Polyamide composition as well as preparation method and application thereof
By adding glass fibers and optimized amide nucleating agents and talc powder to the PA56 material, the crystallization temperature and crystallinity of the polyamide composition are improved, and the problems of long molding cycles and large mold release force of PA56 material are solved, and the problems of long molding cycles and large mold release force are improved. Welding wire strength is suitable for the manufacturing of automotive parts.
Patent Information
- Application Number
- CN202411193018.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-28
AI Technical Summary
The long forming cycle and large mold release force of PA56 material lead to limitations in applications of large automotive parts. At the same time, although the addition of glass fiber increases strength, it reduces the combination effect of crystallinity and weld wires.
Using PA56 resin, glass fiber, amide nucleating agent and talc powder composition, the crystallization temperature and crystallinity of the polyamide composition are improved and the molding cycle is shortened by optimizing the mass ratio and structure of amide nucleating agent and talc powder. And reduce the release force, while increasing the strength of the welded wire.
The high crystallization temperature, low mold release force and good welding wire strength of the polyamide composition are achieved, and are suitable for the manufacturing of automotive parts.
Smart Images

Figure BDA0005015598640000061 
Figure BDA0005015598640000071 
Figure BDA0005015598640000072
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer materials, and more specifically, to a polyamide composition and a preparation method and application thereof. Background Art
[0002] Under the background of the dual carbon strategy, energy conservation and emission reduction have become the trend of automobile development, among which reducing the carbon emissions of the materials used is a very important step. The synthetic monomers of bio-based nylon are partially or completely derived from nature, which has the natural advantage of reducing carbon emissions. Its emissions are only about 50% of petroleum-based nylon. Among them, PA56 in bio-based nylon has received more and more attention from OEMs due to its advantages in carbon reduction and cost, and the demand and development of PA56 materials are becoming more and more common.
[0003] PA56 is obtained by the polymerization of pentamethylenediamine and adipic acid, and has good mechanical properties, hygroscopicity, thermal stability, flame retardancy, dyeing properties, wear resistance and softness. However, due to its special structure, PA56 has a low crystallization temperature and low crystallinity, resulting in a long molding cycle and a large demolding force, which limits its application in large automotive parts. At the same time, in order to meet the requirements of the mechanical properties of the material itself in automotive application scenarios, glass fiber is usually added, but the glass fiber will further reduce the crystallinity of the PA56 material.
[0004] In addition, automotive parts such as engine cylinder covers usually form weld lines during injection molding, so the PA56 material used in the automotive field also needs to pay attention to its weld line strength. The addition of glass fiber will increase the strength of the PA56 material itself, but will cause the bonding effect of the PA56 material weld line position to deteriorate and degrade the weld line strength. Summary of the invention
[0005] The primary purpose of the present invention is to overcome the problems of long molding cycle and large demoulding force of PA56 materials in the prior art and to provide a polyamide composition.
[0006] A further object of the present invention is to provide a method for preparing the above polyamide composition.
[0007] A further object of the present invention is to provide use of the polyamide composition in the preparation of automotive parts.
[0008] The above-mentioned object of the present invention is achieved by the following technical solutions:
[0009] A polyamide composition comprising the following components in parts by weight:
[0010] 39-90 parts of PA56 resin,
[0011] Glass fiber 9-51 parts,
[0012] 1 to 3 parts of composite nucleating agent;
[0013] The composite nucleating agent comprises an amide nucleating agent and talcum powder in a mass ratio of (1.5-4.5):1.
[0014] In the present invention, the addition of glass fiber improves the basic mechanical strength of the polyamide composition.
[0015] The inventors of the present invention have found that in a polyamide composition system with glass fiber added, due to the inherent "defects" in the molecular structure of PA56 resin itself and the steric hindrance effect brought by the glass fiber, the addition of conventional nucleating agents cannot effectively improve the crystallization temperature and crystallinity of the polyamide composition, especially the crystallinity, which makes it difficult to improve the problem of high demolding force of the polyamide composition.
[0016] The inventors of the present invention have found through research that both amide nucleating agents and talc powder have certain nucleating effects. Further utilizing the compatibility of amide nucleating agents and the overlapping effect brought by the flaky structure of talc powder can not only effectively increase the crystallization temperature of the polyamide composition and shorten the molding cycle, but also effectively increase the crystallinity of the polyamide composition and reduce the demolding force. If either the amide nucleating agent or talc powder is missing or one of them is replaced by other conventional nucleating agents, the crystallization temperature and crystallinity of the polyamide composition cannot be increased at the same time.
[0017] In addition, the inventors have also found that in the polyamide composition system of the present invention, the synergistic effect of the amide nucleating agent and talcum powder affects the crystallization behavior of the material during injection molding, thereby effectively improving the weld line strength of the material.
[0018] In the present invention, the amount of PA56 resin added can be 39, 40, 45, 48, 50, 52, 55, 58, 60, 65, 68, 70, 75, 78, 80, 85, 88 or 90 parts by weight; the amount of glass fiber added can be 9, 10, 12, 15, 20, 25, 30, 35, 40, 45, 50 or 51 parts by weight.
[0019] In the present invention, PA56 resin is used as the main resin, and its mass fraction in the polyamide composition is more than 35%.
[0020] Preferably, the relative viscosity of the PA56 resin is 2.2-3.2.
[0021] More preferably, the relative viscosity of the PA56 resin is 2.4 to 2.8. By selecting the PA56 resin with this relative viscosity, the obtained polyamide composition has a lower demoulding force and a higher weld line strength.
[0022] In the present invention, the viscosity of the PA56 resin can be measured under 96% concentrated sulfuric acid conditions according to ISO 307-2019.
[0023] Preferably, the glass fiber is chopped glass fiber.
[0024] Preferably, the average cross-sectional diameter of the glass fiber is 10-13 um.
[0025] Preferably, the average length of the glass fibers is 2 to 4.5 mm.
[0026] In the present invention, the average diameter and average length of the cross section of the glass fiber can be measured by optical microscopy.
[0027] Preferably, the polyamide composition further comprises 1 to 5 parts of a black colorant.
[0028] More preferably, the black colorant is carbon black.
[0029] Further preferably, the black colorant is PE-based carbon black masterbatch.
[0030] Preferably, the composite nucleating agent is added in the form of masterbatch.
[0031] More preferably, the carrier of the masterbatch is PA6 resin.
[0032] Further preferably, the relative viscosity of the PA6 resin is 2.4 to 2.8; the viscosity of the PA6 resin can be measured under 96% concentrated sulfuric acid conditions according to ISO 307-2019.
[0033] More preferably, the content of the composite nucleating agent in the masterbatch is 40-60wt%.
[0034] In the present invention, the mass ratio of the amide nucleating agent to talc can be 1.5:1, 1.8:1, 2:1, 2.5:1, 2.8:1, 3:1, 3.2:1, 3.5:1, 3.8:1, 4:1 or 4.5:1.
[0035] Preferably, the composite nucleating agent comprises an amide nucleating agent and talc in a mass ratio of (3-4): 1. When the mass ratio of the two is controlled within this range, the obtained polyamide composition has a higher crystallization temperature and a lower demoulding force.
[0036] Preferably, the amide nucleating agent is at least one of a succinamide nucleating agent, an adipic diamide nucleating agent, a phthalamide nucleating agent or an organic phosphonic acid nucleating agent.
[0037] More preferably, the succinamide nucleating agent includes but is not limited to diphenyl succinamide.
[0038] More preferably, the adipamide nucleating agent includes but is not limited to diphenyl adipamide.
[0039] More preferably, the phthalamide nucleating agent includes but is not limited to NN dicyclohexyl terephthalamide.
[0040] More preferably, the organic phosphoric acid amide is at least one of diphenyl phosphoramide or diethyl phosphoramide.
[0041] Preferably, the average particle size of the talc is 8 to 18 μm.
[0042] In the present invention, the average particle size of talc can be measured according to GB / T 19077-2016.
[0043] Preferably, the polyamide composition further comprises 0.1 to 4 parts of other additives.
[0044] Preferably, the other auxiliary agent is at least one of a lubricant or an antioxidant.
[0045] Optionally, the lubricant is an ester lubricant, including but not limited to at least one of EBS, stearamide or erucamide.
[0046] Optionally, the antioxidant includes but is not limited to at least one of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate or tris[2,4-di-tert-butylphenyl]phosphite.
[0047] The preparation method of the polyamide composition comprises the following steps: mixing the components, melt-extruding, and granulating to obtain the polyamide composition.
[0048] Preferably, the temperature of the melt extrusion is 220-280° C.; the screw length-to-diameter ratio of the melt extruder is 35-50:1, and the screw speed is 300-600 r / min.
[0049] The application of the above polyamide composition in the preparation of automobile parts is also within the protection scope of the present invention.
[0050] Preferably, the automobile component is a carbon canister, an engine cylinder cover or an oil pan.
[0051] Compared with the prior art, the present invention has the following beneficial effects:
[0052] The present invention uses PA56 resin as the main resin, adds glass fiber, and simultaneously adds amide nucleating agent and talcum powder as a composite nucleating agent. The obtained polyamide composition has not only a high crystallization temperature, but also a low demoulding force and good weld line strength. DETAILED DESCRIPTION
[0053] In order to more clearly and completely describe the technical solution of the present invention, the present invention is further described in detail through specific embodiments below. It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention. Various changes can be made within the scope of the rights of the present invention.
[0054] Some of the reagents selected in the embodiments and comparative examples of the present invention are described as follows:
[0055] PA56 resin 1#: Ecopent-1273, Cathay Biotechnology, relative viscosity 2.8;
[0056] PA56 resin 2#: Ecopent-1251, Cathay Biotechnology, relative viscosity 2.4;
[0057] PA56 resin 3#: Ecopent-3100, Cathay Biotechnology, relative viscosity 3.1;
[0058] Glass fiber: China Jushi, ECS10-03-568H, chopped glass fiber;
[0059] Black colorant 1#: PE2642, Cabot;
[0060] Other additives 1#: lubricant, ethylene bis stearamide, commercially available;
[0061] Other additives 2#: antioxidant, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, commercially available;
[0062] Talc: Huamei, AH-1250N6, average particle size 10-15 μm;
[0063] Amide nucleating agent 1#: diphenyl adipamide, commercially available;
[0064] Amide nucleating agent 2#: NN dicyclohexyl terephthalamide, commercially available;
[0065] Amide nucleating agent 3#: diphenyl succinamide, commercially available;
[0066] Amide nucleating agent 4#: diethylphosphoramide, commercially available;
[0067] Other nucleating agents A#: nanoclay, ADINS CLAY 20, TOLSA;
[0068] Other nucleating agents B#: sodium montanate, LICOMONT NAV101PWD, Clariant;
[0069] Other nucleating agents C#: hydroxyaluminum salt, TMP-6, Shanxi Chemical Research Institute;
[0070] Composite nucleating agent 1#: homemade, the preparation process is as follows: amide nucleating agent 1# and talcum powder are mixed in a mass ratio of 3:1, and then mixed with an equal amount of PA6 resin (Jiangsu Haiyang, PA6HY2500A, relative viscosity 2.4), and then melt blended at a certain temperature (220-250°C) through a single screw extruder to obtain composite nucleating agent 1# (effective ingredient content is 50wt%);
[0071] Composite nucleating agent 2#: homemade, different from composite nucleating agent 1#: the mass ratio of amide nucleating agent 1# and talcum powder is 4:1;
[0072] Composite nucleating agent 3#: homemade, different from composite nucleating agent 1#: the mass ratio of amide nucleating agent 1# and talcum powder is 2:1;
[0073] Composite nucleating agent 4#: homemade, the difference from composite nucleating agent 1# is that amide nucleating agent 1# is replaced by amide nucleating agent 2#;
[0074] Composite nucleating agent 5#: homemade, the difference from composite nucleating agent 1# is that amide nucleating agent 1# is replaced by amide nucleating agent 3#;
[0075] Composite nucleating agent 6#: homemade, the difference from composite nucleating agent 1# is that amide nucleating agent 1# is replaced by amide nucleating agent 4#;
[0076] Composite nucleating agent 7#: homemade, the difference from composite nucleating agent 1# is that talcum powder is replaced with other nucleating agent A#;
[0077] Composite nucleating agent 8#: homemade, the difference from composite nucleating agent 1# is that amide nucleating agent 1# is replaced by other nucleating agent B#;
[0078] Composite nucleating agent 9#: homemade, the difference from composite nucleating agent 1# is that amide nucleating agent 1# is replaced by other nucleating agent C#;
[0079] Single nucleating agent 1#: Homemade, different from composite nucleating agent 1# in that no talcum powder is added.
[0080] Single nucleating agent 2#: Homemade, different from composite nucleating agent 1# in that no amide nucleating agent 1# is added.
[0081] Unless otherwise specified, the components selected in the parallel examples and comparative examples (eg, glass fiber, other additive 1#, other additive 2#) are all the same commercially available products.
[0082] The polyamide compositions of the embodiments of the present invention and the comparative examples are prepared by the following preparation method:
[0083] (1) Weigh each component according to the ratio, put each component into a high-speed mixer, and mix them evenly to obtain a mixture.
[0084] (2) The mixture is fed into a twin-screw extruder, and the extruder temperature is set to 220° C., 240° C., 245° C., 250° C., 260° C., 270° C., 280° C., 275° C., 265° C., and 240° C. according to the temperature of each zone, the rotation speed is 500 r / min, and the screw aspect ratio is 40:1; the polyamide composition is obtained by mixing, melting, homogenizing, and then extruding and granulating.
[0085] The performance of the polyamide compositions provided in the embodiments and comparative examples of the present invention was measured according to the following test methods:
[0086] 1) Crystallization temperature: DSC test was performed according to ISO 11357-2011 standard, and the test was performed at a heating and cooling rate of 10°C / min.
[0087] 2) Demolding force: Use customized demoulding force injection molding machine equipment to inject special parts at a certain temperature and pressure. Inject 5 molds continuously and calculate the average value. Monitor the demoulding force through sensors.
[0088] 3) Weld line strength: Double-sided injection molded weld line tensile test strips are tested according to ISO 527-2019 standard with a tensile rate of 10 mm / min.
[0089] Examples 1 to 10
[0090] Examples 1 to 10 provide a series of polyamide compositions, the formulations of which are shown in Table 1 (the amount of the composite nucleating agent in each example in Table 1 is the amount converted into the effective ingredient).
[0091] Table 1 Formulas of Examples 1 to 10 (parts by weight)
[0092]
[0093]
[0094] Comparative Examples 1 to 5
[0095] Comparative Examples 1 to 5 provide a series of polyamide compositions, whose formulations are shown in Table 2 (the amount of the composite nucleating agent / single nucleating agent in each comparative example in Table 2 is the amount converted into the effective ingredient).
[0096] Table 2 Formulas of Comparative Examples 1 to 5 (parts by weight)
[0097]
[0098] The properties of the polyamide compositions of the embodiments and comparative examples were measured according to the above-mentioned test methods. The test results are shown in Table 3.
[0099] Table 3 Performance test results of polyamide compositions of various embodiments and comparative examples
[0100] Test Results Crystallization temperature(℃) Demolding force (N) Weld line strength (MPa) Example 1 219 580 95 Example 2 220 725 101 Example 3 215 640 80 Example 4 217 565 93 Example 5 216 570 89 Example 6 218 640 85 Example 7 217 650 90 Example 8 216 530 92 Example 9 215 535 94 Example 10 218 610 85 Comparative Example 1 218 975 75 Comparative Example 2 216 980 73 Comparative Example 3 215 990 70 Comparative Example 4 216 1025 65 Comparative Example 5 214 1130 67 .
[0101] From Table 3, we can see that:
[0102] The crystallization temperatures of the polyamide compositions of Examples 1 to 10 are all above 215°C, the demolding forces are all below 725N, and the weld line strengths are all above 80MPa, indicating that the polyamide compositions of the present invention not only have a high crystallization temperature, but also have a low demolding force and good weld line strength.
[0103] The types of composite nucleating agents added in Comparative Examples 1 to 3 are not appropriate, the demoulding force of the polyamide composition is high, and the weld line strength is low. The nucleating agent added in Comparative Example 4 is only an amide nucleating agent, the demoulding force of the polyamide composition is high, and the weld line strength is low. The nucleating agent added in Comparative Example 5 is only talcum powder, the crystallization temperature of the polyamide composition is low, the demoulding force is high, and the weld line strength is low.
[0104] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A polyamide composition, characterized in that The composition comprises the following components in parts by weight: 39-90 parts of PA56 resin, Glass fiber 9-51 parts, 1 to 3 parts of composite nucleating agent, The composite nucleating agent comprises an amide nucleating agent and talcum powder in a mass ratio of (1.5-4.5):
1.
2. The polyamide composition according to claim 1, characterized in that: The relative viscosity of the PA56 resin is 2.2-3.
2.
3. The polyamide composition according to claim 1, characterized in that: The glass fibers are chopped glass fibers.
4. The polyamide composition according to claim 1, characterized in that: The composite nucleating agent is added in the form of masterbatch.
5. The polyamide composition according to claim 1, characterized in that: The amide nucleating agent is at least one of a succinamide nucleating agent, an adipic diamide nucleating agent, a phthalamide nucleating agent or an organic phosphonic acid nucleating agent.
6. The polyamide composition according to claim 1, characterized in that: The talcum powder has an average particle size of 8 to 18 μm.
7. The polyamide composition according to claim 1, characterized in that: The polyamide composition further comprises 0.1 to 4 parts of other auxiliary agents and 1 to 5 parts of black colorant.
8. The polyamide composition according to claim 1, characterized in that: The other auxiliary agent is at least one of a lubricant and an antioxidant.
9. The method for preparing the polyamide composition according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: mixing the components, melt-extruding and granulating to obtain the polyamide composition.
10. Use of the polyamide composition according to any one of claims 1 to 8 in the preparation of automobile parts.
Citation Information
Patent Citations
Polyamide composition for low temperature applications
CN103917600A
Reinforced polyamide 56 composition with improved impact strength and application thereof
CN111117234A
Polyamide compositions capable of increasing laser transmissivity and improving molding defects and applicaion thereof
CN111171564A
Glass fiber reinforced polyamide composite material and preparation method thereof
CN117720810A
Binding band made of resin
JP1998204290A