polyvinyl alcohol acetal polymer. For example, the patent with application number 202211246234.5 discloses a PVA composite porous material and its application, in which PVA is reacted with formaldehyde and a polyurethane prepolymer in a solution and cross-linked to prepare a PVA composite porous material. However, the existing acetalization method for preparing PVA porous materials has the following disadvantages: (1) In the preparation process, a large amount of formaldehyde, acetaldehyde, butyraldehyde and other aldehyde compounds are used as cross-linking agents for condensation reaction, and a large amount of aldehydes remain in the produced porous materials, which are difficult to remove and cause great harm to human health during use; (2) In the preparation process, acids such as sulfuric acid and hydrochloric acid are used as catalysts, and a high amount of acid is required to achieve acetalization. The acidity of the obtained sample after curing is very high, and a large amount of water is required for washing, which produces high-acidity cleaning waste liquid, causing environmental pollution and difficulty in post-processing. Therefore, it is of great theoretical value and practical application value to synthesize a polyvinyl alcohol porous composite material that is free of aldehydes and acids and has excellent water absorption and mechanical properties. Summary of the invention
[0004] In view of the above-mentioned prior art, the purpose of the present invention is to provide a metal oxide / metal ion cross-linked polyvinyl alcohol porous composite material and a preparation method thereof. The present invention adopts surface functionalized Fe3O4@-COOH powder and Na +As a green composite cross-linking agent, it replaces aldehydes and interacts with PVA macromolecules to form a cross-linked network structure. The present invention does not need to add aldehydes as cross-linking agents and does not need acid as a catalyst for polymerization reaction, which solves the problem of high residual aldehyde content in PVA porous materials and the problem of difficulty in removing them, as well as the problem of requiring a large amount of water for washing to produce high-acidity cleaning waste liquid and cause environmental pollution.
[0005] To achieve the above object, the present invention adopts the following technical solutions: The first aspect of the present invention provides a method for preparing a metal oxide / metal ion cross-linked polyvinyl alcohol porous composite material, characterized in that it comprises the following steps: Adding functionalized metal oxide and surfactant to the polyvinyl alcohol solution, stirring evenly, adding alkali solution containing metal ions, stirring at high speed for foaming, and then curing to obtain a metal oxide / metal ion cross-linked polyvinyl alcohol porous composite material; The functionalized metal oxide is a metal oxide with a carboxyl group.
[0006] Preferably, the metal oxide with carboxyl groups is a surface carboxylated iron oxide; the alkali solution containing metal ions is a solution containing Na + of lye.
[0007] Preferably, the surface carboxylated iron oxide is carboxylated Fe3O4; + The alkali solution is NaOH solution, sodium carbonate solution or sodium bicarbonate solution.
[0008] Preferably, the amount of the carboxylated Fe3O4 added is 0.5-20% of the mass of the polyvinyl alcohol solution; the mass concentration of the NaOH solution is 15-30%, and the amount of the NaOH solution added is 40-120% of the mass of the polyvinyl alcohol solution.
[0009] Preferably, the polyvinyl alcohol solution is obtained by adding polyvinyl alcohol to distilled water, and heating and stirring in a constant temperature water bath until the polyvinyl alcohol is completely dissolved; the concentration of the polyvinyl alcohol solution is 0.15-0.23 g / mL.
[0010] Preferably, the surfactant is an anionic surfactant; the anionic surfactant is selected from at least one of sodium methyl taurate, sodium coconut oil methyl taurate, and sodium lauroyl methyl taurate; the added amount of the surfactant accounts for 0.05-2.0% of the mass of the polyvinyl alcohol solution.
[0011] The anionic surfactant selected in the present invention has a strong foaming ability. The hydrophilic group and the hydrophobic group in the molecular structure work together to significantly reduce the surface tension of the solution during the foaming process, making it easier for the gas to form stable bubbles in the liquid.
[0012] Preferably, the stirring time is 1 to 6 hours.
[0013] Preferably, the high-speed stirring and foaming time is 1-3 minutes, and the stirring speed of the high-speed stirring and foaming is 1000-3000 r / min; the curing temperature is 70-90° C., and the curing time is 5-15 hours.
[0014] The second aspect of the present invention provides a metal oxide / metal ion cross-linked polyvinyl alcohol porous composite material obtained by the above preparation method.
[0015] The third aspect of the present invention provides the use of a metal oxide / metal ion cross-linked polyvinyl alcohol porous composite material in improving the mechanical properties and water absorption of a cross-linked polyvinyl alcohol porous composite material.
[0016] Beneficial effects of the present invention: (1) The present invention uses surface functionalized Fe3O4@-COOH powder and Na + As a green composite cross-linking agent, the alternative aldehydes interact with PVA macromolecules to form a cross-linked network structure, solving the problem of high residual aldehyde content in PVA porous materials and the problem of difficulty in removal.
[0017] (2) The present invention does not require acid as a catalyst for the polymerization reaction, thereby eliminating the influence of the acid catalyst and solving the problem that the PVA porous material is highly acidic and requires a large amount of water for washing to produce a highly acidic cleaning waste liquid and cause environmental pollution.
[0018] (3) The PVA porous material prepared by the present invention is aldehyde-free and acid-free, easy to wash and pollution-free, and has excellent mechanical properties and water absorption properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 :Fe3O4 / Na prepared by the present invention + / Preparation mechanism diagram of PVA porous composite materials; Figure 2 :Fe3O4 / Na2O4 of Example 2 + / Physical picture of PVA porous composite material; Figure 3 :Fe3O4 / Na2O4 of Example 2 + / PVA porous composite material pore morphology (SEM photo); Figure 4 :Fe3O4 / Na2O4 of Example 2 + XRD spectrum of / PVA porous composite material; Figure 5 :Fe3O4 / Na2O4 of Example 2 + / PVA porous composite material tensile stress-strain curve; Figure 6 :Fe3O4 / Na2O4 of Example 2 + / DSC test graph of PVA porous composite material; Figure 7 :Fe3O4 / Na2O4 of Example 2 + / PVA porous composite material water absorption curve. DETAILED DESCRIPTION
[0020] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0021] As introduced in the background technology section, polyvinyl alcohol porous materials are prepared by acetalization of PVA and aldehyde monomers under an acidic catalyst. Aldehyde compounds are used as cross-linking agents for condensation reaction, and a large amount of aldehydes remain in the produced porous materials, which are difficult to remove and cause great harm to human health during use; in the preparation process, acids such as sulfuric acid and hydrochloric acid are used as catalysts, and a high amount of acid is required to achieve acetalization. The acidity of the sample obtained after curing is very high, and a large amount of water is required for washing, which produces a high-acidity cleaning waste liquid, causing environmental pollution and making post-processing difficult.
[0022] Based on this, the purpose of the present invention is to provide a metal oxide / metal ion cross-linked polyvinyl alcohol porous composite material and a preparation method. The present invention uses surface functionalized Fe3O4@-COOH powder and metal sodium ions Na + As a green composite crosslinking agent, it can be crosslinked with PVA to prepare porous materials. PVA macromolecule chains contain a large number of -OH groups, and the surface-modified functionalized Fe3O4 powder has a large number of -COOH groups, which can produce esterification, coordination and hydrogen bonding with PVA macromolecules under alkaline conditions. At the same time, the OH in the NaOH solution - Ions attack the -OH on the PVA macromolecular chain to deprotonate and form a portion of O - Group, and free Na + Ionic interactions form complexes, in short, with functionalized Fe3O4 and Na + The synergistic effect forms a multi-crosslinked network structure with PVA macromolecules. At the same time, anionic surfactants are used to reduce the surface tension of the solution, thereby forming a PVA porous material with a uniform and stable pore structure. Figure 1 The cross-linking degree and performance of the porous material can be controlled by adjusting the amount of functionalized Fe3O4 and the concentration of NaOH solution.
[0023] In order to enable those skilled in the art to more clearly understand the technical solution of the present application, the technical solution of the present application will be described in detail below in conjunction with specific embodiments.
[0024] Note: The functionalized Fe3O4 in the present invention is Fe3O4@-COOH, and its preparation method is as follows: 20 g of Fe3O4 was dissolved in 100 mL of anhydrous ethanol and dispersed by ultrasonication, and then 1 g of malonic acid was added. After ultrasonic stirring, the mixture was dried at 85°C for about 5 h to obtain surface functionalized Fe3O4@-COOH powder.
[0025] The test materials used in the examples of the present invention are all conventional test materials in the art and can be purchased through commercial channels.
[0026] Embodiment 1: In this example, the amount of functionalized Fe3O4 is 9 g, and 15% NaOH solution is used. The preparation steps are as follows: (1) Place a four-necked flask equipped with a thermometer, a stirring paddle, and a condenser in a constant temperature water bath. Take 17 g of polyvinyl alcohol granules and add them to the four-necked flask. Add 83 g of distilled water to the four-necked flask. Mechanically stir and dissolve the polyvinyl alcohol in a constant temperature water bath at 90°C for 10 hours until the polyvinyl alcohol is completely dissolved. Reduce the temperature and cool to obtain a completely dissolved viscous and transparent polyvinyl alcohol solution.
[0027] (2) Take 60 g of the completely dissolved polyvinyl alcohol solution in step (1), add 0.05 g of sodium methyl taurine and 9 g of functionalized Fe3O4, and stir thoroughly at a stirring speed of 100 r / min to evenly mix the polyvinyl alcohol, surfactant and functionalized Fe3O4.
[0028] (3) Add 25 g of 15% NaOH solution to the mixed solution in step (2), stir and disperse at 1000 r / min for 2 min to foam, and quickly put the melt into an oven for curing at 80° C. for 10 h after foaming. After curing, wash the material with distilled water to obtain a metal oxide / metal ion cross-linked polyvinyl alcohol porous composite material (denoted as Fe3O4 / Na + / PVA porous composite material).
[0029] Example 2 In this embodiment, the amount of functionalized Fe3O4 is 7 g, and 20% NaOH solution is used. The preparation steps are as follows: (1) Place a four-necked flask equipped with a thermometer, a stirring paddle, and a condenser in a constant temperature water bath. Take 17 g of polyvinyl alcohol granules and add them to the four-necked flask. Add 83 g of distilled water to the four-necked flask. Mechanically stir and dissolve the polyvinyl alcohol in a constant temperature water bath at 90°C for 10 hours until the polyvinyl alcohol is completely dissolved. Reduce the temperature and cool to obtain a completely dissolved viscous and transparent polyvinyl alcohol solution.
[0030] (2) Take 60 g of the completely dissolved polyvinyl alcohol solution in step (1), add 0.05 g of sodium methyl taurine and 7 g of functionalized Fe3O4, and stir thoroughly at a stirring speed of 100 r / min to evenly mix the polyvinyl alcohol, surfactant and functionalized Fe3O4.
[0031] (3) Add 25 g of 20% NaOH solution to the mixed solution in step (2), stir and foam for 2 min using a high-speed stirring disperser at 1000 r / min, and quickly put the melt into an oven for curing at 90° C. for 10 h after foaming. After curing, wash the material with distilled water to obtain a metal oxide / metal ion cross-linked polyvinyl alcohol porous composite material (denoted as Fe3O4 / Na + / PVA porous composite material).
[0032] Example 3 In this embodiment, the amount of functionalized Fe3O4 is 5 g, and 25% NaOH solution is used. The preparation steps are as follows: (1) Place a four-necked flask equipped with a thermometer, a stirring paddle, and a condenser in a constant temperature water bath. Take 17 g of polyvinyl alcohol granules and add them to the four-necked flask. Add 83 g of distilled water to the four-necked flask. Mechanically stir and dissolve the polyvinyl alcohol in a constant temperature water bath at 90°C for 10 hours until the polyvinyl alcohol is completely dissolved. Reduce the temperature and cool to obtain a completely dissolved viscous and transparent polyvinyl alcohol solution.
[0033] (2) Take 60 g of the completely dissolved polyvinyl alcohol solution in step (1), add 0.05 g of sodium cocoyl methyl taurate and 5 g of functionalized Fe3O4, and stir thoroughly at a stirring speed of 100 r / min to evenly mix the polyvinyl alcohol, surfactant and functionalized Fe3O4.
[0034] (3) Add 25 g of 25% NaOH solution to the mixed solution in step (2), stir and foam for 2 min using a high-speed stirring disperser at 1000 r / min, and quickly put the melt into an oven for curing at 70° C. for 10 h after foaming. After curing, wash the material with distilled water to obtain a metal oxide / metal ion cross-linked polyvinyl alcohol porous composite material (denoted as Fe3O4 / Na + / PVA porous composite material).
[0035] Example 4 In this embodiment, the amount of functionalized Fe3O4 is 3 g, and 30% NaOH solution is used. The preparation steps are as follows: (1) Place a four-necked flask equipped with a thermometer, a stirring paddle, and a condenser in a constant temperature water bath. Take 17 g of polyvinyl alcohol granules and add them to the four-necked flask. Add 83 g of distilled water to the four-necked flask. Mechanically stir and dissolve the polyvinyl alcohol in a constant temperature water bath at 90°C for 10 hours until the polyvinyl alcohol is completely dissolved. Reduce the temperature and cool to obtain a completely dissolved viscous and transparent polyvinyl alcohol solution.
[0036] (2) Take 60 g of the completely dissolved polyvinyl alcohol solution in step (1), add 0.05 g of sodium lauroyl methyl taurate and 3 g of functionalized Fe3O4, and stir thoroughly at a stirring speed of 100 r / min to evenly mix the polyvinyl alcohol, surfactant and functionalized Fe3O4.
[0037] (3) Add 25 g of 30% NaOH solution to the mixed solution in step (2), stir and foam for 2 min using a high-speed stirring disperser at 1000 r / min, and quickly put the melt into an oven for curing at 80° C. for 10 h after foaming. After curing, wash the material with distilled water to obtain a metal oxide / metal ion cross-linked polyvinyl alcohol porous composite material (denoted as Fe3O4 / Na + / PVA porous composite material). Comparative Example 1 The difference from Example 2 is that no functionalized Fe3O4 is added, and the metal ion cross-linked polyvinyl alcohol porous composite material (denoted as Na + / PVA composite material).
[0038] Comparative Example 2 The difference from Example 2 is that: no 20% NaOH solution is added, and a metal oxide cross-linked polyvinyl alcohol composite material (denoted as Fe3O4 / PVA composite material) is finally obtained.
[0039] Comparative Example 3 The difference from Example 2 is that the 20% NaOH solution is replaced by an equal amount of 5% NaOH solution, and finally a cross-linked polyvinyl alcohol composite material is obtained.
[0040] Comparative Example 4 The difference from Example 2 is that the 20% NaOH solution is replaced by an equal amount of 40% NaOH solution, and finally a cross-linked polyvinyl alcohol porous composite material is obtained.
[0041] Comparative Example 5 According to the patent application number CN200410014019.8, in this comparative example, formaldehyde is used as a cross-linking agent, sulfuric acid is added for foaming to obtain a cross-linked polyvinyl alcohol porous material, and the preparation steps are as follows: (1) Place a four-necked flask equipped with a thermometer, a stirring paddle, and a condenser in a constant temperature water bath. Take 17 g of polyvinyl alcohol granules and add them to the four-necked flask. Add 83 g of distilled water to the four-necked flask. Mechanically stir and dissolve the polyvinyl alcohol in a constant temperature water bath at 90°C for 10 hours until the polyvinyl alcohol is completely dissolved. Reduce the temperature and cool to obtain a completely dissolved viscous and transparent polyvinyl alcohol solution.
[0042] (2) Take 60 g of the completely dissolved polyvinyl alcohol solution in step (1), add 0.05 g of sodium lauroyl methyl taurate and 14 g of liquid armor, and stir thoroughly at a stirring speed of 100 r / min to mix the polyvinyl alcohol, surfactant and liquid armor evenly.
[0043] (3) Add 10 g of 62% H2SO4 solution to the mixed solution in step (2), stir for 2 min at 1000 r / min using a high-speed stirring disperser to foam, and quickly put the melt into an oven for curing at 80°C for 18 h after foaming. After curing, wash the material with distilled water to obtain a polyvinyl alcohol acetal porous composite material (referred to as PVA formalin porous composite material).
[0044] Test example 1. Mechanical properties testing The tensile properties of the PVA porous composite materials prepared in Examples 1-4 and Comparative Examples 1-5 were tested using an Instron-5569 electronic universal tensile testing machine. The PVA porous material was made into a regular rectangular parallelepiped (length 25 mm, width 10 mm, thickness 2 mm) for tensile properties testing.
[0045] 2. Water absorption test The water absorption rate of the samples was tested according to GB / T8810-2005. The PVA porous composite materials prepared in Examples 1-4 and Comparative Examples 1-5 were placed in an oven for drying, and a small sample was taken and weighed using an electronic balance. m 0 Allow the PVA porous composite material to absorb water freely without any external force, and weigh the mass of the sponge after the material has completely absorbed water. m c , use formula 1-1 to calculate the water absorption rate.
[0046] .
[0047] 3.DSC test The glass transition temperature (Tg) of the PVA porous composite materials prepared in Examples 1-4 and Comparative Examples 1-5 was tested using a 910S differential thermal analyzer. The PVA porous composite materials were placed in an oven for drying, and then taken out and cut into thin sheets. Then, about 10 mg of the sample was weighed and placed in an aluminum crucible, and the starting temperature was set to room temperature, the ending temperature was set to 150°C, and the program heating rate was set to 5°C / min.
[0048] The results of the above three experiments are shown in Table 1.
[0049] Table 1 Performance test results of polyvinyl alcohol composite materials prepared in Examples 1-4 and Comparative Examples 1-5 It can be seen from Comparative Examples 1-2 in Table 1 that without adding NaOH solution, the material prepared by functionalized Fe3O4 and PVA has no pores. + The porous material formed by the crosslinking agent and PVA contains only a small number of pores. Therefore, the present invention uses surface functionalized Fe3O4 metal oxide and metal sodium ion Na + Polyvinyl alcohol porous materials were prepared as green composite cross-linking agent.
[0050] It can be seen from Comparative Examples 3-4 in Table 1 that when the concentration of the NaOH solution is low or high, the prepared porous material contains only a small amount of pores, so the concentration of the NaOH solution is 15-30%.
[0051] Depend on Figure 1 It can be seen that the Fe3O4 / Na + / PVA porous composite materials form a stable network structure through multiple cross-linking.
[0052] Depend on Figure 2 , Figure 3 It can be seen that the Fe3O4 / Na2O4 prepared in Example 2 + / PVA porous composite material has a three-dimensional network porous structure.
[0053] Depend on Figure 4 It can be seen that the functionalized Fe3O4 and PVA in Example 2 were successfully composited to prepare Fe3O4 / Na + / PVA porous composite material.
[0054] Depend on Figure 5~Figure 7 It can be seen that the Fe3O4 / Na2O4 prepared in Example 2 + / PVA porous composite material has a high degree of cross-linking and excellent mechanical properties. At the same time, due to its porous structure, it has excellent water absorption performance.
[0055] The present invention adopts functionalized Fe3O4 and Na+ As a green composite cross-linking agent for polyvinyl alcohol, it replaces aldehydes and interacts with polyvinyl alcohol macromolecules to form a cross-linked network structure. Under alkaline conditions, esterification, coordination and hydrogen bonding occur between functionalized Fe3O4 and polyvinyl alcohol macromolecules, while the introduction of metal ions Na + The composite cross-linking agent synergistically forms a stable multi-cross-linked network structure by complexing with the polyvinyl alcohol macromolecular chain, thereby preparing a polyvinyl alcohol porous composite material that is formaldehyde-free and acid-free, easy to wash and pollution-free, and has excellent mechanical properties and water absorption properties.
[0056] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A method for preparing a metal oxide / metal ion cross-linked polyvinyl alcohol porous composite material, It is characterized in that The following steps are involved: Adding functionalized metal oxide and surfactant to the polyvinyl alcohol solution, stirring evenly, adding alkali solution containing metal ions, stirring at high speed for foaming, and then curing to obtain a metal oxide / metal ion cross-linked polyvinyl alcohol porous composite material; The functionalized metal oxide is a metal oxide with a carboxyl group.
2. The preparation method according to claim 1, It is characterized in that The metal oxide with carboxyl groups is a surface carboxylated iron oxide; the alkali solution containing metal ions is a solution containing Na + of lye.
3. The preparation method according to claim 2, It is characterized in that The surface carboxylated iron oxide is carboxylated Fe 3 O 4 ; The Na + The alkali solution is NaOH solution, sodium carbonate solution or sodium bicarbonate solution.
4. The preparation method according to claim 3, It is characterized in that The carboxylated Fe 3 O 4 The amount of NaOH added is 0.5-20% of the mass of the polyvinyl alcohol solution; the mass concentration of the NaOH solution is 15-30%, and the amount of NaOH added is 40-120% of the mass of the polyvinyl alcohol solution.
5. The preparation method according to claim 1, It is characterized in that The polyvinyl alcohol solution is obtained by adding polyvinyl alcohol into distilled water, heating and stirring in a constant temperature water bath until the polyvinyl alcohol is completely dissolved; the mass concentration of the polyvinyl alcohol solution is 0.15-0.23 g / mL.
6. The preparation method according to claim 1, It is characterized in that The surfactant is an anionic surfactant; the anionic surfactant is selected from at least one of sodium methyl taurate, sodium coconut oil methyl taurate, and sodium lauroyl methyl taurate; the added amount of the surfactant accounts for 0.05-2.0% of the mass of the polyvinyl alcohol solution.
7. The preparation method according to claim 1, It is characterized in that The stirring time is 1 to 6 hours.
8. The preparation method according to claim 1, It is characterized in that The high-speed stirring and foaming time is 1-3 minutes, and the stirring speed of the high-speed stirring and foaming is 1000-3000 r / min; the curing temperature is 70-90° C., and the curing time is 5-15 hours.
9. The metal oxide / metal ion cross-linked polyvinyl alcohol porous composite material obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the metal oxide / metal ion cross-linked polyvinyl alcohol porous composite material according to claim 9 in improving the mechanical properties and water absorption of the cross-linked polyvinyl alcohol porous composite material.
Citation Information
Patent Citations
Preparation method of high-strength wear-resistant polyvinyl alcohol hydrogel
CN111333865A
Preparation method of metal ion cross-linked toughened cellulose nanofiber material
CN115434072A
Polymer particles made of polyvinyl alcohol and comprising a contrast agent for chemoembolization
WO1999012577A1